Method for producing metal carbide and hydrocarbon, and carbon-containing member

The method of using a molten salt and carbon electrode to produce metal carbides at lower temperatures addresses the inefficiencies and high emissions of existing methods, achieving efficient metal carbide and hydrocarbon production with enhanced yield.

WO2024214618A1PCT designated stage expired Publication Date: 2024-10-17DAIKIN INDUSTRIES LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013772
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-25
Filing Date
2024-04-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current methods for producing metal carbides require high temperatures, resulting in low energy efficiency and significant carbon dioxide emissions, and existing methods for producing lithium carbide have low yields and require high-temperature processes.

Method used

A method involving the use of a molten salt containing alkali or alkaline earth metal ions and a carbon electrode to produce metal carbides at relatively low temperatures, followed by hydrolysis to obtain hydrocarbons, with the molten salt being substantially free of carbonate ions to enhance yield.

Benefits of technology

This method allows for the efficient production of metal carbides and hydrocarbons at lower temperatures, improving energy efficiency and increasing the yield of metal carbides while reducing carbon dioxide emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013772_17102024_PF_FP_ABST
    Figure JP2024013772_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for producing metal carbide comprises: preparing a molten salt containing at least one type of first metal ions selected from the group consisting of alkali metal ions and alkaline earth metal ions; readying an electrode containing carbon; and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing carbide of the first metal.
Need to check novelty before this filing date? Find Prior Art

Description

METHOD FOR PRODUCING METAL CARBIDE AND HYDROCARBON, AND CARBON-CONTAINING MEMBER

[0001] The present invention relates to a method for producing metal carbides and hydrocarbons, and to a carbon-containing component.

[0002] Acetylene is an industrially important substance as a raw material for various organic compounds. Acetylene is usually obtained by the reaction of metal carbide (mainly calcium carbide) with water.

[0003] Calcium carbide is generally obtained by heating a mixture of quicklime (calcium oxide) and coke to a high temperature in an electric furnace (see, for example, Patent Document 1). Patent Document 2, regarding the production of calcium carbide, proposes that coke is briquetted in advance and then mixed with quicklime. Patent Document 3 proposes a method for producing lithium carbide by reacting metallic lithium obtained by melt electrolysis of lithium chloride with carbon powder such as carbon black. Non-Patent Document 1 proposes a method for producing lithium carbide by reacting metallic lithium obtained by molten salt electrolysis of lithium hydroxide with a carbon source such as carbon dioxide. Non-Patent Document 2 proposes a method for producing lithium carbide by reacting metallic lithium with carbon.

[0004] JP-A No. 61-178412 JP-A No. 2018-35328 JP-A No. 2-256626

[0005] McEnaney JM, Rohr BA, Nielander AC, Singh AR, King LA, Norskov JK, Jaramillo TF, “A cyclic electrochemical strategy to produce acetylene from CO2, CH4, or alternative carbon sources.”, Sustain Energy Fuels 4:2, 752-2759 (2020)Uwe Ruschewitz, “Binary and ternary carbides of alkali and alkaline-earth Coordination Chemistry Reviews 244, 115-136 (2003)

[0006] To produce metal carbide, raw materials usually need to be heated to 2000°C or higher. This results in low energy efficiency and the generation of large amounts of carbon dioxide. Furthermore, Patent Documents 1 to 3 use carbon itself as the carbon source for metal carbide. Non-Patent Document 1 describes that when carbon dioxide is used as a carbon source, the theoretical yield of lithium carbide does not exceed 20%, but that the yield of lithium carbide can be increased by using carbon as a carbon source. However, no experimental data supporting this claim is presented. Non-Patent Document 2 describes the use of amorphous carbon or graphite as a carbon source, but to produce crystalline lithium carbide, it is necessary to contact metallic lithium vapor at 800°C to 900°C or to contact metallic lithium in an arc melting furnace at approximately 3500°C or higher.

[0007] The present disclosure aims to provide a production method in which a reaction proceeds quickly at a relatively low temperature (for example, 800°C or lower) and metal carbide can be efficiently obtained. The present disclosure also provides a method for producing hydrocarbons from the obtained metal carbide. In addition, the present disclosure provides a carbon-containing member supporting metal carbide.

[0008] The present disclosure includes the following aspects: [1] A method for producing metal carbide, comprising: preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; preparing an electrode containing carbon; and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing carbide of the first metal.

[0009] [2] The method for producing metal carbide according to the above [1], wherein the molten salt does not substantially contain carbonate ions.

[0010] [3] The method for producing metal carbide according to the above [1] or [2], wherein the electrode contains at least one material selected from the group consisting of glassy carbon, natural graphite, isotropic graphite, highly oriented pyrolytic graphite, plastic-formed carbon, and conductive diamond.

