Steel material
The steel material with a tailored chemical composition and microstructure addresses the challenge of achieving high yield strength and low-temperature toughness, enabling effective CO2 storage and press-fitting in low-temperature environments.
Patent Information
- Application Number
- PCT/JP2024/010335
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-17
AI Technical Summary
Current steel materials used in carbon dioxide storage technology lack both high yield strength and low-temperature toughness, particularly in extremely low-temperature environments such as -70°C or lower, which is essential for efficient CO2 storage and press-fitting in depleted oil wells.
A steel material with a specific chemical composition, including C: 0.26-0.35%, Si: 0.10-1.00%, Mn: 1.00-1.40%, and a controlled number of coarse carbides, combined with a microstructure of tempered martensite and tempered bainite, that satisfies the ratio of prior austenite grain size to block diameter (DA/DB) between 2.5 and 10.0, achieving both high yield strength and excellent low-temperature toughness.
The steel material achieves a yield strength of 552 to 655 MPa and excellent low-temperature toughness in cryogenic environments, ensuring stability and efficiency in CO2 storage and press-fitting applications.
Smart Images

Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
steel material
[0001] The present disclosure relates to steel products, and more particularly to steel products used in CO2 storage technologies.
[0002] Currently, the rise in carbon dioxide (CO2) concentrations on land has become a global problem. As a result, efforts to curb CO2 emissions are underway. Among these efforts to curb CO2 emissions, CCUS has been attracting particular attention.
[0003] CCUS is an abbreviation for Carbon Dioxide Capture, Utilization, and Storage. In other words, CCUS includes three technologies: CO2 capture, utilization, and storage. Of these, a CO2 storage technology that has been attracting attention is one that captures CO2 emitted from industrial facilities such as power plants and factories and stores it by injecting it into depleted oil wells.
[0004] Steel materials used in such CO2 storage technologies are required to have a yield strength of, for example, 80 ksi or more (552 MPa or more). To date, steel materials having a yield strength of 80 ksi or more have been proposed in JP 2002-115028 A (Patent Document 1) and WO 2017 / 149570 (Patent Document 2).
[0005] The steel material disclosed in Patent Document 1 is a steel pipe for oil wells, characterized in that it has a yield stress YS of 552 MPa (80 ksi) or more and an L-direction absorbed energy E (J) at 0°C that satisfies the formula (E≧−0.4169×YS+480). Patent Document 1 discloses that this steel material can withstand crushing caused by strong external pressure from the outer surface, which is required for casing.
[0006] The steel material disclosed in Patent Document 2 is a low-alloy, high-strength seamless steel pipe for oil wells, which contains, in mass %, C: 0.23 to 0.27%, Si: 0.01 to 0.35%, Mn: 0.45 to 0.70%, P: 0.010% or less, S: 0.001% or less, O: 0.0015% or less, Al: 0.015 to 0.080%, Cu: 0.02 to 0.09%, C: 0.23 to 0.27%, Si: 0.01 to 0.35%, Mn: 0.45 to 0.70%, The steel material contains r: 0.8 to 1.5%, Mo: 0.5 to 1.0%, Nb: 0.02 to 0.05%, B: 0.0015 to 0.0030%, Ti: 0.005 to 0.020%, and N: 0.005% or less, and has a composition in which the ratio of the Ti content to the N content (Ti / N) is 3.0 to 4.0, with the balance being Fe and unavoidable impurities. This steel material further has a value of the ratio of the stress at 0.7% strain to the stress at 0.4% strain in a stress-strain curve (σ 0.7 / σ 0.4 ) is 1.02 or less, and the yield strength is 655 MPa or more. This steel material has high strength equal to or higher than API standard T95 class, and also has a stable high K ISSC Patent Document 2 discloses that it is possible to provide a low-alloy, high-strength seamless steel pipe for oil wells that exhibits high strength.
[0007] JP 2002-115028 A International Publication No. 2017 / 149570
[0008] When injecting CO2 into depleted oil wells, the CO2 gas may be compressed and pressurized to a supercritical state to increase the injection efficiency. However, if CO2 leaks, the CO2 gas will transition from a supercritical state to a gaseous state, and its temperature will drop rapidly due to a sudden drop in pressure. In this case, the ambient temperature may fall far below normal, possibly even dropping to -70°C or below. Therefore, steel materials intended for application to such carbon dioxide storage technologies are required to have not only high strength but also low-temperature toughness in cryogenic environments of -70°C or below. However, Patent Documents 1 and 2 do not consider low-temperature toughness in cryogenic environments of -70°C or below.
[0009] An object of the present disclosure is to provide a steel material that combines a yield strength of 80 ksi or more (552 MPa or more) with excellent low-temperature toughness in an extremely low-temperature environment of -70°C or less.
[0010] The steel material according to the present disclosure contains, in mass %, C: 0.26 to 0.35%, Si: 0.10 to 1.00%, Mn: 1.00 to 1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15 to 0.50%, Mo: 0.05 to 0.25%, sol. Al: 0.001 to 0.070%, N: 0.0010 to 0.0080%, V: 0 to 0.60%, Nb: 0 to 0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: 0 to 0.0050%, Co: 0 to 0.50%, Ni: 0 to 0.30%, Cu: 0 to 0.50%, Sn: 0 to 0.100%, Ca: 0 to 0.0035%, Mg: 0 to 0.0035%, B: 0 to 0.0010%, rare earth elements: 0 to 0.0050%, and the balance: Fe and impurities, and the steel material has a yield strength of 552 to less than 655 MPa, 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 When the prior austenite grain size is defined as DA and the block diameter is defined as DB, the DA and DB satisfy the formula (1): 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in the formula (1), and the block diameter (unit: μm) is substituted for DB in the formula (1).
[0011] The steel material according to the present disclosure can achieve both a yield strength of 80 ksi or more (552 MPa or more) and excellent low-temperature toughness in an extremely low-temperature environment of -70°C or less.
[0012] The present inventors first investigated obtaining a steel material having a yield strength of 552 to less than 655 MPa, with the aim of applying it to carbon dioxide storage technology. That is, the present inventors investigated and considered methods for obtaining a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment in a steel material expected to be applied to carbon dioxide storage technology. As a result, the present inventors obtained the following findings.
[0013] The inventors first focused on the chemical composition to investigate obtaining a steel material having a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in cryogenic environments, and as a result, found a steel material containing, in mass%, C: 0.26 to 0.35%, Si: 0.10 to 1.00%, Mn: 1.00 to 1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15 to 0.50%, Mo: 0.05 to 0.25%, sol. The inventors considered that a steel material consisting of Al: 0.001 to 0.070%, N: 0.0010 to 0.0080%, V: 0 to 0.60%, Nb: 0 to 0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: 0 to 0.0050%, Co: 0 to 0.50%, Ni: 0 to 0.30%, Cu: 0 to 0.50%, Sn: 0 to 0.100%, Ca: 0 to 0.0035%, Mg: 0 to 0.0035%, B: 0 to 0.0010%, rare earth elements: 0 to 0.0050%, and the balance: Fe and impurities could potentially achieve a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment.
[0014] Next, the inventors focused on fine particles in the steel material and attempted to obtain a steel material that combines a yield strength of 552 to less than 655 MPa with excellent low-temperature toughness in a cryogenic environment. The inventors particularly focused on relatively coarse particles and tried to find a method for improving low-temperature toughness in a cryogenic environment while maintaining yield strength. As a result, they obtained the following findings.
[0015] In steel materials having the above-mentioned chemical composition, when an attempt is made to obtain a yield strength of less than 552 to 655 MPa, coarse carbides may be formed. As a result of detailed studies by the present inventors, it has become clear that when a large number of carbides having an equivalent circle diameter of 2 μm or more are formed in the steel material, the low-temperature toughness in an extremely low temperature environment decreases. Specifically, in steel materials having the above-mentioned chemical composition, carbides having an equivalent circle diameter of 2 μm or more are formed at a density of 10 particles / mm 2By reducing the diameter to or below this value, it may be possible to achieve both a yield strength of 552 to less than 655 MPa and low-temperature toughness in a cryogenic environment. Hereinafter, in this specification, carbides with an equivalent circle diameter of 2 μm or more will also be referred to as "coarse carbides." Note that in this specification, the equivalent circle diameter means the diameter of a circle when the area of an observed precipitate in a visual field in structural observation is replaced with a circle having the same area.
[0016] On the other hand, the steel sheet has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 Even when the content of carbides is reduced to or below 552 MPa, there are cases where low-temperature toughness in a cryogenic environment cannot be obtained. Therefore, the present inventors have developed a steel sheet having the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and in which the number density of coarse carbides having a circle equivalent diameter of 2 μm or more is 10 particles / mm 2 Various methods for improving the low-temperature toughness in cryogenic environments were investigated for the following steel materials.
