Method for producing polyester ether and method for producing molded body
The method of copolymerizing alkylene oxide with an oxygen-containing heterocyclic structure in the presence of a multimetal cyanide complex catalyst and organic solvent addresses the moldability issues of conventional polyester ether production, achieving high molecular weight and biodegradability, thus enabling effective polyester ether molding without increasing molecular weight with isocyanates.
Patent Information
- Application Number
- PCT/JP2024/013925
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional methods for producing polyester ether result in low molecular weight materials that are not suitable for molding, as they either remain as liquids or require increased molecular weight with isocyanates, limiting their moldability and usability as resins.
A method involving copolymerization of alkylene oxide with a compound having an oxygen-containing heterocyclic structure in the presence of a multimetal cyanide complex catalyst and a specific organic solvent, achieving a weight average molecular weight of 40,000 or more, allowing for the production of polyester ether that can be molded without increasing molecular weight with isocyanates.
The method enables the production of polyester ether with enhanced moldability, achieving a maximum point cohesive force of 5.0 N/mm² and maximum point elongation of 5% or more, while maintaining biodegradability and suitable for various applications such as agricultural and civil engineering materials.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Method for producing polyester ether and method for producing molded article
[0001] The present invention relates to a method for producing a polyester ether and a method for producing a molded article.
[0002] Forming a film by reacting a polyester ether polyol with an isocyanate has been conventionally practiced (see, for example, Patent Document 1). Also, producing a polyester ether poly(mono)ol has been conventionally practiced by ring-opening addition polymerization (copolymerization) of an alkylene oxide and a compound having an oxygen-containing heterocyclic structure to an initiator having a hydroxyl group in the presence of a composite metal cyanide complex catalyst (hereinafter also referred to as "DMC catalyst") (see, for example, Patent Document 2). Furthermore, producing a polyether polyol has been conventionally practiced by ring-opening addition polymerization of an alkylene oxide to an initiator in the presence of a DMC catalyst and an organic solvent (see, for example, Patent Document 3).
[0003] International Publication No. WO 2011 / 034030 International Publication No. WO 2007 / 020879 International Publication No. WO 2013 / 157486
[0004] However, the polyester ether polyol described in Patent Document 1 has a small molecular weight of 300 to 5,000, and therefore requires polymerization with isocyanate in order to be molded into a resin. Furthermore, the polyester ether poly(mono)ol produced by the method described in Patent Document 2 has the problem that it cannot be used as a resin for molding as is. Furthermore, the polyether polyol produced by the method described in Patent Document 3 is a liquid and does not become a solid resin, so it has the problem of not exhibiting moldability. Under these circumstances, there has been a demand for the development of a polyester ether that can be molded without polymerization with isocyanate or the like.
[0005] The present invention has been made to solve such problems, and provides a method for producing a polyester ether that can produce a moldable polyester ether without increasing the molecular weight with isocyanates or the like, and a method for producing a molded article by molding the polyester ether to produce a molded article.
[0006] The present inventors conducted extensive research to solve the above-mentioned problems, and as a result, discovered that the above-mentioned problems can be solved by copolymerizing a specific compound (hereinafter also referred to as an "initiator compound") with a specific alkylene oxide and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and an ester bond in the presence of a DMC catalyst and a predetermined amount of a specific organic solvent, thereby completing the present invention. The present invention includes the following items [1] to
[10] . [1] A method for producing a polyester ether, comprising copolymerizing a compound having at least one active hydrogen atom per molecule with an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and an ester bond in the presence of a double metal cyanide complex catalyst and an organic solvent, to obtain a polyester ether having a weight-average molecular weight of 40,000 or more, wherein the organic solvent has a relative dielectric constant of 18.0 or less and 10 to 400 parts by mass of the organic solvent is used per 100 parts by mass of the polyester ether. [2] The method for producing a polyester ether according to [1] above, wherein the organic solvent is used in an amount of 20 to 150 parts by mass per 100 parts by mass of the polyester ether. [3] The method for producing a polyester ether according to [1] or [2] above, wherein the compound having an oxygen-containing heterocyclic structure is a cyclic ester or an acid anhydride. [4] The method for producing a polyester ether according to any one of [1] to [3] above, wherein the alkylene oxide is at least one selected from the group consisting of ethylene oxide and propylene oxide. [5] The method for producing a polyester ether according to any one of [1] to [4] above, wherein the mass ratio of the alkylene oxide to the compound having an oxygen-containing heterocyclic structure (alkylene oxide:compound having an oxygen-containing heterocyclic structure) is 20:80 to 99:1. [6] The method for producing a polyester ether according to any one of [1] to [5] above, wherein the glass transition temperature of the polyester ether is −50° C. or lower. [7] The method for producing a polyester ether according to any one of [1] to [6] above, wherein the melting point of the polyester ether is 50° C. or higher. [8] The method for producing a polyester ether according to any one of [1] to [7] above, wherein the polyester ether is biodegradable.[9] A method for producing a molded article by molding the polyester ether obtained by the method according to the above [1] or [2].
[10] The molded article has a maximum cohesive strength of 5.0 N / mm. 2
[11] The method for producing a molded article according to the above [9], wherein the molded article has a maximum elongation of 5% or more.
[0007] According to the present invention, there are provided a method for producing a polyester ether that can produce a moldable polyester ether without increasing the molecular weight with isocyanate or the like, and a method for producing a molded article by molding the polyester ether.
[0008] The meanings and definitions of terms used in this specification are as follows. In this specification, "alkylene oxide" means "a compound in which the unsaturated group of a monoalkene has been epoxidized." In this specification, the "relative permittivity of an organic solvent" is "a numerical value obtained by rounding off to one decimal place the relative permittivity value described in the Chemistry Handbook, Basic Edition, Revised 5th Edition, edited by the Chemical Society of Japan, I-770 to 777." In this specification, a numerical range expressed as "to" means a numerical range in which the numerical values before and after "to" are the lower and upper limits. In this specification, for preferred numerical ranges (e.g., ranges of content, etc.), the lower and upper limits described in stages can be independently combined. For example, from the description "preferably 10 to 90, more preferably 30 to 60," the "preferable lower limit (10)" and the "more preferable upper limit (60)" can be combined to form "10 to 60." In this specification, "an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring" is sometimes simply referred to as "alkylene oxide." In the description herein of "a compound having an oxygen-containing heterocyclic structure other than the (above-mentioned) alkylene oxide having an ester bond," it is not the "alkylene oxide" that has the ester bond but the "compound having an oxygen-containing heterocyclic structure." Furthermore, in the present specification, the "compound having an oxygen-containing heterocyclic structure other than the (above-mentioned) alkylene oxide having an ester bond" may also be simply referred to as the "compound having an oxygen-containing heterocyclic structure."
[0009] [Method for Producing Polyester Ether] The method for producing a polyester ether of the present invention involves copolymerizing a compound having at least one active hydrogen atom per molecule with an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring, and a compound other than the alkylene oxide and having an ester bond and an oxygen-containing heterocyclic structure, in the presence of a composite metal cyanide complex catalyst and an organic solvent, to obtain a polyester ether having a weight-average molecular weight of 40,000 or more, wherein the organic solvent has a relative dielectric constant of 18.0 or less, and 10 to 400 parts by mass of the organic solvent is used per 100 parts by mass of the polyester ether. This method for producing a polyester ether enables the production of a moldable polyester ether without increasing the molecular weight with isocyanate or the like.
[0010] <Polyester Ether> The polyester ether produced by the production method of the present invention is obtained by copolymerizing an initiator compound with a compound having an oxygen-containing heterocyclic structure containing a specific alkylene oxide in the presence of a DMC catalyst and a specific organic solvent, and is not particularly limited as long as it has a weight-average molecular weight (Mw) of 40,000 or more. It usually has an ether bond and an ester bond, and is preferably biodegradable. Biodegradability refers to the property of being decomposed by the action of microorganisms present in nature. Specifically, the biodegradability in the present invention preferably exhibits a decomposition rate of 60% or more in 28 days in the evaluation according to OECD TG301C.
[0011] The weight average molecular weight (Mw) of the polyester ether is not particularly limited as long as it is 40,000 or more, but from the viewpoint of deterioration resistance, it is preferably 40,000 to 200,000, more preferably 40,000 to 90,000, and particularly preferably 40,000 to 70,000. The weight average molecular weight (Mw) is measured by the method described in the examples.
[0012] The molecular weight distribution (Mw / Mn) of the polyester ether is not particularly limited, but from the viewpoint of achieving a uniform melting point, it is preferably 1.0 to 3.5, more preferably 1.2 to 3.2, and particularly preferably 1.4 to 2.9. The molecular weight distribution (Mw / Mn) is measured by the method described in the Examples.
[0013] The glass transition temperature of the polyester ether is not particularly limited, but from the viewpoint of ensuring flexibility, it is preferably −10° C. or lower, more preferably −70 to −20° C., and particularly preferably −70 to −50° C. The glass transition temperature is measured by the method described in the examples.