[0011] [4] The method for producing metal carbide according to any one of [1] to [3] above, wherein the electrode contains highly oriented pyrolytic graphite.

[0012] [5] The method for producing metal carbide according to any one of the above [1] to [4], wherein the molten salt contains at least one of a halide ion and an oxide ion as an anion.

[0013] [6] The method for producing metal carbide according to any one of the above [1] to [5], wherein the molten salt contains both halide ions and oxide ions as anions.

[0014] [7] The method for producing metal carbide according to the above [5] or [6], wherein the molten salt contains chloride ions as the halide ions.

[0015] [8] The method for producing metal carbide according to the above [5] or [6], wherein the molten salt contains fluoride ions as the halide ions.

[0016] [9] The method for producing metal carbide according to any one of [1] to [8] above, wherein the metal carbide composition further contains at least one selected from the group consisting of carbon, an elemental substance, a halide, a carbonate, an oxide, a hydride, and a peroxide of the first metal.

[0017]

[10] The method for producing metal carbide according to any one of the above [1] to [9], wherein the molten salt contains, as the first metal ions, at least one selected from the group consisting of lithium ions, sodium ions, and potassium ions, and calcium ions.

[0018]

[11] A method for producing hydrocarbons, comprising: preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; preparing an electrode containing carbon; applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing carbide of the first metal; and hydrolyzing the carbide of the first metal to obtain a gas containing hydrocarbons.

[0019]

[12] The method for producing hydrocarbons according to the above

[11] , wherein the hydrocarbon is acetylene.

[0020]

[13] The method for producing hydrocarbons according to

[11] or

[12] above, wherein the gas contains acetylene as the hydrocarbon and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0021]

[14] A carbon-containing member comprising: a substrate containing carbon; and a metal carbide composition supported on the substrate, the metal carbide composition comprising carbide of at least one first metal selected from the group consisting of alkali metals and alkaline earth metals.

[0022] According to the present disclosure, it is possible to provide a production method in which a reaction proceeds quickly at a relatively low temperature and metal carbide can be efficiently obtained, a method for producing hydrocarbons from the obtained metal carbide, and a carbon-containing member supporting metal carbide.

[0023] 1 is a flowchart illustrating a method for producing metal carbides according to the present disclosure; 2 is a flowchart illustrating a method for producing hydrocarbons according to the present disclosure;

[0024] In the method for producing metal carbide according to the present disclosure, a voltage is applied to a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions to obtain metal carbide. According to the method using this molten salt, the reaction proceeds quickly at a relatively low temperature of 800°C or less, and metal carbide can be obtained efficiently.

[0025] The present disclosure also encompasses the hydrolysis of metal carbides obtained by the above-mentioned method to obtain hydrocarbons, which can be efficiently obtained with high purity.

[0026] The present disclosure encompasses a carbon-containing component supported with a metal carbide, which can be utilized in the production of hydrocarbons.

[0027] [Method for Producing Metal Carbide] A method for producing metal carbide according to the present disclosure includes preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, preparing an electrode containing carbon, and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing carbide of the first metal. According to the method according to the present disclosure, the first metal carbide can be obtained in high yield. Figure 1 is a flowchart showing the method for producing metal carbide according to the present disclosure.

[0028] (I) Preparation of Molten Salt (S11) A molten salt containing a first metal ion is prepared. The first metal ion is a metal source for the target metal carbide. The molten salt is prepared by ionizing a salt containing the first metal ion (first metal salt). It is not necessary for all of the first metal salt to be ionized. For convenience, the metal salt contained in the electrolytic bath will be referred to as the molten salt, even if it is not completely ionized.

[0029] (First Metal Ion) The first metal ion is at least one selected from the group consisting of alkali metal ions and alkaline earth metal ions. Carbides of alkali metals and alkaline earth metals, also known as acetylides, are easily hydrolyzed to produce acetylene, and are therefore of great industrial value.

[0030] The alkali metal may be at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr). The alkali metal may be at least one selected from the group consisting of Li, Na, K, Rb, and Cs. The alkali metal may particularly be at least one selected from the group consisting of Li, Na, K, and Cs.

[0031] The alkaline earth metal may be at least one selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), and radium (Ra). The alkaline earth metal may be at least one selected from the group consisting of Mg, Ca, Sr, and Ba.

