Composite electrode sheet and preparation method therefor, and lithium-ion battery
The composite pole piece design with alternately stacked active materials and lithium replenishment layers solves the problem of lithium ion consumption and poor lithium replenishment uniformity in lithium-ion batteries, achieving rapid and uniform diffusion of lithium ions and improving battery performance.
Patent Information
- Application Number
- PCT/CN2024/072759
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-01-17
- Publication Date
- 2024-10-17
AI Technical Summary
The SEI film formed during the formation process of lithium-ion batteries consumes lithium ions, resulting in initial capacity loss and reduced cycle life. Existing lithium replenishment methods have poor uniformity and slow replenishment speed, and side reactions may occur when lithium replenishment agents are mixed with active materials. affect battery performance.
A composite pole piece design is adopted in which n layers of active material layers and n-1 layers of lithium replenishing layers are alternately stacked. The side of the composite material layer close to the current collector is the active material layer, which increases the porosity gradient of the lithium replenishing layer. Through evaporation technology Evenly distribute lithium ions and optimize ion diffusion path and speed.
It improves the diffusion rate of lithium ions and the uniformity of lithium replenishment, reduces initial capacity loss, improves cycle performance and energy density, avoids side reactions, and extends the cycle life of the battery.
Smart Images

Figure CN2024072759_17102024_PF_FP_ABST
Abstract
Description
Composite pole piece, preparation method thereof, and lithium-ion battery
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on December 22, 2023, with application number 202311785825.4. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of battery technology, for example, a composite pole piece and a preparation method thereof, and a lithium-ion battery. Background Art
[0003] During the formation process of lithium-ion batteries, the formation of the SEI film consumes the original lithium ions inside the battery, causing problems such as loss of initial capacity and reduced cycle life of the lithium-ion battery, thereby limiting the improvement of the energy density of the lithium-ion battery. In order to compensate for this part of the lithium loss, lithium supplementation is usually performed.
[0004] Current methods for replenishing lithium in negative electrodes primarily include spraying ultrafine metallic lithium powder on the surface of the negative electrode, spraying a slurry of ultrafine lithium powder on the negative electrode surface, or rolling and laminating ultrathin lithium ribbons onto the negative electrode sheet. However, these methods result in poor lithium replenishment uniformity and slow penetration of the lithium replenisher into the electrode, which limits the rate and efficiency of lithium ion replenishment, thereby reducing the effectiveness of lithium replenishment. The primary method for replenishing lithium in positive electrodes is to add lithium-rich compounds such as Li2NiO2, Li5FeO4, Li3N, Li2O2, or Li2S to the positive electrode active material. However, uneven mixing can lead to uneven distribution of lithium in the battery, potentially resulting in over-replenishment in some areas and under-replenishment in others, which in turn affects battery performance and lifespan. Furthermore, when the lithium replenisher mixes with the positive electrode active material, side reactions may occur, resulting in the production of undesirable chemical substances. These byproducts can negatively impact the battery's electrochemical performance.
[0005] Therefore, there is an urgent need to provide a lithium replenishment method that can improve the replenishment speed and efficiency of the lithium replenishment agent, improve the uniformity of lithium replenishment, and avoid side reactions caused by mixing the lithium replenishment agent with the electrode active material.
[0006] Summary of the Invention
[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0008] The present application provides a composite electrode, a method for preparing the same, and a lithium-ion battery. The composite electrode of the present application comprises n layers of active material and n-1 layers of lithium replenishment, and defines the active material layer as the side of the composite material layer closest to the current collector. This allows for multiple lithium replenishment layers to be spaced apart within the composite material layer, resulting in closer contact between the lithium replenishment layer and the active material layer. This shortens the lithium ion diffusion path and accelerates the lithium ion diffusion rate, helping to improve the rate and efficiency of lithium replenishment, as well as the uniformity of lithium replenishment and preventing side reactions caused by direct mixing of the lithium replenishment material and the active material.
[0009] In a first aspect, an embodiment of the present application provides a composite electrode sheet, comprising a current collector and a composite material layer disposed on at least one surface of the current collector (e.g., one surface or both surfaces), wherein the composite material layer comprises n active material layers and n-1 lithium replenishing layers alternately stacked, where n ≥ 3 and n is an integer (e.g., 3, 4, 5, 6, 8, 10, 12, or 15, etc.);
[0010] The layer of the composite material layer close to the current collector is the active material layer;
[0011] The porosity gradient of the n-1 lithium-supplementing layer increases along a direction away from the current collector.
[0012] It should be noted that the composite electrode sheet may be a positive composite electrode sheet or a negative composite electrode sheet.
[0013] The present application provides a composite electrode, which is provided by alternately stacking n layers of active material layers and n-1 layers of lithium replenishment layers, and defining the side of the composite material layer close to the current collector as the active material layer, so that multiple lithium replenishment layers are spaced apart inside the composite material layer, and the contact between the lithium replenishment layer and the active material layer is closer, thereby shortening the diffusion path of lithium ions and accelerating the diffusion rate of lithium ions, which helps to improve the rate and efficiency of lithium replenishment, and can improve the uniformity of lithium replenishment, avoiding the direct mixing of lithium replenishment materials and active materials to produce side reactions; and, by limiting the porosity of the n-1 layer of lithium replenishment layer to increase gradiently in the direction away from the current collector, lithium ions can be better embedded from the surface of the electrode to the interior of the electrode or removed in the opposite direction. Therefore, the composite electrode of the present application can reduce initial capacity loss and improve cycle performance, thereby improving energy density.
