All-solid-state battery and manufacturing method thereof

The all-solid-state battery design with a specially structured insulating support frame addresses the issues of damage and waviness during roll pressing by controlling Young's modulus, ensuring the battery's integrity and performance.

WO2024214146A1PCT designated stage expired Publication Date: 2024-10-17NISSAN MOTOR CO LTD

Patent Information

Application Number
PCT/JP2023/014566
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The manufacturing of all-solid-state batteries faces challenges with roll pressing, where a high Young's modulus in the insulating support frame can cause damage, while a low modulus leads to waviness at the boundary between the positive electrode active material layer and the support frame.

Method used

The design incorporates an insulating support frame with a first side and second side having a slope that thins towards the outside, and third and fourth sides with a smaller slope, where the Young's modulus of the first side is lower than that of the third and fourth sides, allowing for controlled roll pressing that prevents damage and waviness.

Benefits of technology

This configuration effectively prevents damage and waviness during roll pressing by managing the load distribution, ensuring the integrity of the battery structure and maintaining performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023014566_17102024_PF_FP_ABST
    Figure JP2023014566_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This all-solid-state battery comprises an insulating support frame disposed on a positive electrode current collector foil so as to surround a positive electrode active material layer. The insulating support frame has a first side and a second side that are inclined, and a third side and a fourth side that are inclined to a lesser degree than the first side and the second side. The Young's modulus of the first side is smaller than the Young's moduli of the third side and the fourth side.
Need to check novelty before this filing date? Find Prior Art

Description

All-solid-state battery and method for manufacturing the same

[0001] The present invention relates to an all-solid-state battery and a method for manufacturing the same.

[0002] An all-solid-state battery is a secondary battery in which substantially all of its components, including the electrolyte, are made of solid materials. An all-solid-state battery generally has a configuration in which a positive electrode current collector foil, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector foil are stacked in this order.

[0003] Known all-solid-state batteries include one in which an insulating support frame is provided to surround a positive electrode active material layer. An example of such an all-solid-state battery is described in Patent Document 1 (JP2021-077644A). Patent Document 1 describes an all-solid-state secondary battery including a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer includes a positive electrode current collector, a positive electrode active material layer disposed on the positive electrode current collector, and an inactive member disposed on at least one side of the positive electrode active material layer, and the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on the negative electrode current collector.

[0004] Incidentally, when manufacturing an all-solid-state battery, roll pressing may be performed from the viewpoint of productivity, etc. When manufacturing an all-solid-state battery having an insulating support frame, first, a positive electrode active material layer and an insulating support frame are formed on a positive electrode current collector foil. Then, the obtained laminate is roll pressed. Here, if the Young's modulus of the insulating support frame is large, an excessive load may be applied to the insulating support frame at the pressing start position in the roll press, which may cause the insulating support frame to break. On the other hand, if the Young's modulus of the insulating support frame is small, waviness may occur at the boundary between the positive electrode active material layer and the insulating support frame.

[0005] Therefore, an object of the present invention is to provide an all-solid-state battery that can prevent breakage and undulation caused by roll pressing, and a method for manufacturing the same.

[0006] In one aspect of the present invention, an all-solid-state battery includes a positive electrode current collector foil, a positive electrode active material layer disposed on the positive electrode current collector foil, a solid electrolyte layer disposed on the positive electrode active material layer, a negative electrode active material layer or a negative electrode current collector foil disposed on the solid electrolyte layer, and an insulating support frame disposed on the positive electrode current collector foil so as to surround the positive electrode active material layer. The insulating support frame has a first side and a second side facing each other, the first side and the second side being inclined so as to become thinner toward the outside, and a third side and a fourth side connecting the first side and the second side and having a smaller inclination than the first side and the second side. The Young's modulus of the first side is smaller than the Young's modulus of the third side and the fourth side.

[0007] In another aspect of the present invention, a method for manufacturing an all-solid-state battery includes the steps of forming a positive electrode active material layer on a positive electrode current collector foil, forming an insulating support frame on the positive electrode current collector foil so as to surround the positive electrode active material layer, and fabricating a positive electrode structure having the positive electrode current collector foil, the positive electrode active material layer, and the insulating support frame, and pressing the positive electrode structure by roll pressing. The insulating support frame has a first side and a second side facing each other, and a third side and a fourth side connecting the first side and the second side, respectively. The Young's modulus of the first side is smaller than the Young's modulus of the third side and the fourth side. The pressing step includes a step of performing roll pressing so that pressing starts at the first side and ends at the second side.