[0017] Specifically, the inventors focused on the microstructure of steel material. To date, a method of reducing the prior austenite grain size (hereinafter, the prior austenite grain size is also referred to as "prior γ grain size DA") in the microstructure of steel material has been known as a method for improving the low-temperature toughness of steel material. On the other hand, a steel having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa, and a number density of coarse carbides of 10 particles / mm 2 In the following steel materials, even if the prior γ grain size DA was small, there were cases where low-temperature toughness in an extremely low temperature environment could not be obtained. This point will be specifically explained using a table.
[0018]
[0019] Table 1 is an excerpt from some of the examples described below. Test numbers 13, 14, and 49 all had the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides was 10 pieces / mm 2The following was satisfied. Referring to Table 1, a comparison of Test Nos. 13 and 14 with Test No. 49 shows that, although Test Nos. 13 and 14 have a larger prior γ grain size DA than Test No. 49, Test Nos. 13 and 14 have a lower fracture appearance transition temperature vTrs (°C), which is an index of low temperature toughness, than Test No. 49. Note that, as will be described in detail later, a lower fracture appearance transition temperature vTrs indicates better low temperature toughness of the steel material. In other words, it can be confirmed that Test Nos. 13 and 14, which have a larger prior γ grain size DA, exhibit better low temperature toughness in a cryogenic environment than Test No. 49, which has a smaller prior γ grain size DA.
[0020] As a result of detailed studies by the present inventors, it was found that the steel sheet has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 It has been revealed that in the following steel materials, not only the prior γ grain size DA but also the size of the blocks, which are substructures, affect low-temperature toughness in a cryogenic environment. Here, the microstructure of a steel material having the above-mentioned chemical composition and a yield strength of less than 552 to 655 MPa and excellent low-temperature toughness is mainly composed of tempered martensite and tempered bainite. Here, in the martensite substructure, a group of laths with approximately the same orientation is called a martensite block. Similarly, in the bainite substructure, a group of bainite laths with approximately the same orientation is called a bainite block. In this specification, the martensite block and the bainite block are collectively referred to as a block. Furthermore, in this specification, the average grain size of the martensite block and the average grain size of the bainite block are collectively referred to as a "block diameter DB."
[0021] As described above, steel materials with a finer prior γ grain size (DA) generally tend to exhibit superior low-temperature toughness. Similarly, the present inventors suspected that steel materials with a finer block diameter (DB) would also exhibit superior low-temperature toughness. However, referring to Table 1, it was confirmed that, contrary to the present inventors' expectations, test numbers 13 and 14, which had a larger prior γ grain size (DA) and larger block diameter (DB), exhibited superior low-temperature toughness in a cryogenic environment compared to test number 49, which had a smaller prior γ grain size (DA) and smaller block diameter (DB).
[0022] As a result of further detailed studies by the present inventors based on the above findings, it was found that a steel sheet having the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa and a number density of coarse carbides of 10 particles / mm 2 It has been revealed that the following steel materials can obtain excellent low-temperature toughness in cryogenic environments if the prior γ grain size DA and the block diameter DB satisfy the following formula (1): 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0023] Fn1 is defined as Fn1 = DA / DB. Fn1 has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 This is an index of low-temperature toughness in a cryogenic environment for the following steel material. When Fn1 exceeds 10.0 in the steel material, the prior γ grain size DA is too large relative to the block diameter DB. As a result, excellent low-temperature toughness in a cryogenic environment cannot be obtained. Also, if Fn1 is 2.5 or more in the steel material, low-temperature toughness in a cryogenic environment can be stably obtained. Therefore, if the steel material has the above chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 / mm 2 In the following steel materials, when Fn1 satisfies 2.5 to 10.0, they have excellent low-temperature toughness even in an extremely low-temperature environment.
[0024] In addition, the steel sheet has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 pieces / mm 2 The details of why the following steel materials have excellent low-temperature toughness even in cryogenic environments as a result of satisfying Fn1 of 2.5 to 10.0 are not clear. However, it is known that the steel materials have the above-mentioned chemical composition, a yield strength of 552 to less than 655 MPa, and a number density of coarse carbides of 10 particles / mm 2 In the steel materials listed below, Fn1 satisfies 2.5 to 10.0, and as a result, they have excellent low-temperature toughness even in an extremely low-temperature environment, as proven by the examples described below.
[0025] The gist of the steel material according to this embodiment, which was completed based on the above findings, is as follows.
[0026] [1] A steel material comprising, in mass%, C: 0.26 to 0.35%, Si: 0.10 to 1.00%, Mn: 1.00 to 1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15 to 0.50%, Mo: 0.05 to 0.25%, sol. Al: 0.001 to 0.070%, N: 0.0010 to 0.0080%, V: 0 to 0.60%, Nb: 0 to 0.03%, Ti: 0 to 0.05%, W: 0 to 0.50%, Zr: 0 to 0.0050%, Co: 0 to 0.50%, Ni: 0 to 0.30%, Cu: 0 to 0.50%, Sn: 0 to 0.100%, Ca: 0 to 0.0035%, Mg: 0 to 0.0035%, B: 0 to 0.0010%, rare earth elements: 0 to 0.0050%, and the balance: Fe and impurities, and the steel material has a yield strength of 552 to less than 655 MPa, 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 A steel material in which, when the prior austenite grain size is defined as DA and the block diameter is defined as DB, the DA and DB satisfy the following formula (1): 2.5≦DA / DB≦10.0 (1) Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0027] [2] The steel material according to [1], containing one or more elements selected from the group consisting of V: 0.01 to 0.60%, Nb: 0.01 to 0.03%, Ti: 0.01 to 0.05%, W: 0.01 to 0.50%, Zr: 0.0001 to 0.0050%, Co: 0.01 to 0.50%, Ni: 0.01 to 0.30%, Cu: 0.01 to 0.50%, Sn: 0.001 to 0.100%, Ca: 0.0001 to 0.0035%, Mg: 0.0001 to 0.0035%, B: 0.0001 to 0.0010%, and rare earth elements: 0.0001 to 0.0050%.
[0028] [3] The steel material according to [1] or [2], wherein the steel material is a steel pipe.
[0029] The shape of the steel material according to this embodiment is not particularly limited. The steel material according to this embodiment may be a steel pipe, a round bar (solid material), or a steel plate. Note that round bar refers to a steel bar having a circular cross section perpendicular to the axial direction. The steel pipe may be a seamless steel pipe or a welded steel pipe.
[0030] The steel material according to this embodiment will be described in detail below. Unless otherwise specified, "%" regarding elements means mass %.
[0031] [Chemical Composition] The chemical composition of the steel material according to this embodiment contains the following elements.
[0032] C: 0.26 to 0.35% Carbon (C) improves the hardenability of steel and increases its strength. C also refines the block diameter DB of the steel. If the C content is too low, the above effects cannot be fully achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the C content is too high, the strength of the steel becomes too high, even if the contents of other elements are within the ranges of this embodiment, and the low-temperature toughness of the steel decreases. Therefore, the C content is 0.26 to 0.35%. The preferred lower limit of the C content is 0.27%, more preferably 0.28%, and even more preferably 0.29%. The preferred upper limit of the C content is 0.34%, more preferably 0.33%, and even more preferably 0.32%.
[0033] Si: 0.10 to 1.00% Silicon (Si) deoxidizes steel. If the Si content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Si content is too high, the low-temperature toughness of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Si content is 0.10 to 1.00%. A preferred lower limit of the Si content is 0.12%, more preferably 0.14%, and even more preferably 0.15%. A preferred upper limit of the Si content is 0.95%, more preferably 0.90%, and even more preferably 0.80%.
[0034] Mn: 1.00 to 1.40% Manganese (Mn) improves the hardenability of steel and increases its strength. If the Mn content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content is too high, Mn segregates to grain boundaries together with impurities such as P and S, reducing the low-temperature toughness of the steel, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mn content is 1.00 to 1.40%. The preferred lower limit of the Mn content is 1.02%, more preferably 1.05%. The preferred upper limit of the Mn content is 1.35%, more preferably 1.30%.
[0035] P: 0.015% or less Phosphorus (P) is an impurity. That is, the lower limit of the P content is greater than 0%. If the P content is too high, even if the contents of other elements are within the ranges of this embodiment, P segregates at grain boundaries, reducing the low-temperature toughness of the steel material. Therefore, the P content is 0.015% or less. A preferred upper limit of the P content is 0.014%, more preferably 0.013%. The P content is preferably as low as possible. However, an extreme reduction in the P content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.003%.