[0014] In one embodiment, the porosity of the active material layer is 35-45%, for example, it may be 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44% or 45%.
[0015] In one embodiment, the porosity gradient of the n-layer active material layer increases along a direction away from the current collector.
[0016] In the present application, when the porosity of the n-layer active material layer increases gradiently in the direction away from the current collector, ion transport and diffusion can be improved, the utilization rate of the active material is increased, and the internal resistance of the battery is reduced.
[0017] This application optimizes the path and speed of ion diffusion and improves the charge and discharge rate and cycle life of the battery by designing different layers and pore structures of the active material layer and the lithium replenishment layer.
[0018] In one embodiment, the active material layer includes an active material and a conductive agent.
[0019] In one embodiment, the active material includes a positive electrode active material or a negative electrode active material.
[0020] The present application does not specifically limit the type of positive electrode active material, including but not limited to lithium iron phosphate, lithium nickel cobalt manganese oxide (NMC) or manganese oxide lithium salts.
[0021] The present application does not specifically limit the type of negative electrode active material, including but not limited to graphite, silicon oxycarbon or lithium titanate.
[0022] In one embodiment, based on the total mass of the active material layer being 100%, the mass content of the active material is 96-98%, for example, 96%, 97% or 98%.
[0023] In one embodiment, the active material content of the n active material layers increases gradually in a direction away from the current collector.
[0024] In the present application, when the active material content of the n-layer active material layer increases gradiently in a direction away from the current collector, the electrode reaction rate can be increased, the material can be used more effectively, and the cost can be reduced.
[0025] In one embodiment, the particle size D50 of the active material is 0.4-20 μm, for example, 0.4 μm, 0.8 μm, 1.2 μm, 1.6 μm, 2 μm, 5 μm, 8 μm, 11 μm, 14 μm, 17 μm or 20 μm; the particle size of the conductive agent is in the range of 0.01-0.1 μm.
[0026] In one embodiment, the particle size D50 of the active material in the n active material layers increases gradually along a direction away from the current collector.
[0027] In the present application, when the active material particle size D50 of the n-layer active material layer increases gradiently in a direction away from the current collector, the electrode reaction rate can be increased and the energy density can be increased.
[0028] In one embodiment, the thickness of the active material layer is 3-30 μm, for example, it can be 3 μm, 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm, 17 μm, 19 μm, 2 μm, 23 μm, 25 μm, 27 μm, 29 μm or 30 μm.
[0029] In one embodiment, the thickness gradient of the n-layer active material layer increases along a direction away from the current collector.
[0030] In the present application, when the thickness of the n-layer active material layer increases gradually in a direction away from the current collector, the energy density of the battery can be improved and the internal resistance of the battery can be reduced.
[0031] This application can precisely control the composition and structure of the active material layer and the lithium replenishment layer according to specific battery needs and performance requirements. By adjusting the material combination, thickness, porosity and content of different layers, the electrochemical properties such as the capacity and cycle life of the electrode can be customized.
[0032] In one embodiment, the porosity of the lithium replenishing layer is 5-20%, for example, 5%, 7%, 9%, 10%, 12%, 14%, 16%, 18% or 20%.
[0033] In the present application, the lithium replenishing material filled in the lithium replenishing layer is relatively dense.
[0034] In one embodiment, the lithium replenishing material in the lithium replenishing layer includes metallic lithium or a lithium-containing compound.
[0035] In the present application, when the active material is a positive electrode active material, the lithium-containing compound is a lithium-supplementing material; when the active material is a negative electrode active material, the metallic lithium is a lithium-supplementing material.
[0036] Optionally, the lithium-containing compound includes at least one of Li2NiO2, Li5FeO4, Li3N, Li2O2 and Li2S.
[0037] In one embodiment, the particle size D50 of the lithium replenishing material in the lithium replenishing layer is 0.01-15 μm, for example, it can be 0.01 μm, 0.02 μm, 0.05 μm, 0.08 μm, 0.1 μm, 0.12 μm, 0.15 μm, 0.2 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, etc.
[0038] In one embodiment, the particle size gradient of the lithium-replenishing material of the n-1 lithium-replenishing layer increases along a direction away from the current collector.
[0039] In the present application, when the particle size of the lithium replenishing material of the n-1 lithium replenishing layer increases gradually in the direction away from the current collector, the cycle life and stability of the battery can be improved and the battery capacity attenuation can be reduced.
[0040] In one embodiment, the thickness of the lithium replenishing layer is 0.02-1 μm, for example, it can be 0.02 μm, 0.03 μm, 0.05 μm, 0.07 μm, 0.1 μm, 0.12 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm or 1 μm.
[0041] In this application, if the thickness of each lithium replenishing layer is too thin, it will lead to loss of battery capacity, reduced battery cycle life, and unstable battery performance; if the thickness of each lithium replenishing layer is too thick, it will reduce the battery energy density, increase the battery weight, and increase the battery cost.
[0042] In one embodiment, the thickness gradient of the n-1 lithium replenishing layer increases along a direction away from the current collector.
[0043] In the present application, when the thickness of the n-1 lithium replenishing layer increases gradually in the direction away from the current collector, the cycle life of the battery can be increased, the performance stability of the battery can be improved, and the degradation rate of the electrode material can be reduced.
[0044] In a second aspect, an embodiment of the present application provides a method for preparing the composite electrode according to the first aspect, the method comprising:
[0045] (1) evaporating an active material onto at least one surface of a current collector to form an active material layer;
[0046] (2) evaporating a lithium replenishing agent onto the surface of the active material layer formed in step (1) to form a lithium replenishing layer;
[0047] (3) evaporating an active material onto the surface of the lithium replenishing layer formed in step (2) to form an active material layer;
[0048] (4) Repeat steps (2) and (3) at least once (for example, once, twice, three times, four times, five times, eight times, ten times, twelve times, or fifteen times) to obtain the composite electrode.