[0008] FIG. 1 is a schematic cross-sectional view showing a main part of an all-solid-state battery according to an embodiment. FIG. 2 is a plan view showing a positive electrode active material layer and an insulating support frame. FIG. 3A is a view showing a cross section AA of FIG. 2. FIG. 3B is a view showing a cross section BB of FIG. 2. FIG. 4 is a view showing an outline of a method for manufacturing an all-solid-state battery. FIG. 5 is a schematic view showing a roll press process. FIG. 6 is a graph showing the relationship between the transport position and the load when the Young's modulus of the first side is large. FIG. 7 is a graph showing the relationship between the transport position and the load when the Young's modulus of the first side is small. FIG. 8 is a schematic view showing the mechanism by which undulations occur. FIG. 9 is a plan view showing the position by which undulations occur. FIG. 10 is a schematic view showing an example of a manufacturing process of an insulating support frame. FIG. 11 is a schematic cross-sectional view showing a modified example of the embodiment. FIG. 12 is a schematic view showing the mechanism by which an end of a solid electrolyte layer slides off.

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0010] In this specification, an "all-solid-state battery" refers to a secondary battery using a solid electrolyte layer. The electrolyte in the solid electrolyte layer is primarily a solid electrolyte, but may contain a small amount of liquid electrolyte. Similarly, when the positive electrode layer and the negative electrode layer contain an electrolyte, the main component thereof is a solid electrolyte, but a small amount of liquid electrolyte may be contained.

[0011] Fig. 1 is a schematic cross-sectional view showing a main part of an all-solid-state battery 1 according to this embodiment. As shown in Fig. 1, the all-solid-state battery 1 includes a positive electrode current collector foil 2, a positive electrode active material layer 3 disposed on the positive electrode current collector foil 2, a solid electrolyte layer 4 disposed on the positive electrode active material layer 3, a negative electrode active material layer 5 disposed on the solid electrolyte layer 4, and a negative electrode current collector foil 6 disposed on the negative electrode active material layer 5. Specifically, a plurality of positive electrode current collector foils 2 and a plurality of negative electrode current collector foils 6 are alternately arranged along the stacking direction. The positive electrode active material layer 3, the solid electrolyte layer 4, and the negative electrode active material layer 5 are provided between the positive electrode current collector foil 2 and the negative electrode current collector foil 6 adjacent to each other in the stacking direction.

[0012] The all-solid-state battery 1 according to this embodiment is a secondary battery that is charged and discharged by the movement of lithium ions. During charging, lithium ions move from the positive electrode active material layer 3 through the solid electrolyte layer 4 to the negative electrode active material layer 5, and lithium is absorbed in the negative electrode active material layer 5. Alternatively, lithium is precipitated in the negative electrode active material layer 5. During discharging, on the other hand, lithium ions move from the negative electrode active material layer 5 through the solid electrolyte layer 4 to the positive electrode active material layer 3, and lithium is absorbed in the positive electrode active material layer 3.

[0013] The all-solid-state battery 1 according to this embodiment may be a so-called all-precipitation type all-solid-state battery. An all-precipitation type all-solid-state battery is an all-solid-state battery that uses metallic lithium as the negative electrode active material, and during full discharge, all of the metallic lithium as the negative electrode active material is occluded in the positive electrode active material layer. In such an all-solid-state battery, during full discharge, the negative electrode active material layer 5 is not present. That is, during full discharge, the negative electrode current collector foil 6 is disposed directly on the solid electrolyte layer 4.

[0014] Here, the all-solid-state battery 1 further includes an insulating support frame 7. The insulating support frame 7 is disposed on the positive electrode current collector foil 2 so as to surround the positive electrode active material layer 3. The insulating support frame 7 is provided to support the end of the solid electrolyte layer 4. That is, when viewed along the stacking direction, the outer shape of the positive electrode active material layer 3 is located inside the outer shape of the solid electrolyte layer 4. Therefore, the end of the solid electrolyte layer 4 is not supported by the positive electrode active material layer 3. If the end of the solid electrolyte layer 4 is not supported, defects may occur in the end of the solid electrolyte layer 4 during a pressing step or the like during manufacturing. To prevent such defects from occurring, the insulating support frame 7 is provided around the positive electrode active material layer 3.

