Integrated infusion technological process for pultruded spar cap of wind turbine blade
By arranging flow-blocking partitions and flow-blocking tapes on the pultruded main beams of wind turbine blades, independent infusion of each pultruded plate layer is achieved, which solves the problem of interlayer defects caused by uneven resin flow speed and improves the stability of wind turbine blades. and fatigue performance of the main beam.
Patent Information
- Application Number
- PCT/CN2024/087495
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
During the infusion process of the existing pultruded main beam of wind turbine blades, the inter-layer glass fiber cloth surrounding defects caused by uneven resin flow speeds lead to a high risk of inter-layer failure of the main beam and affect the stability of the blade.
Set up a flow-blocking partition on the continuous felt under the main beam, and design a flow-blocking tape and main beam glue injection pipeline on the flow guide net of each pultruded plate layer to ensure that each pultruded plate layer is poured independently and the resin passes through during infusion. The synergistic effect of the flow-blocking tape and the glue injection pipeline slows down the flow speed and prevents the resin from flowing through the butt joints.
The infusion defects between the layers of the pultruded main beam are completely eliminated, and the interlayer fatigue performance of the main beam and the operating stability of the overall blade are improved.
Smart Images

Figure CN2024087495_17102024_PF_FP_ABST
Abstract
Description
A wind turbine blade pultrusion main beam integrated casting process Technical Field
[0001] The present invention belongs to the technical field of non-metallic composite material processing and forming, and in particular relates to a wind turbine blade pultrusion main beam integral pouring process method. Background Art
[0002] With the trend toward larger wind turbine blades, to reduce the overall weight of wind turbine blades and improve the stability of the main beam's mechanical properties, the industry's current fiberglass main beams are assembled using a stacked pultruded sheet process, which is then infused with the blade shell layer. Existing pultruded main beams are generally assembled using uniaxial pultruded sheet metal with a thickness of 5mm and a width of 100-200mm. Two to six pultruded sheets are spliced across the width of the beam, and eight to 20 sheets are stacked across the thickness to form the wind turbine blade main beam. To ensure interlaminar adhesion between the pultruded sheet layers, 200g / ㎡ of biaxial fiberglass cloth is placed between each layer.
[0003] The current pouring scheme for the pultruded main beam area of wind turbine blades in the industry is shown in Figure 1. When laying the blade shell, the main beam lower cloth layer 1, the main beam lower continuous felt 2, the pultruded main beam 3, the shell core material 4, the guide net 5, the guide net partition 6, the glue injection pipeline 7, and the VAP vacuum bag 8 are laid on the main mold in sequence. After laying is completed, vacuum is established. When pouring the pultruded main beam area, the resin is first injected from the glue injection pipe 7, and infiltrates along the guide net 6 on the upper surface of the pultruded main beam 3 toward the front edge, and along the continuous felt 2 under the main beam on the lower surface of the pultruded main beam 3 toward the front edge. Between the pultruded plate layers of the pultruded main beam 3, the resin infiltrates the fiberglass cloth between the pultruded plate layers from the gap 10 between the pultruded main beam 3 and the shell core material 4. Since the flow rate of the resin on the continuous felt 2 and the guide net 5 is much greater than the flow rate on the fiberglass cloth between the pultruded plate layers, the resin on the upper and lower surfaces of the pultruded main beam 3 will first flow into the pultruded plate joint 9. At this time, the fiberglass cloth on the side of the joint 9 facing the trailing edge of the blade has not been completely infiltrated with the resin. The resin at the joint 9 surrounds the fiberglass cloth between the pultruded plate layers A, B...N at the trailing edge, forming a pouring defect. There is currently no repair method for this defect, and the impact on the blade has not been verified by the wind farm. The risk of failure between the layers of the pultruded main beam is relatively high, which reduces the stability of the wind turbine blade operation. Summary of the Invention
[0004] In order to solve the defects caused by the surrounding glass fiber cloth infusion between the layers of the pultruded main beam, the present invention proposes an integrated infusion process method for the pultruded main beam of a wind turbine blade. By designing independent infusion schemes for each pultruded plate layer of the pultruded main beam, the defects of the glass fiber cloth infusion between the layers of the pultruded main beam of the wind turbine blade are eliminated, the risk of failure between the layers of the pultruded main beam is reduced, and the operating stability of the wind turbine blade is improved.