[0036] S: 0.0020% or less Sulfur (S) is an impurity. That is, the lower limit of the S content is greater than 0%. If the S content is too high, even if the contents of other elements are within the ranges of this embodiment, S segregates at grain boundaries, reducing the low-temperature toughness of the steel material. Therefore, the S content is 0.0020% or less. A preferred upper limit of the S content is 0.0019%, more preferably 0.0018%, and even more preferably 0.0016%. The S content is preferably as low as possible. However, an extreme reduction in the S content significantly increases manufacturing costs. Therefore, considering industrial production, a preferred lower limit of the S content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%.
[0037] Cr: 0.15 to 0.50% Chromium (Cr) improves the hardenability of steel and increases its strength. Cr also concentrates in cementite in the steel, suppressing cementite coarsening. As a result, the low-temperature toughness of the steel is improved. If the Cr content is too low, the above effects cannot be sufficiently achieved even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content is too high, the low-temperature toughness of the steel is reduced even if the contents of other elements are within the ranges of this embodiment. Therefore, the Cr content is 0.15 to 0.50%. The preferred lower limit of the Cr content is 0.18%, more preferably 0.20%. The preferred upper limit of the Cr content is 0.45%, more preferably 0.40%.
[0038] Mo: 0.05 to 0.25% Molybdenum (Mo) improves the hardenability of steel and increases its strength. If the Mo content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mo content is too high, even if the contents of other elements are within the ranges of this embodiment, excessive Mo carbides are formed, reducing the low-temperature toughness of the steel. Therefore, the Mo content is 0.05 to 0.25%. The preferred lower limit of the Mo content is 0.06%, more preferably 0.07%. The preferred upper limit of the Mo content is 0.24%, more preferably 0.20%, and even more preferably 0.18%.
[0039] Sol. Al: 0.001 to 0.070% Aluminum (Al) deoxidizes steel. If the Al content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Al content is too high, coarse oxide-based inclusions are formed, reducing the low-temperature toughness of the steel material even if the contents of other elements are within the ranges of this embodiment. Therefore, the Al content is 0.001 to 0.070%. A preferred lower limit of the Al content is 0.005%, more preferably 0.010%. A preferred upper limit of the Al content is 0.065%, more preferably 0.060%. In this specification, the "Al" content refers to the content of "acid-soluble Al," that is, "sol. Al."
[0040] N: 0.0010 to 0.0080% Nitrogen (N) forms nitrides and refines the prior γ grain size DA of the steel material through a pinning effect. As a result, the low-temperature toughness of the steel material is improved. If the N content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the N content is too high, coarse nitrides are formed, reducing the low-temperature toughness of the steel material, even if the contents of other elements are within the ranges of this embodiment. Therefore, the N content is 0.0010 to 0.0080%. The preferred lower limit of the N content is 0.0015%, more preferably 0.0020%, and even more preferably 0.0025%. The preferred upper limit of the N content is 0.0075%, more preferably 0.0070%.
[0041] The balance of the chemical composition of the steel material according to this embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or the manufacturing environment, during industrial production of the steel material, and are acceptable within a range that does not adversely affect the steel material according to this embodiment.
[0042] [Optional Elements] The chemical composition of the above-described steel material may further contain one or more elements selected from the group consisting of V, Nb, Ti, W, and Zr in place of a portion of Fe. All of these elements are optional elements, and they increase the temper softening resistance of the steel material and increase the strength of the steel material.
[0043] V: 0 to 0.60% Vanadium (V) is an optional element and does not necessarily need to be contained. That is, the V content may be 0%. When contained, V forms fine carbides during tempering, increasing the temper softening resistance of the steel material and increasing the strength of the steel material. Even if even a small amount of V is contained, the above effects can be obtained to some extent. However, if the V content is too high, the low-temperature toughness of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the V content is 0 to 0.60%. The preferred lower limit of the V content is more than 0%, more preferably 0.01%, even more preferably 0.02%, even more preferably 0.04%, and even more preferably 0.06%. The preferred upper limit of the V content is 0.40%, more preferably 0.30%, and even more preferably 0.20%.
[0044] Nb: 0 to 0.03% Niobium (Nb) is an optional element and does not necessarily need to be contained. That is, the Nb content may be 0%. When contained, Nb forms fine carbides during tempering, increasing the temper softening resistance of the steel material and increasing the strength of the steel material. Even if even a small amount of Nb is contained, the above effects can be obtained to some extent. However, if the Nb content is too high, even if the contents of other elements are within the ranges of this embodiment, excessive carbonitrides and the like are formed, resulting in a decrease in the low-temperature toughness and SSC resistance of the steel material. Therefore, the Nb content is 0 to 0.03%. The preferred lower limit of the Nb content is more than 0%, more preferably 0.01%, and even more preferably 0.02%. The preferred upper limit of the Nb content is less than 0.03%.
[0045] Ti: 0 to 0.05% Titanium (Ti) is an optional element and does not necessarily need to be contained. That is, the Ti content may be 0%. When contained, Ti forms fine carbides, which increase the tempering softening resistance of the steel material and increase the strength of the steel material. Even if even a small amount of Ti is contained, the above effects can be obtained to some extent. However, if the Ti content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse nitrides are formed, reducing the low-temperature toughness of the steel material. Therefore, the Ti content is 0 to 0.05%. The preferred lower limit of the Ti content is more than 0%, more preferably 0.01%, and even more preferably 0.02%. The preferred upper limit of the Ti content is less than 0.05%, more preferably 0.04%.
[0046] W: 0 to 0.50% Tungsten (W) is an optional element and does not necessarily need to be contained. That is, the W content may be 0%. When contained, W forms fine carbides during tempering, increasing the temper softening resistance of the steel material and increasing the strength of the steel material. Even if even a small amount of W is contained, the above effects can be obtained to some extent. However, if the W content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse carbides are formed, reducing the low-temperature toughness of the steel material. Therefore, the W content is 0 to 0.50%. The preferred lower limit of the W content is more than 0%, more preferably 0.01%, and even more preferably 0.02%. The preferred upper limit of the W content is 0.45%, more preferably 0.40%.
[0047] Zr: 0 to 0.0050% Zirconium (Zr) is an optional element and does not necessarily need to be contained. That is, the Zr content may be 0%. When contained, Zr forms fine carbides during tempering, increasing the temper softening resistance of the steel material and increasing the strength of the steel material. Even if even a small amount of Zr is contained, the above effects can be achieved to some extent. However, if the Zr content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse oxides will form, reducing the low-temperature toughness of the steel material. Therefore, the Zr content is 0 to 0.0050%. The preferred lower limit of the Zr content is greater than 0%, more preferably 0.0001%, even more preferably 0.0003%, even more preferably 0.0006%, and even more preferably 0.0010%. The preferred upper limit of the Zr content is 0.0045%, more preferably 0.0040%, and even more preferably 0.0035%.
[0048] The chemical composition of the steel material described above may further contain one or more elements selected from the group consisting of Co and Ni in place of a portion of Fe. All of these elements are optional elements, and they improve the hardenability and strength of the steel material.
[0049] Cobalt (Co) is an optional element and does not necessarily need to be contained. That is, the Co content may be 0%. When contained, Co improves the hardenability of the steel material and increases its strength. Even if even a small amount of Co is contained, the above effects can be obtained to some extent. However, if the Co content is too high, even if the contents of other elements are within the ranges of this embodiment, the hardenability of the steel material will decrease and the strength of the steel material will decrease. Therefore, the Co content is 0 to 0.50%. The preferred lower limit of the Co content is more than 0%, more preferably 0.01%, even more preferably 0.02%, even more preferably 0.03%, and even more preferably 0.05%. The preferred upper limit of the Co content is 0.45%, more preferably 0.40%.
[0050] Ni: 0 to 0.30% Nickel (Ni) is an optional element and does not necessarily need to be contained. That is, the Ni content may be 0%. When contained, Ni improves the hardenability of the steel material and increases its strength. Even if even a small amount of Ni is contained, these effects can be obtained to some extent. However, if the Ni content is too high, localized corrosion is promoted and the corrosion resistance of the steel material decreases, even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ni content is 0 to 0.30%. The preferred lower limit of the Ni content is more than 0%, more preferably 0.01%, and even more preferably 0.02%. The preferred upper limit of the Ni content is 0.28%, more preferably 0.25%.
[0051] The chemical composition of the steel material may further contain one or more elements selected from the group consisting of Cu and Sn in place of a portion of Fe. All of these elements are optional elements and increase the strength of the steel material.