[0014] The melting point of the polyester ether is not particularly limited, but from the viewpoint of moldability, it is preferably 50° C. or higher, more preferably 50 to 230° C., and particularly preferably 50 to 200° C. The melting point is measured by the method described in the examples.
[0015] The product produced by the production method of the present invention is only required to contain a polyester ether, and may also contain polyethers other than polyester ether. The content of the polyester ether in the product produced by the production method of the present invention is not particularly limited, but is preferably 40 mass% or more, more preferably 50 mass% or more, even more preferably 70 mass% or more, and particularly preferably 80 mass% or more.
[0016] <Double metal cyanide complex catalyst (DMC catalyst)> The double metal cyanide complex catalyst used in the production method of the present invention is not particularly limited as long as it is a DMC catalyst that is commonly used in the production of polyester ethers. For example, a compound represented by the following general formula (1) can be mentioned.
[0017] M 1 a [M 2 b (CN) c ] d e(M 3 f X g ) h(H 2 O)i(L)...(1) (In formula (1), M 1 ~M 3represents a metal, X represents a halogen atom, L represents an organic ligand, and a, b, c, d, e, f, g, h, and i represent numbers that may change depending on the valence of the metal, the coordination number of the organic ligand, etc.)
[0018] In the above general formula (1), M 1 and M 3 The metal represented by the formula (1) is preferably a metal selected from the group consisting of Zn(II), Fe(II), Fe(III), Co(II), Ni(II), Mo(IV), Mo(VI), Al(III), V(V), Sr(II), W(IV), W(VI), Mn(II), Cr(III), Cu(II), Sn(II), and Pb(II), and more preferably Zn(II) or Fe(II). 2 The metal represented by the formula (1) is preferably a metal selected from Fe(II), Fe(III), Co(II), Co(III), Cr(II), Cr(III), Mn(II), Mn(III), Ni(II), V(IV), and V(V), and more preferably Co(III) or Fe(III). The Roman numerals II, III, IV, V, etc. in parentheses following the metal element symbol indicate the atomic valence. In the formula (1), M 1 and M 3 may be the same as or different from each other, but are preferably the same as each other.
[0019] In the general formula (1), L representing the organic ligand is preferably at least one compound selected from the group consisting of alcohols, ethers, ketones, esters, amines, and amides. Among these, water-soluble organic ligands such as tert-butyl alcohol, n-butyl alcohol, sec-butyl alcohol, iso-butyl alcohol, tert-pentyl alcohol, iso-pentyl alcohol, N,N-dimethylacetamide, ethylene glycol dimethyl ether (also called glyme), diethylene glycol dimethyl ether (also called diglyme), triethylene glycol dimethyl ether (also called triglyme), ethylene glycol mono-tert-butyl ether, isopropyl alcohol, and dioxane are more preferred. As the dioxane, either 1,4-dioxane or 1,3-dioxane may be used, with 1,4-dioxane being preferred.
[0020] In the DMC catalyst used in the production method of the present invention, more preferred organic ligands L are tert-butyl alcohol alone or a combination of tert-butyl alcohol and one of the compounds exemplified above. Among these, tert-butyl alcohol alone and a combination of tert-butyl alcohol and ethylene glycol mono-tert-butyl ether are particularly preferred. DMC catalysts having such organic ligands exhibit high catalytic activity in the copolymerization reaction (ring-opening addition polymerization reaction) of alkylene oxide or the like with the initiator compound used in the production method of the present invention, and can produce polyester ethers with a narrow molecular weight distribution and low viscosity.
[0021] The DMC catalyst used in the production method of the present invention can be produced by a conventionally known production method. The conventionally known production method is not particularly limited, and the catalyst can be produced using any production method. As a production method for a DMC catalyst having an organic ligand that is preferably used in the present invention, for example, the method described in JP-A-2003-117403 can be used. More specifically, examples of the method include (i) a method in which an organic ligand is coordinated to the reaction product obtained by reacting a metal halide salt with a cyanometallate acid and / or an alkali metal cyanometalate in an aqueous solution, followed by separating the resulting solid component and washing the separated solid component with an organic ligand aqueous solution, or (ii) a method in which a metal halide salt is reacted with a cyanometallate acid and / or an alkali metal cyanometalate in an organic ligand aqueous solution, separating the resulting reaction product (solid component), and washing the separated solid component with an organic ligand aqueous solution, followed by filtering and separating the resulting cake (solid component) and drying the resulting cake.
[0022] The metal constituting the cyanometalate of the alkali metal cyanometalate used in producing a DMC catalyst is preferably one or more metals selected from the group consisting of Fe(II), Fe(III), Co(II), Co(III), Cr(II), Cr(III), Mn(II), Mn(III), Ni(II), V(IV) and V(V), more preferably Co(III) or Fe(III), and particularly preferably Co(III).
[0023] The cyanometallate acids and alkali metal cyanometallates used as raw materials for producing the DMC catalyst include H 3 [Co(CN) 6 ], Na 3 [Co(CN) 6 ], or K 3 [Co(CN) 6 ] is preferred, and Na 3 [Co(CN) 6 ] or K 3 [Co(CN) 6 ] is more preferred.
[0024] Furthermore, in the method for producing a DMC catalyst, a polyether compound can be mixed with a liquid obtained by dispersing a solid component in an aqueous organic ligand solution at a stage before filtering and separating the cake, and water and excess organic ligand can be distilled off from the resulting mixed liquid to prepare a slurry DMC catalyst mixture in which the DMC catalyst is dispersed in the polyether compound (hereinafter also referred to as a "slurry DMC catalyst").
[0025] The polyether compound used to prepare the slurry DMC catalyst can be separated from the DMC catalyst during the production of polyester ether, and the separated DMC catalyst can be used in the production of polyester ether. However, this polyether compound is preferably used as part or all of the initiator compound described below. This polyether compound is copolymerized with an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound other than the alkylene oxide having an ester bond and an oxygen-containing heterocyclic structure to obtain the desired polyester ether. The polyether compound used for this purpose preferably has 1 to 8 hydroxyl groups and a number average molecular weight (Mn) of 300 to 5,000. This is preferred because it increases the catalytic activity of the DMC catalyst and does not increase the viscosity of the slurry DMC catalyst, making it easy to handle.
[0026] The amount of DMC catalyst added is not particularly limited, but from the viewpoint of narrowing the molecular weight distribution, it is preferably 10 to 500 ppm by mass, more preferably 20 to 300 ppm by mass, and even more preferably 30 to 200 ppm by mass, relative to 100% by mass of the polyester ether produced by the production method of the present invention.
[0027] <Organic Solvent> The organic solvent used in the production method of the present invention is not particularly limited as long as it has a dielectric constant of 18.0 or less. However, organic solvents having a dielectric constant of 1.0 to 8.0 are preferred, organic solvents having a dielectric constant of 1.5 to 8.0 are more preferred, and organic solvents having a dielectric constant of 1.7 to 3.0 are even more preferred. When the dielectric constant is 18.0 or less, a high molecular weight polyester ether can be produced. The lower limit of the dielectric constant of the organic solvent is not particularly limited, but is typically 1.0 or more. When the dielectric constant is within the preferred range, the organic solvent does not deactivate the DMC catalyst and does not inhibit the copolymerization reaction between an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and having an ester bond, and therefore it is presumed that a preferred polyester ether can be produced.
[0028] In the present invention, the amount of organic solvent used is expressed as a mass ratio relative to 100 parts by mass of the polyester ether produced. Since the total mass of the polyester ether produced is equal to the combined mass of the initiator compound, alkylene oxide, and the cyclic ester and acid anhydride in the compound having an oxygen-containing heterocyclic structure, this mass ratio is the same as the combined mass of the initiator compound, alkylene oxide, and the cyclic ester and acid anhydride in the compound having an oxygen-containing heterocyclic structure, relative to 100 parts by mass.
[0029] Specific examples of such organic solvents and their dielectric constants (indicated by the numbers in parentheses) include hexane (1.9), octane (1.9), 1,4-dioxane (2.2), carbon tetrachloride (2.2), toluene (2.4), diethyl ether (4.2), ethyl acetate (6.0), acetic acid (6.2), tetrahydrofuran (7.6), dichloromethane (8.9), cyclohexanol (15.0), 1-butanol (17.5), etc. Among these, hexane, toluene, and tetrahydrofuran are preferred in view of their suitability as organic solvents that do not react with the initiator compound, alkylene oxide, and compound having an oxygen-containing heterocyclic structure, their odor, environmental impact, and boiling point.
[0030] Furthermore, when the polyester ether is used as a raw material for products such as urethane prepolymers and modified silicone polymers without removing the organic solvent, it is preferable to use the organic solvent used in the products in the production of the polyester ether.