[0005] The objective of the present invention is achieved by the following technical solution. A method for integrally casting a pultruded main beam for a wind turbine blade is proposed according to the present invention, comprising the following steps: sequentially laying a main beam lower fabric layer, a main beam lower continuous felt, a pultruded main beam, a shell core material, a guide net, and a glue injection pipeline on a mold according to existing blade laying processes; the pultruded main beam comprises a pultruded plate layer formed by stacking multiple pultruded plates and glass fiber cloth between the layers; and further comprising the following steps:
[0006] A flow-blocking partition is made on the continuous felt under the main beam. The flow-blocking partition is located at the joint between the first and second pultruded plate layers at the rear edge of the pultruded main beam.
[0007] Flow-blocking tapes and main beam glue injection pipelines are installed on the guide net corresponding to the pultruded main beam area. Flow-blocking tapes are installed on the guide net above each pultruded plate layer; main beam glue injection pipelines are installed between every two flow-blocking tapes;
[0008] Before pouring, establish vacuum and connect pipelines according to existing process requirements;
[0009] During pouring, the glue injection pipeline is opened first. Each main beam glue injection pipeline is opened when the resin front reaches the adjacent flow-blocking tape on its leading edge. The pipeline is closed when the entire pultruded main beam area is fully poured.
[0010] After the entire blade is poured, the heating process is started according to the existing process requirements to heat and solidify it to form a blade without defects between the pultruded main beam layers.
[0011] Furthermore, the flow-blocking partition has a width of 50-150 mm.
[0012] Furthermore, the flow-blocking partition is symmetrical with respect to the butt joint between the first and second pultruded plate layers at the rear edge of the pultruded main beam.
[0013] Furthermore, the flow-blocking tape is a sealing tape with a thickness of 1-3 mm and a width of 10-20 mm.
[0014] Furthermore, multiple flow-blocking tapes are evenly distributed in the infiltration direction during pouring of the pultruded main beam, and the extending direction of the flow-blocking tapes is perpendicular to the infiltration direction.
[0015] Furthermore, the main beam glue injection pipeline is a φ10-30 ohm tube or a spiral tube.
[0016] Furthermore, the main beam glue injection pipeline is opposite to the corresponding butt joint position.
[0017] Compared with the existing technology, the benefits of the present invention are: based on the existing technology, the present invention makes a flow-blocking partition on the injection source side of the continuous felt under the main beam, and designs a flow-blocking tape and a main beam injection pipeline on the guide net of each pultruded plate layer area of the pultruded main beam, so as to realize the independent partitioning of each pultruded plate layer (A / B / ... / N) of the pultruded main beam, and there is a flow-blocking tape on the guide net on the upper side of each pultruded plate layer in the pultruded main beam, and there is a resin source partition on the continuous felt under the main beam. During the injection, the flow speed of the resin in the glass fiber cloth between the pultruded plate layers is greater than the flow speed on the upper and lower sides of the pultruded main beam, which solves the risk of the resin surrounding the glass fiber cloth between each pultruded plate layer when flowing through the pultruded plate joint, thereby completely eliminating the interlayer injection defect of the pultruded main beam.
[0018] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following preferred embodiments are specifically cited and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a cross-sectional view of a conventional wind turbine blade pultrusion main beam integral casting process;
[0020] FIG2 is a cross-sectional view of an embodiment of a method for integrally pouring a pultruded main beam of a wind turbine blade according to the present invention. Reference numerals
[0021] 1- cloth layer under the main beam, 2- continuous felt under the main beam, 3- pultruded main beam, 4- shell core material, 5- guide net, 6- guide net partition, 7- glue injection pipeline, 8- VAP vacuum bag, 9- butt joint, 10- gap, 11- flow blocking partition, 12- flow blocking tape, 13- glue injection pipeline of the main beam. Modes for Carrying Out the Invention
[0022] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0023] An embodiment of a pultruded main beam integrated casting process method for a wind turbine blade according to the present invention is shown in Figure 2. When the blade shell is laid, the main beam lower cloth layer 1, the main beam lower continuous felt 2, the flow-blocking partition 11, the pultruded main beam 3, the shell core material 4, the guide net 5, the glue injection pipeline 7, the flow-blocking tape 12, and the main beam glue injection pipeline 13 are laid on the main mold in sequence; the glue injection pipeline 7 is close to the trailing edge of the wind turbine blade, and the pultruded main beam 3 includes a plurality of spliced and stacked pultruded plates, and the plurality of pultruded plates are stacked in the thickness direction to form a plurality of pultruded plate layers, and the plurality of pultruded plate layers are respectively A, B...N in Figure 2, and are spliced in the width direction to form a pultruded main beam, and the pultruded plates in the plurality of pultruded plate layers are spliced one by one, and fiberglass cloth is arranged between the pultruded plates at the same height and the adjacent pultruded plates in the plurality of pultruded plate layers.