[0052] Cu: 0 to 0.50% Copper (Cu) is an optional element and does not necessarily need to be contained. That is, the Cu content may be 0%. When contained, Cu increases the strength of the steel material. Even if even a small amount of Cu is contained, the above effect can be obtained to some extent. However, if the Cu content is too high, even if the contents of other elements are within the ranges of this embodiment, the strength of the steel material becomes too high and the low-temperature toughness of the steel material decreases. Therefore, the Cu content is 0 to 0.50%. The preferred lower limit of the Cu content is more than 0%, more preferably 0.01%, even more preferably 0.02%, and even more preferably 0.05%. The preferred upper limit of the Cu content is 0.45%, more preferably 0.35%, and even more preferably 0.25%.
[0053] Sn: 0 to 0.100% Tin (Sn) is an optional element and does not necessarily need to be contained. That is, the Sn content may be 0%. When contained, Sn increases the strength of the steel material. Even if even a small amount of Sn is contained, the above effect can be obtained to some extent. However, if the Sn content is too high, the hot workability of the steel material will decrease even if the contents of other elements are within the ranges of this embodiment. Therefore, the Sn content is 0 to 0.100%. The preferred lower limit of the Sn content is more than 0%, more preferably 0.001%, even more preferably 0.002%, and even more preferably 0.003%. The preferred upper limit of the Sn content is 0.095%, more preferably 0.090%, even more preferably 0.080%, and even more preferably 0.070%.
[0054] The chemical composition of the steel material described above may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Ca, Mg, B, and rare earth elements. All of these elements are optional elements, and improve the hot workability of the steel material.
[0055] Ca: 0 to 0.0035% Calcium (Ca) is an optional element and does not necessarily need to be contained. That is, the Ca content may be 0%. When contained, Ca renders S in the steel harmless as sulfides, improving the hot workability of the steel. Even if even a small amount of Ca is contained, the above effects can be obtained to some extent. However, if the Ca content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse oxides will be generated, reducing the low-temperature toughness of the steel. Therefore, the Ca content is 0 to 0.0035%. The preferred lower limit of the Ca content is more than 0%, more preferably 0.0001%, even more preferably 0.0003%, even more preferably 0.0006%, and even more preferably 0.0010%. The preferred upper limit of the Ca content is 0.0033%, more preferably 0.0030%.
[0056] Mg: 0 to 0.0035% Magnesium (Mg) is an optional element and does not necessarily need to be contained. That is, the Mg content may be 0%. When contained, Mg renders S in the steel harmless as sulfides, improving the hot workability of the steel. Even if even a small amount of Mg is contained, the above effects can be obtained to some extent. However, if the Mg content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse oxides are formed, reducing the low-temperature toughness of the steel. Therefore, the Mg content is 0 to 0.0035%. The preferred lower limit of the Mg content is more than 0%, more preferably 0.0001%, even more preferably 0.0003%, even more preferably 0.0006%, and even more preferably 0.0010%. The preferred upper limit of the Mg content is 0.0033%, more preferably 0.0030%.
[0057] B: 0 to 0.0010% Boron (B) is an optional element and does not necessarily need to be contained. That is, the B content may be 0%. When contained, B suppresses the segregation of S to grain boundaries in the steel material, improving the hot workability of the steel material. Even if even a small amount of B is contained, the above effects can be obtained to some extent. However, if the B content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse nitrides are formed, reducing the low-temperature toughness of the steel material. Therefore, the B content is 0 to 0.0010%. The preferred lower limit of the B content is more than 0%, more preferably 0.0001%, and even more preferably 0.0002%. The preferred upper limit of the B content is 0.0009%, more preferably 0.0008%.
[0058] Rare earth elements (REM): 0 to 0.0050% Rare earth elements (REM) are optional elements and may not be contained. That is, the REM content may be 0%. When contained, REM renders S in the steel harmless as sulfides, improving the hot workability of the steel. Even if even a small amount of REM is contained, the above effects can be obtained to some extent. However, if the REM content is too high, even if the contents of other elements are within the ranges of this embodiment, coarse oxides are formed, reducing the low-temperature toughness of the steel. Therefore, the REM content is 0 to 0.0050%. The preferred lower limit of the REM content is greater than 0%, more preferably 0.0001%, even more preferably 0.0003%, and even more preferably 0.0006%. The preferred upper limit of the REM content is 0.0045%, more preferably 0.0040%.
[0059] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.
[0060] [Yield strength] The yield strength of the steel material according to this embodiment is 552 to less than 655 MPa (80 to less than 95 ksi). The yield strength in this specification means the 0.2% offset yield strength (MPa) obtained by a tensile test at room temperature (24±3°C) in accordance with ASTM E8 / E8M (2021).
[0061] In this embodiment, the yield strength of the steel material can be determined by the following method. Specifically, a tensile test is performed according to ASTM E8 / E8M (2021). A round bar test piece is prepared from the steel material according to this embodiment. When the steel material is a steel plate, the round bar test piece is prepared from the center of the plate thickness. In this case, the axial direction of the round bar test piece is parallel to the rolling direction of the steel plate. When the steel material is a steel pipe, the round bar test piece is prepared from the center of the wall thickness. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the steel pipe. When the steel material is a round bar, the round bar test piece is prepared from the R / 2 position. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the round bar. In this specification, the R / 2 position refers to the center position of the radius R in a cross section perpendicular to the axial direction of the round bar. The size of the round bar test piece is, for example, 6 mm in parallel diameter and 30 mm in gauge length. A tensile test was performed using a round bar test piece in the air at room temperature (24±3°C), and the obtained 0.2% offset proof stress (MPa) was defined as the yield strength (MPa). In this embodiment, the yield strength (MPa) is a value obtained by rounding off the obtained value to one decimal place.
[0062] [Number Density of Coarse Carbides] The steel material according to this embodiment has the above-described chemical composition and a yield strength of 552 to less than 655 MPa, and further has a number density of coarse carbides (carbides with a circle equivalent diameter of 2 μm or more) of 10 particles / mm 2 As a result, the steel material according to this embodiment has excellent low-temperature toughness in a cryogenic environment, provided that the other configurations of this embodiment are satisfied. As described above, in this specification, the circle-equivalent diameter means the diameter of a circle having the same area as the area of an observed precipitate in a visual field in microstructural observation.
[0063] In steel materials having the above-mentioned chemical composition, coarse carbides are likely to be formed. In particular, if carbides remain without being dissolved in the quenching process described below, the remaining carbides tend to coarsen and become coarse carbides in the subsequent tempering process. On the other hand, if the number of coarse carbides is less than 10 / mm 2If the precipitation exceeds 10 / mm , there is a concern that the low-temperature toughness of the steel material will be reduced. In particular, this effect becomes significant in an extremely low-temperature environment such as -70°C or lower. Therefore, the steel material according to this embodiment has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and further has a number density of coarse carbides of 10 / mm . 2 The following applies.
[0064] In this embodiment, the preferred upper limit of the number density of coarse carbides is 9 pieces / mm 2 and more preferably 8 pieces / mm 2 and more preferably 7 pieces / mm 2 and more preferably 6 pieces / mm 2 and more preferably 5 pieces / mm 2 The lower limit of the number density of the coarse carbides is not particularly limited, and is 0 particles / mm 2 1 piece / mm 2 may be.
[0065] In this embodiment, the number density of coarse carbides in a steel material can be determined by the following method. First, a test piece is prepared from the steel material according to this embodiment. Specifically, when the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with a plane including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the wall thickness, with a plane including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared with a plane including the R / 2 position in the center and including the axial and radial directions as the observation surface.
[0066] The observation surface of the prepared test piece is polished to a mirror finish before measurement. The area of the observation surface is not limited, but for example, 300 mm 2The sample is measured in a size of 20 mm x 15 mm. The number of carbides with a circle-equivalent diameter of 2 μm or more is determined on the observation surface. Specifically, particles on the observation surface are first identified based on contrast. Each identified particle is subjected to element concentration analysis (EDS analysis) using energy dispersive X-ray spectrometry (EDS). In the EDS analysis, an acceleration voltage is set to 20 kV, and the target elements are quantified as C, N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb. If C is detected and the Fe content is 50 mass% or more based on the EDS analysis results of each particle, the particle is identified as a "carbide." Here, in this specification, "C is detected" means that a characteristic X-ray peak identified as C is confirmed. It should be noted that a person skilled in the art would naturally be able to confirm the characteristic X-ray peak identified as C.
[0067] Of the carbides identified on the observation surface, those with a circle-equivalent diameter of 2 μm or more (coarse carbides) are identified, and the total number of coarse carbides is determined. The circle-equivalent diameter of the carbides can be determined by a well-known method, for example, by image analysis. Based on the total number of coarse carbides and the total area of the observation surface, the number density of the coarse carbides (pieces / mm 2 In this embodiment, the number density of coarse carbides (pieces / mm 2 ) is obtained by rounding off the obtained value to one decimal place. The number density of coarse carbides can be measured using an apparatus (SEM-EDS apparatus) in which a composition analysis function is added to a scanning electron microscope (SEM). As the SEM-EDS apparatus, for example, an automatic analyzer manufactured by FEI (ASPEX) under the trade name of Metals Quality Analyzer can be used.
