Resin composition, laminated film, and decorative film
The addition of a phosphite-based antioxidant to resin compositions with vinylidene fluoride and propylene glycol units addresses the issue of yellowing, achieving transparent and chemically resistant films for automotive and architectural applications.
Patent Information
- Application Number
- PCT/JP2024/014730
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-17
AI Technical Summary
Resin compositions containing vinylidene fluoride resin produced with polypropylene glycol emulsifiers tend to yellow due to propylene glycol units, which is undesirable for appearance and cannot be prevented by conventional techniques.
Incorporating a phosphite-based antioxidant into the resin composition, specifically with a vinylidene fluoride resin, a methacrylic acid ester resin, and a compound having a propylene glycol unit, to suppress yellowing, with preferred antioxidants like tris(2,4-di-tert-butylphenyl)phosphite, resulting in a resin composition with a yellowness index of 6.0 or less.
The resin composition effectively suppresses yellowing and maintains high transparency and chemical resistance, suitable for use in decorative films and surface materials for automobiles and architectural applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Resin composition, laminated film and decorative film
[0001] The present invention relates to a resin composition, a laminate film, and a decorative film.
[0002] Taking advantage of their weather resistance, chemical resistance, and stain resistance, vinylidene fluoride resins have been widely used as surface materials for outdoor signs, wrapping films for mobility, repair films in the infrastructure field, etc. In recent years, vinylidene fluoride resins have also been used as surface materials for decorative films used in the interior or exterior of automobiles and buildings, or in electrical appliance components, and research and development into these resins is progressing from various perspectives.
[0003] In recent years, designs have become increasingly diverse and complex, particularly in automotive interiors, and high transparency is required for the outermost layer of decorative films to preserve color and texture. In particular, metallic decorative films, which are produced by metal deposition on resin films to impart a metallic design, require an outermost layer with high transparency. For this reason, technologies have been developed to improve the transparency of resin films containing vinylidene fluoride resins.
[0004] Patent Document 1 proposes a film containing a vinylidene fluoride resin (A) and an acrylic resin (B), in order to provide a film with high crystallinity, transparency, and surface smoothness, and having an arithmetic mean roughness of at least one surface of 0.1 to 20 nm, a heat of crystalline fusion of 18 to 40 J / g as measured by a differential scanning calorimeter, and a haze value of 3.5 or less.
[0005] Patent Document 2 describes the successful production of a novel fluororesin film that can be used for vehicle interior and exterior component applications and that is excellent in transparency, surface hardness, chemical resistance, and stain resistance, by using a fluorine-containing (meth)acrylic resin containing a fluorine-containing alkyl (meth)acrylate polymer component. This document specifically discloses a fluororesin-laminated acrylic resin film in which a fluororesin film layer is laminated on at least one side of a film layer made of an acrylic resin (A), the fluororesin film layer being formed from a fluororesin (C) containing a fluorine-containing (meth)acrylic resin (B) that contains a fluorine-containing alkyl (meth)acrylate polymer component.
[0006] Patent Document 3 discloses that the film can be prevented from becoming cloudy by providing a protective layer made of a plurality of mixed resin layers containing a vinylidene fluoride resin and an acrylic ester resin.
[0007] International Publication No. 2011 / 142453 Japanese Patent Application Laid-Open No. 2012-187934 Japanese Patent Application Laid-Open No. 2021-123082
[0008] Traditionally, fluorine-based emulsifiers have been used to polymerize vinylidene fluoride to produce vinylidene fluoride-based resins. However, due to their bioaccumulation potential, their use may be subject to future restrictions. Polypropylene glycol-based emulsifiers are an emulsifier that can be used instead of fluorine-based emulsifiers during the production of vinylidene fluoride-based resins. However, it has been found that resin compositions containing vinylidene fluoride-based resins produced using polypropylene glycol-based emulsifiers tend to yellow due to the presence of compounds containing propylene glycol units derived from the emulsifier. A yellowish tinge in the resin composition is undesirable from the standpoint of the appearance of products obtained by molding the resin composition. However, such yellowing cannot be prevented using conventional techniques.
[0009] One aspect of the present invention has been made in view of the above circumstances, and an object of the present invention is to suppress yellowing in a resin composition that contains, in addition to a vinylidene fluoride resin, a compound having a propylene glycol unit.