[0031] The amount of organic solvent used is not particularly limited as long as it is 10 to 400 parts by mass per 100 parts by mass of the polyester ether to be produced, but is preferably 15 to 300 parts by mass, more preferably 20 to 150 parts by mass, even more preferably 25 to 130 parts by mass, and particularly preferably 30 to 110 parts by mass. A use amount equal to or greater than the lower limit of the preferred range is preferred in that a polyester ether with a low viscosity can be produced. On the other hand, a use amount equal to or less than the upper limit of the preferred range is preferred in that a polyester ether with an extremely high molecular weight can be easily produced.
[0032] After the copolymerization reaction is complete, the organic solvent can be removed by degassing under reduced pressure or the like, but it is also possible not to remove it, or to leave a necessary amount of the organic solvent. By leaving the organic solvent in the polyester ether, when it is used as a raw material for a urethane prepolymer or a modified silicone polymer, it is easy to handle due to its low viscosity, and the organic solvent can be used as it is as a raw material for producing the product.
[0033] When the organic solvent is to be removed sufficiently, the amount of the organic solvent used is preferably 10 to 150 parts by mass per 100 parts by mass of the polyester ether to be produced.
[0034] <Initiator Compound> The initiator compound used in the production method of the present invention is a compound having at least one active hydrogen atom per molecule. As the compound having an active hydrogen atom, a compound having a hydroxyl group is preferred in that it does not inhibit the activity of the DMC catalyst, and more specifically, a compound having 1 to 12 hydroxyl groups and a weight average molecular weight (Mw) of 18 to 30,000 is preferred. When the initiator compound has one hydroxyl group, a polyester ether having one hydroxyl group, such as a polyester ether monool, is obtained. When the initiator compound has two or more hydroxyl groups, a polyester ether having two or more hydroxyl groups, such as a polyester ether polyol, is obtained.
[0035] Specific examples of the initiator compound include monohydric alcohols such as methanol, ethanol, 2-propanol, n-butanol, iso-butanol, 2-ethylhexanol, decyl alcohol, lauryl alcohol, tridecanol, cetyl alcohol, stearyl alcohol, and oleyl alcohol; water; ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,4-cyclohexanediol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanediol, and polyethylene. dihydric alcohols such as glycol, polypropylene glycol, polycarbonate diol, and polytetramethylene glycol; trihydric or higher polyhydric alcohols such as glycerin, diglycerin, trimethylolpropane, pentaerythritol, dipentaerythritol, and tripentaerythritol; sugars or derivatives thereof such as glucose, sorbitol, dextrose, fructose, sucrose, and methyl glucoside; phenols such as bisphenol A, bisphenol F, bisphenol S, novolak, resol, and resorcinol; and esters such as polycaprolactone and polylactic acid. These compounds can be used alone or in combination of two or more.
[0036] Polyester ethers obtained by polymerizing these compounds with alkylene oxides having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than alkylene oxides having an ester bond using known methods can also be used as initiator compounds. The weight-average molecular weight (Mw) of these polyester ethers is not particularly limited, but from the viewpoint of not requiring further molecular weight increase using isocyanates, it is preferably 10,000 to 30,000, more preferably 15,000 to 30,000, and particularly preferably 20,000 to 25,000. The number of hydroxyl groups per molecule of these polyols is not particularly limited, but is preferably 1 to 12, more preferably 1 to 8, and particularly preferably 1 to 6. Using an initiator compound with a hydroxyl group count equal to or less than the above upper limit tends to narrow the molecular weight distribution of the resulting polyester ether. When two or more compounds are used in combination as initiator compounds, the average number of hydroxyl groups per molecule is preferably 1 to 12, more preferably 1 to 8, and particularly preferably 1 to 4.
[0037] The weight-average molecular weight (Mw) of the initiator compound is not particularly limited, and is preferably 18 to 30,000, more preferably 400 to 25,000, and particularly preferably 700 to 20,000. By using an initiator compound with a weight-average molecular weight (Mw) of 400 or more, the time until the initial process using alkylene oxide in the presence of a DMC catalyst begins can be shortened. Using an initiator compound with a weight-average molecular weight (Mw) of 20,000 or less is preferable because the viscosity is not too high when the initiator compound is charged into a reactor. The molecular weight distribution (weight-average molecular weight (Mw) / number-average molecular weight (Mn)) of the initiator compound is not particularly limited, and from the viewpoint of uniforming the melting point, it is preferably 1.000 to 2.000, more preferably 1.100 to 1.700, and particularly preferably 1.200 to 1.500.
[0038] In addition, when the initiator compound is composed only of molecules of the same molecular weight, such as a low-molecular-weight alcohol, the molecular weight calculated from the chemical formula is the weight-average molecular weight (Mw). The weight-average molecular weight (Mw) of the initiator compound is lower than the weight-average molecular weight (Mw) of the polyester ether obtained using it. The difference between the weight-average molecular weight of the initiator compound and the weight-average molecular weight of the polyester ether obtained using it (i.e., the amount of units formed by ring-opening of an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and an ester bond) is preferably 5,000 or more, and particularly preferably 10,000 or more. When the difference in weight-average molecular weight is 5,000 or more, the amount of polymerization in the presence of a DMC catalyst increases, making it easier to obtain the benefits of polymerization in the presence of a DMC catalyst. Furthermore, in the production method of the present invention, even a small amount of the initiator compound increases the apparent mass by reacting with an organic solvent, making it less susceptible to the limitations of the stirring device and cooling device in the stirrer. Therefore, even when the difference in weight-average molecular weight between the initiator compound and the polyester ether is large, production is more feasible than without using an organic solvent.
[0039] When the resulting polyester ether is used as a raw material for resins such as polyurethane or modified silicones, the number of hydroxyl groups in the polyester ether is preferably 1 to 12, more preferably 2 to 8, and particularly preferably 2 to 6. Therefore, the number of hydroxyl groups in the initiator compound for producing such polyester ether is preferably 1 to 12, more preferably 2 to 8, and particularly preferably 2 to 6. When two or more initiator compounds are used, the average number of hydroxyl groups in the initiator compounds is preferably 1.5 to 8, more preferably 1.8 to 6, and particularly preferably 1.8 to 3.
[0040] The amount of the initiator compound to be added is not particularly limited, but from the viewpoint of sufficient stirring and utilizing as much of the free space in the reaction vessel as possible for the copolymerization reaction, it is preferably 1 to 30% by volume of the reactor volume, more preferably 5 to 20% by volume, and even more preferably 6 to 15% by volume. When the amount of the initiator compound charged is small, an organic solvent having a relative dielectric constant of 18.0 or less can also be used in combination.
[0041] <Alkylene oxide, compound having an oxygen-containing heterocyclic structure> In the production method of the present invention, the compound copolymerized with the initiator compound is an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring, and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and having an ester bond. The term "compound having an oxygen-containing heterocyclic structure" generally refers to a compound having an oxygen-containing heterocyclic structure composed of two or more carbon atoms and one or more oxygen atoms. Because the production method of the present invention is a method for producing polyester ethers, the compound having an oxygen-containing heterocyclic structure used in the production method of the present invention contains components derived from ester bonds, such as cyclic esters and acid anhydrides. Examples of compounds having an oxygen-containing heterocyclic structure include cyclic esters, acid anhydrides, and cyclic carbonates. The compound having an oxygen-containing heterocyclic structure used in the production method of the present invention is preferably a cyclic ester or acid anhydride.
[0042] In the production method of the present invention, specific examples of a method of using in combination an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than an alkylene oxide and an ester bond include a method of reacting a mixture of an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and a compound having an oxygen-containing heterocyclic structure other than an alkylene oxide and an ester bond with an initiator compound, and a method of reacting the two compounds separately. When the compound having an oxygen-containing heterocyclic structure other than an alkylene oxide having an ester bond is a compound that is difficult to copolymerize alone (such as a carboxylic acid anhydride), it is preferable to use it in a mixture with an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring.
[0043] <<Alkylene oxide having 2 to 20 carbon atoms and having an epoxy ring>> The number of carbon atoms in the alkylene oxide having 2 to 20 carbon atoms and having an epoxy ring is not particularly limited as long as it is 2 to 20, and 2 to 6 is preferred. Examples of alkylene oxides having 2 to 20 carbon atoms and having an epoxy ring include ethylene oxide (hereinafter referred to as "EO"), propylene oxide (hereinafter referred to as "PO"), 1,2-butene oxide, 2,3-butene oxide, and epoxidized products of 5 to 12 α-olefins. Two or more types of alkylene oxides having 2 to 20 carbon atoms and having an epoxy ring to be reacted with the initiator compound may be used. When two or more types are used, they may be reacted as a mixture or separately. EO and PO are particularly preferred as the alkylene oxide having 2 to 20 carbon atoms and having an epoxy ring to be used in the production method of the present invention. EO and PO can be reacted alone, as a mixture, or separately.
[0044] The amount of the alkylene oxide having 2 to 20 carbon atoms and an epoxy ring to be added is not particularly limited, but from the viewpoint of ensuring biodegradability, it is preferably 10 to 95 parts by mass, more preferably 15 to 85 parts by mass, and even more preferably 20 to 75 parts by mass, relative to 100 parts by mass of the polyester ether of the present invention.