[0032] In terms of industrial value, the first metal ion may include an alkaline earth metal ion. The first metal ion may include an alkali metal ion together with the alkaline earth metal ion. This is because the alkali metal ion facilitates ionization of the alkaline earth metal salt, promoting the generation of alkaline earth metal ions, and lowering the melting point of the molten salt, enabling electrolysis at lower temperatures, thereby providing excellent electrolyte functions. The first metal ion may include at least one alkali metal ion selected from the group consisting of Li, Na, K, Rb, and Cs ions, and at least one alkaline earth metal ion selected from the group consisting of Be, Mg, Ca, Sr, and Ba ions. In particular, the first metal ion may include at least one Li, Na, and K ion, and Ca ions.

[0033] The amount of the first metal ions contained in the molten salt is not particularly limited. From the viewpoint of reaction efficiency, the number of moles of the first metal ions is preferably 1 mol% or more, more preferably 2 mol% or more, and particularly preferably 3 mol% or more, relative to the total number of moles of cations in the electrolytic bath. The number of moles of the first metal ions is preferably 20 mol% or less, more preferably 15 mol% or less, and particularly preferably 10 mol% or less, relative to the total number of moles of cations in the electrolytic bath. In one embodiment, the number of moles of the first metal ions is 1 mol% or more and 20 mol% or less, relative to the total number of moles of cations in the electrolytic bath.

[0034] (Other Metal Ions) The molten salt may contain metal ions (second metal ions) other than the first metal ions. The second metal ions are not particularly limited as long as they can stably precipitate the first metal carbide, which is the target substance. It is preferable that the salt of the second metal ions ionize at a temperature of 800°C or less.

[0035] The second metal may be at least one selected from the group consisting of rare earth elements, aluminum (Al), gallium (Ga), indium (In), thallium (Tl), zinc (Zn), cadmium (Cd), gold (Au), silver (Ag), and copper (Cu). The rare earth elements may include scandium (Sc), yttrium (Y), lanthanoid elements, and actinoid elements.

[0036] (Anion) Examples of counter ions (anions) of the first and second metal ions include halide ions, sulfate ions, phosphate ions, nitrate ions, acetate ions, carboxylate ions, and oxide ions (O 2- ) At least one selected from the group consisting of

[0037] The anions may include at least one of halide ions and oxide ions. In particular, the anions may include both halide ions and oxide ions. While oxides of the first metal are readily available, they tend to have high melting temperatures. Halides of the first metal are commonly used as molten salts. However, halide ions can generate halogen gas at the anode, which has high oxidizing power (and can cause corrosion). When the molten salt includes both halide ions and oxide ions, the generation of halogen gas can be suppressed while the melting temperature of the molten salt can be lowered.

[0038] The halogen may be at least one selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I), and astatine (At). The halogen may be at least one selected from the group consisting of F, Cl, Br, and I, and may particularly be F and / or Cl.

[0039] The first metal salt used in preparing the molten salt is, for example, a first metal salt containing an alkaline earth metal ion, specifically, CaO, CaCl 2 , CaF 2 , CaBr 2 , CaI 2 , CaH 2 , Ca 3 P 2 Specific examples of the first metal salt containing an alkali metal ion include LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI.

[0040] The molten salt is carbonate ions (CO 3 2- ) is preferably substantially free of 2CO. If the molten salt contains carbonate ions, they react with electrons generated by the discharge of the first metal (Equation 1), and carbon is likely to be produced. This reduces the yield of the first metal carbide. If the molten salt is substantially free of carbonate ions, this side reaction is suppressed, and the yield of the first metal carbide increases. (Equation 1) 2CO 32- +8e - → 2C + 6O 2-

[0041] "Substantially free of carbonate ions" allows for the presence of carbonate ions to an extent that they are not involved in the electrolytic reaction. The molten salt may contain, for example, about 1.0 mol% or less of carbonate ions. The carbonate ion concentration in the molten salt may be 0.5 mol% or less, 0.3 mol% or less, or 0 mol%.

[0042] (II) Preparation of carbon-containing electrode (S12) An electrode containing carbon (hereinafter, sometimes referred to as a "carbon electrode") is prepared. The carbon electrode functions as a cathode during electrolysis. The carbon contained in the carbon electrode serves as a carbon source for the target metal carbide.

[0043] The carbon may be present at least on the surface of the carbon electrode, where the surface of the carbon electrode is the portion that can come into contact with the first metal ion.

[0044] The raw material of the carbon electrode may be, for example, at least one carbon material selected from the group consisting of glassy carbon (GC), graphite, isotropic graphite, highly oriented pyrolytic graphite (HOPG), plastic-formed carbon (PFC) and conductive diamond. Among them, from the viewpoint of Faraday efficiency, a carbon material having a high degree of crystallinity may be used, such as HOPG. Other carbon materials having a high degree of crystallinity include, for example, graphene, carbon nanotubes, carbon nanohorns, and carbon fibers. The carbon electrode may be obtained by molding the above carbon material, for example, in the form of a woven fabric, nonwoven fabric, or felt.