[0010] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, they found that a phosphite ester-based antioxidant is effective in suppressing yellowing of a resin composition containing a vinylidene fluoride resin produced using a polypropylene glycol-based emulsifier, i.e., a resin composition containing a compound having a propylene glycol unit in addition to a vinylidene fluoride resin, and thus arrived at the present invention.
[0011] [Aspect 1] A resin composition comprising: 100 parts by mass of a mixed resin of 60 to 95 parts by mass of a vinylidene fluoride resin and 5 to 40 parts by mass of a methacrylate ester resin; a compound having a propylene glycol unit; and 0.05 to 1 part by mass of a phosphite ester antioxidant relative to 100 parts by mass of the mixed resin.
[0012] [Aspect 2] The resin composition according to Aspect 1, wherein the content of the propylene glycol unit in the compound having the propylene glycol unit is 0.001 parts by mass or more and 0.1 parts by mass or less per 100 parts by mass of the vinylidene fluoride unit content of the vinylidene fluoride resin.
[0013] [Aspect 3] The resin composition according to Aspect 1 or 2, wherein the phosphite antioxidant is at least one selected from the group consisting of tris(2,4-di-tert-butylphenyl)phosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, 2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocine, and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane.
[0014] [Embodiment 4] The resin composition according to any one of embodiments 1 to 3, wherein the resin composition is in a pellet form and has a yellowness index of 6.0 or less.
[0015] [Aspect 5] The resin composition according to any one of Aspects 1 to 4, wherein the total content of the vinylidene fluoride resin, the methacrylate ester resin, and the phosphite ester antioxidant is 90 mass% or more based on the total amount of the resin composition.
[0016] [Aspect 6] A laminated film comprising: a surface layer made of the resin composition according to any one of aspects 1 to 5; and a back layer made of a resin composition containing a methacrylic acid ester-based resin, laminated on one side of the surface layer.
[0017] [Embodiment 7] The laminate film according to embodiment 6, wherein the laminate film has a haze of 3.0% or less as measured in accordance with JIS K7136:2000.
[0018] [Embodiment 8] A decorative film comprising: the laminate film according to embodiment 6 or 7; and a decorative layer having a design, laminated directly or indirectly on the back surface layer side of the laminate film.
[0019] According to one aspect of the present invention, yellowing can be suppressed in a resin composition containing a compound having a propylene glycol unit in addition to a vinylidene fluoride resin.
[0020] Furthermore, resin compositions containing vinylidene fluoride resins used in surface materials may be required to have low opacity when formed into a film, high transparency, and high chemical resistance. In contrast, by forming a film from a resin composition according to one aspect of the present invention, a film with low opacity, high transparency, and high chemical resistance can be obtained. In another aspect, the present invention can provide a laminate film comprising such a resin composition. In another aspect, the present invention can provide a decorative film comprising such a laminate film. In other words, the resin composition can be suitably used as various surface materials, for example, decorative films, in the automotive and architectural fields.
[0021] 1 is a schematic cross-sectional view showing a laminate structure of a laminate film according to one embodiment of the present invention.
[0022] The following describes embodiments of the present invention. The embodiments described below are illustrative of typical embodiments of the present invention, and are not intended to narrow the technical scope of the present invention.
[0023] (1. Resin Composition) A resin composition according to one embodiment of the present invention contains a vinylidene fluoride resin, a methacrylate ester resin, a compound having a propylene glycol unit, and a phosphite ester antioxidant.
[0024] The resin composition may be in the form of, for example, pellets or a film. The yellowness index of the resin composition is preferably 6.0 or less, more preferably 5.5 or less, and even more preferably 5.0 or less. From the viewpoint of suppressing variation in color tone of products obtained by molding the resin composition, the yellowness index of the resin composition is preferably 2.0 or more, more preferably 3.0 or more, and even more preferably 4.0 or more. The yellowness index of the resin composition is, for example, preferably 2.0 or more and 6.0 or less, more preferably 3.0 or more and 5.5 or less, and even more preferably 4.0 or more and 5.0 or less. When the resin composition is in the form of pellets, it is particularly preferable that the yellowness index of the resin composition (pellets) is within the above range. In this specification, a pellet refers to a pellet having a volume measured from the outer dimensions of one particle of 6.5 to 50 mm 3 Also, in this specification, yellowness refers to yellowness index (YI) measured in accordance with ASTM E313.