[0015] FIG. 2 is a plan view showing the positive electrode active material layer 3 and the insulating support frame 7. The positive electrode active material layer 3 is rectangular. Therefore, the insulating support frame 7 is also rectangular. The insulating support frame 7 has a first side 7-1, a second side 7-2, a third side 7-3, and a fourth side 7-4. The first side 7-1 and the second side 7-2 face each other, and the third side 7-3 and the fourth side 7-4 face each other. The third side 7-3 and the fourth side 7-4 also serve as sides connecting the first side 7-1 and the second side 7-2, respectively. That is, the third side 7-3 and the fourth side 7-4 are sandwiched between the first side 7-1 and the second side 7-2. The lengths of the third side 7-3 and the fourth side 7-4 (L in FIG. 2) are A ) is the length of the positive electrode active material layer 3 (L in the figure) 1 On the other hand, the length of the first side 7-1 and the second side 7-2 (L B ) is the length of the positive electrode active material layer 3 (in the figure, L 2 ) is larger than

[0016] 3A is a diagram showing the AA cross section of FIG. 2, and FIG. 3B is a diagram showing the BB cross section of FIG. 2. As shown in FIG. 3B, the first side 7-1 and the second side 7-2 are each inclined. Specifically, the first side 7-1 and the second side 7-2 are each inclined so that their thicknesses become thinner toward the outside. This inclination is formed during roll pressing. In other words, the first side 7-1 and the second side 7-2 correspond to the press start position and press end position during roll pressing, which will be described later.

[0017] On the other hand, as shown in FIG. 3A , the third side 7-3 and the fourth side 7-4 are hardly inclined. The inclination of the third side 7-3 and the fourth side 7-4 is smaller than that of the first side 7-1 and the second side 7-2. In this specification, "small inclination" means that the angle between the outer end surface of the insulating support frame 7 and the surface of the positive current collector foil 2 is close to a right angle. As shown in FIG. 3A , in this embodiment, the outer end surfaces of the third side 7-3 and the fourth side 7-4 are approximately perpendicular to the surface of the positive current collector foil 2 and are not substantially inclined. As a result, the inclination of the third side 7-3 and the fourth side 7-4 is smaller than that of the first side 7-1 and the second side 7-2.

[0018] Furthermore, in this embodiment, the Young's modulus of the first side 7-1 is smaller than the Young's modulus of the third side 7-3 and the fourth side 7-4.

[0019] The above is a schematic configuration of the all-solid-state battery 1 according to this embodiment. With such a configuration, it is possible to prevent breakage and undulation caused by roll pressing. This point will be described below based on the manufacturing method of the all-solid-state battery 1.

[0020] FIG. 4 is a diagram schematically showing a method for manufacturing the all-solid-state battery 1.

[0021] 4(a) , in manufacturing the all-solid-state battery 1, first, a positive electrode active material layer 3 is formed on a positive electrode current collector foil 2. The positive electrode active material layer 3 can be formed by, for example, a coating method, a transfer method, or the like.

[0022] 4(b), an insulating support frame 7 is formed on the positive electrode current collector foil 2. The insulating support frame 7 can be formed, for example, by applying a slurry containing the constituent materials of the insulating support frame 7 onto the positive electrode current collector foil 2. In this way, a positive electrode structure 8 including the positive electrode current collector foil 2, the positive electrode active material layer 3, and the insulating support frame 7 is produced.

[0023] 4(c) and 4(d), a solid electrolyte layer 4 is formed on the positive electrode active material layer 3 and the insulating support frame 7. The solid electrolyte layer 4 can be formed by using, for example, a coating method, a transfer method, or the like. In this way, a positive electrode-solid electrolyte layer assembly 9 is obtained.