[0068] [Fn1 (=DA / DB)] The steel material according to this embodiment has the above-described chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 pieces / mm 2or less, and further, the prior austenite grain size DA and the block diameter DB satisfy the following formula (1): 2.5≦DA / DB≦10.0 (1) As a result, the steel material according to this embodiment can achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in an extremely low-temperature environment. Here, the prior austenite grain size (unit: μm) is substituted for DA in formula (1), and the block diameter (unit: μm) is substituted for DB in formula (1).
[0069] As described above, in this specification, the prior austenite grain size in the microstructure of the steel material is also referred to as the "prior γ grain size DA." Furthermore, in this specification, the average grain size of the martensite blocks and the average grain size of the bainite blocks are collectively referred to as the "block diameter DB." Note that, as described above, the microstructure of the steel material according to this embodiment is mainly composed of tempered martensite and tempered bainite. Therefore, in this specification, the martensite blocks and the bainite blocks are collectively referred to as blocks.
[0070] Fn1 (=DA / DB) has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 Fn1 is an index of low-temperature toughness in a cryogenic environment for the following steel materials. If Fn1 exceeds 10.0, excellent low-temperature toughness in a cryogenic environment cannot be obtained. On the other hand, if the steel has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 In the following steel material, if Fn1 is 2.5 or more, low-temperature toughness in a cryogenic environment can be stably obtained. Therefore, the steel material according to this embodiment has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 particles / mm 2 The following conditions are satisfied, and Fn1 is set to 2.5 to 10.0.
[0071] As described above, in a steel material having the above-described chemical composition, if carbides remain without dissolving in the quenching process described below, the remaining carbides tend to coarsen and become coarse carbides in the subsequent tempering process. On the other hand, if an attempt is made to dissolve the carbides sufficiently in the quenching process, the prior γ grain size DA and / or the block diameter DB tend to become large. In this case, if either the prior γ grain size DA or the block diameter DB becomes too large, Fn1 becomes less than 2.5 or exceeds 10.0. As a result, excellent low-temperature toughness cannot be stably obtained in an extremely low-temperature environment. On the other hand, if carbides dissolve in the quenching process described below and the number density of coarse carbides becomes 10 / mm 2 If Fn1 satisfies the range of 2.5 to 10.0 after being reduced to the above range, excellent low-temperature toughness can be stably obtained even in an extremely low-temperature environment.
[0072] In the steel material according to this embodiment, the prior γ grain size DA and block diameter DB are not particularly limited as long as Fn1 satisfies the range of 2.5 to 10.0. However, if the steel material has the above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 pieces / mm 2 In the following steel materials, the prior γ grain size DA is, for example, 10.0 to 200.0 μm. In the present embodiment, a preferable upper limit of the prior γ grain size DA is 180.0 μm, more preferably 160.0 μm, and even more preferably 150.0 μm. In the steel material according to the present embodiment, even if the prior γ grain size DA is, for example, 15.0 μm or more, 20.0 μm or more, 30.0 μm or more, 40.0 μm or more, or even coarse to 50.0 μm or more, by satisfying Fn1 of 2.5 to 10.0, it is possible to achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment.
[0073] The above-mentioned chemical composition and a yield strength of 552 to less than 655 MPa, and the number density of coarse carbides is 10 / mm 2In the following steel materials, the block diameter DB is, for example, 2.0 to 30.0 μm. In this embodiment, the upper limit of the block diameter DB is preferably 25.0 μm, more preferably 20.0 μm, and even more preferably 15.0 μm. In the steel material according to this embodiment, even if the block diameter DB is, for example, 5.0 μm or more, 7.0 μm or more, 8.0 μm or more, 10.0 μm or more, or even coarse to 11.0 μm or more, by satisfying Fn1 of 2.5 to 10.0, it is possible to achieve both a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment.
[0074] In this embodiment, the lower limit of Fn1 is preferably 3.0, more preferably 3.5, and even more preferably 4.0. In this embodiment, the upper limit of Fn1 is preferably 9.8, more preferably 9.5, and even more preferably 9.0.
[0075] In this embodiment, Fn1 can be determined by the following method. First, the prior γ grain size DA of the steel material according to this embodiment is determined. Specifically, a test piece for measuring the prior γ grain size DA is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with the observation surface being a plane including the rolling direction and the plate thickness direction. When the steel material is a steel pipe, a test piece is prepared from the center of the wall thickness, with the observation surface being a plane including the pipe axial direction and the pipe radial direction. When the steel material is a round bar, a test piece is prepared with the R / 2 position in the center and the observation surface being a plane including the axial and radial directions.
[0076] The test piece is embedded in resin, and the observation surface is polished to a mirror finish. Then, it is immersed for about 60 seconds in a solution of saturated aqueous picric acid mixed with an appropriate amount of surfactant, and the prior γ grain boundaries are revealed by etching. The area of the observation surface is not limited, but for example, 100 mm 2(10 mm x 10 mm). The grain size number G is determined by optical microscope observation based on the cutting method in accordance with JIS G 0551 (2020). The obtained grain size number G is converted to the average grain size M (μm) based on the following formulas (2) and (3). In this embodiment, the average grain size M obtained by the above method is defined as the prior γ grain size DA (μm). In other words, in this embodiment, the prior austenite grain size DA (μm) means the average grain size of prior austenite grains determined based on the cutting method in accordance with JIS G 0551 (2020). n = 2 G+3 (2) M=1000 / n 1 / 2 (3)
[0077] Next, the block diameter DB of the steel material according to this embodiment is determined. Specifically, a test piece for measuring the block diameter DB is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece having an observation surface of 25 μm × 25 μm is prepared from the center of the plate thickness. When the steel material is a steel pipe, a test piece having an observation surface of 25 μm × 25 μm is prepared from the center of the wall thickness. When the steel material is a round bar, a test piece having an observation surface of 25 μm × 25 μm that includes the R / 2 position in the center is prepared.
[0078] Measurements are performed on the observation surface of the test piece using electron backscatter diffraction (EBSD). EBSD measurements are performed at an acceleration voltage of 20 kV, with a field of view of 25 μm × 25 μm at a pitch of 0.1 μm. The orientation of the body-centered cubic structure (iron) is identified from the Kikuchi line pattern obtained by the EBSD measurement. A crystal orientation diagram is obtained from the orientation of the body-centered cubic structure (iron). From the crystal orientation diagram, areas surrounded by an orientation misorientation of 15° or more with adjacent crystals are identified to obtain a crystal orientation map. An area surrounded by an orientation misorientation of 15° or more is defined as one block.
[0079] For the defined blocks, the average grain size DB (μm) is calculated from the area of each block. Specifically, the total number of blocks in the crystal orientation map is k, and the area of each block is SBi (i is a natural number equal to or less than k) (μm 2 ), the area of the crystal orientation map is ST (μm 2) In this case, the average particle size DB (μm) of the blocks is defined by the following formula (4). Here, the total number of blocks in the crystal orientation map (a natural number) is substituted for k in equation (4), and the area (μm 2 ) is substituted, π is substituted with the constant of the circumference of the circle, and ST is the total area (μm 2 ) is substituted.
[0080] Fn1 (= DA / DB) is calculated from the obtained prior γ grain diameter DA (μm) and block diameter DB (μm). In this embodiment, the prior γ grain diameter DA (μm) is a value obtained by rounding off the obtained numerical value to one decimal place. Furthermore, in this embodiment, the block diameter DB (μm) is a value obtained by rounding off the obtained numerical value to one decimal place. Furthermore, in this embodiment, Fn1 is a value obtained by rounding off the obtained numerical value to one decimal place.
[0081] [Low temperature toughness] The steel material according to this embodiment has the above-mentioned chemical composition and has a number density of coarse carbides of 10 particles / mm 2 or less, and Fn1 is 2.5 to 10.0. As a result, the steel material according to this embodiment has a yield strength of 552 to less than 655 MPa and excellent low-temperature toughness in a cryogenic environment. In this embodiment, excellent low-temperature toughness in a cryogenic environment is defined as follows.
[0082] A Charpy impact test in accordance with ASTM E23 (2018) is performed on the steel material according to this embodiment. First, a V-notch test specimen is prepared from the steel material according to this embodiment in accordance with ASTM E23 (2018). Specifically, when the steel material is a steel plate, a V-notch test specimen is prepared from the center of the plate thickness, having a notch surface perpendicular to the plate thickness direction and a longitudinal direction parallel to the plate width direction. When the steel material is a steel pipe, a V-notch test specimen is prepared from the center of the wall thickness, having a notch surface perpendicular to the pipe axial direction and a longitudinal direction perpendicular to the pipe axial direction and the pipe radial direction. When the steel material is a round bar, a V-notch test specimen is prepared from the R / 2 position on a cross section perpendicular to the axial direction, having a notch surface perpendicular to the axial direction and a longitudinal direction perpendicular to the axial direction and the cross-sectional radial direction.