[0049] Traditional multilayer coating often uses multiple nozzles to simultaneously spray different electrode materials, mixing them in a laminar flow to form a multilayer electrode structure. However, the coating formed by spraying is relatively thick. Excessively thick coatings can easily lead to uneven coating, which can cause inconsistent electrode performance and potentially lead to battery performance fluctuations and instability. It can also increase the diffusion distance of ions or molecules in the electrode, resulting in increased resistance to charge and mass transfer. This can slow the battery's response speed and reduce its power performance. It can also lead to a poor interface between the electrode and the electrolyte, limiting ion transport and charge conduction, which can affect the battery's cycle life and stability.
[0050] This application uses evaporation to obtain a uniform active material layer and lithium replenishment layer, which can more evenly distribute lithium ions and ensure balanced migration of lithium ions during the charge and discharge process, thereby improving the cycle life and performance stability of the battery. The evaporation method forms a multi-layer composite structure on the foil surface, achieving a refined design at the electrode level. In addition, the evaporation method coating has a controllable thickness and is applicable to a wide range of electrode materials.
[0051] Before evaporation, the current collector needs to be pre-treated to remove surface dirt, grease and impurities to ensure that the coating can be evenly attached to its surface.
[0052] In one embodiment, when the active material is evaporated, the temperature of the evaporation source is 500-2500°C, for example, 500°C, 600°C, 700°C, 900°C, 1000°C, 1200°C, 1500°C, 2000°C, 2200°C or 2500°C.
[0053] In this application, when evaporating the active material, when the evaporation source temperature is low, a lower evaporation rate generally favors the formation of larger particles, while when the evaporation source temperature is high, a higher evaporation rate generally leads to the formation of smaller particles. By controlling the evaporation time and the evaporation source temperature, the thickness of the active material layer can be controlled. Repeated evaporation can also be performed to increase the thickness of the active material layer.
[0054] In one embodiment, when evaporating the active material, the distance between the substrate to be evaporated and the evaporation source is 10-50 cm, for example, 10 cm, 20 cm, 30 cm, 40 cm or 50 cm.
[0055] In one embodiment, when the lithium supplement agent is evaporated, the temperature of the evaporation source is 500-2500°C, for example, 500°C, 600°C, 700°C, 900°C, 1000°C, 1200°C, 1500°C, 2000°C, 2200°C or 2500°C.
[0056] In this application, when evaporating the lithium-replenishing agent, when the evaporation source temperature is low, the lower evaporation rate generally favors the formation of larger particle sizes, while when the evaporation source temperature is high, the higher evaporation rate generally leads to the formation of smaller particle sizes. By controlling the evaporation time and the evaporation source temperature, the thickness of the lithium-replenishing layer can be controlled. Repeated evaporation can also be performed to increase the thickness of the lithium-replenishing layer.
[0057] In one embodiment, when the lithium supplementing agent is evaporated, the distance between the substrate to be evaporated and the evaporation source is 10-50 cm, for example, 10 cm, 20 cm, 30 cm, 40 cm or 50 cm.
[0058] In this application, when evaporating active materials or lithium replenishers, the distance between the substrate to be deposited and the evaporation source affects the accumulation and growth behavior of the particles. Adjusting the distance between the evaporation source and the substrate can control the deposition pattern and particle size. Furthermore, by controlling the temperature of the evaporation source and the distance between the substrate to be deposited and the evaporation source, the particle size of the material in the active material layer or lithium replenisher layer can be changed.
[0059] In one embodiment, after each evaporation, an inert gas (such as nitrogen) is introduced to cool and solidify the film.
[0060] Maintaining a constant inert gas flow rate within the vacuum chamber accelerates the cooling process of the substrate and the film. This helps stabilize the film and ensures its adhesion to the substrate.
[0061] In a third aspect, an embodiment of the present application provides a lithium-ion battery, wherein the lithium-ion battery includes the composite electrode described in the first aspect.
[0062] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to limited space and for the sake of simplicity, this application no longer exhaustively lists the specific point values included in the range.
[0063] Compared with the related art, the beneficial effects of this application are:
[0064] The present application provides a composite electrode, which is provided by alternately stacking n layers of active material layers and n-1 layers of lithium replenishment layers, and defining the side of the composite material layer close to the current collector as the active material layer, so that multiple lithium replenishment layers are spaced apart inside the composite material layer, and the contact between the lithium replenishment layer and the active material layer is closer, thereby shortening the diffusion path of lithium ions and accelerating the diffusion rate of lithium ions, which helps to improve the rate and efficiency of lithium replenishment, and can improve the uniformity of lithium replenishment, avoiding the direct mixing of lithium replenishment materials and active materials to produce side reactions; and, by limiting the porosity of the n-1 layer of lithium replenishment layer to increase gradiently in the direction away from the current collector, lithium ions can be better embedded from the surface of the electrode to the interior of the electrode or removed in the opposite direction. Therefore, the composite electrode of the present application can reduce initial capacity loss and improve cycle performance, thereby improving energy density.
[0065] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] FIG1 is a schematic structural diagram of a composite electrode provided in Example 1 of the present application;
[0067] Among them, 1 is the current collector; 2 is the first active material layer; 3 is the first lithium replenishing layer; 4 is the second active material layer; 5 is the second lithium replenishing layer; and 6 is the third active material layer. DETAILED DESCRIPTION
[0068] The technical solution of this application is further explained below through specific implementation methods.