[0045] <<Compound Having an Oxygen-Containing Heterocyclic Structure Other than Alkylene Oxide Having an Ester Bond>> Examples of compounds having an oxygen-containing heterocyclic structure other than an alkylene oxide having an ester bond include cyclic esters, acid anhydrides, and cyclic carbonates. These may be used alone or in combination of two or more. The number of ester bonds in one molecule of the compound having an oxygen-containing heterocyclic structure other than an alkylene oxide having an ester bond is not particularly limited as long as it is one or more, but is preferably 1 to 4, more preferably 1 to 3, and particularly preferably 1.
[0046] (Cyclic Ester) The cyclic ester is not particularly limited, and examples thereof include cyclic ester compounds having 3 to 9 carbon atoms, so-called lactones. The cyclic ester compound is not particularly limited, and examples thereof include β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, methyl-ε-caprolactone, α-methyl-β-propiolactone, β-methyl-β-propiolactone, methoxy-ε-caprolactone, methoxy-ε-caprolactone, ethoxy-ε-caprolactone, glycolide, and the like. These may be used alone or in combination of two or more. Among these, ε-caprolactone, δ-valerolactone, and γ-butyrolactone are preferred, and ε-caprolactone is more preferred.
[0047] (Acid Anhydride) The acid anhydride is not particularly limited, and examples thereof include polycarboxylic acid anhydrides. Among these, dicarboxylic acid anhydrides are preferred. The dicarboxylic acid anhydride is not particularly limited, and examples thereof include aliphatic dicarboxylic acid anhydrides such as maleic anhydride, succinic anhydride, dodecenyl succinic anhydride, and octadecenyl succinic anhydride; aromatic dicarboxylic acid anhydrides such as phthalic anhydride; and alicyclic dicarboxylic acid anhydrides such as hexahydrophthalic anhydride, tetrahydrophthalic anhydride, 3-methyl-hexahydrophthalic anhydride, 4-methyl-hexahydrophthalic anhydride, 3-methyl-1,2,3,6-tetrahydrophthalic anhydride, and 4-methyl-1,2,3,6-tetrahydrophthalic anhydride. These may be used alone or in combination of two or more. Among these, maleic anhydride, phthalic anhydride, and tetrahydrophthalic anhydride are preferred, with phthalic anhydride and tetrahydrophthalic anhydride being more preferred.
[0048] Cyclic polycarboxylic acid anhydrides do not undergo ring-opening addition reaction alone, but form polyester chains by alternating polymerization with cyclic ethers. Therefore, cyclic polycarboxylic acid anhydrides are used in combination with an equimolar or greater amount of cyclic ether, and the mixture is used as a compound having an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring and an oxygen-containing heterocyclic structure other than the alkylene oxide and having an ester bond. In this case, cyclic ethers in an amount exceeding equimolar to the cyclic polycarboxylic acid anhydride polymerize with themselves to form ether bonds.
[0049] (Cyclic Carbonate) The cyclic carbonate is not particularly limited, and examples thereof include ethylene carbonate, propylene carbonate, trimethylene carbonate, and substituted products thereof.
[0050] The amount of the compound having an oxygen-containing heterocyclic structure to be added is not particularly limited, but from the viewpoint of ensuring biodegradability, it is preferably 5 to 90 parts by mass, more preferably 15 to 85 parts by mass, and even more preferably 25 to 80 parts by mass, relative to 100 parts by mass of the polyester ether of the present invention.
[0051] <Mass Ratio of Alkylene Oxide Having 2 to 20 Carbon Atoms and Epoxy Ring to Compound Having an Oxygen-Containing Heterocyclic Structure Other Than the Alkylene Oxide and Having an Ester Bond> The mass ratio of the alkylene oxide having 2 to 20 carbon atoms and epoxy ring to the compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and having an ester bond (alkylene oxide:compound having an oxygen-containing heterocyclic structure) is not particularly limited, but is preferably 1:99 to 99:1, more preferably 20:80 to 80:20, and particularly preferably 30:70 to 70:30.
[0052] <Other Additives> To prevent deterioration during long-term storage until subsequent use, the polyester ether obtained by the production method of the present invention may contain an additive selected from hindered phenol-based and hindered amine-based antioxidants, benzotriazole-based non-ferrous corrosion inhibitors, triazole-based and benzophenone-based ultraviolet absorbers, and boron compound-based reducing agents.
[0053] Other examples of suitable acids for adjusting the pH include mineral acids such as phosphoric acid, phosphorous acid, hypophosphorous acid, pyrophosphoric acid, hydrochloric acid, sulfuric acid, and sulfurous acid; organic acids such as formic acid, oxalic acid, succinic acid, acetic acid, maleic acid, benzoic acid, paratoluenesulfonic acid, and dodecylbenzenesulfonic acid; alkali metal hydroxides or alkaline earth metal hydroxides such as sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, and barium hydroxide; alkali metal carbonates or alkaline earth metal carbonates such as lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, and barium carbonate; carbonates It is possible to add a compound selected from the group consisting of alkali metal hydrogen carbonates or alkaline earth metal hydrogen carbonates, such as lithium hydrogen carbonate, potassium hydrogen carbonate, sodium hydrogen carbonate, and cesium hydrogen carbonate; phosphates, such as lithium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, lithium monohydrogen phosphate, sodium monohydrogen phosphate, potassium monohydrogen phosphate, and sodium acid pyrophosphate; hydrogen sulfates, such as lithium hydrogen sulfate, sodium hydrogen sulfate, and potassium hydrogen sulfate; fatty acid amines, such as ethylenediamine, diethylenetriamine, and hexamethylenediamine; aromatic amines, such as tolylenediamine and diphenylmethanediamine; and organic alkaline compounds, such as alkanolamine.
[0054] <Method for Producing Polyester Ethers> A method for producing polyester ethers using an initiator compound, an alkylene oxide, and a compound having an oxygen-containing heterocyclic structure as raw materials is described below. A preferred method for producing polyester ethers of the present invention includes an initial step (a) in which a portion of the alkylene oxide to be copolymerized with the initiator compound (hereinafter, sometimes referred to as "initial step alkylene oxide") is supplied to a reaction solution containing an initiator compound, a DMC catalyst, and a compound having an oxygen-containing heterocyclic structure, preferably in an amount of 5 to 20 parts by mass per 100 parts by mass of the initiator compound contained in the reaction solution, and the reaction is allowed to proceed; and a polymerization step (b) in which, after the initial step (a), additional alkylene oxide is supplied and copolymerized. The organic solvent may be added at any step in the polyester ether production process. If necessary, the organic solvent may be added to a reaction vessel and degassed prior to the initial step for dehydration. This method is preferably carried out batchwise, but may also be a continuous process. Specifically, it can be carried out as follows.
[0055] The mixing means in the initial step (a) of the production method of the present invention is not particularly limited as long as it can sufficiently mix the initiator compound, the DMC catalyst, and the compound having an oxygen-containing heterocyclic structure (including components added as needed). A stirring means is usually used as the mixing means. The stirring power of the stirring means is 4 to 500 kW / m 3 is preferred, and 8 to 500 kW / m 3 More preferably, 12 to 500 kW / m 3 is particularly preferred. Here, the stirring power is a value calculated from known values, and this value is the power required per unit liquid volume of the contents, calculated from the volume and viscosity of the contents in the pressure-resistant reaction vessel, the shape of the reaction vessel, and the shape and rotation speed of the stirring blades. In the present invention, the reaction liquid corresponds to the contents in the pressure-resistant reaction vessel.
[0056] Specific examples of the stirring means used in the initial step (a) of the production method of the present invention include stirring blades, bubbling with an inert gas such as nitrogen gas, electromagnetic waves, and ultrasonic waves, but stirring with stirring blades is preferred. Preferred examples of stirring blades include the stirring blades described in JP 2003-342361 A. Large stirring blades are particularly preferred, and large blades such as the FULLZONE (registered trademark) blade manufactured by Kobe Steel Pantech Co., Ltd. and the MAXBLEND (registered trademark) blade manufactured by Sumitomo Heavy Industries, Ltd. can be used. Paddle blades, pitch paddle blades, turbine blades, and propeller blades can also be used. In this case, the stirring blade radius is preferably 20 to 99%, more preferably 30 to 90%, and particularly preferably 40 to 80% of the inner diameter (inner radius) of the pressure-resistant reaction vessel.
[0057] The pressure-resistant reaction vessel used in the initial step (a) of the present invention may be of any shape or material, but is preferably made of heat-resistant glass or metal.
[0058] As a means for supplying alkylene oxide into the reaction vessel, alkylene oxide supply means for discharging alkylene oxide into the liquid at two or more locations may be provided.