[0025] The content of the vinylidene fluoride resin may be 55% by mass or more, 60% by mass or more, 62.5% by mass or more, 65% by mass or more, 70% by mass or more, or 75% by mass or more, based on the total amount of the resin composition, and may be 95% by mass or less, 92.5% by mass or less, 90% by mass or less, or 85% by mass or less.
[0026] The mixing ratio of the vinylidene fluoride resin and the methacrylate ester resin in the resin composition (also referred to herein as the "mixed resin") is preferably 60 to 95 parts by mass:5 to 40 parts by mass, more preferably 60 to 80 parts by mass:20 to 40 parts by mass, even more preferably 62.5 to 77.5 parts by mass:22.5 to 37.5 parts by mass, and even more preferably 65 to 75 parts by mass:25 to 35 parts by mass, per 100 parts by mass of the mixed resin. When the vinylidene fluoride resin is 60 parts by mass or more per 100 parts by mass of the mixed resin, properties such as chemical resistance, weather resistance, and contamination resistance can be improved. Furthermore, by setting the content of the methacrylate ester-based resin to 5 parts by mass or more per 100 parts by mass of the mixed resin, when the resin composition is formed into a film to form a surface layer, the adhesiveness and adhesion to the back surface layer can be improved. Furthermore, since the methacrylate ester-based resin has a higher compatibility with antioxidants than the vinylidene fluoride-based resin, there is also the advantage that the film is less likely to become cloudy.
[0027] In this specification, vinylidene fluoride resins include homopolymers of vinylidene fluoride and copolymers of vinylidene fluoride and monomers copolymerizable with vinylidene fluoride. Examples of monomers copolymerizable with vinylidene fluoride include vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, hexafluoroisobutylene, trifluoroethylene chloride, and fluorinated alkyl vinyl ethers. The monomer may be a known vinyl monomer such as styrene, ethylene, butadiene, or propylene. These monomers may be used alone or in combination of two or more. Among these, at least one selected from the group consisting of vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluoroethylene chloride is preferred, with hexafluoropropylene being more preferred.
[0028] Polymerization reactions for obtaining vinylidene fluoride resins include known polymerization reactions such as radical polymerization and anionic polymerization. Furthermore, in order to reduce environmental impact, emulsion polymerization using a propylene glycol-based emulsifier is a suitable method for polymerizing vinylidene fluoride resins. Polypropylene glycol-based emulsifiers are substances with a low environmental impact because they have a lower bioaccumulation tendency than fluorine-based emulsifiers. When a propylene glycol-based emulsifier is used as an emulsifier, compounds having propylene glycol units derived from the propylene glycol-based emulsifier remain as impurities in the vinylidene fluoride resin. The resin composition according to this embodiment can suppress yellowing even when it contains a compound having a propylene glycol unit in addition to a vinylidene fluoride resin.
[0029] Examples of propylene glycol-based emulsifiers include polypropylene glycol acrylate, polypropylene glycol, polypropylene glycol methacrylate, and polypropylene glycol dimethacrylate. One type of propylene glycol-based emulsifier may be used alone, or two or more types may be used in combination. Furthermore, a copolymer such as a block copolymer of at least one unit selected from the group consisting of an ethylene glycol unit and a tetramethylene glycol unit with a propylene glycol unit may also be used.
[0030] The resin composition may contain the above-mentioned propylene glycol-based emulsifier itself as the compound having a propylene glycol unit, or may contain a compound derived from the above-mentioned propylene glycol-based emulsifier. That is, the compound having a propylene glycol unit may be a propylene glycol-based emulsifier or a compound derived therefrom. The compound derived from a propylene glycol-based emulsifier may be, for example, a decomposition product of the propylene glycol-based emulsifier.
[0031] In one embodiment, the content of the propylene glycol unit in the compound having the propylene glycol unit may be 0.001 parts by mass or more and 0.1 parts by mass or less, 0.01 parts by mass or more and 0.09 parts by mass or less, or 0.02 parts by mass or more and 0.08 parts by mass or less, relative to 100 parts by mass of the vinylidene fluoride unit content of the vinylidene fluoride resin.