[0069] Example 1
[0070] This embodiment provides a composite electrode sheet, which is a positive electrode sheet, as shown in FIG1 , comprising a current collector 1 (i.e., aluminum foil) and composite material layers disposed on both sides of the aluminum foil. The composite material layers comprise three alternating active material layers and two lithium replenishing layers, which are sequentially labeled as a first active material layer 2, a first lithium replenishing layer 3, a second active material layer 4, a second lithium replenishing layer 5, and a third active material layer 6 in a direction away from the current collector 1.
[0071] Each active material layer is composed of lithium iron phosphate positive electrode active material and carbon black conductive agent. The mass content of active material in the first active material layer 2, the second active material layer 4 and the third active material layer 6 are 96%, 97% and 98% respectively. The active material particle size D50 in the first active material layer 2, the second active material layer 4 and the third active material layer 6 are 0.6μm, 1μm and 1.4μm respectively. The particle size range of the carbon black conductive agent in the three active material layers is 0.01-0.1μm. The porosity of the first active material layer 2, the second active material layer 4 and the third active material layer 6 are 35%, 40% and 45% respectively. The thickness of the first active material layer 2, the second active material layer 4 and the third active material layer 6 are 5μm, 10μm and 15μm respectively.
[0072] Each lithium replenishment layer is composed of lithium-rich lithium nickelate (Li2NiO2); the particle size D50 of the lithium replenishment material in the first lithium replenishment layer 3 and the second lithium replenishment layer 5 is 1.3μm and 1.5μm respectively; the porosity of the first lithium replenishment layer 3 and the second lithium replenishment layer 5 is 6% and 12% respectively; the thickness of the first lithium replenishment layer 3 and the second lithium replenishment layer 5 is 0.05μm and 0.1μm respectively.
[0073] This embodiment also provides a method for preparing the composite electrode, which comprises the following steps:
[0074] (1) Lithium iron phosphate and carbon black powder in a mass ratio of 96:4 were mixed and placed in an evaporation source; the chamber in the first evaporation device was evacuated to a high vacuum state to 10 -4 ~10 -7 kPa, to avoid oxidation and denaturation of the material in a high-temperature environment; at the same time, vacuum evaporation can provide a uniform atmosphere, so that the coating can be deposited on the foil with relatively uniform density and structure; ensure that the air pressure in the chamber is controlled and monitored to achieve the required evaporation environment;
[0075] (2) The foil to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the foil and the evaporation source is ensured to be 25 cm; the evaporation source heating device is used to heat the material to its sublimation temperature of 1000°C, so that the material sublimates and forms vapor. The sublimated material vapor is deposited on the surface of the foil in a vacuum environment for 0.15 hours; then nitrogen is introduced to cool and solidify, and the resulting active material layer is the first active material layer 2;
[0076] (3) The foil on which the first active material layer 2 has been deposited (i.e., the substrate to be deposited) is transferred to the second deposition device, and lithium nickelate (Li2NiO2) powder is placed at the evaporation source; the chamber in the deposition device is re-evacuated to a high vacuum state to 10 -4 ~10 -7kPa, to prevent the lithium supplement from reacting with oxygen at high temperatures and denaturing; at the same time, vacuum evaporation can provide a uniform atmosphere, allowing the coating to be deposited on the substrate with relatively uniform density and structure;
[0077] (4) The substrate to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the substrate and the evaporation source is ensured to be 25 cm. The lithium supplement agent is heated to its sublimation temperature of 500°C using the evaporation source heating device, so that the lithium supplement agent sublimates and forms vapor. The sublimated lithium supplement agent vapor is deposited on the surface of the substrate to be evaporated in a vacuum environment for 0.15 hours; then nitrogen gas is introduced to cool and solidify, and the obtained lithium supplement layer is the first lithium supplement layer 3;
[0078] (5) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 97:3, the distance between the substrate to be evaporated and the evaporation source to 20 cm, the temperature of the evaporation source to 1100° C., and the deposition time to 0.1 h, thereby obtaining a second active material layer 4;
[0079] (6) Repeat steps (3) and (4), and adjust the deposition time to 0.15 h, the distance between the substrate to be evaporated and the evaporation source to 15 cm, the temperature of the evaporation source to 600 ° C, and the deposition time to 0.1 h, thereby obtaining a second lithium replenishment layer 5;
[0080] (7) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 98:2, the distance between the substrate to be evaporated and the evaporation source to 15 cm, the temperature of the evaporation source to 1200° C., and the deposition time to 0.05 h, thereby obtaining a third active material layer 6.
[0081] Example 2
[0082] This embodiment provides a composite electrode sheet, which is a positive electrode sheet, including a current collector (i.e., aluminum foil) and a composite material layer disposed on one surface of the aluminum foil. The composite material layer includes five active material layers and four lithium replenishing layers alternately stacked, which are sequentially labeled as the first active material layer, the first lithium replenishing layer, the second active material layer, the second lithium replenishing layer, the third active material layer, the third lithium replenishing layer, the fourth active material layer, the fourth lithium replenishing layer, and the fifth active material layer in the direction away from the current collector.
