High-current-density combined passivated back-contact battery and preparation method therefor

By setting up a specific doping region and layer structure in the back contact cell, combined with the tunnel oxide layer and anti-reflection layer, the problems of parasitic absorption and high equipment cost caused by the amorphous silicon layer are solved, and high current density and efficient conversion are achieved. Efficiency improves market competitiveness.

WO2024212770A1PCT designated stage expired Publication Date: 2024-10-17GOLD STONE (FUJIAN) ENERGY CO LTD

Patent Information

Application Number
PCT/CN2024/082386
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-19
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Parasitic absorption and attenuation problems caused by amorphous silicon or microcrystalline silicon layers in existing back-contact heterojunction solar cells, as well as the high cost of plate-type PECVD equipment, limit cell conversion efficiency and market competitiveness.

Method used

Designing a high current density jointly passivated back-contact cell by arranging a second shallowly doped region and a first heavily doped region with a specific surface doping index ratio on the silicon substrate, combined with a tunneling oxide layer and anti-reflection layer, avoiding the use of amorphous silicon or microcrystalline silicon layers to achieve field passivation and chemical passivation effects.

Benefits of technology

While ensuring high current density, it avoids parasitic absorption and attenuation problems, reduces equipment costs, improves fill factor and photoelectric conversion efficiency, and enhances component stability and market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082386_17102024_PF_FP_ABST
    Figure CN2024082386_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure belongs to the technical field of back-contact batteries, and particularly relates to a high-current-density combined passivated back-contact battery and a preparation method therefor. The high-current-density combined passivated back-contact battery comprises: a silicon substrate, which has a front face and a back face; a first semiconductor layer and a second semiconductor layer, which are provided on the back face; and a front passivation layer and an anti-reflection layer, which are provided on the front face, wherein the first semiconductor layer comprises a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer. The side of the first doped silicon crystal layer that is away from the silicon substrate is provided with a first heavily doped region, and the front face of the silicon substrate is provided with a second lightly doped region, which is in contact with the front passivation layer; and the ratio of a face doping index of the first heavily doped region to that of the second lightly doped region is 10-40:1, and the ratio of the thickness of the second lightly doping region to that of the tunneling oxide layer is 2-10:1 The present disclosure can ensure a high current density, without providing an amorphous silicon layer or a microcrystalline silicon layer.
Need to check novelty before this filing date? Find Prior Art

Description

A high current density combined passivation back contact battery and its preparation method

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to Chinese patent application No. 2023103689848 filed with the Patent Office of China on April 10, 2023, entitled “A high current density combined passivated back contact battery and its preparation method,” the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0003] The present disclosure belongs to the technical field of back contact batteries, and particularly relates to a high current density combined passivation back contact battery and a preparation method thereof. Background Art

[0004] In the prior art, the front of a back-contact heterojunction solar cell is generally deposited with an amorphous silicon or microcrystalline silicon layer superimposed with an anti-reflection layer to ensure the passivation effect while increasing transmittance and improving short-circuit current. However, the amorphous silicon or microcrystalline silicon layer has certain light absorption properties, which will produce parasitic absorption, affecting the improvement of short-circuit current. At the same time, the amorphous silicon or microcrystalline silicon layer will experience PID (potential induced degradation) or LID (light induced degradation) during long-term outdoor operation. Moreover, the amorphous silicon or microcrystalline silicon layer deposited in the back-contact cell is generally deposited using plate-type PECVD deposition. The plate-type equipment is relatively expensive and is not conducive to improving market competitiveness.

[0005] The applicant of the present disclosure, in its earlier research results, CN115207137B, disclosed a combined passivated back-contact cell and its preparation method. The cell comprises an N-type doped silicon substrate having a light-receiving surface and a back surface, a first semiconductor layer and a second semiconductor layer disposed on the back surface, the second semiconductor layer comprising an intrinsic silicon layer and a P-type doped silicon layer sequentially disposed in a direction perpendicular to the back surface and outward, and the first semiconductor layer comprising a tunneling oxide layer and an N-type doped silicon crystal layer sequentially disposed in a direction perpendicular to the back surface and outward; an amorphous silicon or microcrystalline silicon layer superimposed with an antireflection layer is deposited on the light-receiving surface (i.e., the front surface). Compared to conventional heterojunction cells, this combined passivated back-contact cell can significantly improve fill factor (FF), photoelectric conversion efficiency, and yield, among other things. Furthermore, the preparation method is relatively simple and industrializable, facilitating mass production efficiency and offering significant market advantages.

[0006] However, in the combined passivated back-contact cells that have great advantages in mass production, the parasitic absorption problem of the back polycrystalline and front amorphous film layers limits the improvement of the cell conversion efficiency to a certain extent. Therefore, how to overcome the above-mentioned parasitic absorption and attenuation problems caused by the amorphous silicon or microcrystalline silicon layer in the combined passivated cell structure and the high cost of deposition equipment, and further improve market competitiveness, has not been reported in the existing technology.

[0007] Summary of the Invention

[0008] The purpose of the present disclosure is to overcome the parasitic absorption and attenuation problems caused by the back polycrystalline and front deposited amorphous silicon or microcrystalline silicon layers and the defects of high deposition equipment cost in the prior art, and to provide a high current density combined passivation back contact cell and a preparation method thereof. The combined passivation back contact cell can achieve good passivation effect without setting an amorphous silicon or microcrystalline silicon layer while ensuring high current density (that is, taking into account the comprehensive effects of better short-circuit current Isc, open-circuit voltage Voc, fill factor FF, and battery conversion efficiency), while avoiding the above-mentioned parasitic absorption and attenuation problems caused by the back polycrystalline and amorphous silicon or microcrystalline silicon layers and the problem of high deposition equipment cost.

[0009] In order to achieve the above-mentioned objectives, in a first aspect, the present disclosure provides a high current density combined passivation back contact cell, comprising a silicon substrate having a front side and a back side, a first semiconductor layer and a second semiconductor layer arranged on the back side, and a front passivation layer and an anti-reflection layer arranged on the front side, wherein the first semiconductor layer comprises a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer; a first heavily doped region is provided on a side of the first doped silicon crystal layer away from the silicon substrate, a second shallowly doped region is provided on the front side of the silicon substrate, the second shallowly doped region is in contact with the front passivation layer, and a ratio of the surface doping index of the first heavily doped region to the second shallowly doped region is 10-40:1, wherein the surface doping index is the ratio of the effective doping concentration of the corresponding doping layer to the thickness of the doping layer; and the ratio of the thickness of the second shallowly doped region to the tunneling oxide layer is 2-10:1.

[0010] In some optional embodiments of the present disclosure, the side of the first doped silicon crystal layer close to the silicon substrate is an original shallow doping region, and the ratio of the surface doping index of the original shallow doping region to the first heavily doped region and the second shallow doping region is 0.3-2:10-40:1.

[0011] More optionally, the ratio of the surface doping index of the second doped silicon layer to the original shallow doped region is 5-30:1.

[0012] In some optional embodiments of the present disclosure, the thickness of the first heavily doped region is 1 / 10-1 / 2 of the thickness of the first doped silicon crystal layer.