[0024] On the other hand, a negative electrode current collector foil 6 is prepared as shown in Fig. 4(e). Then, as shown in Figs. 4(f) and 4(g), a negative electrode active material layer 5 is formed on the negative electrode current collector foil 6 to produce a negative electrode structure 10. Note that when an all-precipitation type all-solid-state battery 1 is produced, the negative electrode active material layer 5 may be omitted.

[0025] 4(h), the positive electrode-solid electrolyte layer assemblies 9 and the negative electrode structures 10 are alternately stacked, and then necessary members such as tabs are combined to obtain the all-solid-state battery 1.

[0026] The above is an outline of the entire manufacturing method of the all-solid-state battery 1. Here, in the above-described manufacturing method, after the cathode structure 8 is fabricated (see FIG. 4( b)), the cathode structure 8 is pressed by roll pressing at least once. For example, roll pressing is performed after fabrication of the cathode structure 8 and before formation of the solid electrolyte layer 4. Alternatively, when forming the solid electrolyte layer 4 by a transfer method, roll pressing may be performed when transferring the solid electrolyte layer 4. Alternatively, roll pressing may be performed after formation of the solid electrolyte layer 4 or when laminating the cathode-solid electrolyte layer assembly 9 and the anode structure 10.

[0027] FIG. 5 is a schematic diagram showing the roll press process. As described above, roll press is performed so that pressing begins at the first edge 7-1 and ends at the second edge 7-2. At this time, the roll 11 rides up onto the first edge 7-1, which is the pressing start position. If the Young's modulus of the first edge 7-1 is large, excessive load is applied to the first edge 7-1. FIG. 6 is a graph showing the relationship between the workpiece transport position and load when the Young's modulus of the first edge 7-1 is large (specifically, 175 GPa). As shown in FIG. 6, if the Young's modulus of the first edge 7-1 is large, excessive load is applied at the pressing start position (see A in the figure). As a result, cracks are more likely to occur on the first edge 7-1.

[0028] In contrast, Figure 7 is a graph showing the relationship between the workpiece transport position and the load when the Young's modulus of the first edge 7-1 is small (specifically, 10 GPa). As shown in Figure 7, when the Young's modulus is low, excessive load is not applied at the press start position (see A in the figure). Therefore, the small Young's modulus of the first edge 7-1 suppresses the occurrence of cracks at the press start position. By suppressing cracks, it is possible to prevent a decrease in battery performance due to short circuits or stacking misalignment.

[0029] As described above, reducing the Young's modulus of the first edge 7-1 can suppress cracking. However, reducing the Young's modulus of not only the first edge 7-1 but also the third edge 7-3 and the fourth edge 7-4 increases the likelihood of waviness during roll pressing. This point will be explained with reference to FIG. 8 . FIG. 8 is a schematic diagram illustrating the waviness generation mechanism. In a typical all-solid-state battery, the positive electrode active material layer 3 has a large Young's modulus. Reducing the Young's modulus of the insulating support frame 7 to a level that suppresses cracking increases the difference between the Young's modulus of the positive electrode active material layer 3 and the Young's modulus of the insulating support frame 7. This difference in Young's modulus causes differences in the way loads are applied during roll pressing between the positive electrode active material layer 3 and the insulating support frame 7. As a result, differences occur in the magnitude of the load applied to the underlying positive electrode current collector foil 2, resulting in differences in the elongation of the positive electrode current collector foil 2. This causes waviness. FIG. 9 is a plan view showing the location of waviness 12. According to the findings of the present inventors, the undulations 12 caused by roll pressing tend to occur along the roll feed direction (the direction from the first side 7-1 to the second side 7-2). That is, the undulations 12 tend to occur along the third side 7-3 and the fourth side 7-4.

[0030] In contrast, in this embodiment, the Young's modulus of the third side 7-3 and the fourth side 7-4 is set to a value greater than that of the first side 7-1. Therefore, the difference between the Young's modulus of the positive electrode active material layer 3 and the Young's modulus of the third side 7-3 and the fourth side 7-4 is small, making it difficult for a difference to occur in the load applied to the positive electrode current collector foil 2. As a result, undulation is suppressed.

[0031] For the reasons explained above, in this embodiment, the Young's modulus of the first side 7-1 is small and the Young's modulus of the third side 7-3 and the fourth side 7-4 is large, so that both cracks and undulations during roll pressing can be prevented.