[0024] The flow-blocking partition 11 is arranged on the continuous felt 2 under the main beam and is located below the butt joint 9 between the first and second pultruded plate layers at the rear edge of the pultruded main beam 3 to slow down the flow rate of the resin during infusion. In this embodiment, the two ends of the flow-blocking partition 11 are symmetrical with respect to the butt joint 9 between the first and second pultruded plate layers at the rear edge of the pultruded main beam 3. The flow-blocking partition is 50-150 mm wide to further slow down the flow rate of the resin during infusion. A flow-blocking tape 12 is arranged on the guide net above each pultruded plate layer. As shown in FIG2 , a flow-blocking tape 12 is arranged on the guide net above the A, B···N pultruded plate layers. In this embodiment, multiple flow-blocking tapes are provided. The flow tape 12 is evenly distributed in the infiltration direction during the pouring of the pultruded main beam 3, and the infiltration direction is from the trailing edge to the leading edge of the wind turbine blade. The flow-blocking tape 12 is a sealing tape with a thickness of 1-3 mm and a width of 10-20 mm, and the extension direction of the flow-blocking tape 12 is perpendicular to the infiltration direction to achieve a better flow-blocking effect; a main beam glue injection pipeline 13 is arranged between every two flow-blocking tapes 12. In this embodiment, the main beam glue injection pipeline 13 adopts a φ10-30 ohm tube or a spiral tube. The main beam glue injection pipeline 13 is opposite to the corresponding butt joint position, and the resin quickly reaches the butt joint to achieve a better pouring effect.
[0025] After laying is complete, a vacuum is established. When pouring the pultruded main beam 3 area, resin is preferentially injected through the glue injection line 7, where it infiltrates along the guide mesh 5 from the upper surface of the pultruded main beam 3 toward the leading edge. Each main beam glue injection line 13 begins injecting resin when the resin reaches the adjacent flow-blocking tape 12 on its leading edge. That is, during pouring, the resin first passes through the corresponding joint of the main beam injection line 13 and reaches the flow-blocking tape 12 on the leading edge before the main beam glue injection line 13 begins injecting resin to ensure that defects in the pultruded plate layer are eliminated. Resin injection ceases after pouring the pultruded main beam 3 area. After pouring is complete and heating and curing according to process requirements, a blade shell (a half-blade shell in a wind turbine blade) free of defects between the pultruded main beam layers is obtained.
[0026] The key technology of the present invention is to make a flow-blocking partition 11 on the injection source side of the continuous felt 2 under the main beam on the basis of the existing technology, and design a flow-blocking tape 12 and a main beam injection pipeline 13 on the guide net 5 of each pultruded plate area of the pultruded main beam 3, so as to realize the independent partitioning and injection of each pultruded plate (A / B / ... / N) of the pultruded main beam 3. There is a flow-blocking tape 12 on the guide net 5 on the upper side of each pultruded plate in the pultruded main beam, and there is a resin source partition on the continuous felt 2 under the main beam. During injection, the flow rate of the resin in the glass fiber cloth between the pultruded plate layers is greater than the flow rate on the upper and lower sides of the pultruded main beam 3, which solves the risk of the resin surrounding the glass fiber cloth between the layers of each pultruded plate when flowing through the pultruded plate joint 9, thereby completely eliminating the interlayer injection defect of the pultruded main beam.
[0027] By designing an integrated infusion scheme for the pultruded main beam of a wind turbine blade using the method of the present invention, defects in the interlayer glass fiber infusion of the pultruded main beam can be eliminated, and the fatigue performance of the interlayer of the pultruded main beam can be improved.
[0028] The specific steps of an embodiment of a method for integrally pouring a pultruded main beam of a wind turbine blade are as follows:
[0029] 1. According to the blade process, the main beam lower cloth layer 1, the main beam lower continuous felt 2, the pultruded main beam 3, the shell core material 4, the guide net 5, and the glue injection pipeline 7 are laid in the mold in sequence. Among them, the flow-blocking partition 11 is made on the continuous felt 2 under the main beam. The flow-blocking partition 11 is symmetrical with respect to the joint of the first and second pultruded plates at the rear edge of the pultruded main beam, and the partition width is 50-150mm.