[0013] In some optional embodiments of the present disclosure, the ratio of the thickness of the second shallow doped region to the intrinsic silicon layer and the tunneling oxide layer is 5-15:5-10:1.

[0014] In some optional embodiments of the present disclosure, the ratio of the thickness of the second shallowly doped region to the front passivation layer and the anti-reflection layer is 1:0.1-2:5-30.

[0015] In some optional embodiments of the present disclosure, the anti-reflection layer is a phosphorus-doped silicon layer.

[0016] More optionally, the ratio of the surface doping index of the anti-reflection layer to that of the second shallowly doped region is 0.2-11:1.

[0017] More optionally, the phosphorus-doped silicon layer is phosphorus-doped with at least one selected from silicon oxynitride, silicon nitride, silicon dioxide or silicon oxide.

[0018] In some optional embodiments of the present disclosure, the anti-reflection layer is composed of two or more layers, and along the outward direction from the front side of the silicon substrate, the phosphorus doping concentration of each anti-reflection layer is 1×1018-1×1021 cm-3, and the refractive index is 1.2-2.3, optionally 1.4-2.3, and the absolute value A of the difference in phosphorus doping concentration and the absolute value B of the difference in refractive index between adjacent anti-reflection layers satisfy a specific relationship: A / B>10.

[0019] In some optional embodiments of the present disclosure, one of the first doped silicon crystal layer and the second doped silicon layer is N-type and the other is P-type, and the second shallow doped region and the first doped silicon crystal layer have the same doping element.

[0020] Optionally in the present disclosure, the front side of the silicon substrate is a textured surface or a polished surface, and the back side is a polished surface.

[0021] Optionally in the present disclosure, the front passivation layer is an oxide layer.

[0022] In some optional embodiments of the present disclosure, the first semiconductor layer is spaced apart on the back side of the silicon substrate, and a second semiconductor opening region is formed at the spaced apart location for setting a portion of the second semiconductor layer; and a portion of the second semiconductor layer is also set in the outward direction of the first semiconductor layer, and a first semiconductor opening region is opened in the middle of the portion of the second semiconductor layer.

[0023] More optionally, the width of the first semiconductor opening region Wb is 100-300 μm, and the width of the second semiconductor opening region Wa is 300-700 μm.

[0024] In some optional embodiments of the present disclosure, the combined passivation back contact cell further comprises:

[0025] A conductive film layer is disposed outward from the first semiconductor layer and the second semiconductor layer; an isolation trench is formed on the conductive film layer, and the isolation trench is located between the first semiconductor opening region and the second semiconductor opening region;

[0026] Metal electrodes are respectively arranged in the first semiconductor opening region and the second semiconductor opening region.

[0027] In a second aspect, the present disclosure provides a method for preparing the combined passivation back contact cell according to the first aspect, comprising the following steps:

[0028] S1. Providing a silicon substrate with a textured or polished front surface and a first semiconductor layer disposed on the back surface;

[0029] S2. Doping the front and back sides of the silicon substrate obtained in S1 so as to form a second shallowly doped region on the front side of the silicon substrate and a first heavily doped region on the first doped silicon crystal layer in the first semiconductor layer on the back side; the doping conditions are such as to satisfy a desired ratio of the surface doping index of the first heavily doped region to the second shallowly doped region and a desired thickness of the second shallowly doped region;

[0030] S3, forming a second semiconductor layer on the back side of the silicon substrate obtained in S2;

[0031] S4. Depositing a front passivation layer and an anti-reflection layer on the front side of the silicon substrate obtained in S3.

[0032] In some optional embodiments of the present disclosure, the deposition process of the anti-reflection layer in S4 includes: depositing multiple layers of anti-reflection layers in sequence and co-doping them, and the deposition conditions and co-doping conditions are such as to meet the required doping concentration, refractive index and thickness of each anti-reflection layer.

[0033] In some optional embodiments of the present disclosure, the preparation method further includes: in S4, before depositing the front passivation layer, pretreatment is performed to repair dangling bonds, and the pretreatment process includes: under plasma conditions, introducing hydrogen, ammonia, or a mixture of one or two of them and an inert gas.

[0034] More optionally, the pretreatment conditions include: a pretreatment temperature of 300-500° C., and a pretreatment time of 0.5-1.5 h.

[0035] In some optional embodiments of the present disclosure, the process of providing a silicon substrate having a textured or polished front surface and a first semiconductor layer disposed on the back surface in S1 includes:

[0036] S101, depositing a first semiconductor layer on the back side of a silicon substrate with both the front and back sides polished;

[0037] S102, depositing a mask layer on the outward surface of the first semiconductor layer in S101;

[0038] S103 , texturing the front surface obtained in S102 , and removing the mask layer to expose the first semiconductor layer.

[0039] In some optional embodiments of the present disclosure, the process of forming a second semiconductor layer on the back side of the silicon substrate obtained in S2 in S3 includes:

[0040] S301, removing a portion of the first semiconductor layer on the back side of the silicon substrate obtained in S2 to form a second semiconductor opening region;

[0041] S302 , depositing a second semiconductor layer in the second semiconductor opening region obtained in S301 .

[0042] In some optional embodiments of the present disclosure, the preparation method further comprises:

[0043] S5, etching the middle portion of the second semiconductor layer on the outer surface of the first semiconductor layer on the back side of the silicon substrate obtained in S4 to expose the first semiconductor layer, thereby forming a first semiconductor opening region;

[0044] S6, depositing a conductive film layer on the back side of the silicon substrate obtained in S5;

[0045] S7, etching the conductive film layer on the back side of the silicon substrate obtained in S6 to form an isolation trench, wherein the isolation trench is located between the first semiconductor opening region and the second semiconductor opening region;

[0046] S8. Form metal electrodes respectively at the first semiconductor opening region and the second semiconductor opening region on the back side of the silicon substrate obtained in S7. Beneficial effects:

[0047] The present disclosure provides a front second lightly doped region and a back first heavily doped region with a specific doping index ratio and a specific thickness ratio in a combined passivation structure, and cooperates with a first semiconductor layer, a front passivation layer, and an anti-reflection layer to enable the front layer structure and the back layer structure of the silicon substrate to synergistically form a good and appropriate field passivation and chemical passivation effect. Thus, while ensuring a high current density (i.e., taking into account the comprehensive effect of a relatively good short-circuit current Isc, open-circuit voltage Voc, fill factor FF, and battery conversion efficiency), there is no need to provide an amorphous silicon or microcrystalline silicon layer, thereby avoiding the above-mentioned parasitic absorption and attenuation problems caused by the back polycrystalline and amorphous silicon or microcrystalline silicon layers, as well as the high cost of deposition equipment. Under the same conditions, if the ratio of the corresponding surface doping index is too large, the impurities will be excessive due to the high doping concentration, affecting the passivation effect; if the ratio of the corresponding surface doping index is too small, the field passivation effect will be weakened, resulting in less than expected passivation and a reduced passivation level. Under the same conditions, if the ratio of the thickness of the second shallow doped region to the tunnel oxide layer is too large, the front impurity doping will dominate and the back passivation will be unsatisfactory, resulting in serious carrier recombination at the interface and serious damage to the opening voltage and short-circuit current. If it is too small, the potential barrier formed by the tunnel oxide layer will be too large, which will prevent the carriers from tunneling out, affecting the conductive performance and thus affecting the FF.