[0045] Alternatively, the carbon electrode may be a molded body of a metal such as Ag, Cu, Ni, Pb, Hg, Tl, Bi, In, Sn, Cd, Au, Zn, Pd, Ga, Ge, Fe, Pt, Ru, Ti, Cr, Mo, W, V, Nb, Ta, Zr, or an alloy thereof, coated with the above-mentioned carbon material. The carbon electrode does not need to contain the first metal.

[0046] The material of the other electrode (anode) is not particularly limited. Examples of the material of the anode include Pt, conductive metal oxides, and the above-mentioned carbon materials. Examples of electrodes made of conductive metal oxides include transparent conductive electrodes called ITO electrodes in which a mixed oxide of indium and tin is formed on glass, electrodes called DSA electrodes (trademark of De Nora Permelec Electrodes Co., Ltd.) in which an oxide of a platinum group metal such as ruthenium or iridium is formed on a substrate such as titanium, and La 1-x Sr x FeO 3-δ (0≦x≦0.5 (particularly, 0.1≦x≦0.5), 0≦δ≦0.5), etc. Among these, conductive metal oxide anodes are preferred because they are less susceptible to consumption due to oxidation reactions.

[0047] (III) Applying a Voltage (S13) Subsequently, a voltage is applied to the molten salt. Carbon is reduced on the cathode (C≡C 2- ), reacts with the first metal ion to obtain a composition containing the first metal carbide (metal carbide composition). The application of voltage can also promote ionization of the first metal salt that has not been ionized in the molten salt.

[0048] When the first metal is Ca, calcium carbide (CaC 2 ) is produced (Equation 2). Calcium carbide typically deposits on the cathode. Metallic calcium may also be produced on the cathode through a side reaction (Equation 3). Some or all of the metallic calcium produced in this side reaction may further react to form calcium carbide. (Equation 2) Ca 2+ +2C +2e - → CaC 2 (Formula 3) Ca 2+ +2e - → Ca

[0049] The voltage is applied at a temperature at which the molten salt can be maintained in a molten state. The temperature of the electrolytic bath may be, for example, 350°C or higher, or 400°C or higher. The temperature of the electrolytic bath may be, for example, 800°C or lower, or 700°C or lower. According to the present disclosure, the reaction proceeds at such a relatively low temperature, resulting in high energy efficiency.

[0050] The applied voltage is set so that the cathode potential is lower (more noble) than the potential (Emc) at which the first metal precipitates on the carbon electrode. This can further improve the selectivity of the first metal carbide. If the cathode potential is excessively high (more noble), the desired first metal carbide is difficult to produce. If the cathode potential is excessively low (more noble), the first metal carbide is produced, but metals contained in the molten salt whose redox potential is higher (more noble) than the set cathode potential precipitate. If the molten salt contains multiple metals with similar redox potentials, an alloy of the multiple metals may precipitate depending on the set cathode potential. The potential Emc can be determined by performing cyclic voltammetry measurements in the molten salt using the carbon electrode (e.g., a HOPG electrode).

[0051] When constant current electrolysis is performed, the set current value may be appropriately set so that the cathode potential during electrolysis falls within the above-described potential range.

[0052] The metal carbide composition includes a carbide of a first metal. The first metal carbide is a major component of the metal carbide composition. A major component is a component that accounts for 50 mass% or more of the total mass of the metal carbide composition. The content of the first metal carbide may be 80 mass% or more, or 90 mass% or more, of the mass of the metal carbide composition. The content of the first metal carbide may be 99.9 mass% or less, or 99 mass% or less, of the mass of the metal carbide composition. In one embodiment, the content of the first metal carbide is 80 mass% or more and 99.9 mass% or less of the mass of the metal carbide composition.

[0053] The metal carbide composition is usually obtained in a state supported on a cathode (strictly speaking, a substrate derived from the carbon electrode used as the cathode). When a molten salt in which the first metal carbide has excellent solubility is used, the first metal carbide is obtained in a state in which it is partially or entirely dissolved in the molten salt. If the first metal carbide is dissolved in the molten salt in advance, the first metal carbide obtained by electrolysis is more likely to be deposited on the carbon electrode and is more likely to be obtained in a state in which it is supported on the substrate derived from the carbon electrode.

[0054] The metal carbide composition may include at least one selected from the group consisting of carbon, an elemental form, a halide, a carbonate, an oxide, a hydride, and a peroxide of a first metal, and may further include at least one selected from the group consisting of an elemental form, a halide, a carbonate, an oxide, and a carbide of a second metal.

[0055] The metal carbide composition may also contain at least one selected from the group consisting of solidified electrolytes (other metal salts), halides, oxides, metals, and hydrates of the materials constituting the device.