[0032] Specifically, the Young's modulus of the first side 7-1 is preferably approximately the same as that of the solid electrolyte layer 4. The Young's modulus of the solid electrolyte layer 4 is usually smaller than that of the positive electrode active material layer 3. If the Young's modulus of the first side 7-1 is approximately the same as that of the solid electrolyte layer 4, excessive load can be prevented from being applied at the pressing start position. The Young's modulus of the first side 7-1 is, for example, 1 to 30 GPa.

[0033] On the other hand, the Young's modulus of the third side 7-3 and the fourth side 7-4 is preferably equivalent to that of the positive electrode active material layer 3. Here, "equivalent to that of the positive electrode active material layer 3" means that the Young's modulus of the third side 7-3 and the fourth side 7-4 is within a range of ±5% of the Young's modulus of the positive electrode active material layer 3. The Young's modulus of the third side 7-3 and the fourth side 7-4 is, for example, 50 to 300 GPa.

[0034] The Young's modulus of the second side 7-2 corresponding to the pressing end position is not particularly limited.

[0035] From one perspective, it is preferable that the Young's modulus of the second side 7-2 is smaller than those of the third side 7-3 and the fourth side 7-4, similar to that of the first side 7-1. More preferably, the Young's modulus of the second side is the same as that of the first side 7-1. By adopting such a configuration, the difference in the amount of compression between the first side 7-1 and the second side 7-2 during roll pressing can be reduced, and the difference in film thickness between the first side 7-1 and the second side 7-2 can be reduced. This makes it less likely that transfer defects will occur when the solid electrolyte layer 4 is formed by transfer. Furthermore, when the solid electrolyte layer 4 is formed by a coating method, the coating accuracy can be improved, and differences in adhesion between the solid electrolyte layer 4 and the insulating support frame 7 can be prevented.

[0036] On the other hand, from another perspective, it is preferable that the second side 7-2 have the same composition as the third side 7-3 and the fourth side 7-4. In other words, it is preferable that the Young's modulus of the second side 7-2 is the same as the Young's modulus of the third side 7-3 and the fourth side 7-4. Such a configuration makes it possible to easily manufacture the insulating support frame 7. This point will be explained with reference to FIG. 10. FIG. 10 is a schematic diagram showing an example of a manufacturing process for the insulating support frame 7. The insulating support frame 7 can be formed, for example, by applying a slurry containing the constituent material of the insulating support frame 7 using a dispenser or the like. In this case, if the second side 7-2, the third side 7-3, and the fourth side 7-4 have the same composition, the second side 7-2, the third side 7-3, and the fourth side 7-4 can be successively coated. As a result, the manufacturing process can be simplified.

[0037] Next, the insulating support frame 7 will be described in detail.

[0038] The insulating support frame 7 is preferably 10 5 The insulating support frame 7 has an electrical resistivity of 10 Ωcm or more. 6 If the insulating support frame 7 has such an electrical resistivity, the electrode reaction (exchange of lithium ions) will occur uniformly at the interface between the positive electrode active material layer 3 and the solid electrolyte layer 4. In addition, short-circuiting between the positive electrode side and the negative electrode side will be more reliably prevented.

[0039] The width of the insulating support frame 7 is not particularly limited, but is, for example, 1 to 30 mm, and preferably 1 to 10 mm.

[0040] In the insulating support frame 7, it is preferable that there be zero clearance at the portions where the sides are connected to each other. In other words, it is preferable that there be no gaps between the sides.

[0041] It is preferable that the clearance between the insulating support frame 7 and the positive electrode active material layer 3 is zero. That is, it is preferable that the insulating support frame 7 is disposed so as to contact the outer peripheral end surface of the positive electrode active material layer 3.

[0042] The thickness of the insulating support frame 7, excluding the inclined portions of the first side 7-1 and the second side 7-2, is preferably the same as the thickness of the positive electrode active material layer 3. The thickness of the insulating support frame 7 is, for example, 30 to 1000 μm, and preferably 30 to 100 μm.

[0043] The constituent material of the insulating support frame 7 is not particularly limited as long as it is insulating. The insulating support frame 7 can be formed from, for example, an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, or a sulfide-based solid electrolyte.