[0048] The use of a specific front-side second shallowly doped region replaces the traditional front-side deposited amorphous silicon or microcrystalline layer, creating a field passivation effect that reduces parasitic absorption from the amorphous silicon or microcrystalline silicon film layer. The absence of an amorphous silicon or microcrystalline silicon film layer on the front side reduces the likelihood of PID or LID, increasing component stability. The front-side second shallowly doped region can be formed by diffusion, using only tube-type equipment, replacing plate-type amorphous silicon deposition equipment and reducing equipment investment. Furthermore, the first heavily doped region of the first semiconductor can be formed through secondary diffusion, further enhancing film conductivity and contributing to improved fill factor and conversion efficiency.

[0049] In the optional scheme disclosed herein, a multi-layer anti-reflection layer doped with phosphorus of different concentrations and different refractive indices that meets specific conditions is used on the front side, which is more conducive to enhancing the field passivation effect and improving the passivation level, while increasing the transmittance and being more conducive to improving the short-circuit current.

[0050] In the optional scheme disclosed herein, a front passivation layer is deposited after pre-treatment, so that defects at the interface of the second shallowly doped layer are repaired due to the intervention of pre-treatment hydrogen, thereby further improving the passivation level, reducing carrier recombination losses, and being more conducive to improving battery conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0052] FIG1 is a schematic cross-sectional view of a silicon wafer after double-sided polishing and cleaning in Example 1 of the present disclosure;

[0053] FIG2 is a schematic cross-sectional view of a first semiconductor layer formed sequentially on a silicon wafer surface in Example 1 of the present disclosure;

[0054] FIG3 is a schematic cross-sectional view of the embodiment 1 of the present disclosure after a mask layer is deposited on the back side of the silicon wafer;

[0055] FIG4 is a schematic cross-sectional view of forming a pyramid texture surface on the front side of a silicon wafer and removing a back side mask layer by texture cleaning in Example 1 of the present disclosure;

[0056] FIG5 is a schematic cross-sectional view of the embodiment 1 of the present disclosure after the second lightly doped region is formed on the front side and the first heavily doped region is formed on the back side;

[0057] FIG6 is a schematic cross-sectional view of the silicon wafer after a portion of the first semiconductor layer is removed from the back side of the silicon wafer in Example 1 of the present disclosure;

[0058] FIG7 is a schematic cross-sectional view of a second semiconductor layer deposited on the back side of a silicon wafer in Example 1 of the present disclosure;

[0059] FIG8 is a schematic cross-sectional view of the silicon wafer after front surface pretreatment and sequential deposition of a front passivation layer and an anti-reflection layer in Example 1 of the present disclosure;

[0060] FIG9 is a schematic cross-sectional view of forming a first semiconductor opening region on the back side of a silicon wafer in Example 1 of the present disclosure;

[0061] FIG10 is a schematic cross-sectional view of a conductive film layer deposited on the back side of a silicon wafer in Example 1 of the present disclosure;

[0062] 11 is a schematic cross-sectional view of forming an isolation trench between a first semiconductor opening region and a second semiconductor opening region on the back side of a silicon wafer in Example 1 of the present disclosure;

[0063] FIG12 is a schematic cross-sectional view of the embodiment 1 of the present disclosure after metal electrodes are formed in two semiconductor opening regions on the back side of the silicon wafer.

[0064] Explanation of the accompanying symbols: 1. Silicon wafer, 2. Tunneling oxide layer, 3. N-type doped polysilicon layer, 3.1. Original shallowly doped region, 3.2. First heavily doped region, 3.3. Second shallowly doped region, 4. Mask layer, 5. Intrinsic amorphous silicon layer, 6. Second doped silicon layer, 7.1. Front passivation layer, 7.2. First anti-reflection layer, 7.3. Second anti-reflection layer, 8. Conductive film layer, 9. Metal electrode. DETAILED DESCRIPTION

[0065] In the description of this disclosure, the terms "first" and "second" are configured for descriptive purposes only and should not be understood to indicate or imply relative importance or implicitly specify the number of the technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this disclosure, the meaning of "plurality" is two or more, unless otherwise explicitly and specifically defined.

[0066] In the present disclosure, unless otherwise expressly specified or limited, when a first feature is "above" or "below" a second feature, it may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Furthermore, when a first feature is "above," "above," or "above" a second feature, it may mean that the first feature is directly above or diagonally above the second feature, or simply means that the first feature is at a higher level than the second feature. When a first feature is "below," "below," or "below" a second feature, it may mean that the first feature is directly below or diagonally below the second feature, or simply means that the first feature is at a lower level than the second feature.

[0067] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Among them, the terms "optional" and "optional" all mean that they may be included or not (or may be present or not).

[0068] In the present disclosure, the direction away from the silicon substrate is referred to as outward, and the direction close to the silicon substrate is referred to as inward.

[0069] In the first aspect, the present disclosure provides a high current density combined passivation back contact cell, comprising a silicon substrate having a front and a back, a first semiconductor layer and a second semiconductor layer arranged on the back, and a front passivation layer and an anti-reflection layer arranged on the front, wherein the first semiconductor layer comprises a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer; a first heavily doped region is provided on a side of the first doped silicon crystal layer away from the silicon substrate, a second shallowly doped region is provided on the front side of the silicon substrate, the second shallowly doped region is in contact with the front passivation layer, and a ratio of the surface doping index of the first heavily doped region to the second shallowly doped region is 10-40:1, wherein the surface doping index is the ratio of the effective doping concentration of the corresponding doping layer to the thickness of the doping layer; and a ratio of the thickness of the second shallowly doped region to the tunneling oxide layer is 2-10:1.

[0070] Optionally, the ratio of the surface doping index of the first heavily doped region to the second lightly doped region is 10-30: 1. This option is more conducive to achieving a better comprehensive effect of Isc, Voc, FF and battery conversion efficiency.

[0071] Optionally, the ratio of the thickness of the second shallowly doped region to the tunnel oxide layer is 4-10: 1. In this option, a better comprehensive effect of Isc, Voc, FF and battery conversion efficiency is achieved.

[0072] The silicon substrate disclosed in the present disclosure may be a single crystal silicon wafer or a single cast silicon wafer, optionally a single crystal silicon wafer.

[0073] In some optional embodiments of the present disclosure, the side of the first doped silicon crystal layer closest to the silicon substrate is a primary shallowly doped region, and the ratio of the surface doping index of the primary shallowly doped region to the first heavily doped region and the second shallowly doped region is 0.3-2:10-40:1, or optionally 0.3-1.5:10-30:1. In this optional solution, the surface doping index ratio of the primary shallowly doped region to the first heavily doped region and the second shallowly doped region is appropriate, achieving both conductivity and passivation without compromising the passivation effect, thereby further improving overall battery conversion efficiency and other effects.

[0074] More optionally, the ratio of the surface doping index of the second doped silicon layer to the original shallow doped region is 5-30:1, more optionally 10-30:1. Under the optional solution disclosed herein, the surface doping index ratio of the original shallow doped region to the second doped silicon layer is appropriate, which can ensure the passivation effect and conductive performance, and is more conducive to improving Isc, Voc, FF and battery conversion efficiency.