[0059] Next, the pressure-resistant reactor is preferably purged with nitrogen. This removes oxygen from the reaction solution. The amount of oxygen in the reaction solution is preferably 1% by mass or less relative to the amount of nitrogen. The pressure in the pressure-resistant reactor in the initial step (a) of the present invention is preferably 1.020 MPaA or less in absolute pressure. An absolute pressure of 1.015 MPaA or less is more preferred, and an absolute pressure of 1.010 MPaA or less is particularly preferred. An absolute pressure exceeding 1.020 MPaA is not preferred because the pressure rises sharply due to the reduction in the volume of space in the pressure-resistant reactor associated with polymerization. Note that venting the pressure-resistant reactor does not have the effect of improving the activity of the catalyst, but may be carried out if necessary for the process when the initiator compound contains too much water.
[0060] Next, the reaction solution is heated with stirring to raise the temperature, and then, while the temperature of the reaction solution is at a predetermined initial temperature, an initial step alkylene oxide is supplied and reacted. In this specification, the initial temperature refers to the temperature of the reaction solution at the start of supplying the initial step alkylene oxide. The initial temperature of the reaction solution is 120 to 165°C, preferably 125 to 150°C, and more preferably 130 to 140°C. When the initial temperature is at least the lower limit of the above range, catalytic activity is significantly improved, and when it is at most the upper limit of the above range, there is no risk of thermal decomposition of the components contained in the reaction solution themselves.
[0061] Specifically, it is preferable to heat the reaction solution to the initial temperature while stirring, and then start the supply of alkylene oxide while the temperature of the reaction solution is maintained. For example, heating is stopped when the reaction solution reaches a predetermined initial temperature, and the supply of alkylene oxide is started before the temperature of the reaction solution starts to drop. The time from stopping heating to starting the supply of alkylene oxide is not particularly limited, but from the viewpoint of efficiency, it is preferably within 1 hour. The temperature-raising time for raising the reaction solution to the predetermined temperature is preferably 10 minutes to 24 hours, and particularly preferably 15 minutes to 2 hours. When the temperature-raising time is equal to or greater than the lower limit of the above range, the reaction solution can be heated uniformly, and when it is equal to or less than the upper limit of the above range, time efficiency is good.
[0062] The initial step alkylene oxide is an alkylene oxide that is polymerized with an initiator compound in the production of polyester ether. If the amount of the initial step alkylene oxide supplied is too small, the DMC catalyst will not be activated sufficiently, and if it is too large, a runaway reaction will occur. Therefore, the amount of the initial step alkylene oxide supplied is preferably 5 to 20 parts by mass, more preferably 8 to 15 parts by mass, and particularly preferably 10 to 12 parts by mass, per 100 parts by mass of the initiator compound contained in the reaction solution.
[0063] The alkylene oxide for the initial step is supplied while the pressure-resistant reactor is sealed. Immediately after the alkylene oxide is supplied to the reaction solution, the internal pressure of the pressure-resistant reactor increases due to the vaporization of unreacted alkylene oxide. Next, when the DMC catalyst is initially activated, a reaction occurs between the alkylene oxide and the initiator compound, and the internal pressure of the pressure-resistant reactor begins to decrease, while the temperature of the reaction solution increases due to the heat of reaction. When the entire amount of alkylene oxide supplied has reacted, the internal pressure of the pressure-resistant reactor decreases to the same level as before the supply, and the temperature increase of the reaction solution due to the heat of reaction disappears. Depending on the amount of organic solvent, there may be little temperature increase of the reaction solution due to the heat of reaction, and an increase in internal pressure may be observed. In this specification, the initial step (a) refers to the process from the start of supplying the alkylene oxide for the initial step to the completion of the reaction of the alkylene oxide. The completion of the reaction of the alkylene oxide for the initial step can be confirmed by a decrease in the internal pressure of the pressure-resistant reactor. That is, the end of the initial step (a) refers to the time when the internal pressure of the pressure-resistant reactor has decreased to the same level as before the alkylene oxide was supplied. The initial step is preferably for 10 minutes to 24 hours, more preferably for 15 minutes to 3 hours. When the initial step is at least the lower limit of the above range, the DMC catalyst can be activated, and when the initial step is at most the upper limit of the above range, time efficiency is good.
[0064] After the initial step is completed, alkylene oxide is newly supplied to the reaction system, the temperature of the reaction solution is adjusted to a predetermined polymerization temperature, and the copolymerization reaction is carried out while stirring to obtain the target polyester ether. A pressure-resistant autoclave vessel is preferably used as the heat-resistant reaction vessel used in the polymerization step (b) of the production method of the present invention, but if the boiling points of the alkylene oxide, the compound having an oxygen-containing heterocyclic structure, the organic solvent, etc. are high, a pressure-resistant vessel is not necessary. There are no particular restrictions on the material. The vessel used in the initial step (a) can be used as the reaction vessel.
[0065] In the polymerization step (b) of the production method of the present invention, during the reaction of the product of the initial step (a) (a compound obtained by reacting an initiator compound with an alkylene oxide and a compound having an oxygen-containing heterocyclic structure) with an alkylene oxide and any compound having an oxygen-containing heterocyclic structure in the presence of a DMC catalyst, the reaction solution is heated at a power of preferably 4 to 500 kW / m, similar to the initial step (a). 3 , more preferably 8 to 500 kW / m 3 , particularly preferably 12 to 500 kW / m 3 It is preferable to stir using a stirring power of 1000 W or less. As for the stirring blades, propeller blades, paddle blades, Max Blend blades, and disc turbines can be used, with large blades being preferred for uniform mixing within the reaction vessel. Other suitable blades include a Disper, Homomixer, Colloid Mill, and Nauta Mixer, which are used for emulsification and dispersion. Ultrasonic mixing may also be used without using stirring blades. These stirring methods may be used in combination. When using a stirring method that uses a general stirring blade, it is preferable to increase the rotation speed of the stirring blades as much as possible within a range that does not result in a decrease in stirring efficiency due to a large amount of gas from the gas phase of the reactor being taken into the reaction liquid.
[0066] The polymerization method in the polymerization step (b) of the present invention includes a batch method and a continuous method, and the batch method is preferred from the viewpoint of ease of control to obtain the desired molecular weight. The continuous method is a method in which the addition of a mixture containing alkylene oxide, the product of the initial step (a), and a DMC catalyst and the withdrawal of the polyester ether, which is the product of the polymerization step (b), are carried out simultaneously. In particular, when an organic solvent is used, the viscosity of the entire system can be reduced, and therefore, when the number average molecular weight per hydroxyl group of the initiator compound is 500 to 10,000, the continuous method increases productivity.
[0067] The temperature of the reaction solution (polymerization temperature) when reacting the polyester ether in the polymerization step (b) is preferably 125 to 180°C, more preferably 125 to 160°C. When the polymerization temperature is equal to or higher than the lower limit of the above range, a good reaction rate can be obtained, and the amount of unreacted material remaining in the final product can be reduced. Furthermore, when the polymerization temperature is equal to or lower than the upper limit of the above range, the high activity of the DMC catalyst can be well maintained, and the molecular weight distribution can be narrowed. After the reaction of the alkylene oxide in the polymerization step (b) is completed, it is preferable to cool the reaction solution and purify the reaction product.
[0068] The supply rate of the alkylene oxide in the polymerization step (b) is preferably as slow as possible because this narrows the molecular weight distribution of the resulting polymer, but this also reduces production efficiency, so it is preferable to determine this rate by comparing these factors. A specific supply rate is preferably 1 to 200 mass% / hour based on the total mass of the polyester ether intended as the final product. The supply rate may be changed gradually during the copolymerization reaction.
[0069] The reaction time in the polymerization step (b) of the present invention is preferably 10 minutes to 40 hours, more preferably 30 minutes to 24 hours. When the reaction time is equal to or greater than the lower limit of the above range, the reaction can be controlled, but when the reaction time is equal to or less than the upper limit of the above range, it is preferable in terms of efficiency.
[0070] The pressure in the pressure-resistant reactor in the polymerization step (b) of the present invention is preferably 2 MPaA or less in absolute pressure, particularly preferably 1.8 MPaA or less, in terms of ease of operation and equipment. The polyester ether obtained by polymerization using a DMC catalyst as described above may be copolymerized with an alkylene oxide and a compound having an oxygen-containing heterocyclic structure using a polymerization catalyst other than the DMC catalyst to obtain the final polyester ether. The copolymerization reaction can be carried out by a known method using an alkali metal catalyst such as potassium hydroxide as the polymerization catalyst.
[0071] If necessary, the polyester ether obtained by the production method of the present invention may be subjected to a DMC catalyst removal treatment and a DMC catalyst deactivation treatment. Examples of such methods include an adsorption method using an adsorbent selected from synthetic silicates (magnesium silicate, aluminum silicate, etc.), ion exchange resins, and activated clay, a neutralization method using organic acids and salts thereof such as amines, alkali metal hydroxides, phosphoric acid, lactic acid, succinic acid, adipic acid, and acetic acid, or inorganic acids such as sulfuric acid, nitric acid, and hydrochloric acid, and a method combining a neutralization method and an adsorption method. Even when primary hydroxyl group conversion is performed using the alkali metal catalyst, the alkali metal catalyst can be similarly deactivated and removed.