[0083] Each active material layer is composed of lithium iron phosphate positive electrode active material and carbon black conductive agent. The mass content of active material in the first active material layer, the second active material layer, the third active material layer, the fourth active material layer and the fifth active material layer is 96%, 96.5%, 97%, 97.5% and 98% respectively; the active material particle size D50 in the first active material layer, the second active material layer, the third active material layer, the fourth active material layer and the fifth active material layer is 0.6μm, 0.8μm, 1μm, 1.2μm, respectively. μm and 1.4 μm, the particle size range of the carbon black conductive agent in the five active material layers is 0.01-0.1 μm; the porosity of the first active material layer, the second active material layer, the third active material layer, the fourth active material layer and the fifth active material layer are 35%, 37.5%, 40%, 42.5% and 45% respectively; the thickness of the first active material layer, the second active material layer, the third active material layer, the fourth active material layer and the fifth active material layer are 2 μm, 4 μm, 6 μm, 8 μm and 10 μm respectively;
[0084] Each lithium replenishment layer is composed of lithium-rich lithium nickelate (Li2NiO2); the particle size D50 of the lithium replenishment material in the first lithium replenishment layer, the second lithium replenishment layer, the third lithium replenishment layer and the fourth lithium replenishment layer are 1.3μm, 1.4μm, 1.5μm and 1.6μm respectively; the porosity of the first lithium replenishment layer, the second lithium replenishment layer, the third lithium replenishment layer and the fourth lithium replenishment layer are 6%, 8%, 10% and 12% respectively; the thickness of the first lithium replenishment layer, the second lithium replenishment layer, the third lithium replenishment layer and the fourth lithium replenishment layer are 0.015μm, 0.03μm, 0.045μm and 0.06μm respectively.
[0085] This embodiment also provides a method for preparing the composite electrode, which comprises the following steps:
[0086] (1) Lithium iron phosphate and carbon black powder in a mass ratio of 96:4 were mixed and placed in an evaporation source; the chamber in the first evaporation device was evacuated to a high vacuum state to 10 -4 ~10 -7 kPa, to avoid oxidation and denaturation of the material in a high-temperature environment; at the same time, vacuum evaporation can provide a uniform atmosphere, so that the coating can be deposited on the foil with relatively uniform density and structure; ensure that the air pressure in the chamber is controlled and monitored to achieve the required evaporation environment;
[0087] (2) The foil to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the foil and the evaporation source is ensured to be 40 cm; the evaporation source heating device is used to heat the material to its sublimation temperature of 1000°C, so that the material sublimates and forms vapor. The sublimated material vapor is deposited on the surface of the foil in a vacuum environment for 0.2 hours; then nitrogen is introduced for cooling and solidification, and the resulting active material layer is the first active material layer;
[0088] (3) The foil on which the first active material layer has been evaporated (i.e., the substrate to be evaporated) is transferred to the second evaporation device, and lithium nickelate (Li2NiO2) powder is placed at the evaporation source; the chamber in the evaporation device is re-evacuated to a high vacuum state to 10 -4 10 -7 kPa, to prevent the lithium supplement agent from reacting with oxygen at high temperature and denaturing; at the same time, vacuum evaporation can provide a uniform atmosphere, so that the coating can be deposited on the substrate with relatively uniform density and structure;
[0089] (4) The substrate to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the substrate and the evaporation source is ensured to be 40 cm. The lithium replenishing agent is heated to its sublimation temperature of 1000° C. using the evaporation source heating device, so that the lithium replenishing agent sublimates and forms vapor. The sublimated lithium replenishing agent vapor is deposited on the surface of the substrate to be evaporated for 0.1 h in a vacuum environment; then nitrogen is introduced for cooling and solidification, and the obtained lithium replenishing layer is the first lithium replenishing layer;
[0090] (5) Repeating steps (1) and (2), adjusting the mass ratio of the active material to the conductive agent to 96.5:3.5, adjusting the distance between the substrate to be evaporated and the evaporation source to 35 cm, adjusting the temperature of the evaporation source to 1100° C., and adjusting the deposition time to 0.17 h, thereby obtaining a second active material layer;
[0091] (6) Repeat steps (3) and (4), and adjust the deposition time to 0.17 h, the distance between the substrate to be evaporated and the evaporation source to 35 cm, the temperature of the evaporation source to 1100 ° C, and the deposition time to 0.17 h to obtain a second lithium replenishment layer;
[0092] (7) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 97:3, the distance between the substrate to be evaporated and the evaporation source to 30 cm, the temperature of the evaporation source to 1200° C., and the deposition time to 0.14 h, thereby obtaining a third active material layer;
[0093] (8) Repeat steps (3) and (4), and adjust the deposition time to 0.14 h, the distance between the substrate to be evaporated and the evaporation source to 30 cm, the temperature of the evaporation source to 1200 ° C, and the deposition time to 0.14 h to obtain a third lithium replenishment layer;
[0094] (9) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 97.5:2.5, the distance between the substrate to be evaporated and the evaporation source to 25 cm, the temperature of the evaporation source to 1300° C., and the deposition time to 0.11 h, thereby obtaining a fourth active material layer;
[0095] (10) Repeat steps (3) and (4), and adjust the deposition time to 0.11 h, the distance between the substrate to be evaporated and the evaporation source to 25 cm, the temperature of the evaporation source to 1300 ° C, and the deposition time to 0.11 h, thereby obtaining a fourth lithium replenishment layer;
[0096] (11) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 98:2, the distance between the substrate to be evaporated and the evaporation source to 20 cm, the temperature of the evaporation source to 1400° C., and the deposition time to 0.08 h to obtain a fifth active material layer.
[0097] Example 3
[0098] This embodiment provides a composite electrode sheet, which is a negative electrode sheet and includes a current collector (i.e., copper foil) and a composite material layer disposed on one surface of the copper foil. The composite material layer includes three active material layers and two lithium replenishing layers alternately stacked, which are sequentially designated as the first active material layer, the first lithium replenishing layer, the second active material layer, the second lithium replenishing layer, and the third active material layer in the direction away from the current collector.