[0075] In some optional embodiments of the present disclosure, the thickness of the first heavily doped region is 1 / 10-1 / 2, more preferably 1 / 5-1 / 2, of the thickness of the first doped silicon crystal layer. In these optional solutions of the present disclosure, this optimal thickness ratio can improve the overall conductivity of the film layer, further contributing to improvements in Isc, FF, and battery conversion efficiency.

[0076] In some optional embodiments of the present disclosure, the thickness ratio of the second shallowly doped region to the intrinsic silicon layer and tunneling oxide layer is 5-15:5-10:1. In this optional solution, the thickness ratio is appropriate, which can ensure the selectivity of carrier transport and the stability of passivation, and is more conducive to improving the overall comprehensive effects of Isc, Voc, FF, and battery conversion efficiency.

[0077] In the present disclosure, the doping concentration and thickness of the original shallow doping region, the first heavily doped region, and the second shallow doping region, as well as the thickness of the tunneling oxide layer and the intrinsic silicon layer, only need to satisfy the above-mentioned required proportional relationship. Those skilled in the art can select within the conventional range of the prior art based on the above-mentioned proportional relationship. For example, in some embodiments, the thickness of the tunneling oxide layer is 0.5-5nm, the thickness of the intrinsic silicon layer is 5-15nm, the thickness of the first doped silicon crystal layer is 50-300nm, the doping concentration of the original shallow doping region is 1×1019-1×1020cm-3, the doping concentration of the second shallow doping region is 1×1018-1×1019cm-3, and the thickness of the second shallow doping region is 1-15nm.

[0078] The intrinsic silicon layer may be an intrinsic amorphous silicon layer or a microcrystalline silicon layer. The first doped silicon crystal layer may be a doped polycrystalline silicon layer, and the second doped silicon layer may be a doped amorphous silicon layer or a microcrystalline silicon layer.

[0079] In some optional embodiments of the present disclosure, the thickness ratio of the second shallowly doped region to the front passivation layer and anti-reflection layer is 1:0.1-2:5-30, more preferably 1:0.2-1:5-20. It will be understood that if the anti-reflection layer is multi-layered, the thickness of the anti-reflection layer here refers to the total thickness. In this optional solution, the thickness ratio is optimal, balancing passivation effect and light transmission performance, and is more conducive to improving the overall comprehensive effect of Isc, Voc, FF, and cell conversion efficiency.

[0080] In some optional embodiments of the present disclosure, the anti-reflection layer is a phosphorus-doped silicon layer, which is more conducive to enhancing the field passivation effect and the optical effect of enhancing transmission such as the refractive index.

[0081] More optionally, the ratio of the surface doping index of the antireflection layer to the second shallowly doped region is 0.2-11:1. When the antireflection layer is multi-layered, each antireflection layer satisfies this ratio. In this optional solution, the doping of the antireflection layer enables the second shallowly doped region on the front side of the silicon substrate to be superimposed on the phosphorus-doped silicon layer, forming a negative fixed charge field with appropriately variable doping concentration, thereby enhancing the field passivation effect of the battery and further improving the overall passivation level, thereby improving Isc, Voc, FF, and battery conversion efficiency.

[0082] More optionally, the phosphorus-doped silicon layer is phosphorus-doped and selected from at least one of silicon oxynitride, silicon nitride, silicon dioxide or silicon oxide, and more optionally phosphorus-doped silicon oxynitride.

[0083] In some optional embodiments of the present disclosure, the anti-reflection layer comprises two or more layers, and the concentration, refractive index, and thickness of each anti-reflection layer are the same or different, and can be different.

[0084] More optionally, along the outward direction from the front surface of the silicon substrate, the phosphorus doping concentration of each antireflection layer is 1×1018-1×1021 cm-3, and the refractive index is 1.2-2.3, optionally 1.4-2.3. Furthermore, the absolute value of the difference in phosphorus doping concentration (A) and the absolute value of the difference in refractive index (B) between adjacent antireflection layers satisfy the specific relationship: A / B>10. This option achieves both passivation and enhanced photon transmission performance in the film, further improving the overall effects of Isc, Voc, FF, and cell conversion efficiency.

[0085] In the present disclosure, the specific values ​​of the doping concentration and refractive index of each anti-reflection layer only need to satisfy the above-mentioned required ranges and specific relationships.

[0086] In some optional embodiments of the present disclosure, one of the first doped silicon crystal layer and the second doped silicon layer is N-type and the other is P-type, and the second shallowly doped region and the first doped silicon crystal layer are doped with the same element. It is understood that when the silicon substrate is P-type, the first doped silicon crystal layer is P-type, the second doped silicon layer is N-type, the front side is the second shallowly doped region doped with boron, and the first heavily doped region of the first doped silicon crystal layer is heavily P-type doped. When the silicon substrate is N-type, the first doped silicon crystal layer is N-type, the second doped silicon layer is P-type, the front side is the second shallowly doped region doped with phosphorus, and the first heavily doped region of the first doped silicon crystal layer is heavily N-type doped.

[0087] Optionally in the present disclosure, the front side of the silicon substrate is a textured surface or a polished surface, and the back side is a polished surface.

[0088] Optionally in the present disclosure, the front passivation layer is an oxide layer, such as a silicon dioxide layer.

[0089] In some optional embodiments of the present disclosure, the first semiconductor layer is spaced apart on the back side of the silicon substrate, and a second semiconductor opening region is formed at the spaced apart location for setting a portion of the second semiconductor layer; and a portion of the second semiconductor layer is also set in the outward direction of the first semiconductor layer, and a first semiconductor opening region is opened in the middle of the portion of the second semiconductor layer.

[0090] More optionally, the width of the first semiconductor opening region Wb is 100-300 μm, and the width of the second semiconductor opening region Wa is 300-700 μm.

[0091] In some optional embodiments of the present disclosure, the combined passivated back contact cell further includes: a conductive film layer disposed outwardly of the first semiconductor layer and the second semiconductor layer; and an isolation trench is formed on the conductive film layer, the isolation trench being located between the first semiconductor opening region and the second semiconductor opening region;

[0092] Metal electrodes are respectively arranged in the first semiconductor opening region and the second semiconductor opening region.

[0093] The isolation trench is configured to isolate two semiconductor layers to reduce short circuit or leakage. More optionally, the width Wg of the isolation trench is 50-200 μm.

[0094] In the present disclosure, a wide range of options is provided for the conductive film layer, metal electrode, and isolation trench. The conductive film layer may be a transparent conductive film or a composite film layer composed of a transparent conductive film and a metal conductive film. The transparent conductive film may be indium oxide doped with zinc, tin, tungsten, titanium, or silicon, or zinc oxide doped with aluminum, boron, or gallium. The metal conductive film may be at least one of aluminum, copper, silver, a nickel alloy, and a titanium alloy. Optionally, the conductive film layer may be a composite film layer of tin-doped indium oxide, copper, or a nickel-copper alloy. More optionally, the sheet resistance of the conductive film layer may be less than 0.2Ω / □.