[0056] The carbon contained in the metal carbide composition is at least one selected from the group consisting of nanocarbon materials such as graphite, amorphous carbon, glassy carbon, carbon nanotubes, diamond, nanodiamond, and graphene. By subsequently performing the electrolysis of the above method, the first metal carbide can be further obtained from the carbon contained in the metal carbide composition. In this case, the yield can be further increased.

[0057] The presence of the first metal carbide, the first metal itself, compounds containing the first metal, and other impurities can be confirmed and their quantities can be determined, for example, by Raman spectroscopic analysis and X-ray diffraction (XRD) analysis of the composition.

[0058] [Carbon-Containing Member] The present disclosure encompasses a carbon-containing member comprising a substrate containing carbon and a metal carbide composition supported on the substrate, the metal carbide composition comprising a carbide of at least one first metal selected from the group consisting of alkali metals and alkaline earth metals. The carbon-containing member according to the present disclosure can be used for producing hydrocarbons.

[0059] The carbon-containing member can be obtained by, for example, the above-described method for producing a metal carbide. That is, the carbon-containing member can correspond to the carbon electrode obtained by electrolyzing the above-described molten salt using the above-described carbon electrode. In this case, the substrate is derived from the above-described carbon electrode.

[0060] The metal carbide composition may be supported on at least a portion of the surface of the substrate. The surface of the substrate typically corresponds to the portion of the carbon electrode that was in contact with the first metal ion. "Supported" includes a state in which at least a portion of the surface of the substrate is covered with the metal carbide composition.

[0061] However, after the carbon contained in the carbon electrode is consumed as a carbon source for the first metal carbide, it is again precipitated as the first metal carbide. Therefore, the substrate usually does not retain the original shape of the carbon electrode. In addition, the carbon electrode may contain metal carbide. Therefore, it may not be possible to clearly distinguish between the metal carbide contained in the carbon electrode before electrolysis and the metal carbide generated by electrolysis. In this case, for example, it is possible to confirm whether or not the carbon-containing member according to the present disclosure is a carbon-containing member as follows.

[0062] When elemental analysis is performed by energy dispersive X-ray analysis (EDX) on a cross section passing through the center (or center of gravity) of a carbon-containing component, a first metal and carbon are detected in the cross section. Because the substrate (carbon electrode) typically does not contain the first metal, the detection of the first metal and carbon can be safely considered to indicate the presence of a first metal carbide. Furthermore, if the concentration of the first metal is higher near the outer edge of the cross section than near the center, it can be safely considered that a substrate and a metal carbide composition supported thereon are present. This is because carbon present on the outer side of a carbon electrode is typically more reactive (more likely to become the first metal carbide) than the center. According to the above method, even if the boundary between the substrate and the metal carbide composition is unclear, it is possible to confirm whether the component is a carbon-containing component according to the present disclosure.

[0063] [Method for Producing Hydrocarbons] The present disclosure encompasses a method for producing hydrocarbons from a first metal carbide. That is, the method for producing hydrocarbons according to the present disclosure includes preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions, preparing an electrode containing carbon (carbon electrode), applying a voltage to the molten salt using the carbon electrode to obtain a metal carbide composition containing the first metal carbide, and hydrolyzing the first metal carbide to obtain a gas containing hydrocarbons. Figure 2 is a flowchart showing the method for producing hydrocarbons according to the present disclosure.

[0064] (1) Preparation of Molten Salt (S21) A molten salt is prepared in the same manner as in the preparation of molten salt (S11) in the above-described method for producing metal carbide.

[0065] (2) Preparation of carbon-containing electrode (S22) A carbon electrode is prepared in the same manner as in (II) Preparation of carbon-containing electrode (S12) in the above-mentioned method for producing metal carbide.

[0066] (3) Applying Voltage (S23) A voltage is applied to the molten salt in the same manner as in the voltage application (S13) in the above-described method for producing a metal carbide, thereby obtaining a composition containing the first metal carbide.

[0067] (4) Hydrolysis of Metal Carbide (S24) Next, the first metal carbide is brought into contact with water to hydrolyze it. This results in the production of a gas containing the target hydrocarbon. According to the present disclosure, the Faraday efficiency e for the production of hydrocarbons is improved. Hydrocarbons generally have low solubility in water. Therefore, the produced hydrocarbons are quickly released into the gas phase and recovered.

[0068] The first metal carbide may be isolated from the metal carbide composition and then hydrolyzed. Isolation is performed, for example, by pulverizing the metal carbide composition and utilizing the difference in specific gravity. Alternatively, the metal carbide composition may be hydrolyzed as is. For example, an electrode (which may be a "carbon-containing member" according to the present disclosure) on which the metal carbide composition has been deposited is brought into contact with water as is. In this case, the second metal carbide that may be contained in the metal carbide composition may also be hydrolyzed to produce hydrocarbons.