[0083] The prepared V-notch test specimens are subjected to a Charpy impact test in accordance with ASTM E23 (2018). Specifically, the test temperature is set to eight levels (-120°C, -100°C, -80°C, -60°C, -40°C, -20°C, 0°C, and 20°C) in increments of 20°C within the range of -120°C to 20°C. The Charpy impact test is performed using two test specimens for each test temperature. Under the above conditions, the brittle fracture surface ratio (%) of the test specimens after testing at each temperature is determined. An approximation curve is obtained by plotting the test temperature (°C) and the obtained brittle fracture surface ratio (%). From the obtained approximation curve, the temperature (°C) at which the brittle fracture surface ratio becomes 50% is determined and defined as the fracture transition temperature vTrs (°C). In this embodiment, if the fracture transition temperature vTrs is -70°C or lower, it is determined that the specimen has excellent low-temperature toughness in a cryogenic environment.
[0084] [Microstructure] As described above, the microstructure of the steel material according to this embodiment is mainly composed of tempered martensite and tempered bainite. Specifically, the microstructure of the steel material according to this embodiment has a total volume fraction of tempered martensite and tempered bainite of 90% or more. The remainder of the microstructure is, for example, ferrite or pearlite. The above-mentioned chemical composition, a yield strength of 552 to less than 655 MPa, and a density of 10 pieces / mm 2 In a steel material that satisfies the following number density of coarse carbides and Fn1 of 2.5 to 10.0, if the steel material has a microstructure in which the total volume fraction of tempered martensite and tempered bainite is 90% or more, it will have excellent low-temperature toughness in an extremely low-temperature environment. 2 If a steel material that satisfies the number density of coarse carbides below and Fn1 of 2.5 to 10.0 has excellent low-temperature toughness in an extremely low-temperature environment, the microstructure of the steel material is determined to have a total volume fraction of tempered martensite and tempered bainite of 90% or more.
[0085] When the volume fractions of tempered martensite and tempered bainite are determined by observation, they can be determined by the following method. First, a test piece having a specific observation surface is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with the observation surface being a plane including the rolling direction and the plate thickness direction. When the steel material is a steel pipe, a test piece is prepared from the center of the wall thickness, with the observation surface being a plane including the pipe axial direction and the pipe radial direction. When the steel material is a round bar, a test piece is prepared with the R / 2 position in the center, with the observation surface being a plane including the axial and radial directions.
[0086] The observation surface of the test piece is polished to a mirror finish, and then immersed in a nital etching solution for about 10 seconds to reveal the structure by etching. The etched observation surface is observed using a SEM in 10 fields of view as secondary electron images. The field area is, for example, 0.01 mm. 2 (Magnification: 1000x). In each field of view, tempered martensite and tempered bainite are identified from the contrast. The area fractions of the identified tempered martensite and tempered bainite are calculated. The method for calculating the area fractions is not particularly limited, and any known method may be used. For example, the area fractions of tempered martensite and tempered bainite can be calculated by image analysis. In this embodiment, the arithmetic mean values of the area fractions of tempered martensite and tempered bainite calculated in all fields of view are defined as the volume fractions of tempered martensite and tempered bainite.
[0087] [Manufacturing method] A method for manufacturing a steel material according to this embodiment will be described below. A method for manufacturing a seamless steel pipe will be described below as an example of a steel material according to this embodiment. The method for manufacturing a seamless steel pipe includes a step of preparing a mother pipe (preparation step) and a step of quenching and tempering the mother pipe to form a seamless steel pipe (quenching step and tempering step). Note that the manufacturing method according to this embodiment is not limited to the manufacturing method described below. Each step will be described in detail below.
[0088] [Preparation step] In the preparation step, an intermediate steel material having the above-mentioned chemical composition is prepared. As long as the intermediate steel material has the above-mentioned chemical composition, there is no particular limitation on the method for manufacturing the intermediate steel material. The intermediate steel material referred to here is a plate-shaped steel material if the final product is a steel plate, a mother pipe if the final product is a steel pipe, or a steel material with a circular cross section perpendicular to the axial direction if the final product is a round steel bar.
[0089] The preparation step may include a step of preparing a material (material preparation step) and a step of hot working the material to produce an intermediate steel material (hot working step). Below, the case where the material preparation step and the hot working step are included will be described in detail.
[0090] [Material Preparation Step] In the material preparation step, a material is produced using molten steel having the above-described chemical composition. The method for producing the material is not particularly limited and may be a well-known method. Specifically, a cast piece (slab, bloom, or billet) may be produced using the molten steel by a continuous casting method. An ingot may be produced using the molten steel by an ingot casting method. If necessary, the slab, bloom, or ingot may be subjected to blooming to produce a billet. The material (slab, bloom, or billet) is produced through the above steps.
[0091] [Hot working process] In the hot working process, a prepared raw material is hot worked to produce an intermediate steel material. When the steel material is a seamless steel pipe, the intermediate steel material corresponds to a mother pipe. First, a billet is heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The billet extracted from the heating furnace is hot worked to produce a mother pipe (seamless steel pipe). The hot working method is not particularly limited, and a well-known method may be used.
[0092] For example, a mother pipe may be produced by carrying out the Mannesmann process as the hot working. In this case, a round billet is pierced and rolled using a piercing mill. When piercing and rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The piercing-rolled round billet is further hot-rolled using a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative area reduction rate in the hot working process is, for example, 20 to 70%.
[0093] Other hot working methods may be used to produce a mother pipe from the billet. For example, in the case of a short, thick-walled steel material such as a coupling, the mother pipe may be produced by forging using the Erhardt method or the like. A mother pipe is produced through the above steps. The thickness of the mother pipe is not particularly limited, but is, for example, 9 to 60 mm.
[0094] When the steel material is round steel, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The material extracted from the heating furnace is subjected to hot working to produce an intermediate steel material having a circular cross section perpendicular to the axial direction. The hot working is, for example, blooming using a blooming mill or hot rolling using a continuous rolling mill. The continuous rolling mill has horizontal stands each having a pair of grooved rolls arranged side by side in the vertical direction, and vertical stands each having a pair of grooved rolls arranged side by side in the horizontal direction, arranged alternately.
[0095] When the steel material is a steel plate, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The material extracted from the heating furnace is hot-rolled using a blooming mill and a continuous rolling mill to produce an intermediate steel material in the shape of a steel plate.
[0096] The mother pipe produced by hot working may be air-cooled (as-rolled). The mother pipe produced by hot working may be quenched directly after the hot working without being cooled to room temperature, or may be quenched after being reheated after the hot working.
[0097] When quenching is performed directly after hot working or after reheating, cooling may be stopped or slow cooling may be performed during quenching. In this case, the occurrence of quench cracks in the mother pipe can be suppressed. When quenching is performed directly after hot working or after reheating, stress relief annealing (SR) may be performed after quenching and before the next heat treatment. In this case, residual stress in the mother pipe is removed.
[0098] As described above, in the preparation step, an intermediate steel material is prepared. The intermediate steel material may be manufactured by the above-mentioned preferred process, or may be manufactured by a third party, or may be manufactured in a factory or business establishment other than the factory where the quenching and tempering steps described below are performed. The quenching step will be described in detail below.
[0099] [Quenching Process] In the quenching process, a prepared intermediate steel material (blank pipe) is quenched. In this specification, "quenching" means rapidly cooling an intermediate steel material at or above the A3 point. Herein, the temperature of the intermediate steel material immediately before rapid cooling when quenching is performed is also referred to as the quenching temperature. Preferably, in the quenching process according to this embodiment, heating is performed in two stages, followed by rapid cooling. That is, the quenching process according to this embodiment includes a first heating process, a second heating process, and a rapid cooling process. Each process will be described in detail below.
[0100] [First Heating Step] Preferably, in the first heating step according to this embodiment, the prepared intermediate steel material (blank pipe) is heated to a heating temperature T1 (°C) and held for a heating time t1 (minutes). If the heating temperature T1 is too low, the austenite transformation may not be completed. In this case, the produced steel material will not have a yield strength of less than 552 to 655 MPa. On the other hand, if the heating temperature T1 is too high, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the produced steel material will not exhibit excellent low-temperature toughness in a cryogenic environment. Therefore, the heating temperature T1 (°C) in the first heating step is preferably set to 900 to 980°C.