[0095] In a second aspect, the present disclosure provides a method for preparing the combined passivation back contact cell according to the first aspect, comprising the following steps:

[0096] S1. Providing a silicon substrate with a textured or polished front surface and a first semiconductor layer disposed on the back surface;

[0097] S2. Doping the front and back sides of the silicon substrate obtained in S1 so as to form a second shallowly doped region on the front side of the silicon substrate and a first heavily doped region on the first doped silicon crystal layer in the first semiconductor layer on the back side; the doping conditions are such as to satisfy a desired ratio of the surface doping index of the first heavily doped region to the second shallowly doped region and a desired thickness of the second shallowly doped region;

[0098] S3, forming a second semiconductor layer on the back side of the silicon substrate obtained in S2;

[0099] S4. Depositing a front passivation layer and an anti-reflection layer on the front side of the silicon substrate obtained in S3.

[0100] The doping conditions described in S2 only need to meet the required doping concentration and thickness of each layer. Those skilled in the art can select within the scope of the existing technology. Generally, the doping described in S2 is doping by diffusing phosphorus oxychloride. For example, when performing phosphorus diffusion doping, the doping process includes: first entering a first stage of pre-deposition, in which at least one of phosphorus oxychloride, nitrogen, and oxygen is introduced to form a phosphorus element and a PSG layer through a chemical reaction. The reaction temperature of the first stage is 750-850°C, and the reaction time is 5-180 minutes; then entering a second stage of temperature-increasing phosphorus diffusion. The second stage is carried out in an oxygen atmosphere. While the temperature is increased to promote phosphorus diffusion, an undoped oxide layer is formed between the PSG layer and the tunneling oxide layer. The temperature of the second stage is 800-900°C, and the reaction time is 10-300 minutes. The phosphorus diffusion can be carried out in a high-temperature phosphorus diffusion furnace.

[0101] Optionally, in the present disclosure, S4 further includes: doping the anti-reflection layer, for example, phosphorus diffusion doping.

[0102] In some optional embodiments of the present disclosure, the deposition process of the anti-reflection layer in S4 includes: depositing multiple layers of anti-reflection layers in sequence and co-doping, and the deposition conditions and co-doping conditions are such that the required doping concentration, refractive index and thickness of each anti-reflection layer are satisfied. Generally, the doping of the anti-reflection layer in S4 is to introduce a gas such as phosphine during the deposition of the anti-reflection layer to perform co-reaction doping (or co-doping), generally using a plasma doping method. For example, the formation process of the anti-reflection layer includes: under plasma conditions, introducing a reaction gas including silane, nitrogen, ammonia and phosphine to perform in-situ doping to form a film, adjusting the refractive index of the corresponding film layer by controlling the ratio of ammonia to silane, and controlling the doping amount of the corresponding film layer by adjusting the ratio of phosphine to silane. It is a prior art to control each parameter by adjusting the ratio of the reaction gas. Those skilled in the art can select and adjust according to the required parameters, and will not be described in detail here.

[0103] In some optional embodiments of the present disclosure, the preparation method further includes: in S4, before depositing the front passivation layer, pre-treatment is performed to repair dangling bonds.

[0104] More optionally, the pre-treatment process includes: introducing hydrogen, ammonia, or a mixture of one or two of them with an inert gas under plasma conditions. That is, hydrogen, ammonia, a mixture of hydrogen and an inert gas, or a mixture of ammonia and an inert gas can be introduced. In the optional pre-treatment scheme disclosed herein, under plasma conditions, hydrogen or ammonia gas molecules decompose H atoms or ions to repair dangling bonds on the silicon surface, which is beneficial to improving the passivation level, thereby being more beneficial to improving the overall comprehensive effect of Isc, Voc, FF and battery conversion efficiency.

[0105] After the above-mentioned pre-treatment, the present invention can enhance the passivation level, which is beneficial to improving the Voc of the battery. Since some dangling bonds are repaired, the front passivation layer (oxide layer) can be thinner, so that the thickness ratio of the second shallowly doped region to the front passivation layer and the anti-reflection layer is 1:0.1-1:5-20.

[0106] More optionally, the pretreatment conditions include: a pretreatment temperature of 300-500° C., and a pretreatment time of 0.5-1.5 h.

[0107] In some optional embodiments of the present disclosure, the process of providing a silicon substrate having a textured or polished front surface and a first semiconductor layer disposed on the back surface in S1 includes:

[0108] S101, depositing a first semiconductor layer on the back side of a silicon substrate with both the front and back sides polished;

[0109] S102, depositing a mask layer on the outward surface of the first semiconductor layer in S101;

[0110] S103, texturing the front surface obtained in S102, and removing the mask layer to expose the first semiconductor layer. The texturing forms a textured surface with an anti-reflection effect on the front surface of the silicon substrate.

[0111] The mask layer disclosed herein is configured to protect the first semiconductor layer from corrosion in a strong acid or alkali solution used in texturing. The mask layer may be made of at least one of silicon nitride, silicon oxynitride, silicon carbide, and an organic protective ink.

[0112] In some optional embodiments of the present disclosure, the process of forming a second semiconductor layer on the back side of the silicon substrate obtained in S2 in S3 includes:

[0113] S301, removing a portion of the first semiconductor layer on the back side of the silicon substrate obtained in S2 to form a second semiconductor opening region;

[0114] S302 , depositing a second semiconductor layer in the second semiconductor opening region obtained in S301 .

[0115] In some optional embodiments of the present disclosure, the preparation method further comprises:

[0116] S5, etching the middle portion of the second semiconductor layer on the outer surface of the first semiconductor layer on the back side of the silicon substrate obtained in S4 to expose the first semiconductor layer, thereby forming a first semiconductor opening region;

[0117] S6, depositing a conductive film layer on the back side of the silicon substrate obtained in S5;

[0118] S7, etching the conductive film layer on the back side of the silicon substrate obtained in S6 to form an isolation trench, wherein the isolation trench is located between the first semiconductor opening region and the second semiconductor opening region;

[0119] S8. Form metal electrodes respectively at the first semiconductor opening region and the second semiconductor opening region on the back side of the silicon substrate obtained in S7.

[0120] The following describes embodiments of the present disclosure in detail, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only configured to explain the present disclosure and are not to be construed as limiting the present disclosure.

[0121] Example 1

[0122] A high current density combined passivation back contact battery is prepared by the following method:

[0123] S1. Providing a silicon substrate with a textured surface on the front side and a first semiconductor layer on the back side:

[0124] S100, as shown in FIG1 , providing a double-sided polished silicon wafer 1, which is a single crystal silicon wafer;

[0125] S101. As shown in FIG2 , a first semiconductor layer is deposited on the back side of the silicon wafer 1. The first semiconductor layer comprises a tunneling oxide layer 2 and an N-type doped polysilicon layer 3. The tunneling oxide layer 2 has a thickness of 1 nm, the N-type doped polysilicon layer 3 has a thickness of 220 nm, and the doping concentration is 1×10 20 cm -3 .

[0126] S102, as shown in FIG3, continuing to deposit a mask layer 4 on the first semiconductor layer. The mask layer is silicon nitride, and its purpose is to protect the first semiconductor layer from being corroded by the strong acid or alkali solution.

[0127] S103, as shown in FIG4, the silicon wafer 1 obtained in the above S102 is textured to form a textured surface with an anti-reflection effect on the front side of the silicon wafer 1, and the mask layer on the back side (first semiconductor layer) is removed to expose the first semiconductor layer.