[0044] However, when the solid electrolyte layer 4 contains a sulfide solid electrolyte, the insulating support frame 7 is preferably formed of a material dispersible in a low-polarity solvent. When fabricating the cathode structure 8, the insulating support frame 7 is preferably formed by dispersing the material for forming the insulating support frame 7 in a low-polarity solvent to prepare a slurry for the insulating support frame, and then applying the prepared insulating support frame slurry to the cathode current collector foil 2. When the solid electrolyte layer 4 contains a sulfide solid electrolyte, residues of the solvent used in fabricating the insulating support frame 7 may react with the sulfide solid electrolyte. However, low-polarity solvents are less likely to react with the sulfide solid electrolyte. Therefore, using a low-polarity solvent can prevent the reaction between the sulfide solid electrolyte and the residual solvent. This ensures the insulating properties of the solid electrolyte layer 4 and suppresses dendrite formation. Examples of low-polarity solvents include trimethylbenzene, dimethylbenzene, and butyl acetate.

[0045] Next, a modified example regarding the position of the end of the insulating support frame 7 will be described. FIG. 11 is a schematic cross-sectional view showing this modified example. In this modified example, when viewed along the stacking direction, the end of the insulating support frame 7 is located outward from the end of the solid electrolyte layer 4. This configuration can prevent the end of the solid electrolyte layer 4 from sliding off. FIG. 12 is a schematic diagram showing the mechanism by which the end of the solid electrolyte layer 4 slides off. FIG. 12( a) shows a case in which the end of the insulating support frame 7 is aligned with the end of the solid electrolyte layer 4. In the example shown in FIG. 12( a), when the solid electrolyte layer 4 stretches due to pressure applied by the roll press, the end of the solid electrolyte layer 4 protrudes outward from the end of the insulating support frame 7. As a result, the end of the solid electrolyte layer 4 is no longer supported and is prone to sliding off. End sliding off should be avoided because it can cause contamination and short circuits. 12( b), if the end of the insulating support frame 7 is located outward from the end of the solid electrolyte layer 4, even if the solid electrolyte layer 4 stretches slightly, the end of the solid electrolyte layer 4 is still supported by the insulating support frame 7. Therefore, the end of the solid electrolyte layer 4 is prevented from slipping off.

[0046] In this modification, the positions of the ends of the insulating support frame 7 are preferably located outside the ends of the solid electrolyte layer 4 on all of the first side 7-1 to the fourth side 7-4. However, the end of the insulating support frame 7 may be located outside the end of the solid electrolyte layer 4 on at least one of the first side 7-1 to the fourth side 7-4. Even in such a case, a certain effect can be obtained because the end of the solid electrolyte layer 4 can be prevented from slipping off on that at least one side.

[0047] Next, the configuration other than the insulating support frame 7 will be described.

[0048] The solid electrolyte layer 4 is solid and may be made of any material as long as it functions as an electrolyte layer in a secondary battery. The solid electrolyte layer 4 includes, for example, a resin binder and a solid electrolyte dispersed in the resin binder. The solid electrolyte preferably includes a sulfide solid electrolyte. The thickness of the solid electrolyte layer 4 is, for example, 5 to 100 μm.

[0049] The positive electrode active material layer 3 may be formed of any material capable of releasing lithium ions during charging and absorbing lithium ions during discharging. The positive electrode active material layer 3 may be formed, for example, of a material containing a resin binder and a positive electrode active material dispersed in the resin binder. The positive electrode active material is not particularly limited, but may be, for example, an NMC-based positive electrode active material. The thickness of the positive electrode active material layer 3 is, for example, 30 to 1000 μm, preferably 10 to 500 μm.

[0050] For example, a metal foil is used as the positive electrode current collector foil 2. For example, an aluminum foil or the like can be used as the positive electrode current collector foil 2. The thickness of the positive electrode current collector foil 2 is, for example, 5 to 50 μm, and preferably 8 to 20 μm.

[0051] For example, a metal foil is also used as the negative electrode current collector foil 6. For example, SUS and copper foil can be used as the negative electrode current collector foil 6. The thickness of the negative electrode current collector foil 6 is, for example, 5 to 50 μm, and preferably 8 to 20 μm.