[0069] The hydrocarbons obtained include, for example, methane, ethane, ethylene, acetylene (C 2 H 2 ), methylacetylene, propane, propylene, butane, and butene. When an isolated first metal carbide is used or when the amount of impurities (particularly simple metals) contained in the composition is small, acetylene is obtained as the main component. The main component is a component that accounts for 50% by mass or more of the total mass of the recovered gas. Acetylene is an industrially important hydrocarbon.

[0070] The resulting gas may contain impurities such as water vapor, hydrogen, nitrogen, and oxygen in addition to hydrocarbons. The amount of impurities is preferably 10% by mass or less, more preferably 1% by mass or less, of the recovered gas. The amount of impurities may be 0.0001% by mass or more, or even 0.001% by mass or more, of the recovered gas. In one embodiment, the amount of impurities is 0.0001% by mass or more and 1% by mass or less of the recovered gas.

[0071] The resulting gas contains acetylene as a hydrocarbon, and may further contain at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene, and hydrogen.

[0072] The presence of hydrocarbons and impurities can be confirmed and their quantity can be determined, for example, by gas chromatography-mass spectrometry (GC-MS analysis), Fourier transform infrared absorption spectrometry (FT-IR analysis) equipped with a gas cell, or ultraviolet-visible absorption spectrometry (UV-Vis analysis) of the recovered gas.

[0073] The amount of water to be brought into contact with the composition is appropriately determined depending on the mass of the composition. The amount of water is, for example, at least the amount necessary for hydrolysis of the metal carbide and metal contained in the composition. In addition, it is desirable to use an amount of water that allows the entire composition to be immersed and that takes into account evaporation due to heat generated during hydrolysis.

[0074] Hydrolysis of the first metal carbide produces hydrocarbons as well as hydroxides of the first metal. For example, hydrolysis of calcium carbide produces calcium hydroxide along with acetylene (Equation 4). (Equation 4) CaC 2 +2H 2 O → C 2 H 2 + Ca(OH) 2

[0075] Although the embodiments of the present disclosure have been described above in detail, the present disclosure is not limited thereto.

[0076] In the above embodiments, examples of the carbon electrode include a metal compact coated with a carbon material and an electrode obtained by molding a carbon material. However, the present invention is not limited to these. The carbon electrode may be an electrode (typically a metal electrode) on which a carbon-containing composition is deposited (hereinafter referred to as a "third carbon electrode"). The third carbon electrode can be obtained, for example, by electrolyzing a molten salt containing a first metal ion derived from a first metal carbonate and carbonate ions. The third carbon electrode can also be obtained, for example, by electrolyzing a molten salt containing the first metal ion in the presence of carbonate ions derived from carbon dioxide. In these cases, the third carbon electrode is obtained as a cathode after the electrolysis.

[0077] The present invention will be explained in more detail with reference to the following examples, but the present invention is not limited to these examples.

[0078] [Example 1-1] (Production of Metal Carbide) Eutectic composition of LiCl, KCl, and CaCl 2 (LiCl / KCl / CaCl 2 = 52.3 mol% / 11.6 mol% / 36.1 mol% and 3.0 mol% CaO was mixed (i.e., LiCl / KCl / CaCl 2 / CaO = 50.8 mol% / 11.3 mol% / 35.0 mol% / 2.9 mol%) and dried in vacuum at 200°C and 100 Pa or less for 24 hours or more. Each of these mixed salts was placed in a glass container, placed in an electric furnace, and heated to 450°C. 2 A molten salt of CaO was obtained.

[0079] Next, a working electrode (1 cm x 1.5 cm HOPG), a counter electrode (coiled platinum wire), and a reference electrode (Ag + / Ag) was attached and the container was sealed with this lid. Subsequently, a voltage was applied for 30 minutes using a potentio-galvanostat while maintaining the potential of the working electrode relative to the reference electrode at 0.3 V. It was confirmed that a deposit had been deposited on the working electrode. All experimental operations were carried out in a glove box maintained in a high-purity argon atmosphere. The potential of the working electrode was measured between the reference electrode (Ag+ / Ag) and the cathode and calibrated using the Li-Ca alloy deposition potential as a standard.

[0080] (Production of Hydrocarbons) The precipitate was placed in a sealed test tube. Pure water was added to the test tube in small amounts at room temperature (23°C) to hydrolyze the precipitate. The total amount of water added was 2.5 ml. After confirming that foaming had occurred in the test tube, the test tube was left to stand until foaming no longer occurred. Subsequently, 100 μl (microliters) of gas was collected from the test tube using a gas-tight syringe.