[0128] S2. As shown in FIG5 , phosphorus diffusion doping is performed on both sides of the silicon wafer 1, forming a second shallowly doped region 3.3 on the front side of the silicon wafer 1. A portion of the N-type doped polysilicon layer 3 on the back side of the silicon wafer 1 is heavily doped a second time to form a first heavily doped region 3.2, with the remaining portion serving as the original shallowly doped region 3.1. The phosphorus diffusion doping process comprises: first, a pre-deposition first stage, in which phosphorus oxychloride, nitrogen, and oxygen are introduced to chemically react to form a phosphorus element and a PSG layer. The reaction temperature for the first stage is 750°C, and the reaction time is 15 minutes. Then, a second stage of phosphorus diffusion is performed at an elevated temperature. The second stage is conducted in an oxygen atmosphere. While the temperature is elevated to promote phosphorus diffusion, an undoped oxide layer is formed between the PSG layer and the tunneling oxide layer. The temperature for the second stage is 900°C, and the reaction time is 35 minutes. The phosphorus diffusion doping process results in a thickness of 10 nm for the second shallowly doped region 3.3, with a phosphorus doping concentration of 1×1019 cm-3. The doping concentration of the N-type doped polysilicon layer 3 is increased from 1×1020 cm-3 in the original shallowly doped region 3.1 to 1×1021 cm-3 in the first heavily doped region 3.2. The depth of the first heavily doped region 3.2 is 1 / 4 the thickness of the original N-type doped polysilicon layer 3. The ratio of the surface doping index of the original shallowly doped region 3.1, the first heavily doped region 3.2, and the second shallowly doped region 3.3 is 0.6:18:1, where the surface doping index is the ratio of the effective doping concentration of the corresponding doped layer to the thickness of the doped layer.

[0129] S3, forming a second semiconductor layer on the back side of the silicon substrate obtained in S2:

[0130] S301, as shown in FIG6, forming a second semiconductor opening region on the back surface, the width of the second semiconductor layer opening region is Wa, and the width Wa is 500 μm;

[0131] S302. As shown in FIG7 , a second semiconductor layer is deposited in the second semiconductor opening region. The second semiconductor layer comprises an intrinsic amorphous silicon layer 5 and a second doped silicon layer 6, which is an amorphous silicon P layer. The thickness of the second doped silicon layer 6 is 12 nm, and the ratio of the doping index of the second doped silicon layer 6 to that of the original shallowly doped region 3.1 is 12.7:1. The thickness ratio of the second shallowly doped region 3.3 to the intrinsic amorphous silicon layer 5 and the tunneling oxide layer 2 is 10:8:1.

[0132] S4. Depositing a front passivation layer and an anti-reflection layer on the front side of the silicon substrate obtained in S3:

[0133] As shown in FIG8 , the front surface is pretreated and a front passivation layer 7.1 (oxide layer) and two anti-reflection layers are deposited. The anti-reflection layers are then co-doped with phosphorus diffusion to form a first anti-reflection layer 7.2 and a second anti-reflection layer 7.3 of different thicknesses. The pretreatment is performed by introducing a mixture of hydrogen and inert argon gas under plasma conditions for 0.5 h. The anti-reflection layer formation process includes: in-situ doping and film formation by introducing reaction gases including silane, nitrogen, ammonia, and phosphine under plasma conditions, adjusting the refractive index of the film by controlling the ratio of ammonia to silane, and controlling the doping level of the film by adjusting the ratio of phosphine to silane. The anti-reflection layer is ultimately formed into two phosphorus-doped silicon oxynitride layers with different concentrations and refractive indices. Specifically, the phosphorus doping concentrations on the front side from the outside to the inside are 1×1021 cm-3 and 1×1020 cm-3, respectively, and the refractive indices from the outside to the inside are 1.46 and 2.0, respectively. The thickness ratio of the second shallowly doped region 3.3 to the front passivation layer 7.1 and the total thickness of the two anti-reflection layers is 1:0.1:24. The thickness ratio of the first anti-reflection layer 7.2 to the second anti-reflection layer 7.3 is 1:1.45.

[0134] S5. As shown in FIG9 , the second semiconductor layer on the back side of the first semiconductor layer is removed to expose the first semiconductor layer, thereby forming a first semiconductor opening region Wb with a width of 200 μm.

[0135] S6. As shown in FIG10 , a conductive film layer 8 is deposited on the back of the battery. The conductive film layer 8 is a composite film layer of tin-doped indium oxide, metallic copper, and nickel-copper alloy, with a square resistance of 0.1Ω / □.

[0136] S7. As shown in FIG11 , a gap isolation trench with a width of Wg is formed between the first semiconductor opening region and the second semiconductor opening region. The width of Wg is 150 μm, mainly for isolating the two semiconductor layers to reduce short circuit or leakage.

[0137] S8. As shown in FIG12 , gate lines are printed on the back of the battery, and metal electrodes 9 are formed at the first semiconductor opening region and the second semiconductor opening region of the silicon wafer 1 .

[0138] The short-circuit current Isc, open-circuit voltage Voc, fill factor FF, and battery conversion efficiency of the obtained combined passivated back contact battery were tested, and the results are shown in Table 1.

[0139] Example 2

[0140] The method of Example 1 is referred to, except that in S4, no pre-treatment is performed on the front surface, but the front passivation layer (oxide layer) and two anti-reflection layers are directly deposited.

[0141] The corresponding tests were carried out and the results are shown in Table 1.

[0142] Example 3

[0143] The method of Example 1 is referred to, except that in S4, only a first anti-reflection layer is deposited on the front surface, and the second anti-reflection layer is not deposited.

[0144] The corresponding tests were carried out and the results are shown in Table 1.

[0145] Example 4

[0146] The method of Example 1 is referred to, except that in S2, the doping concentration of the first heavily doped region is adjusted so that the ratio of the surface doping index of the first heavily doped region to that of the second lightly doped region is 16:1, and the conditions for controlling phosphorus diffusion doping are correspondingly to increase the diffusion gas pressure by 5% and extend the diffusion time by 8%. Under the same diffusion conditions, the diffusion rate on polysilicon is 1.5 times that on bulk silicon (silicon substrate).

[0147] The corresponding tests were carried out and the results are shown in Table 1.

[0148] Example 5

[0149] The method of Example 1 is referred to, except that in S2, the doping concentration of the first heavily doped region is adjusted so that the ratio of the surface doping index of the first heavily doped region to that of the second lightly doped region is 35:1, and the conditions for controlling phosphorus diffusion doping are correspondingly controlled by reducing the diffusion gas pressure by 20% and the diffusion temperature by 10%.

[0150] The corresponding tests were carried out and the results are shown in Table 1.

[0151] Example 6

[0152] The method of Example 1 is referred to, except that in S101 the thickness of the tunnel oxide layer is adjusted so that the ratio of the thickness of the second shallowly doped region to the thickness of the tunnel oxide layer is 2.2:1.

[0153] The corresponding tests were carried out and the results are shown in Table 1.