[0052] The embodiment and modifications of the present invention have been described above. The following summarizes the relationship between the configuration and the effects of the present invention.

[0053] In one embodiment, an all-solid-state battery 1 includes a positive electrode current collector foil 2, a positive electrode active material layer 3 disposed on the positive electrode current collector foil 2, a solid electrolyte layer 4 disposed on the positive electrode active material layer 3, an anode active material layer 5 or an anode current collector foil 6 disposed on the solid electrolyte layer 4, and an insulating support frame 7 disposed on the positive electrode current collector foil 2 so as to surround the positive electrode active material layer 3. The insulating support frame 7 has a first side 7-1 and a second side 7-2 facing each other, the first side 7-1 and the second side 7-2 having a slope such that the thickness decreases toward the outside, and a third side 7-3 and a fourth side 7-4 connecting the first side 7-1 and the second side 7-2, respectively, and having a slope smaller than that of the first side 7-1 and the second side 7-2. The Young's modulus of the first side 7-1 is smaller than that of the third side 7-3 and the fourth side 7-4. With this configuration, since the Young's modulus of the first side 7-1 is small, it is possible to prevent excessive load from being applied at the press start position during roll pressing, thereby suppressing the occurrence of cracks. Also, since the Young's modulus of the third side 7-3 and the fourth side 7-4 is large, it is possible to suppress the occurrence of swells.

[0054] From one perspective, it is preferable that the Young's modulus of the second side 7-2 be smaller than those of the third side 7-3 and the fourth side 7-4. With this configuration, the Young's moduli of the first side 7-1 and the second side 7-2 can be made approximately the same. As a result, the difference in film thickness between the first side 7-1 and the second side 7-2 can be reduced. This makes it easier to form the solid electrolyte layer 4 with high reliability.

[0055] From another viewpoint, it is preferable that the second side 7-2, the third side 7-3, and the fourth side 7-4 have the same composition. This configuration makes it possible to continuously produce the second side 7-2 to the fourth side 7-4, thereby simplifying the manufacturing process.

[0056] Preferably, the Young's modulus of the third side 7-3 and the fourth side 7-4 is equal to the Young's modulus of the positive electrode active material layer 3. According to this configuration, the occurrence of undulations can be more reliably prevented.

[0057] Preferably, at least one of the first side 7-1 to the fourth side 7-4, the end of the insulating support frame 7 is located outside the end of the solid electrolyte layer 4. This configuration can more reliably prevent the end of the solid electrolyte layer 4 from slipping off.

[0058] Preferably, the electrical resistivity of the insulating support frame 7 is 10 5 According to this configuration, the electrode reaction (exchange of lithium ions) occurs uniformly at the interface between the positive electrode active material layer 3 and the solid electrolyte layer 4, and short circuits between the positive electrode side and the negative electrode side are more reliably prevented.

[0059] Preferably, the solid electrolyte layer 4 contains a sulfide solid electrolyte. Furthermore, the insulating support frame 7 is formed from a material that is dispersible in a low-polarity solvent. With this configuration, the insulating support frame 7 can be formed using a low-polarity solvent. As a result, reaction between the sulfide solid electrolyte and residues of the solvent used when forming the insulating support frame 7 can be suppressed.

[0060] In one embodiment, a method for manufacturing an all-solid-state battery 1 includes the steps of forming a cathode active material layer 3 on a cathode current collector foil 2, forming an insulating support frame 7 on the cathode current collector foil 2 so as to surround the cathode active material layer 3, and fabricating a cathode structure 8 having the cathode current collector foil 2, the cathode active material layer 3, and the insulating support frame 7, and pressing the cathode structure 8 by roll pressing. The insulating support frame 7 has a first side 7-1 and a second side 7-2 that face each other, and a third side 7-3 and a fourth side 7-4 that connect the first side 7-1 and the second side 7-2, respectively. The Young's modulus of the first side 7-1 is smaller than the Young's modulus of the third side 7-3 and the fourth side 7-4. The pressing step includes a step of performing roll pressing so that pressing starts at the first side 7-1 and ends at the second side 7-2. According to this method, since the Young's modulus of the first side 7-1 is small, it is possible to prevent excessive load from being applied at the press start position during roll pressing, thereby suppressing the occurrence of cracks. Also, since the Young's modulus of the third side 7-3 and the fourth side 7-4 is large, it is possible to suppress the occurrence of undulations.