[0101] Furthermore, if the heating time t1 is too short, the austenite transformation may not be completed. In this case, the produced steel material will not have a yield strength of less than 552 to 655 MPa. On the other hand, if the heating time t1 is too long, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the produced steel material will not exhibit excellent low-temperature toughness in an extremely low-temperature environment. Therefore, it is preferable to set the heating time t1 (minutes) of the first heating step to 5 to 15 minutes.
[0102] [Second Heating Step] Preferably, in the second heating step according to this embodiment, the intermediate steel material (blank pipe) heated in the first heating step is heated to a heating temperature T2 (°C) and maintained for a heating time t2 (minutes). If the heating temperature T2 is too low, carbides may not be sufficiently dissolved. In this case, the number density of coarse carbides in the produced steel material may be too high, and the produced steel material will not exhibit excellent low-temperature toughness in a cryogenic environment. On the other hand, if the heating temperature T2 is too high, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the produced steel material will not exhibit excellent low-temperature toughness in a cryogenic environment. Therefore, the heating temperature T2 (°C) in the second heating step is preferably set to 1000 to 1100°C.
[0103] Furthermore, if the heating time t2 is too short, the carbides may not be sufficiently solid-dissolved. In this case, the number density of coarse carbides in the produced steel material will be too high, and the steel material will not exhibit excellent low-temperature toughness in a cryogenic environment. On the other hand, if the heating time t2 is too long, the prior γ grain size DA may become coarse, and Fn1 may become too large. In this case, the produced steel material will not exhibit excellent low-temperature toughness in a cryogenic environment. Therefore, it is preferable to set the heating time t2 (minutes) of the second heating step to 3 to 10 minutes.
[0104] [Quenching Step] In the quenching step, the intermediate steel material (mother pipe) heated in the second heating step is quenched. In the quenching step, the intermediate steel material (mother pipe) is continuously cooled to continuously lower the surface temperature of the mother pipe. The method of continuous cooling is not particularly limited, and any well-known method may be used. Examples of continuous cooling methods include a method of immersing the mother pipe in a water bath for cooling, or a method of accelerated cooling of the mother pipe by shower water cooling or mist cooling.
[0105] If the cooling rate during quenching is too slow, the microstructure will not be mainly composed of tempered martensite and tempered bainite after the tempering step described below, and the mechanical properties specified in this embodiment will not be obtained. Here, in the rapid cooling step according to this embodiment, the average cooling rate during quenching when the surface temperature of the intermediate steel material (blank pipe) is in the range of 800 to 500°C is defined as the cooling rate during quenching, CR 800-500 Specifically, the cooling rate during quenching, CR 800-500is determined from the temperature measured at the slowest cooling location within the cross section of the intermediate steel being quenched (for example, the center of the thickness of the intermediate steel when both surfaces are forcedly cooled).
[0106] In the quenching step according to this embodiment, a preferred cooling rate during quenching CR 800-500 The cooling rate CR during quenching is preferably 60°C / min or more. 800-500 The lower limit of the cooling rate during quenching, CR, is 300°C / min, and more preferably 600°C / min. 800-500 The upper limit of the quenching rate is not particularly specified, but is, for example, 6000°C / min. The quenching process according to this embodiment can be carried out by the above steps. The tempering process will be described in detail below.
[0107] [Tempering Process] In the tempering process, tempering is carried out after the above-mentioned quenching. In this specification, "tempering" refers to the process of tempering the intermediate steel material after quenching. c1 This means that the steel is reheated to a temperature below the specified holding temperature and held therein. The holding temperature in the tempering process is adjusted as appropriate depending on the chemical composition of the steel and the yield strength to be obtained. In other words, the holding temperature is adjusted for an intermediate steel (blank pipe) having the chemical composition of this embodiment to adjust the yield strength of the steel to 80 to less than 95 ksi (552 to less than 655 MPa). Here, the holding temperature corresponds to the furnace temperature when the intermediate steel is heated and held therein after quenching. The holding time refers to the time from when the temperature of the intermediate steel reaches the specified holding temperature to when it is extracted from the heat treatment furnace.
[0108] The holding temperature is adjusted as appropriate depending on the chemical composition of the steel and the yield strength to be obtained. That is, the holding temperature is adjusted for an intermediate steel (blank pipe) having the chemical composition of this embodiment to adjust the yield strength of the steel to 552 to less than 655 MPa. In the tempering process according to this embodiment, the holding temperature is preferably 640 to 720°C.
[0109] If the holding time is too short, a microstructure mainly composed of tempered martensite and tempered bainite may not be obtained. On the other hand, if the holding time is too long, the above effect saturates. Therefore, in the tempering step of this embodiment, the holding time is preferably 20 to 180 minutes. A more preferable lower limit of the holding time is 30 minutes. A more preferable upper limit of the holding time is 150 minutes, and even more preferably 120 minutes.
[0110] The steel material according to this embodiment can be manufactured by the above manufacturing method. In the above manufacturing method, a method for manufacturing a steel pipe has been described as an example. However, the steel material according to this embodiment may be a steel plate or other shape. Similar to the above manufacturing method, a manufacturing method for a steel plate or other shape also includes, for example, a preparation step, a quenching step, and a tempering step. Furthermore, the above manufacturing method is an example, and the steel material may be manufactured by other manufacturing methods.
[0111] The present invention will be described in more detail below with reference to examples. Note that the examples described below are examples of conditions adopted to confirm the feasibility and effects of the steel material according to this embodiment. In other words, the steel material according to this embodiment is not limited to the examples described below.
[0112] 180 kg of molten steel having the chemical composition shown in Tables 2-1 and 2-2 was produced. Note that "-" in Tables 2-1 and 2-2 means that the content of the corresponding element was at the impurity level. Specifically, the V content, Nb content, Ti content, W content, Co content, Ni content, and Cu content of Test No. 1 were 0% when rounded to two decimal places. The Sn content of Test No. 1 was 0% when rounded to four decimal places. The Zr content, Ca content, Mg content, B content, and REM content of Test No. 1 were 0% when rounded to five decimal places.
[0113]
[0114]
[0115] Using the molten steel of each test number, a round billet was produced by continuous casting. The produced round billet of each test number was heated and hot-worked. Specifically, the round billet of each test number was subjected to hot rolling by the Mannesmann-mandrel method as the hot-working, to produce a mother pipe (seamless steel pipe) of each test number.
[0116] The obtained mother pipes of each test number were subjected to quenching and tempering. The quenching process involved two stages: a first heating stage and a second heating stage. Specifically, the mother pipes of each test number were heated at a heating temperature T1 (°C) for a heating time t1 (minutes) listed in the "Quenching Process" column of Table 3 in the first heating stage, and then at a heating temperature T2 (°C) for a heating time t2 (minutes) in the second heating stage. The heated mother pipes of each test number were water-cooled to perform quenching. The cooling rate CR during quenching of the mother pipes of each test number was 0.015. 800-500 The range of 60 to 6000°C / min was satisfied.
[0117]
[0118] Furthermore, the obtained mother pipes of each test number were tempered. Specifically, the mother pipes of each test number were tempered by holding them at the holding temperature (°C) for the holding time (minutes) shown in the "Tempering step" column in Table 3. Through the above manufacturing process, seamless steel pipes of each test number were obtained.
[0119] [Evaluation Tests] The seamless steel pipes having the respective test numbers after tempering were subjected to the following tensile tests, coarse carbide number density measurement tests, Fn1 measurement tests, and Charpy impact tests.
[0120] [Tensile Test] A tensile test was conducted on each seamless steel pipe according to ASTM E8 / E8M (2021). Specifically, a round bar test specimen with a parallel section diameter of 6 mm and a gauge length of 30 mm was prepared from the center of the wall thickness of each seamless steel pipe. The axial direction of the round bar test specimen was parallel to the axial direction of the seamless steel pipe. Using the prepared round bar tensile test specimen, a tensile test was conducted at room temperature (25°C) in air to obtain the yield strength (MPa) of the seamless steel pipe of each test number. In this example, the 0.2% offset proof stress (MPa) obtained in the tensile test was defined as the yield strength. The obtained yield strength for each test number is shown in Table 4 as "YS (MPa)".
[0121]
[0122] [Measurement test for number density of coarse carbides] A measurement test for number density of coarse carbides was carried out for each seamless steel pipe of each test number by the method described above. Specifically, a test piece was prepared from the center of the wall thickness of each seamless steel pipe of each test number, with the surface including the pipe axis direction and the pipe diameter direction as the observation surface. The observation surface of the prepared test piece was polished to a mirror finish, and then cut into 300 mm pieces. 2 In the observation surface (20 mm × 15 mm), particles identified from the contrast by the above-mentioned method were subjected to EDS analysis by the above-mentioned method to identify carbides. In this example, particles in which C was detected and the Fe content was 50 mass % or more were identified as carbides, similarly to the above-mentioned method.