[0154] Example 7

[0155] The method of Example 1 is referred to, except that in S101, the original doping concentration of the N-type doped polysilicon layer is adjusted so that the ratio of the surface doping index of the original shallow doping region and the first heavily doped region is 0.1:1, and the phosphorus diffusion is adjusted accordingly to obtain the first heavily doped region and the second shallow doped region as in Example 1.

[0156] The corresponding tests were carried out and the results are shown in Table 1.

[0157] Example 8

[0158] The method of Example 1 is referred to, except that in S101, the thickness of the original lightly doped region in the N-type doped polysilicon layer is adjusted so that the thickness of the first heavily doped region is 1 / 6 of the thickness of the N-type doped polysilicon layer, and the thickness of the first heavily doped region remains unchanged.

[0159] The corresponding tests were carried out and the results are shown in Table 1.

[0160] Example 9

[0161] The method of Example 1 is referred to, except that in S302 , the doping concentration of the second doped silicon layer is adjusted so that the ratio of the surface doping index of the second doped silicon layer to that of the original shallowly doped region is 7.5:1.

[0162] The corresponding tests were carried out and the results are shown in Table 1.

[0163] Example 10

[0164] The method of Example 1 is referred to, except that in S4, the total thickness of the two anti-reflection layers is adjusted (the ratio of the thickness of the first anti-reflection layer 7.2 to the second anti-reflection layer 7.3 is 1:2) so that the ratio of the thickness of the second shallowly doped region to the total thickness of the anti-reflection layer is 1:30.

[0165] The corresponding tests were carried out and the results are shown in Table 1.

[0166] Example 11

[0167] The method of Example 1 was followed, except that in S4, the doping concentration of the anti-reflection layer was adjusted so that the doping concentration and refractive index of each anti-reflection layer satisfied the following conditions: the doping concentrations were 1×1018 cm-3 and 1×1019 cm-3, respectively, and the refractive indices were 2.3 and 1.2, respectively; and the absolute value A of the difference in phosphorus doping concentration and the absolute value B of the difference in refractive index of adjacent anti-reflection layers were such that A / B=9.09.

[0168] The corresponding tests were carried out and the results are shown in Table 1.

[0169] Comparative Example 1

[0170] The method of Example 1 is referred to, except that in S2, no second shallowly doped region is provided on the front side, and the N-type doped polysilicon layer on the back side is not heavily doped for the second time to form the first heavily doped region. Instead, a conventional amorphous silicon passivation layer and a silicon nitride anti-reflection layer are used on the front side.

[0171] The corresponding tests were carried out and the results are shown in Table 1.

[0172] Comparative Example 2

[0173] The method of Example 1 is referred to, except that in S2, the silicon wafer is doped with phosphorus diffusion to form a second shallowly doped region only on the front side of the silicon wafer, and the N-type doped polysilicon layer on the back side of the silicon wafer is not heavily doped for the second time to form a first heavily doped region.

[0174] The corresponding tests were carried out and the results are shown in Table 1.

[0175] Comparative Example 3

[0176] The method of Example 1 is referred to, except that in S2, the doping concentration of the first heavily doped region is adjusted so that the ratio of the surface doping index of the first heavily doped region to that of the second shallowly doped region is 45:1, and the second shallowly doped region remains basically unchanged. Accordingly, the conditions for controlling phosphorus diffusion doping are to increase the diffusion concentration of phosphorus oxychloride by 25% and the diffusion temperature by 20-30%, so that the phosphorus doping amount in the first heavily doped region is much greater than that in the second shallowly doped region.

[0177] The corresponding tests were carried out and the results are shown in Table 1.

[0178] Comparative Example 4

[0179] The method of Example 1 is referred to, except that in S2, the doping concentration of the first heavily doped region is adjusted so that the ratio of the surface doping index of the first heavily doped region to that of the second lightly doped region is 7:1, and the conditions for controlling phosphorus diffusion doping are correspondingly controlled by lowering the diffusion temperature and shortening the diffusion time, so that the doping concentration of the first heavily doped region is reduced.

[0180] The corresponding tests were carried out and the results are shown in Table 1.

[0181] Comparative Example 5

[0182] The method of Example 1 is referred to, except that in S101 the thickness of the tunnel oxide layer 2 is adjusted so that the ratio of the thickness of the second shallow doped region to the thickness of the tunnel oxide layer is 13:1.

[0183] The corresponding tests were carried out and the results are shown in Table 1.

[0184] Table 1

[0185] It can be seen from the above embodiments and comparative examples and Table 1 that, compared with the comparative examples, the embodiments of the present disclosure can achieve better comprehensive effects of Isc, Voc, FF and battery conversion efficiency.

[0186] Optionally, it can be seen from Examples 1 and 2 that the use of an additional pre-treatment solution can be more conducive to obtaining a better passivation effect, thereby improving Voc and battery conversion efficiency. It can be seen from Examples 1 and 3, and Examples 10-11 that the use of the anti-reflection layer solution under the optional specific structural parameters of the present disclosure can be more conducive to reducing the reflectivity of the front side and improving the comprehensive transmittance of photons in the film layer, thereby obtaining a high current density and improving Isc, Voc, FF and battery conversion efficiency. It can be seen from Examples 1 and 4-9 that the use of the layer structure solution under the optional specific parameters of the present disclosure can be compatible with the passivation effect while improving the conductivity and light transmittance of the battery, which is more conducive to improving the overall comprehensive effect of the battery's Isc, Voc, FF and battery conversion efficiency.

[0187] The above describes in detail the optional embodiments of the present disclosure, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure can be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as the contents disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability

[0188] The high current density combined passivation back contact cell disclosed in the present invention provides a front second shallowly doped region and a back first heavily doped region with a specific surface doping index ratio and a specific thickness ratio in the combined passivation structure, and cooperates with the first semiconductor layer, the front passivation layer and the anti-reflection layer to enable the front layer structure and the back layer structure of the silicon substrate to cooperate to form a good and appropriate field passivation and chemical passivation effect, so that while ensuring a high current density (that is, taking into account the comprehensive effects of better short-circuit current Isc, open-circuit voltage Voc, fill factor FF, and cell conversion efficiency), there is no need to provide an amorphous silicon or microcrystalline silicon layer, thereby avoiding the above-mentioned parasitic absorption and attenuation problems caused by the back polycrystalline and amorphous silicon or microcrystalline silicon layers and the high cost of deposition equipment.

Claims

1. A high current density joint passivation back contact cell, comprising a silicon substrate having a front side and a back side, a first semiconductor layer and a second semiconductor layer arranged on the back side, and a front passivation layer and an anti-reflection layer arranged on the front side, wherein the first semiconductor layer comprises a tunneling oxide layer and a first doped silicon crystal layer, and the second semiconductor layer comprises an intrinsic silicon layer and a second doped silicon layer; characterized in that: A first heavily doped region is provided on a side of the first doped silicon crystal layer away from the silicon substrate, a second lightly doped region is provided on the front side of the silicon substrate, the second lightly doped region is in contact with the front passivation layer, and a ratio of the surface doping index of the first heavily doped region to the second lightly doped region is 10-40:1, wherein the surface doping index is a ratio of the effective doping concentration of the corresponding doping layer to the thickness of the doping layer; and a ratio of the thickness of the second lightly doped region to the tunneling oxide layer is 2-10:

1.