[0099] Each active material layer is composed of a graphite negative electrode active material and a carbon black conductive agent. The mass content of the active material in the first active material layer, the second active material layer, and the third active material layer is 96%, 97%, and 98%, respectively. The active material particle size D50 in the first active material layer, the second active material layer, and the third active material layer are 15 μm, 16 μm, and 17 μm, respectively. The particle size range of the carbon black conductive agent in the three active material layers is 0.01-0.1 μm. The porosity of the first active material layer, the second active material layer, and the third active material layer are 35%, 40%, and 45%, respectively. The thickness of the first active material layer, the second active material layer, and the third active material layer are 5 μm, 10 μm, and 15 μm, respectively.
[0100] Each lithium replenishment layer is composed of metallic lithium; the particle size D50 of the lithium replenishment material in the first lithium replenishment layer and the second lithium replenishment layer is 0.04μm and 0.06μm respectively; the porosity of the first lithium replenishment layer and the second lithium replenishment layer is 6% and 12% respectively; the thickness of the first lithium replenishment layer and the second lithium replenishment layer is 0.05μm and 0.1μm respectively.
[0101] This embodiment also provides a method for preparing the composite electrode, which comprises the following steps:
[0102] (1) Graphite and carbon black powders with a mass ratio of 96:4 were mixed and placed in an evaporation source; the chamber in the first evaporation device was evacuated to a high vacuum state to 10 -4 10 -7kPa, to avoid oxidation and denaturation of the material in a high-temperature environment; at the same time, vacuum evaporation can provide a uniform atmosphere, so that the coating can be deposited on the foil with relatively uniform density and structure; ensure that the air pressure in the chamber is controlled and monitored to achieve the required evaporation environment;
[0103] (2) The foil to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the foil and the evaporation source is ensured to be 25 cm; the evaporation source heating device is used to heat the material to its sublimation temperature of 800°C, so that the material sublimates and forms vapor. The sublimated material vapor is deposited on the surface of the foil in a vacuum environment for 0.15 hours; then nitrogen is introduced to cool and solidify, and the resulting active material layer is the first active material layer;
[0104] (3) The foil on which the first active material layer has been evaporated (i.e., the substrate to be evaporated) is transferred to the second evaporation device, and the lithium supplement powder is placed at the evaporation source, wherein the lithium supplement powder is metallic lithium; the chamber in the evaporation device is re-evacuated to a high vacuum state to 10 -4 ~10 -7 kPa, to prevent the lithium supplement agent from reacting with oxygen at high temperature and denaturing; at the same time, vacuum evaporation can provide a uniform atmosphere, so that the coating can be deposited on the substrate with relatively uniform density and structure;
[0105] (4) The substrate to be evaporated is conveyed to the top of the evaporation source by the unwinding device and the winding device, and the distance between the substrate and the evaporation source is ensured to be 25 cm. The lithium replenishing agent is heated to its sublimation temperature of 1800° C. using the evaporation source heating device, so that the lithium replenishing agent sublimates and forms vapor. The sublimated lithium replenishing agent vapor is deposited on the surface of the substrate to be evaporated in a vacuum environment for 0.15 h; then nitrogen is introduced for cooling and solidification, and the obtained lithium replenishing layer is the first lithium replenishing layer;
[0106] (5) Repeating steps (1) and (2), adjusting the mass ratio of the active material to the conductive agent to 97:3, adjusting the distance between the substrate to be evaporated and the evaporation source to 20 cm, adjusting the temperature of the evaporation source to 900° C., and adjusting the deposition time to 0.1 h, thereby obtaining a second active material layer;
[0107] (6) Repeat steps (3) and (4), and adjust the deposition time to 0.1 h, the distance between the substrate to be evaporated and the evaporation source to 20 cm, the temperature of the evaporation source to 2000 ° C, and the deposition time to 0.1 h to obtain a second lithium replenishment layer;
[0108] (7) Repeat steps (1) and (2), and adjust the mass ratio of the active material to the conductive agent to 98:2, the distance between the substrate to be evaporated and the evaporation source to 15 cm, the temperature of the evaporation source to 1000°C, and the deposition time to 0.05 h to obtain a third active material layer.
[0109] Example 4
[0110] The difference between this embodiment and embodiment 1 is that the thickness of the first lithium replenishing layer is adjusted to 0.5 μm, and the thickness of the second lithium replenishing layer is adjusted to 1 μm. The rest is exactly the same as embodiment 1.
[0111] Example 5
[0112] The difference between this embodiment and embodiment 1 is that the thickness of the first lithium replenishing layer is adjusted to 0.02 μm, and the thickness of the second lithium replenishing layer is adjusted to 0.04 μm. The rest is exactly the same as embodiment 1.
[0113] Example 6
[0114] The difference between this embodiment and embodiment 1 is that the thickness of the first lithium replenishing layer and the second lithium replenishing layer are the same, both 0.1 μm. The rest is exactly the same as embodiment 1.
[0115] Example 7
[0116] The difference between this embodiment and embodiment 1 is that the particle size D50 of the lithium replenishing material in the first lithium replenishing layer and the second lithium replenishing layer is the same, both 1.3 μm. The rest is exactly the same as embodiment 1.
[0117] Example 8
[0118] The difference between this embodiment and embodiment 1 is that the active material mass content of the first active material layer, the second active material layer, and the third active material layer is the same, namely, 96%.