[0123] Among the identified carbides, carbides with a circle equivalent diameter of 2 μm or more were identified using image analysis. Based on the total number of coarse carbides and the total area of the observation surface, the number density of the coarse carbides (pieces / mm 2 The number density of coarse carbides (pieces / mm 2 ) are shown in Table 4.
[0124] [Fn1 Measurement Test] For each seamless steel pipe of each test number, the prior γ grain size DA (μm), block diameter DB (μm), and Fn1 (= DA / DB) were determined by the above-mentioned method. Specifically, a test piece for measuring the prior γ grain size DA was prepared from the center of the wall thickness of each seamless steel pipe of each test number, with the plane including the pipe axis direction and the pipe diameter direction as the observation surface. The prepared test piece was embedded in resin, and the observation surface was polished to a mirror finish. After that, it was immersed for about 60 seconds in a solution of saturated aqueous picric acid mixed with an appropriate amount of surfactant, and the prior γ grain boundaries were revealed by etching. The etched 100 mm 2 The observation surface (10 mm × 10 mm) was observed with an optical microscope, and the grain size number was determined based on the cutting method in accordance with JIS G 0551 (2020). Using the determined grain size number, the prior austenite grain size (prior γ grain size DA) was determined by the method described above.
[0125] Next, test specimens for measuring the block diameter DB were prepared from the center of the wall thickness of each seamless steel pipe. EBSD measurements were performed on the test specimen's observation surface. EBSD measurements were performed at an acceleration voltage of 20 kV, with a field of view of 25 μm × 25 μm and a pitch of 0.1 μm. A crystal orientation diagram was obtained from the obtained Kikuchi line pattern, and regions surrounded by an orientation misorientation of 15° or more with adjacent crystals were identified to obtain a crystal orientation map. A region surrounded by an orientation misorientation of 15° or more was defined as one block. For the defined blocks, the average grain size (block diameter DB) of the block was determined using the method described above.
[0126] The prior γ grain size DA (μm) obtained for each test number is shown in the "DA (μm)" column of Table 4. The block diameter DB (μm) obtained for each test number is shown in the "DB (μm)" column of Table 4. Fn1 (= DA / DB) was calculated from the prior γ grain size DA (μm) and block diameter DB (μm) obtained for each test number. Table 4 shows the Fn1 obtained for each test number.
[0127] [Charpy Impact Test] A Charpy impact test in accordance with ASTM E23 (2018) was conducted on each seamless steel pipe of each test number. Specifically, a V-notch test specimen was prepared from the center of the wall thickness of each seamless steel pipe of each test number, with a notch surface perpendicular to the pipe axis direction and a longitudinal direction perpendicular to the pipe axis direction and the pipe diameter direction. A Charpy impact test was conducted on the prepared V-notch test specimen in accordance with ASTM E23 (2018). The test temperature was varied in 20°C increments from -120 to 20°C, with eight levels (-120°C, -100°C, -80°C, -60°C, -40°C, -20°C, 0°C, and 20°C). Two test specimens were used for each test temperature, and the brittle fracture surface ratio (%) of the test specimen after testing at each temperature was determined. The temperature (°C) at which the brittle fracture rate reached 50% was determined from an approximate curve obtained by plotting the test temperature (°C) versus the brittle fracture rate (%), thereby obtaining the fracture transition temperature vTrs (°C). The fracture transition temperature vTrs (°C) for each test number is shown in the "vTrs (°C)" column of Table 4.
[0128] [Evaluation Results] With reference to Tables 2-1, 2-2, 3, and 4, the seamless steel pipes of test numbers 1 to 38 had appropriate chemical compositions and the manufacturing methods also satisfied the preferred conditions described in the specification. As a result, these seamless steel pipes had a yield strength of 552 to less than 655 MPa and a coarse carbide number density of 10 / mm 2 or less, and Fn1 satisfied the range of 2.5 to 10.0. As a result, these seamless steel pipes had a fracture appearance transition temperature vTrs of -70°C or less, and had excellent low-temperature toughness even in an extremely low-temperature environment. It was also determined that the total volume fraction of tempered martensite and tempered bainite in all of these seamless steel pipes was 90% or more.
[0129] On the other hand, the seamless steel pipe of test number 39 had an excessively low C content and an excessively low Fn1. As a result, this seamless steel pipe had a fracture appearance transition temperature vTrs exceeding −70° C., and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0130] The seamless steel pipe of test number 40 had an excessively high Mn content, resulting in a fracture appearance transition temperature vTrs exceeding −70° C., and the seamless steel pipe did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0131] The seamless steel pipe of test number 41 had an excessively high P content. As a result, this seamless steel pipe had a fracture appearance transition temperature vTrs exceeding −70° C., and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0132] The seamless steel pipe of test number 42 had an excessively high S content. As a result, this seamless steel pipe had a fracture appearance transition temperature vTrs exceeding −70° C., and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0133] The seamless steel pipe of test number 43 had an excessively low Cr content, resulting in a fracture appearance transition temperature vTrs exceeding −70° C. and thus not having excellent low-temperature toughness in an extremely low-temperature environment.
[0134] The seamless steel pipe of test number 44 had an excessively high Cr content. As a result, the seamless steel pipe had a yield strength of 655 MPa or more, which was not the desired yield strength. As a result, the seamless steel pipe had a fracture appearance transition temperature (vTrs) exceeding -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0135] The seamless steel pipe of test number 45 had an excessively high Mo content, resulting in a fracture appearance transition temperature vTrs exceeding −70° C., and the seamless steel pipe did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0136] The seamless steel pipe of test number 46 had a holding temperature in the tempering process that was too low. As a result, the seamless steel pipe had a yield strength of 655 MPa or more, which was not the desired yield strength. As a result, the seamless steel pipe had a fracture appearance transition temperature (vTrs) exceeding -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0137] The seamless steel pipe of test number 47 was not subjected to the second heating step in the quenching process. As a result, the number density of coarse carbides in this seamless steel pipe was 10 pieces / mm 2 As a result, this seamless steel pipe had a fracture appearance transition temperature vTrs exceeding −70° C., and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0138] The seamless steel pipe of test number 48 had an excessively high heating temperature T2 in the second heating step of the quenching process. As a result, the seamless steel pipe had an Fn1 value of more than 10.0. As a result, the seamless steel pipe had a fracture appearance transition temperature vTrs of more than -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0139] The seamless steel pipe of test number 49 had an excessively long heating time t2 in the second heating step of the quenching process. As a result, the seamless steel pipe had an Fn1 value of more than 10.0. As a result, the seamless steel pipe had a fracture appearance transition temperature vTrs of more than -70°C, and did not have excellent low-temperature toughness in an extremely low-temperature environment.
[0140] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments within the scope of the present disclosure.
Claims
1. A steel material having the following components, in mass percent: C: 0.26-0.35%, Si: 0.10-1.00%, Mn: 1.00-1.40%, P: 0.015% or less, S: 0.0020% or less, Cr: 0.15-0.50%, Mo: 0.05-0.25%, sol. The steel material has an average yield strength of 552 to less than 655 MPa, and in which: 10 carbides per mm with a circle equivalent diameter of 2 μm or more 2 A steel material, wherein, when a prior austenite grain size is defined as DA and a block diameter is defined as DB, the DA and the DB satisfy formula (1): 2.5≦DA / DB≦10.0 (1) In formula (1), the prior austenite grain size (unit: μm) is substituted for DA, and the block diameter (unit: μm) is substituted for DB in formula (1).
2. The steel material according to claim 1, containing one or more elements selected from the group consisting of V: 0.01-0.60%, Nb: 0.01-0.03%, Ti: 0.01-0.05%, W: 0.01-0.50%, Zr: 0.0001-0.0050%, Co: 0.01-0.50%, Ni: 0.01-0.30%, Cu: 0.01-0.50%, Sn: 0.001-0.100%, Ca: 0.0001-0.0035%, Mg: 0.0001-0.0035%, B: 0.0001-0.0010%, and rare earth elements: 0.0001-0.0050%.
3. A steel material according to claim 1 or 2, which is a steel pipe.
Citation Information
Patent Citations
Steel pipe for oil well having excellent collapse strength, and testing method thereof
JP2002115028A
Low-alloy, high-strength seamless steel pipe for oil well
WO2017149570A1
CO2 corrosion resistant steel tube and preparation method thereof
CN112921250A
Seamless steel tube with high toughness and high corrosion resistance
JP2001073086A
Steel material with high toughness and method for manufacturing steel pipe thereof
JP2003041341A
Cited By
Seamless steel pipe and method for manufacturing seamless steel pipe
WO2026116398A1