[0081] The obtained gas was analyzed by GC-MS using a gas chromatograph (GC) and found to contain C as the main component. 2 H 2 It was confirmed that methane, ethane, and hydrogen were produced as by-products. The gas also contained water, carbon dioxide, nitrogen, oxygen, and argon. The amount of each component produced was also confirmed. 2 H 2 The mass proportion of was sufficiently more than 50 mass%. 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0082] C 2 H 2 The faradaic efficiency for gas production was calculated to be about 0.7%. It can be said that the higher the faradaic efficiency for hydrocarbon gas production, the higher the faradaic efficiency for metal carbide production.

[0083] [Example 1-2] A deposit and hydrocarbons were obtained in the same manner as in Example 1, except that a voltage was applied for 30 minutes while maintaining the potential of the working electrode relative to the reference electrode at 0.1 V. The hydrocarbons contained C as the main component. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes 2 H 2 The faradaic efficiency for gas production was calculated to be about 8.8%.

[0084] Examples 1-3 to 1-6 Precipitates and hydrocarbons were obtained in the same manner as in Example 1-1, except that constant-current electrolysis was performed while maintaining the current density at the value shown in Table 1. The hydrocarbons contained C as the main component. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 In Examples 1-4, the molten salt was previously added with CaC 2 was added in an amount of 2.0 mol % to the molten salt.

[0085]

[0086] Examples 2-1 to 2-5 Deposits and hydrocarbons were obtained in the same manner as in Example 1-1, except that graphite was used for the working electrode and electrolysis was performed under the conditions shown in Table 2. The hydrocarbons contained C as the main component. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0087]

[0088] [Examples 3-1 and 3-2] Precipitates and hydrocarbons were obtained in the same manner as in Example 1-1, except that GC was used as the working electrode and electrolysis was performed under the conditions shown in Table 3. The hydrocarbons contained C as the main component. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0089]

[0090] [Examples 4-1 to 4-7] Molten salts: NaCl, KCl, CaCl 2 (NaCl / KCl / CaCl 2 = 33.4 mol% / 11.6 mol% / 55.0 mol%), 3.0 mol% CaO and 7.0 mol% CaC 2 a mixture of NaCl, KCl, and CaCl 2 / CaO / CaC 2 Precipitates and hydrocarbons were obtained in the same manner as in Example 1-1, except that electrolysis was performed under the conditions shown in Table 4 using a ZnO / FeO mixture of 30.4 mol % / 10.5 mol % / 50.0 mol % / 2.7 mol % / 6.4 mol %. The potential of the working electrode was measured using a reference electrode (Ag + The potential between the electrode and the cathode was measured and calibrated using the Na-K-Ca alloy deposition potential as a standard. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0091]

[0092] [Examples 5-1 to 5-12] Molten salts: NaCl, KCl, CaCl 2 (NaCl / KCl / CaCl 2= 33.4 mol % / 11.6 mol % / 55.0 mol %), graphite was used for the working electrode, and electrolysis was performed at 550°C under the conditions shown in Table 5. In Examples 5-3 to 5-5, precipitates and hydrocarbons were obtained in the same manner as in Example 1-1. 2 was added to the molten salt at 1.0 mol %. In Examples 5-6 to 5-12, CaC 2 was added in an amount of 7.0 mol % to the molten salt.

[0093] The amount of gas (mL) generated by hydrolysis and the C calculated by analyzing the gas 2 H 2 The Faraday efficiency for the production is shown in Table 5. Tables 6 to 8 also show the gas production amount and the Faraday efficiency. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0094]

[0095] [Examples 6-1 to 6-10] Precipitates and hydrocarbons were obtained in the same manner as in Example 5-1, except that GC (glassy carbon) was used as the working electrode and electrolysis was performed under the conditions shown in Table 6. In Examples 6-3 to 6-5, CaC 2 was added to the molten salt at 1.0 mol %. In Examples 6-6 to 6-10, CaC 2 The hydrocarbon was added in an amount of 7.0 mol% to the molten salt. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0096]

[0097] [Examples 7-1 to 7-4] Precipitates and hydrocarbons were obtained in the same manner as in Example 5-1, except that HOPG (highly oriented pyrolytic graphite) was used as the working electrode and electrolysis was performed under the conditions shown in Table 7. In Examples 7-3 to 7-4, CaC 2 The hydrocarbon was added at 1.0 mol % to the molten salt. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0098]