[0119] Example 9
[0120] The difference between this embodiment and embodiment 1 is that the thicknesses of the first active material layer, the second active material layer, and the third active material layer are the same, namely, 10 μm. The rest is exactly the same as embodiment 1.
[0121] Example 10
[0122] The difference between this embodiment and embodiment 1 is that the particle size D50 of the first active material layer, the second active material layer, and the third active material layer is the same, namely, 1 μm. The rest is exactly the same as embodiment 1.
[0123] Example 11
[0124] The difference between this embodiment and embodiment 1 is that the porosity of the first active material layer, the second active material layer, and the third active material layer are the same, namely, 35%. The rest is exactly the same as embodiment 1.
[0125] Comparative Example 1
[0126] The difference between this comparative example and Example 1 is that the porosity of the first lithium replenishing layer and the second lithium replenishing layer are the same, both 12%. The rest is exactly the same as Example 1.
[0127] Comparative Example 2
[0128] This comparative example differs from Example 1 in that the composite material layer includes two alternating active material layers and one lithium-replenishing layer. The two active material layers are the first active material layer and the second active material layer, and the one lithium-replenishing layer is the first lithium-replenishing layer. The remainder of the structure is identical to Example 1.
[0129] Comparative Example 3
[0130] This comparative example provides a positive electrode plate, which includes an aluminum foil and an active material layer arranged on one side of the aluminum foil. The active material layer includes LiFePO4, carbon black, Li2NiO2 and polyvinylidene fluoride (PVDF), with a mass ratio of 7:1:1:1.
[0131] Comparative Example 4
[0132] This comparative example provides a negative electrode plate, which includes a copper foil and an active material layer arranged on one surface of the copper foil, wherein the active material layer includes graphite and carbon black in a mass ratio of 97:3; an ultra-thin lithium strip and the active material layer are rolled and composited to replenish lithium.
[0133] Performance Testing
[0134] The positive electrode sheets provided in Examples 1-2, Examples 4-11 and Comparative Examples 1-3 were assembled into lithium-ion batteries, wherein the negative electrode was a graphite sheet, the electrolyte was LiPF6 electrolyte, and the separator was polyethylene.
[0135] The negative electrode plates provided in Example 3 and Comparative Example 4 were assembled into a lithium-ion battery, wherein the positive electrode was a lithium iron phosphate plate, the electrolyte was LiPF6 electrolyte, and the separator was polyethylene.
[0136] The lithium-ion battery assembled above was tested:
[0137] (1) First charge and discharge efficiency test
[0138] Place the prepared test battery in a constant temperature box, control the temperature at 23℃±2℃, and let it stand for 2h~12h. Then use a lithium-ion battery electrochemical performance tester to test the battery. The charge and discharge system is as follows:
[0139] a) Charging limit voltage: At a rate of 0.1C, constant current charging to 3.65V, then constant voltage charging, constant voltage charging cut-off current 0.05C;
[0140] b) Discharge end voltage: at 0.1C rate, constant current discharge to 2.0V;
[0141] The constant current charge and discharge current at tC rate can be calculated as follows: I t =m×C0×t;
[0142] Among them, I t is the constant charge and discharge current, in mA; m is the mass of the active material in the battery (such as lithium iron phosphate or graphite), in g; C0 is the theoretical specific capacity of the active material, in mA h / g; t is the number of times the charge or discharge is completed in 1 / t time, in / h, which refers to 0.1 / h in this article.
[0143] c) Data Recording:
[0144] After the test battery is charged and discharged for one week, the charge and discharge capacity is recorded and the initial charge and discharge efficiency of the battery is calculated. The initial charge and discharge efficiency of lithium iron phosphate is calculated as follows:
[0145] Among them, Q ID and Q IC The battery is in I t The first discharge capacity and first charge capacity of the charge and discharge test under current.
[0146] (2) Cycle life test
[0147] After the test battery is divided into different capacities, a cycle test is performed using a lithium-ion battery electrochemical performance tester. The charge and discharge voltage limits are as follows:
[0148] a) Charging limit voltage: constant current and constant voltage charging to 3.65V, constant voltage charging cut-off current is 0.05C;
[0149] b) Discharge end voltage: 2.5V;
[0150] c) Charge and discharge system: According to the provisions of GB / T18287, charge and discharge cycles are carried out at 1C / 1C at an ambient temperature of (23±2)℃.
[0151] d) Data recording: record the charge and discharge capacity of the test battery at different cycle times. The discharge capacity at the first cycle when the battery is discharged to the termination voltage is recorded as Q1, and the discharge capacity at the nth cycle when the battery is discharged to the termination voltage is recorded as Q. n The capacity retention rate after 1500 cycles is calculated as follows: η=(Q 1500 / Q1)×100%.
[0152] The test results are shown in Table 1.
[0153] Table 1
[0154] analyze:
[0155] It can be seen from the data of Examples 1-3 and Comparative Examples 3-4 that by alternately stacking the active material layers and the lithium supplement layers, and setting the various gradient parameters, the first charge and discharge efficiency of the composite electrode assembled battery can be improved, the initial capacity loss can be reduced, and the capacity retention rate of the battery can be improved, and the cycle performance can be improved.
[0156] It can be seen from the data of Examples 1 and 4-5 that if the thickness of each lithium replenishing layer is too thick, the battery capacity retention rate will be slightly lower and the cycle performance will be slightly worse; if the thickness of each lithium replenishing layer is too thin, the battery's initial charge and discharge efficiency will be slightly lower, the initial capacity will be lost, the capacity retention rate will be slightly lower, and the cycle performance will be slightly worse.