[0032] The content (parts by mass) of glycol units relative to 100 parts by mass of vinylidene fluoride units is measured by a nuclear magnetic resonance (NMR) spectrometer under the following conditions: NMR spectrometer: AVANCE NEO 500 (Bruker Bio Spin) or a device having equivalent performance Probe: CPBBO 5 mm Observation nucleus: 1H Measurement solvent: DMSO-d6 (measurement temperature 70°C) Sample amount: 100 mg (PVDF resin composition) The propylene glycol units are formed by the CH 3 The range of 1.04 to 1.08 ppm is integrated to determine the molar ratio, which is then converted into parts by mass. The propylene glycol unit is [-CH(CH 3 )-CH 2 The formula weight per unit is calculated as 58. The vinylidene fluoride unit is represented by CH 2 Regarding the head-to-head bond (-CF 2 -CH 2 -CH 2 -CF 2 -): 2.15-2.45ppm Head-to-tail bond (-CF 2 -CH 2 -CF 2 -CH 2 -): 2.60 to 3.10 ppm. The range is integrated, the sum is calculated, the molar ratio is calculated, and then converted into parts by mass. 2 -CH 2 -] and the formula weight per unit is calculated as 64.
[0033] Although the present invention is not intended to be limited by theory, the present inventors speculate as follows: If a compound having a propylene glycol unit remains in a resin composition, an oxidation reaction occurs due to heat during compound processing and film formation, generating peroxides. It is speculated that radicals are generated from the generated peroxides, which oxidize chemical bonds in the resin composition, resulting in yellowing. Therefore, it is desirable to prevent the oxidation of the compound having a propylene glycol unit, or to reduce the compound if it is oxidized. According to the research results of the present inventors, a phosphite-based antioxidant is effective in suppressing yellowing. One type of phosphite-based antioxidant may be used alone, or two or more types may be used in combination.
[0034] The phosphite-based antioxidant may be, but is not limited to, at least one selected from the group consisting of tris(2,4-di-tert-butylphenyl)phosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, 2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane.
[0035] From the viewpoint of enhancing the effect of inhibiting yellowing, the content of the phosphite ester-based antioxidant in the resin composition is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, per 100 parts by mass of the mixed resin. From the viewpoint of preventing cloudiness and bleed-out due to excessive addition, the content of the phosphite ester-based antioxidant in the resin composition is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.6 parts by mass or less, per 100 parts by mass of the mixed resin. The content of the phosphite ester-based antioxidant in the resin composition is preferably 0.05 parts by mass or more and 1 part by mass or less, more preferably 0.1 parts by mass or more and 0.8 parts by mass or less, and even more preferably 0.3 parts by mass or more and 0.6 parts by mass or less, per 100 parts by mass of the mixed resin.
[0036] In this specification, the methacrylic acid ester-based resin includes a homopolymer of a methacrylic acid ester and a copolymer of a methacrylic acid ester and a monomer copolymerizable with the methacrylic acid ester.
[0037] The methacrylic acid ester may be, for example, a methacrylic acid alkyl ester. The number of carbon atoms in the alkyl group in the methacrylic acid alkyl ester may be 1 or more, and may be 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less. The alkyl group may be linear or branched. The methacrylic acid alkyl ester is preferably methyl methacrylate.
[0038] Examples of monomers copolymerizable with methacrylic acid esters include (meth)acrylic acid esters such as butyl acrylate, butyl methacrylate, ethyl acrylate, and ethyl methacrylate; aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, t-butylstyrene, divinylbenzene, and tristyrene; vinyl cyanide monomers such as acrylonitrile and methacrylonitrile; glycidyl group-containing monomers such as glycidyl (meth)acrylate; vinyl carboxylate monomers such as vinyl acetate and vinyl butyrate; olefin monomers such as ethylene, propylene, and isobutylene; diene monomers such as 1,3-butadiene and isoprene; unsaturated carboxylic acid monomers such as maleic acid, maleic anhydride, and (meth)acrylic acid; and enone monomers such as vinyl methyl ketone. These monomers can be used alone or in combination of two or more.