[0099] [Examples 8-1 to 8-5] Precipitates and hydrocarbons were obtained in the same manner as in Example 5-1, except that PFC (plastic formed carbon) was used as the working electrode and electrolysis was performed under the conditions shown in Table 8. In Examples 8-1 to 8-5, CaC 2 The hydrocarbon was added in an amount of 7.0 mol% to the molten salt. 2 H 2 It was confirmed that it contains 2 H 2 Since gas is generated, the deposit on the working electrode is mainly composed of CaC 2 It can be understood that this includes:

[0100]

[0101] C 2 H 2 The Faraday efficiency e for production was calculated as follows: First, the C content in the recovered gas was calculated from the total area of ​​the peaks obtained from the GC-MS analysis and the calibration curve. 2 H 2 The volume ratio of the gas phase in the collection vessel and the volume of the gas phase in the calculated gas were calculated. 2 H 2 From the volume ratio of C 2 H 2 Finally, the volume of generated C 2 H 2was in standard conditions (0°C, 101 kPa), and the Faraday efficiency e (%) was calculated using the following formula.

[0102] As can be seen from Tables 1 to 8, the target first metal carbide was obtained by both constant-potential and constant-current electrolysis. In particular, when HOPG with a high degree of crystallinity was used as the working electrode, acetylene (first metal carbide) was obtained with high faradaic efficiency. 2 By using molten salt, hydrocarbons could be obtained from the resulting precipitate with higher Faraday efficiency. 2 It is desirable to add CaC 2 This is thought to be because the dissolution of the molten salt was suppressed.

[0103] The production method of the present disclosure is useful in various fields because the reaction proceeds quickly at a relatively low temperature and metal carbide can be obtained efficiently.

[0104] This application claims priority based on Japanese Patent Application No. 2023-064932 filed in Japan on April 12, 2023 and Japanese Patent Application No. 2024-048286 filed in Japan on March 25, 2024, the entire contents of which are incorporated herein by reference.

Claims

1. A method for producing metal carbide, comprising: preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; preparing an electrode containing carbon; and applying a voltage to the molten salt using the electrode to obtain a metal carbide composition containing carbide of the first metal.

2. The method for producing metal carbide according to claim 1, wherein the molten salt is substantially free of carbonate ions.

3. The method for producing metal carbide according to claim 1 or 2, wherein the electrode comprises at least one material selected from the group consisting of glassy carbon, natural graphite, isotropic graphite, highly oriented pyrolytic graphite, plastic formed carbon and conductive diamond.

4. A method for producing metal carbide according to any one of claims 1 to 3, wherein the electrode comprises highly oriented pyrolytic graphite.

5. A method for producing metal carbide according to any one of claims 1 to 4, wherein the molten salt contains at least one of halide ions and oxide ions as anions.

6. A method for producing metal carbide according to any one of claims 1 to 5, wherein the molten salt contains both halide ions and oxide ions as anions.

7. The method for producing metal carbide according to claim 5 or 6, wherein the molten salt contains chloride ions as the halide ions.

8. The method for producing metal carbide according to claim 5 or 6, wherein the molten salt contains fluoride ions as the halide ions.

9. The method for producing metal carbide according to any one of claims 1 to 8, wherein the metal carbide composition further comprises at least one selected from the group consisting of carbon, an elemental substance, a halide, a carbonate, an oxide, a hydride, and a peroxide of the first metal.

10. A method for producing metal carbide described in any one of claims 1 to 9, wherein the molten salt contains, as the first metal ion, one selected from the group consisting of lithium ions, sodium ions, and potassium ions, and calcium ions.

11. A method for producing hydrocarbons, comprising: preparing a molten salt containing at least one first metal ion selected from the group consisting of alkali metal ions and alkaline earth metal ions; preparing electrodes containing carbon; applying a voltage to the molten salt using the electrodes to obtain a metal carbide composition containing a carbide of the first metal; and hydrolyzing the carbide of the first metal to obtain a gas containing a hydrocarbon.

12. The method for producing hydrocarbons according to claim 11, wherein the hydrocarbon is acetylene.

13. The method for producing hydrocarbons according to claim 11 or 12, wherein the gas contains acetylene as the hydrocarbon, and further contains at least one selected from the group consisting of ethylene, ethane, methane, methylacetylene, propylene, butene and hydrogen.

14. A carbon-containing member comprising: a substrate comprising carbon; and a metal carbide composition supported on the substrate, the metal carbide composition comprising a carbide of at least one first metal selected from the group consisting of alkali metals and alkaline earth metals.

Citation Information

Patent Citations

  • Production of calcium carbide by blast furnace process

    JP1986178412A

  • Production of high-purity acetylene gas

    JP1990256626A

  • Manufacturing method of briquette and manufacturing method of calcium carbide

    JP2018035328A

  • Thermosetting resin composition, film, and article including the film