[0157] It can be seen from the data of Examples 1 and 6-7 that if the thickness of the first lithium replenishing layer and the second lithium replenishing layer is the same and no gradient is formed, the initial charge and discharge efficiency and cycle performance of the composite electrode assembled battery will be reduced; if the particle size of the lithium replenishing material of the first lithium replenishing layer and the second lithium replenishing layer is the same and no gradient is formed, the battery cycle life will be reduced.
[0158] It can be seen from the data of Examples 1 and 8-11 that if the active material mass content, thickness and porosity of the first active material layer, the second active material layer and the third active material layer are made the same, no gradient is formed, which will lead to reduced cycle performance of the battery.
[0159] It can be seen from the data of Example 1 and Comparative Example 1 that if the porosity of the first lithium replenishing layer and the second lithium replenishing layer is the same and no gradient is formed, it will affect the embedding or reverse extraction of lithium ions from the surface of the electrode to the interior of the electrode, thereby reducing the initial charge and discharge efficiency of the composite electrode assembled battery.
[0160] It can be seen from the data of Example 1 and Comparative Example 2 that if the composite material layer only includes two active material layers and one lithium replenishing layer alternately stacked, the battery cycle performance will be reduced.
[0161] It can be seen from the data of Example 1 and Comparative Example 3 that, for the positive electrode sheet, using a conventional blending method to supplement lithium will lead to a decrease in the cycle performance of the battery.
[0162] It can be seen from the data of Example 1 and Comparative Example 4 that, for the negative electrode, the conventional rolling composite method for lithium replenishment will reduce the initial charge and discharge efficiency of the battery assembled with the composite electrode.
Claims
1. A composite electrode, comprising a current collector and a composite material layer disposed on at least one side of the current collector, wherein the composite material layer comprises n layers of active material layers and n-1 layers of lithium supplement layers alternately stacked, where n≥3 and n is an integer; The side of the composite material layer close to the current collector is an active material layer; Along the direction away from the current collector, the porosity gradient of the n-1 lithium replenishing layer increases.
2. The composite pole piece according to claim 1, wherein: The porosity of the active material layer is 35-45%.
3. The composite pole piece according to claim 1 or 2, wherein: The porosity gradient of the n-layer active material layer increases along a direction away from the current collector.
4. The composite pole piece according to any one of claims 1 to 3, wherein: The active material layer includes active material and conductive agent; Optionally, based on the total mass of the active material layer being 100%, the mass content of the active material is 96-98%; Optionally, the active material content of the n active material layers increases gradiently along a direction away from the current collector; Optionally, the particle size D50 of the active material is 0.4-20 μm; the particle size range of the conductive agent is 0.01-0.1 μm.
5. The composite pole piece according to any one of claims 1 to 4, wherein: The active material particle size D50 of the n active material layers increases gradually along a direction away from the current collector.
6. The composite pole piece according to any one of claims 1 to 5, wherein: The thickness of the active material layer is 3-30 μm.
7. The composite pole piece according to any one of claims 1 to 6, wherein: Along the direction away from the current collector, the thickness gradient of the n active material layers increases.
8. The composite pole piece according to any one of claims 1 to 7, wherein: The porosity of the lithium supplement layer is 5-20%.
9. The composite pole piece according to any one of claims 1 to 8, wherein: The lithium supplement material in the lithium supplement layer includes metallic lithium or a lithium-containing compound; Optionally, the particle size D50 of the lithium replenishing material in the lithium replenishing layer is 0.01-15 μm.
10. The composite pole piece according to any one of claims 1 to 9, wherein: Along the direction away from the current collector, the particle size gradient of the lithium replenishing material of the n-1 lithium replenishing layer increases.
11. The composite pole piece according to any one of claims 1 to 10, wherein: The thickness of the lithium supplement layer is 0.02-1 μm.
12. The composite pole piece according to any one of claims 1 to 11, wherein: Along the direction away from the current collector, the thickness gradient of the n-1 lithium replenishing layer increases.
13. A method for preparing the composite pole piece according to any one of claims 1 to 12, comprising: (1) evaporating an active material onto at least one side of a current collector to form an active material layer; (2) evaporating a lithium replenishing agent onto the surface of the active material layer formed in step (1) to form a lithium replenishing layer; (3) evaporating an active material onto the surface of the lithium replenishing layer formed in step (2) to form an active material layer; (4) Repeat steps (2) and (3) at least once to obtain the composite electrode.
14. The preparation method according to claim 13, wherein: When evaporating the active material, the temperature of the evaporation source is 500-2500° C.; Optionally, when evaporating the active material, the distance between the substrate to be evaporated and the evaporation source is 10-50 cm; Optionally, when evaporating the lithium supplementing agent, the temperature of the evaporation source is 500-2500° C.; Optionally, when the lithium supplementing agent is evaporated, the distance between the substrate to be evaporated and the evaporation source is 10-50 cm.
15. A lithium ion battery, wherein: The lithium-ion battery comprises the composite pole piece according to any one of claims 1 to 12.
Citation Information
Patent Citations
Method for preparing lithium-supplemented anode, lithium-supplemented anode and lithium ion secondary battery
CN109244355A
Lithium-supplementing positive pole piece, preparation method thereof and lithium ion battery
CN115939308A
Lithium-rich thick electrode and preparation method and application thereof
CN116525822A
Pole piece and lithium secondary battery
CN215184062U
Lithium ion secondary battery, and manufacturing method thereof
JP2011198692A
Cited By
Lithium ion secondary battery, assembly for preparing lithium ion secondary battery, preparation method, lithium supplementing negative plate and power utilization device