[0039] From the viewpoint of film strength and flexibility, the methacrylic acid ester resin is preferably a homopolymer of methyl methacrylate or an acrylic rubber-modified methacrylic copolymer in which a monomer mainly composed of methyl methacrylate (including methyl methacrylate) is copolymerized with an acrylic rubber containing butyl (meth)acrylate.
[0040] The content of the methacrylic acid ester resin may be 5% by mass or more, 7% by mass or more, 10% by mass or more, 13% by mass or more, 15% by mass or more, or 17% by mass or more, based on the total amount of the resin composition, and may be 40% by mass or less, 35% by mass or less, 30% by mass or less, or 25% by mass or less.
[0041] Polymerization reactions for obtaining methacrylic acid ester-based resins include known polymerization reactions such as radical polymerization, living radical polymerization, living anionic polymerization, and living cationic polymerization. Furthermore, known polymerization methods include bulk polymerization, suspension polymerization, emulsion polymerization, and solution polymerization. The mechanical properties of the resulting resin vary depending on the polymerization reaction and polymerization method.
[0042] When the vinylidene fluoride resin and the methacrylic acid ester resin are copolymers, the types of copolymers include random copolymers, graft copolymers, block copolymers (for example, linear types such as diblock copolymers, triblock copolymers, and gradient copolymers, star copolymers polymerized by the arm-first method or the core-first method, etc.), copolymers obtained by polymerization using macromonomers, which are polymerizable functional compounds (macromonomer copolymers), and mixtures thereof. Among these, graft copolymers and block copolymers are preferred from the viewpoint of resin productivity.
[0043] The melting point of the vinylidene fluoride resin is preferably 150° C. or higher, more preferably 160° C. or higher, and is preferably 170° C. or lower, which is the same as the melting point of polyvinylidene fluoride (PVDF).
[0044] The glass transition point (Tg) of the methacrylate ester resin is preferably 70° C. or higher, more preferably 80° C. or higher, and preferably 120° C. or lower.
[0045] The melting point of the vinylidene fluoride resin and the Tg of the methacrylic acid ester resin can be measured by heat flux differential scanning calorimetry (heat flux DSC). For example, they can be determined from a DSC curve (first run) obtained by heating a 1.5 mg sample from room temperature to 200°C at a heating rate of 10°C / min using a Bruker AXS DSC3100SA differential scanning calorimeter.
[0046] In addition to the vinylidene fluoride resin, the methacrylate resin, and the phosphite antioxidant, the resin composition may appropriately contain, within the scope of the object of the present invention, other resins, plasticizers, heat stabilizers, other antioxidants, light stabilizers, crystal nucleating agents, antiblocking agents, sealability improvers, mold release agents, colorants, pigments, foaming agents, flame retardants, etc. In one embodiment, the total content of the vinylidene fluoride resin, the methacrylate resin, and the phosphite antioxidant in the resin composition may be 90% by mass or more, 95% by mass or more, or 98% by mass or more, based on the total amount of the resin composition.
[0047] The resin composition may further contain an ultraviolet absorber. When used as a surface layer of a laminate film described below, the resin composition preferably does not contain an ultraviolet absorber from the viewpoints of cost and bleed-out.
[0048] The resin composition can be produced by known methods, such as a melt-kneading method using an extruder. Components such as a vinylidene fluoride resin produced using a propylene glycol-based emulsifier as a polymerization aid, a methacrylate resin, and a phosphite-based antioxidant are premixed in an unmolten state, then melted and uniformly mixed in an extruder. The resulting mixture is then extruded into a strand, cooled, and pelletized in a pelletizer to produce a pelletized resin composition. Common extruders that can be used include single-screw, twin-screw, and tandem types. A twin-screw extruder is preferred from the viewpoint of uniform dispersion. The resulting pelletized resin composition can be processed into a desired shape, such as a film.
[0049] (2. Laminated Film) Fig. 1 shows a schematic cross-sectional view illustrating the laminate structure of a laminated film 1 according to one embodiment of the present invention. The laminated film 1 has a laminate structure including a surface layer 10 and a back surface layer 20 laminated on one side of the surface layer 10. In one embodiment, the surface layer 10 and the back surface layer 20 are in contact with each other without any other layer interposed between them.