2. The combined passivation back contact cell according to claim 1, characterized in that: The side of the first doped silicon crystal layer close to the silicon substrate is an original lightly doped region, and the ratio of the surface doping index of the original lightly doped region to the first heavily doped region and the second lightly doped region is 0.3-2:10-40:

1.

3. The combined passivation back contact cell according to claim 2, characterized in that: The ratio of the surface doping index of the second doped silicon layer to that of the original lightly doped region is 5-30:1, and / or the thickness of the first heavily doped region is 1 / 10-1 / 2 of the thickness of the first doped silicon crystal layer.

4. The combined passivated back contact cell according to any one of claims 1 to 3, characterized in that: The thickness ratio of the second shallowly doped region to the intrinsic silicon layer and the tunneling oxide layer is 5-15:5-10:1, and / or the thickness ratio of the second shallowly doped region to the front passivation layer and the anti-reflection layer is 1:0.1-2:5-30.

5. The combined passivated back contact cell according to any one of claims 1 to 4, characterized in that: The anti-reflection layer is a phosphorus-doped silicon layer.

6. The combined passivation back contact cell according to claim 5, characterized in that: The ratio of the surface doping index of the anti-reflection layer to that of the second shallowly doped region is 0.2-11:

1.

7. The combined passivation back contact cell according to claim 5, characterized in that: The phosphorus-doped silicon layer is phosphorus-doped and is selected from at least one of silicon oxynitride, silicon nitride, silicon dioxide or silicon oxide.

8. The combined passivation back contact cell according to claim 5, characterized in that: The anti-reflection layer has more than two layers, and along the direction from the front side of the silicon substrate to the outside, the phosphorus doping concentration of each anti-reflection layer is 1×1018-1×1021cm-3, and the refractive index is 1.2-2.3, and the absolute value A of the difference in phosphorus doping concentration and the absolute value B of the difference in refractive index between adjacent anti-reflection layers satisfy a specific relationship: A / B>10.

9. The combined passivation back contact cell according to claim 5, characterized in that: One of the first doped silicon crystal layer and the second doped silicon layer is N-type, and the other is P-type, and the second shallowly doped region and the first doped silicon crystal layer have the same doping element.

10. The combined passivation back contact cell according to any one of claims 1 to 9, characterized in that: The front side of the silicon substrate is a textured surface or a polished surface, and the back side is a polished surface; and / or the front side passivation layer is an oxide layer.

11. The combined passivated back contact cell according to any one of claims 1 to 10, characterized in that: The first semiconductor layer is arranged at intervals on the back side of the silicon substrate, and a second semiconductor opening area is formed at the intervals to provide a portion of the second semiconductor layer; and a portion of the second semiconductor layer is also arranged in the outward direction of the first semiconductor layer, and a first semiconductor opening area is opened in the middle of the portion of the second semiconductor layer; wherein the width of the first semiconductor opening area Wb is 100-300 μm, and the width of the second semiconductor opening area Wa is 300-700 μm; The combined passivation back contact cell also includes: A conductive film layer is disposed in the outward direction of the first semiconductor layer and the second semiconductor layer; and an isolation groove is provided on the conductive film layer, and the isolation groove is located between the first semiconductor opening area and the second semiconductor opening area; Metal electrodes are respectively arranged in the first semiconductor opening region and the second semiconductor opening region.

12. A method for preparing a combined passivation back contact cell according to any one of claims 1 to 11, characterized in that: The following steps are involved: S1, providing a silicon substrate with a textured surface or a polished surface on the front side and a first semiconductor layer on the back side; S2, doping the front and back sides of the silicon substrate obtained in S1, so that a second shallowly doped region is formed on the front side of the silicon substrate, and a first heavily doped region is formed on the first doped silicon crystal layer in the first semiconductor layer on the back side; the doping conditions are such that the required ratio of the surface doping index of the first heavily doped region to the second shallowly doped region and the thickness of the second shallowly doped region are satisfied; S3, forming a second semiconductor layer on the back side of the silicon substrate obtained in S2; S4. Depositing a front passivation layer and an anti-reflection layer on the front side of the silicon substrate obtained in S3.

13. The preparation method according to claim 12, characterized in that The deposition process of the anti-reflection layer in S4 includes: depositing multiple layers of anti-reflection layers in sequence and co-doping them, and the deposition conditions and co-doping conditions are such that the required doping concentration, refractive index and thickness of each anti-reflection layer are met; and / or The preparation method also includes: in S4, before depositing the front passivation layer, pretreatment is performed to repair dangling bonds, and the pretreatment process includes: under plasma conditions, hydrogen, ammonia or a mixture of one or two of them and an inert gas is introduced; the pretreatment conditions include: a pretreatment temperature of 300-500°C and a pretreatment time of 0.5-1.5h.

14. The preparation method according to claim 12 or 13, characterized in that The process of providing a silicon substrate with a textured surface or a polished surface on the front side and a first semiconductor layer on the back side in S1 includes: S101, depositing a first semiconductor layer on the back side of a silicon substrate whose front side and back side are polished; S102, depositing a mask layer on the outward surface of the first semiconductor layer in S101; S103, texturing the front surface obtained in S102, and removing the mask layer to expose the first semiconductor layer; And / or, the process of forming a second semiconductor layer on the back side of the silicon substrate obtained in S2 in S3 includes: S301, removing a portion of the first semiconductor layer on the back side of the silicon substrate obtained in S2 to form a second semiconductor opening region; S302 , depositing a second semiconductor layer in the second semiconductor opening region obtained in S301 .

15. The preparation method according to claim 12 or 13, characterized in that The preparation method further comprises: S5, etching the middle portion of the second semiconductor layer on the outer surface of the first semiconductor layer on the back side of the silicon substrate obtained in S4 to expose the first semiconductor layer, thereby forming a first semiconductor opening region; S6, depositing a conductive film layer on the back side of the silicon substrate obtained in S5; S7, etching the conductive film layer on the back side of the silicon substrate obtained in S6 to form an isolation groove, wherein the isolation groove is located between the first semiconductor opening region and the second semiconductor opening region; S8. Form metal electrodes respectively at the first semiconductor opening region and the second semiconductor opening region on the back side of the silicon substrate obtained in S7.

Citation Information

Patent Citations

  • Back-surface tunnel oxidation and passivation inter-digitated type back-to-back contact battery production method

    CN106784069A

  • Combined passivation back contact battery and preparation method thereof

    CN115207137A

  • Back contact solar cell and preparation method thereof

    CN115513308A

  • Double-sided tunneling silicon oxide passivated back contact solar cell and preparation method thereof

    CN115621333A

  • Back contact battery, manufacturing method thereof and photovoltaic module

    CN115832065A

Cited By

  • Combined passivation back contact battery and post-texturing preparation method thereof

    CN119451282A

  • Back contact battery and photovoltaic module

    CN119677225A

  • Back contact battery, non-etching manufacturing method thereof and battery assembly

    CN119744024A

  • Back contact battery capable of resisting hot spot effect and preparation method of back contact battery

    CN120379388A

  • Back contact photovoltaic cell with high-concentration co-doped region as well as preparation method and application of back contact photovoltaic cell

    CN121262889A