[0072] To the polyethers thus obtained, a stabilizer may be added as needed to prevent deterioration during long-term storage. Examples of stabilizers include 2,6-di-t-butyl-4-cresol (BHT); Irganox 1010 (BASF product name, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]), Irganox 1076 (BASF product name, 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate stearyl), and Irganox 1135 (BASF product name, octyl-3,5-di-t-butyl-4-hydroxy-hydroxybenzoate). Additives selected from hindered phenol-based antioxidants such as bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate (product name of BASF) and hindered amine-based antioxidants such as Tinuvin 765 (product name of BASF, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate) and Nonflex DCD (product name of Seiko Chemical Corporation, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine) can be added, benzotriazole-based non-ferrous corrosion inhibitors, triazole-based and benzophenone-based ultraviolet absorbers, and boron compound-based reducing agents can be added. When an antioxidant is added, the amount added is preferably 50 to 5,000 ppm by mass, and more preferably 500 to 4,000 ppm by mass, relative to the obtained polyether polyol.
[0073] Examples of methods for supplying the alkylene oxide and the compound having an oxygen-containing heterocyclic structure include a method of adding the compound having an oxygen-containing heterocyclic structure all at once, a method of adding the compound having an oxygen-containing heterocyclic structure in portions, and a method of mixing the alkylene oxide and the compound having an oxygen-containing heterocyclic structure in a pipe (pipe mixing method).
[0074] In the batch or divided addition method of the compound having an oxygen-containing heterocyclic structure, an initiator compound and a compound having an oxygen-containing heterocyclic structure are charged into a reaction vessel, and alkylene oxide is added through an alkylene oxide supply means previously equipped with a flow control valve or the like. In the batch addition method, the compound having an oxygen-containing heterocyclic structure is charged in its entirety in one go, and then alkylene oxide is added. In the divided addition method, the compound having an oxygen-containing heterocyclic structure is added multiple times, and the alkylene oxide is added multiple times.
[0075] In the pipe mixing method, a pipe for supplying the alkylene oxide and the compound having an oxygen-containing heterocyclic structure, which is previously equipped with a flow control valve or the like, is provided leading to a reactor, and the alkylene oxide and the compound having an oxygen-containing heterocyclic structure are introduced into the reactor while their flow rates are controlled. The alkylene oxide and the compound having an oxygen-containing heterocyclic structure may be introduced independently into the reactor, or the two liquids may be mixed by collision during the introduction. To improve the mixing properties, the mixture may be mixed using a static mixer or a dynamic mixer.
[0076] [Method for producing molded article] <Method for molding polyester ether> The polyester ether of the present invention is thermoplastic, and general molding methods for plastic resins can be applied. Specific examples include injection molding, extrusion molding, blow molding, compression molding, calendar molding, and thermoforming. Among these, injection molding is preferred, and hydraulic injection molding is more preferred. As molding conditions for hydraulic injection molding, the temperature is preferably 80 to 200°C, and more preferably 100 to 150°C. The pressure is preferably 1 to 10 MPaG, and more preferably 2 to 8 MPaG. The pressing time is preferably 1 to 10 minutes, and more preferably 1 to 5 minutes.
[0077] <Molded Article> The polyester ether of the present invention is molded into a molded article by the molding method described above. The molded article refers to any article that can be molded by the molding method described above, and examples thereof include membranous articles such as sheets and films. The thickness of the molded article is preferably 10 to 1000 μm, more preferably 20 to 500 μm, for membranous articles.
[0078] There is no particular limitation on the maximum cohesive strength of the compact, but from the viewpoint of the toughness of the material, it is recommended to set it at 5.0 N / mm 2 More than 5.5 N / mm is preferable. 2 More preferably, 6.0 N / mm 2 The above is particularly preferred. The method for measuring the maximum point cohesive strength is the method described in the Examples.
[0079] The maximum elongation of the molded body is not particularly limited, but from the viewpoint of the elongation resistance of the material, it is preferably 5% or more, more preferably 6% or more, and particularly preferably 7% or more. The maximum elongation is measured by the method described in the Examples.
[0080] <Applications> The polyester ether obtained by the production method of the present invention can be suitably used for biodegradable agricultural and civil engineering materials, biodegradable soft packaging films, biodegradable food containers, coating materials for biodegradable coated fertilizers, biodegradable polymer beads for cosmetics, etc.
[0081] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0082] [Evaluation and Measurement Methods] <Number Average Molecular Weight (Mn) and Weight Average Molecular Weight (Mw)> The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of polymers such as polyester ether are polystyrene-equivalent molecular weights obtained by gel permeation chromatography (GPC) under the following conditions using a calibration curve prepared using standard polystyrene samples of known molecular weights. The measurement results are shown in Table 2. <<GPC Measurement Conditions>> Model used: HLC-8320GPC (manufactured by Tosoh Corporation) Columns used: TSG gel SuperHZ 4000 x 2, 2500 x 2 (manufactured by Tosoh Corporation) Column temperature: 40°C Detector: RI Solvent: tetrahydrofuran Flow rate: 0.35 ml / min Sample concentration: 0.5% Injection volume: 20 μL Standard sample for preparing calibration curve: polystyrene (manufactured by Polymer Laboratory; [EasiCal] PS-2 [polystyrene standard])
[0083] <Glass transition temperature (Tg) and melting point (Tm)> The glass transition temperature (Tg) and melting point (Tm) were measured by DSC analysis of the synthesized samples. The measurement results are shown in Table 2. <<DSC measurement conditions>> Model used: DSC 3500 Sirius (manufactured by NETZSCH) Amount of sample used: Approximately 10 mg Measurement conditions: 22°C (start), temperature decreased to -100°C (temperature decrease rate 10°C / min), temperature increased to 150°C (temperature increase rate: 10°C / min) The two peaks measured during the temperature increase from -100°C to 150°C were taken as the glass transition temperature and melting point. Peak temperature around -70°C to 50°C: glass transition temperature (Tg, °C) Peak temperature around 50°C to 70°C: melting point (Tm, °C)
[0084] <Moldability> A dumbbell-shaped No. 3 test piece sandwiched between two sheets of release PET prepared according to the hydraulic molding conditions described below was visually inspected to see whether the test piece could maintain its shape when removed from the release PET film, and judged as pass or fail. A molded sample that could maintain its shape was judged as pass, and a molded sample that could not maintain its shape, such as when the sample adhered to the release PET and was chipped, was judged as fail. The evaluation results are shown in Table 2. <<Hydraulic molding conditions>> 10 g of the sample was sandwiched between two sheets of release PET film together with a 0.1 mm metal frame spacer plate, and the sample was placed in a hydraulic molding machine (manufactured by Iwaki Kogyo Co., Ltd., maximum output: 50 ton, maximum pressure: 200 kg / cm) at 130°C. 2 ) under 5 MPaG for 2 minutes.
[0085] <Maximum cohesive strength (Tmax) and maximum elongation (Emax)> The pressed sample used in the moldability evaluation was aged at 23°C for 1 day, and then punched into a dumbbell shape No. 3 in accordance with JIS K6251: 2017 to obtain a test piece. The test piece (thickness 0.1 mm) was subjected to a tensile test using a Tensilon testing machine (temperature 23°C, tensile speed 300 mm / min), and the maximum cohesive strength (Tmax) [N / mm 2 The results are shown in Table 2.
[0086] <Soil decomposition (biodegradability) test> The pressed sample used in the moldability evaluation was cut into 2 cm x 2 cm pieces and then placed in a planter so that it was completely buried in soil (horticultural culture soil: manufactured by Togawa Heiwa Farm). After 8 weeks at 25°C, the sample was removed and the changes in the appearance of the film were visually confirmed and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2. <<Evaluation criteria>> A: Decomposition B: No decomposition
[0087] <Preparation of DMC catalyst A> A DMC catalyst obtained by the method described in Example 3 of JP-A-2003-190808 was used. 3 [Co(CN) 6To the reaction solution obtained by reacting the hydroxypropyl methylcellulose and the hydroxypropyl methylcellulose, a mixture of 80 g of tert-butyl alcohol, 1 g of polyoxypropylene glycol (also referred to as "PPG1") having a number average molecular weight of 1,500, a hydroxyl value of 75 mg KOH / g, and two hydroxyl groups, and 80 g of water was added, and the mixture was heated to 60°C. After stirring for 1 hour, a filtration operation (first filtration) was performed to obtain a cake containing a composite metal cyanide complex catalyst organic phase. Next, a mixture of 40 g of tert-butyl alcohol, 1 g of "PPG1," and 70 g of water was added to the cake containing the composite metal cyanide complex catalyst organic phase, and the mixture was stirred for 30 minutes, followed by a filtration operation (second filtration). To the cake containing the composite metal cyanide complex catalyst organic phase obtained by this filtration operation, a mixture of 80 g of tert-butyl alcohol, 1 g of "PPG1," and 10 g of water was further added, stirred, and then a filtration operation (third filtration) was performed. The cake containing the organic phase of the composite metal cyanide complex catalyst obtained by this filtration operation was dried at 80°C until there was no change in mass, and then pulverized to obtain a powdery composite metal cyanide complex catalyst (also referred to as "DMC catalyst A").