[0050] (2-1. Surface Layer) In one embodiment, the surface layer is composed of the above-mentioned resin composition containing 100 parts by mass of a mixed resin of 60 to 95 parts by mass of a vinylidene fluoride resin and 5 to 40 parts by mass of a methacrylic acid ester resin, a compound having a propylene glycol unit, and 0.05 to 1 part by mass of a phosphite ester antioxidant relative to 100 parts by mass of the mixed resin. The embodiments of the resin composition have already been described, so redundant description will be omitted.
[0051] The average thickness of the surface layer is preferably 1 to 40 μm, more preferably 5 to 35 μm, even more preferably 8 to 30 μm, and particularly preferably 10 to 20 μm. When the average thickness of the film is 1 μm or more, film formability is improved and the protective function when used as the outermost layer can be improved. When the average thickness of the film is 40 μm or less, improved transparency and cost reduction can be achieved. The surface layer may be formed as a single layer or as multiple layers, but it is desirable that the total average thickness falls within the above-mentioned average thickness range. The average thickness of the surface layer can be calculated as the average value when thicknesses are measured at multiple locations by observing the cross section of the surface layer using a confocal laser microscope.
[0052] (2-2. Backside Layer) The backside layer is composed of a resin composition containing a methacrylate ester-based resin. The resin composition may further contain a vinylidene fluoride-based resin. In one embodiment, the backside layer may be composed of a resin composition containing 0 to 30 parts by mass of a vinylidene fluoride-based resin and 70 to 100 parts by mass of a methacrylate ester-based resin, totaling 100 parts by mass. The backside layer does not need to contain a vinylidene fluoride-based resin, but it preferably does so because it allows for the reuse of leftover laminate film generated during the manufacturing process as the backside layer. The mixing ratio of the vinylidene fluoride-based resin and the methacrylate ester-based resin in the backside layer is more preferably 5 to 28 parts by mass:72 to 95 parts by mass, and even more preferably 10 to 25 parts by mass:75 to 90 parts by mass, based on a total of 100 parts by mass of both.
[0053] The content of vinylidene fluoride resin in the back surface layer may be 5 mass% or more, 8 mass% or more, 10 mass% or more, 15 mass% or more, or 17 mass% or more, based on the total amount of the resin composition in the back surface layer, and may be 28 mass% or less, 25 mass% or less, or 22 mass% or less.
[0054] The content of the methacrylic acid ester resin in the back surface layer may be 70% by mass or more, 72% by mass or more, or 75% by mass or more, based on the total amount of the resin composition in the back surface layer, and may be 95% by mass or less, 90% by mass or less, 85% by mass or less, or 80% by mass or less.
[0055] Unless otherwise specified, the definitions and embodiments of vinylidene fluoride resins and vinylidene fluoride resins, including preferred embodiments, are as described in the description of the surface layer, and therefore redundant description will be omitted. The emulsifier for the vinylidene fluoride resin in the back layer preferably does not contain a fluorine-based emulsifier. As an alternative to a fluorine-based emulsifier, it is preferable to use a propylene glycol-based emulsifier to the extent that it does not affect yellowing. Furthermore, if a compound having a propylene glycol unit in an amount that affects yellowing remains in the vinylidene fluoride resin, it is preferable to add a phosphite ester-based antioxidant under the conditions described in the description of the surface layer. Since the proportion of vinylidene fluoride resin in the back layer is small, the effect of yellowing can often be ignored.
[0056] The average thickness of the back surface layer is preferably 10 to 100 μm, more preferably 15 to 90 μm, even more preferably 20 to 85 μm, and particularly preferably 25 to 80 μm. An average film thickness of 10 μm or more improves film formability and enhances protective function when used as a protective layer for a decorative film. An average film thickness of 100 μm or less can achieve improved transparency and processability. The back surface layer may be formed as a single layer or multiple layers, but it is desirable that the total average thickness falls within the above-mentioned range. The average thickness of the back surface layer can be calculated as the average value of thicknesses measured at multiple locations by observing the cross section of the back surface layer using a confocal laser microscope.