[0061] Preferably, the method for manufacturing the all-solid-state battery 1 further includes a step of forming a solid electrolyte layer 4 on the positive electrode active material layer 3, and a step of forming a negative electrode active material layer 5 or a negative electrode current collector foil 6 on the solid electrolyte layer 4.

[0062] Preferably, the solid electrolyte layer 4 contains a sulfide solid electrolyte. The process of producing the positive electrode structure 8 includes a step of dispersing a material for forming the insulating support frame 7 in a low-polarity solvent to prepare a slurry for the insulating support frame, and a step of forming the insulating support frame 7 by applying the insulating support frame slurry to the positive electrode current collector foil 2. This method makes it possible to prevent residues of the solvent used in forming the insulating support frame 7 from reacting with the sulfide solid electrolyte.

Claims

1. An all-solid-state battery comprising: a positive electrode current collector foil; a positive electrode active material layer disposed on the positive electrode current collector foil; a solid electrolyte layer disposed on the positive electrode active material layer; a negative electrode active material layer or a negative electrode current collector foil disposed on the solid electrolyte layer; and an insulating support frame disposed on the positive electrode current collector foil so as to surround the positive electrode active material layer, wherein the insulating support frame has a first side and a second side opposed to each other, the first side and the second side being inclined so as to become thinner toward the outside, and a third side and a fourth side respectively connecting the first side and the second side and having a smaller inclination than the first side and the second side, and a Young's modulus of the first side is smaller than the Young's modulus of the third side and the fourth side.

2. The all-solid-state battery according to claim 1, wherein the Young's modulus of the second side is smaller than the Young's modulus of the third side and the fourth side.

3. The all-solid-state battery according to claim 1, wherein the second side, the third side, and the fourth side have the same composition.

4. The all-solid-state battery according to claim 1 or 2, wherein the Young's modulus of the third side and the fourth side is equal to the Young's modulus of the positive electrode active material layer.

5. An all-solid-state battery according to claim 1 or 2, wherein an end of the insulating support frame is positioned outside an end of the solid electrolyte layer in at least one of the first side to the fourth side.

6. The all-solid-state battery according to claim 1 or 2, wherein the electrical resistivity of the insulating support frame is 10 5 An all-solid-state battery having a capacitance of Ωcm or more.

7. An all-solid-state battery according to claim 1 or 2, wherein the solid electrolyte layer contains a sulfide solid electrolyte, and the insulating support frame is formed of a material that can be dispersed in a low-polarity solvent.

8. A method for manufacturing an all-solid-state battery, comprising: a step of forming a positive electrode active material layer on a positive electrode current collector foil; a step of forming an insulating support frame on the positive electrode current collector foil so as to surround the positive electrode active material layer, thereby producing a positive electrode structure having the positive electrode current collector foil, the positive electrode active material layer, and the insulating support frame; and a step of pressing the positive electrode structure by roll pressing, wherein the insulating support frame has a first side and a second side opposed to each other, and a third side and a fourth side each connecting the first side and the second side, respectively, and the Young's modulus of the first side is smaller than the Young's modulus of the third side and the fourth side, and the pressing step includes a step of performing roll pressing so that pressing starts at the first side and ends at the second side.

9. The method according to claim 8, further comprising the steps of: forming a solid electrolyte layer on the positive electrode active material layer; and forming a negative electrode active material layer or a negative electrode current collector foil on the solid electrolyte layer.

10. A manufacturing method according to claim 9, wherein the solid electrolyte layer contains a sulfide solid electrolyte, and the step of producing the positive electrode structure includes the steps of: dispersing a material for forming the insulating support frame in a low-polarity solvent to prepare a slurry for the insulating support frame; and applying the slurry for the insulating support frame onto the positive electrode current collector foil to form the insulating support frame.

Citation Information

Patent Citations

  • Electrode structure and all-solid secondary battery including the same

    JP2022173135A

  • Electrode body for all-solid-state batteries, and method for producing same

    WO2019103008A1

  • Battery

    WO2021230009A1

Cited By

  • Battery

    WO2026021610A1