[0088] <Production Examples> Examples 1, 2, 6, 7, 10 to 12, 14, and 15 are comparative examples, and Examples 3 to 5, 8, 9, 13, and 16 are working examples. [Substances Used] Details of the various substances used in the synthesis examples are shown below. EO: Ethylene oxide Polypropylene glycol (molecular weight 700, EXCENOL 720 manufactured by AGC Inc.) Polyethylene glycol (molecular weight 600, PEG #600 manufactured by NOF Corporation) ε-Caprolactone (manufactured by Daicel Corporation, trade name: PLACCEL M) Phthalic anhydride (manufactured by Air Water Performance Chemicals Inc.) Toluene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade, relative dielectric constant: 2.3) Irganox 1076 (manufactured by BASF Japan Ltd.) Methyl ethyl ketone (manufactured by Junsei Chemical Co., Ltd., special reagent grade, relative dielectric constant: 18.5) Dimethyl sulfoxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade, relative dielectric constant: 46.5) Tetrahydrofuran (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade, relative dielectric constant: 7.6)
[0089] Example 1: Synthesis of Polyester Ether (A), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol Precharged with ε-Caprolactone in One Batch: 1,143 g of polyethylene glycol (PEG #600) was added to a 10 L reactor equipped with a stirrer, stirring blades, a heating jacket, a cooling coil, a nitrogen inlet pipe, and a pressure reduction pipe. Then, 0.4 g of the DMC catalyst A was added to the reactor. After purging with nitrogen gas, the reactor was heated to 130°C and mixed for 1 hour under a reduced pressure of -0.1 MPaG with stirring at 200 rpm. After completion of the pretreatment, the reactor was pressurized to 0.1 MPaG with nitrogen gas, cooled to 80°C, and the internal pressure was adjusted to 0 MPaG. Then, 1,429 g of ε-caprolactone was charged and the temperature was raised to 130°C. At 130°C, 114 g of EO was added for initial activation. After confirming initial activity by a decrease in internal pressure, 1,314 g of EO was fed over 4 hours at 130°C. After aging for 1 hour at 130°C, the reactor was depressurized to -0.1 MPaG, and it was confirmed that there was no unreacted EO or ε-caprolactone. 4.0 g of Irganox 1076 was then added as an antioxidant, and the product, polyester ether (A), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was extracted. The extracted product was subjected to GPC measurement, DSC measurement, and the maximum cohesive strength (Tmax) and maximum elongation (Emax) were measured using the methods described above, and its moldability and soil decomposition properties were evaluated using the methods described above. The measurement and evaluation results are shown in Tables 1 and 2. The following examples were also evaluated in the same manner and are shown in Tables 1 and 2.
[0090] Example 2 Synthesis of Polyester Ether (B), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol, with ε-Caprolactone Charged All at Once 1,161 g of the polyester ether (A), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol described in Example 1, 0.72 g of the DMC catalyst A, 2,420 g of ε-caprolactone, and 1,200 g of toluene were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping. The atmosphere was then purged with nitrogen gas and the temperature was raised to 130°C. At 130°C, 116 g of EO was fed for initial activation. After confirming the occurrence of initial activation by a decrease in internal pressure, 2,304 g of EO was fed at 130°C over 4.5 hours. After aging for 1 hour at 130°C, 6.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which was an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (B), which was an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0091] Example 3 Synthesis of Polyester Ether (C), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol, in Which ε-Caprolactone is Charged All at Once
[0049] To a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping, 1,905 g (including 317 g of toluene) of Polyester Ether (B), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene, as described in Example 2, 0.54 g of the above DMC catalyst A, 1,706 g of ε-caprolactone, and 1,683 g of toluene were added, followed by nitrogen gas substitution and heating to 130°C. At 130°C, 159 g of EO was fed for initial activation. After confirming that initial activation had occurred by a decrease in internal pressure, 1,548 g of EO was fed at 130°C over 3.5 hours. After aging for 1 hour at 130°C, 5.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (C), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0092] Example 4 Synthesis of Polyester Ether (D), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol, in Which ε-Caprolactone is Charged All at Once
[0049] To a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping, 914 g of Polyester Ether B, an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene described in Example 2 (containing 152 g of toluene), 0.32 g of the DMC catalyst A, 1,619 g of ε-caprolactone, and 3,848 g of toluene were added, followed by nitrogen gas substitution and heating to 130°C. 76 g of EO was fed at 130°C for initial activation. After confirming that initial activation had occurred by a decrease in internal pressure, 1,543 g of EO was fed at 130°C over 4.5 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours at 130°C and under reduced pressure of -0.1 MPaG, to obtain polyester ether (D), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0093] Example 5 Synthesis of polyester ether (E), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, prepared by mixing EO (50% by mass) and caprolactone (50% by mass) in a feed pipe. 914 g (including 152 g of toluene) of polyester ether (B), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene, described in Example 2, 0.32 g of the DMC catalyst A, and 3,848 g of toluene were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. The atmosphere was then purged with nitrogen gas and the temperature was raised to 130°C. 76 g of EO was fed for initial activation at 130°C. After confirming that initial activation had occurred by a decrease in internal pressure, 1,543 g of EO and 1,543 g of ε-caprolactone were mixed in the feed pipe and fed at 130°C over 4.5 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (E), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0094] Example 6 Synthesis of Polyester Ether (F), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol, by Mixing EO (35% by mass) and Caprolactone (65% by mass) in a Feed Pipe: 1,286 g of polyethylene glycol (PEG #600) was added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. 0.45 g of the DMC catalyst A was then added, followed by nitrogen gas replacement. The mixture was heated to 130 ° C. and stirred at 200 rpm under reduced pressure of -0.1 MPaG for 1 hour. The reactor pressure was then adjusted to 0.03 MPaG with nitrogen gas, and 239 g of ε-caprolactone was added at 130 ° C., followed by 129 g of EO for initial activation. After confirming that initial activity had occurred due to a decrease in internal pressure, 996 g of EO and 1,851 g of ε-caprolactone were fed over 6.5 hours at 130° C. while being mixed in the feed pipe. After allowing to age for 1 hour at 130° C., 4.5 g of Irganox 1076 was added as an antioxidant, and then polyester ether (F), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product.
[0095] Example 7 Synthesis of Polyester Ether (G), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, prepared by mixing EO (35% by mass) and caprolactone (65% by mass) in a feed pipe. 857 g of polyester ether F, an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol described in Example 6, 0.36 g of the DMC catalyst A, and 900 g of toluene were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. The atmosphere was then purged with nitrogen gas and the temperature was raised to 130°C. After feeding 159 g of ε-caprolactone at 130°C, 86 g of EO was fed for initial activation. After confirming that initial activation had occurred by a decrease in internal pressure, 1,189 g of EO and 2,209 g of ε-caprolactone were mixed in the feed pipe and fed at 130°C over 8.0 hours. After aging for 1 hour at 130°C, 4.5 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (G), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0096] Example 8: Synthesis of polyester ether (H), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, prepared by mixing EO (35% by mass) and caprolactone (65% by mass) in a feed pipe. 914 g of polyester ether G (containing 152 g of toluene), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene, as described in Example 7, 0.32 g of the DMC catalyst A, and 3,848 g of toluene were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. The mixture was then purged with nitrogen gas and heated to 130°C. After feeding 141 g of ε-caprolactone at 130°C, 76 g of EO was fed for initial activation. After confirming that initial activation had occurred by a decrease in internal pressure, 1,057 g of EO and 1,963 g of ε-caprolactone were mixed in the feed pipe and fed at 130°C over 8.0 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (H), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0097] Example 9 Synthesis of Polyester Ether (I), an Ethylene Oxide / ε-Caprolactone Copolymer of Polyethylene Glycol, by Mixing EO (50% by mass) and Caprolactone (50% by mass) in a Feed Pipe Under Reduced Solvent Conditions 914 g (containing 152 g of toluene) of Polyester Ether B, an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene described in Example 2, 0.32 g of the DMC Catalyst A, and 1,448 g of toluene were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. After the mixture was purged with nitrogen gas, the mixture was heated to 130°C. 141 g of ε-caprolactone was fed at 130°C, followed by feeding 76 g of EO for initial activation. After confirming that initial activity had occurred due to a decrease in internal pressure, 1,543 g of EO and 1,478 g of ε-caprolactone were mixed in the feed pipe and fed at 130°C over 8.0 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which was an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, was removed as the product. 1,000 g of the removed sample was placed in a 2-L flask and distilled at 130°C and a reduced pressure of -0.1 MPaG for 4 hours to remove toluene, yielding polyester ether (I), which was an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol.