[0030] 2. On the guide net 5 in the pultruded main beam 3 area, a flow-blocking tape 12 and a main beam glue injection pipeline 13 are installed. The flow-blocking tape is a sealing tape with a thickness of 1-3 mm and a width of 10-20 mm. A flow-blocking tape 12 is installed on the guide net above each pultruded plate; the main beam glue injection pipeline 13 is a φ10-30 ohm tube or a spiral tube, and a main beam glue injection pipeline 13 is installed between every two flow-blocking tapes 12.
[0031] 3. Establish vacuum and connect pipelines according to process requirements.
[0032] 4. During pouring, first open the glue injection pipeline 7. Each main beam glue injection pipeline 13 is opened when the resin front reaches the adjacent flow-blocking tape 12 on its leading edge side. When the entire main beam area is poured, close the pipeline.
[0033] 5. After the entire blade is infused, start the heating program to heat and cure according to the process requirements.
[0034] 6. After curing, a blade shell (half blade shell) without defects between the pultruded main beam layers can be obtained.
[0035] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and alterations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A wind turbine blade pultrusion main beam integral casting process method, comprising the following steps: According to the blade laying process, the main beam lower cloth layer (1), the main beam lower continuous felt (2), the pultruded main beam (3), the shell core material (4), the guide net (5), and the glue injection pipeline (7) are laid in sequence on the mold, and the pultruded main beam includes a pultruded plate layer formed by stacking multiple pultruded plates and glass fiber cloth between the layers, which is characterized by: further comprising the following steps: A flow-blocking partition (11) is provided on the continuous felt (2) under the main beam, and the flow-blocking partition (11) is located at the butt joint (9) between the first and second pultruded plate layers at the rear edge of the pultruded main beam; A flow-blocking tape (12) and a main beam glue injection pipeline (13) are arranged on the guide net (5) corresponding to the pultruded main beam (3) area, and a flow-blocking tape (12) is arranged on the guide net above each pultruded plate layer; and a main beam glue injection pipeline (13) is arranged between adjacent flow-blocking tapes (12); Before pouring, establish vacuum and connect pipelines according to process requirements; During pouring, the glue injection pipeline (7) is opened first, and each main beam glue injection pipeline (13) is opened when the resin front reaches the flow-blocking tape (12) adjacent to its front edge side, and the pipeline is closed when the entire pultruded main beam area is poured; After the entire blade is infused, the heating program is started according to the process requirements for heating and curing.
2. The method for integrally pouring a wind turbine blade pultruded main beam according to claim 1 is characterized in that: The flow-blocking partition (11) has a width of 50-150 mm.
3. The method for integrally pouring a wind turbine blade pultruded main beam according to claim 1 is characterized in that: The flow-blocking partition is symmetrical with respect to the butt joints of the first and second pultruded plate layers at the rear edge of the pultruded main beam.
4. The method for integrally pouring a wind turbine blade pultruded main beam according to claim 1 is characterized in that: The flow-blocking tape (12) is a sealing tape with a thickness of 1-3 mm and a width of 10-20 mm.
5. The method for integrally pouring a wind turbine blade pultrusion main beam according to claim 1 is characterized in that: A plurality of flow-blocking adhesive tapes (12) are evenly distributed in the infiltration direction during pouring of the pultruded main beam (3), and the extending direction of the flow-blocking adhesive tapes (12) is perpendicular to the infiltration direction.
6. The method for integrally pouring a wind turbine blade pultrusion main beam according to claim 1 is characterized in that: The main beam glue injection pipeline (13) is a φ10-30 ohm tube or a spiral tube.
7. The method for integrally pouring a wind turbine blade pultrusion main beam according to claim 1 is characterized in that: The main beam glue injection pipeline (13) is located opposite to the corresponding butt joint (9).
Citation Information
Patent Citations
Method for preparing large-scale composite-material aerogenerator blade
CN102114710A
Main beam for fan blade and manufacturing method thereof
CN113544379A
Wind power blade integrated pouring forming system and method and wind power blade
CN114953503A
Interlayer pouring structure and pouring method for pultrusion plate girder of wind power blade
CN115614214A
Wind power blade pultrusion beam pouring structure and forming method
CN115923196A
Cited By
Method for improving interlayer defect of pultrusion main beam of wind power blade and pultrusion main beam
CN120963091A
Method for improving interlaminar defects in a pultruded spar for a wind turbine blade and pultruded spar
CN120963091B