[0098] Example 10: Synthesis of polyester ether (J), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, by mixing EO (35% by mass) and caprolactone (65% by mass) in a feed pipe under conditions using a further reduced amount of solvent. 914 g of polyester ether B (containing 152 g of toluene), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol containing toluene, as described in Example 2, and 0.32 g of the DMC catalyst A were added to a 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet pipe, and pressure reduction pipe. The atmosphere was then purged with nitrogen gas and the temperature was raised to 130°C. 141 g of ε-caprolactone was fed at 130°C, and then 76 g of EO was fed for initial activation. After it was confirmed that initial activity had occurred due to a decrease in the internal pressure, an attempt was made to feed 1,057 g of EO and 1,963 g of ε-caprolactone at 130°C over 8.0 hours while mixing them in the feed pipe, but the stirrer stopped during the polymerization due to overload caused by an increase in viscosity in the system, and the polymerization was discontinued.
[0099] (Example 11) Synthesis of polyester ether (K), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, prepared by charging ε-caprolactone in one lump using methyl ethyl ketone as the solvent. Synthesis and removal of the solvent in a flask were carried out under the same conditions as in Example 2, except that the solvent used was changed from toluene to methyl ethyl ketone, to obtain a product (polyester ether (K)).
[0100] (Example 12) Synthesis of polyester ether (L), an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, charged all at once under conditions where ε-caprolactone was used as the solvent: A 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping was charged with 1,161 g of polyester ether L, an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol described in Example 1, 0.72 g of the DMC catalyst A, 2,420 g of ε-caprolactone, and 1,200 g of dimethyl sulfoxide. After purging with nitrogen gas, the temperature was raised to 130 ° C. 116 g of EO was fed for initial activation at 130 ° C., but no decrease in internal pressure was confirmed even after 3 hours. It was determined that the DMC catalyst had been deactivated, and the synthesis was discontinued.
[0101] (Example 13) Synthesis of polyester ether (M), which is an ethylene oxide / ε-caprolactone copolymer of polyethylene glycol, obtained by mixing EO (50% by mass) and caprolactone (50% by mass) in a feed pipe using tetrahydrofuran as a solvent. Synthesis and removal of the solvent in a flask were carried out under the same conditions as in Example 5, except that the solvent used was changed from toluene to tetrahydrofuran, and a product (polyester ether (M)) was obtained.
[0102] (Example 14) Synthesis of polyester ether (N), which is an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol using toluene as a solvent and charged in bulk with phthalic anhydride. A 10L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping was charged with 1,333 g of polypropylene glycol (EL-720), followed by the addition of 0.8 g of the DMC catalyst A, and then purged with nitrogen gas. The temperature was raised to 130 ° C., and under a reduced pressure of -0.1 MPaG and stirring at 200 rpm, the mixture was mixed for 1 hour. After completion of the pretreatment, the reactor was pressurized to 0.1 MPaG with nitrogen gas, cooled to 80 ° C., and the pressure in the vessel was set to 0 MPaG. 1,333 g of phthalic anhydride and 400 g of toluene were charged, and the temperature was raised to 130 ° C. 67 g of EO was fed for initial activation at 130 ° C. After confirming initial activity by a decrease in internal pressure, 1,267 g of EO was fed over 4 hours at 130°C. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which was an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol, was removed as the product. 1,000 g of the removed sample was placed in a 2-L flask and distilled under reduced pressure of 130°C and -0.1 MPaG for 4 hours to remove toluene, yielding polyester ether (N), which was an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol.
[0103] (Example 15) Synthesis of polyester ether (O), an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol, using toluene as a solvent and phthalic anhydride all at once. A 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping was charged with 838 g of polyester ether (N), a toluene solution of ethylene oxide / phthalic anhydride copolymer of polypropylene glycol described in Example 14, 0.65 g of the DMC catalyst A, 1,619 g of phthalic anhydride, and 3,924 g of toluene. After purging with nitrogen gas, the temperature was raised to 130 ° C. 38 g of EO was fed for initial activation at 130 ° C. After confirming that initial activation had occurred by a decrease in internal pressure, 1,581 g of EO was fed at 130 ° C. over 4.5 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (O), which is an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol.
[0104] (Example 16) Synthesis of polyester ether (P), an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol, using toluene as a solvent and phthalic anhydride all at once. A 10 L reactor equipped with a stirrer, stirring blade, heating jacket, cooling coil, nitrogen inlet piping, and pressure reduction piping was charged with 1,495 g of polyester ether (O), a toluene solution of ethylene oxide / phthalic anhydride copolymer of polypropylene glycol described in Example 15, 0.65 g of the DMC catalyst A, 1,619 g of phthalic anhydride, and 3,267 g of toluene. After purging with nitrogen gas, the temperature was raised to 130 ° C. 38 g of EO was fed for initial activation at 130 ° C. After confirming that initial activation had occurred by a decrease in internal pressure, 1,581 g of EO was fed at 130 ° C. over 4.5 hours. After aging for 1 hour at 130°C, 4.0 g of Irganox 1076 was added as an antioxidant, and then a toluene solution of polyester ether, which is an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol, was taken out as the product. 1,000 g of the taken out sample was placed in a 2 L flask and the toluene was distilled off for 4 hours under reduced pressure conditions of 130°C and -0.1 MPaG, to obtain polyester ether (P), which is an ethylene oxide / phthalic anhydride copolymer of polypropylene glycol.
[0105]
[0106]
[0107] (Evaluation Results) In Examples 1, 2, 6, 7, 14, and 15, the weight-average molecular weight of the polyester ether was small, and the moldability was unacceptable. In Example 10, the amount of solvent used was small, and polyester ether could not be synthesized. In Example 11, the relative dielectric constant of the solvent was higher than in Example 2. The molecular weight did not increase, and low-molecular-weight compounds were produced, resulting in a small weight-average molecular weight and a large molecular weight distribution, which was unsuitable. In Example 12, the relative dielectric constant of the solvent was higher than in Example 2. The behavior after the addition of EO for initial activation was significantly different, the DMC catalyst was deactivated, and polyester ether could not be synthesized. On the other hand, in Examples 3 to 5, 8, 9, 13, and 16, molding was possible without polymerizing using toxic isocyanates or the like, and physical properties (maximum point cohesion strength (Tmax) and maximum point elongation (Emax)) could be expressed. In addition, the polyester ether that was moldable was biodegradable.
[0108] The polyester ether produced by the method for producing a polyester ether of the present invention can be suitably used for agricultural and civil engineering materials, flexible packaging films, food containers, coating materials for biodegradable coated fertilizers, and the like.
Claims
1. A method for producing a polyester ether, comprising copolymerizing a compound having at least one active hydrogen atom per molecule, an alkylene oxide having 2 to 20 carbon atoms and an epoxy ring, and a compound having an oxygen-containing heterocyclic structure other than the alkylene oxide and having an ester bond in the presence of a composite metal cyanide complex catalyst and an organic solvent to obtain a polyester ether having a weight average molecular weight of 40,000 or more, wherein the organic solvent has a relative dielectric constant of 18.0 or less, and 10 to 400 parts by mass of the organic solvent is used per 100 parts by mass of the polyester ether.
2. The method for producing a polyester ether according to claim 1, wherein the organic solvent is used in an amount of 20 to 150 parts by mass per 100 parts by mass of the polyester ether.
3. The method for producing a polyester ether according to claim 1 or 2, wherein the compound having an oxygen-containing heterocyclic structure is a cyclic ester or an acid anhydride.
4. The method for producing polyester ether according to claim 1 or 2, wherein the alkylene oxide is at least one selected from the group consisting of ethylene oxide and propylene oxide.
5. A method for producing a polyester ether according to claim 1 or 2, wherein the mass ratio of the alkylene oxide to the compound having an oxygen-containing heterocyclic structure (alkylene oxide:compound having an oxygen-containing heterocyclic structure) is 20:80 to 99:
1.
6. The method for producing a polyester ether according to claim 1 or 2, wherein the glass transition temperature of the polyester ether is -50°C or lower.
7. The method for producing a polyester ether according to claim 1 or 2, wherein the melting point of the polyester ether is 50°C or higher.
8. The method for producing a polyester ether according to claim 1 or 2, wherein the polyester ether is biodegradable.
9. A method for producing a molded article, comprising molding the polyester ether obtained by the method according to claim 1 or 2 to produce a molded article.
10. The maximum cohesive strength of the molded body is 5.0 N / mm 2The method for producing a molded article according to claim 9 .
11. The method for producing a molded article according to claim 9, wherein the molded article has a maximum elongation of 5% or more.
Citation Information
Patent Citations
Production of lactide polymer
JP1992359014A
Sustainably hydrophilicizing agent for polyolefin fiber and imparting polyolefin fiber with sustainable hydrophilicity using the same
JP1996226082A
Production of high molecular lactate-based polyether copolymer
JP1999035655A
Biodegradable lubricant composition
JP2007077312A
Method for producing polyether ester polyols
JP2013536286A