[0057] In addition to the methacrylate ester-based resin and the vinylidene fluoride-based resin, the back surface layer may contain, as appropriate, ultraviolet absorbers, other resins, plasticizers, heat stabilizers, antioxidants, light stabilizers, nucleating agents, antiblocking agents, sealability improvers, mold release agents, colorants, pigments, foaming agents, flame retardants, and the like, provided that the object of the present invention is not impaired. In one embodiment, the total content of the methacrylate ester-based resin and the vinylidene fluoride-based resin in the back surface layer may be 90% by mass or more, 95% by mass or more, or 97% by mass or more, based on the total amount of the resin composition. Because the proportion of the vinylidene fluoride-based resin in the back surface layer is small, yellowing of the resin composition for the back surface layer is slight, and there is no need to add a phosphite ester-based antioxidant to the resin composition for the back surface layer. Furthermore, by not adding a phosphite ester-based antioxidant to the resin composition for the back surface layer, cloudiness can be prevented when the resin composition is formed into a film.
[0058] The back surface layer preferably contains an ultraviolet absorber. By containing an ultraviolet absorber in the back surface layer, ultraviolet rays are blocked and weather resistance can be effectively improved. Examples of ultraviolet absorbers include, but are not limited to, hydroquinone-based, triazine-based, benzotriazole-based, benzophenone-based, cyanoacrylate-based, oxalic acid-based, hindered amine-based, and salicylic acid derivatives, and these can be used alone or in combination of two or more. Among these, in terms of the durability of the ultraviolet absorption effect, it is preferable to contain a triazine-based compound, a benzotriazole-based compound, or a mixture thereof.
[0059] The content of the UV absorber in the back surface layer is preferably 0.1 to 10 parts by mass per 100 parts by mass of the mixed resin of vinylidene fluoride resin and methacrylate ester resin in the back surface layer. By making the content of the UV absorber in the back surface layer 0.1 parts by mass or more, preferably 1 part by mass or more, and more preferably 2 parts by mass or more per 100 parts by mass of the mixed resin of vinylidene fluoride resin and methacrylate ester resin in the back surface layer, it is possible to expect improved weather resistance and UV absorption effects. Furthermore, by making the content of the UV absorber in the back surface layer 10 parts by mass or less, preferably 5 parts by mass or less per 100 parts by mass of the mixed resin of vinylidene fluoride resin and methacrylate ester resin in the back surface layer, it is possible to prevent the UV absorber from bleeding out to the film surface and achieve cost reductions.
[0060] (2-3. Properties of Laminated Film) The average thickness of the laminated film may be 40 μm or more, 45 μm or more, or 47 μm or more, and may be 60 μm or less, 55 μm or less, or 52 μm or less.
[0061] The haze of the laminate film according to one embodiment of the present invention, measured in accordance with JIS K7136: 2000, may be 3.0% or less. From the viewpoint of enhancing transparency, the haze is preferably 2.5% or less, more preferably 2.0% or less, and may be, for example, 1.0 to 3.0%.
[0062] The laminate film according to one embodiment of the present invention may have a total light transmittance of 80% or more as measured in accordance with JIS K7361-1: 1997. From the viewpoint of increasing transparency, the total light transmittance is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more, and may be, for example, 80 to 95%.
[0063] (3. Manufacturing Method of Laminated Film) A laminated film according to one embodiment of the present invention can be manufactured by, for example, a melt coextrusion molding method in which multiple resins are bonded and laminated in a molten state using multiple extruders. Examples of melt coextrusion molding methods include a multi-manifold die method, a feed block die method, and a dual slot die method. In the multi-manifold die method, multiple resins are formed into a sheet, and then the layers are brought into contact and bonded at the tip inside a T-die. In the feed block die method, multiple resins are bonded in a merging device (feed block) and then spread into a sheet. In the dual slot die method, multiple resins are molded into a sheet, and then the layers are brought into contact and bonded at the tip outside the T-die. The film can also be manufactured by an inflation molding method using a round die.
[0064] The laminated film can be produced, for example, by carrying out the following steps: Step 1: A step of melt-co-extrusion molding a resin composition for the surface layer and a resin composition for the back layer into a film shape through a T-die at a temperature of 200 to 260°C so that each has a predetermined thickness. Step 2: A step of contacting at least the surface of the melt-co-extruded film, which has been extruded from the outlet of the T-die and is facing the resin composition for the surface layer, with the surface of a metal roll whose temperature is adjusted to 20 to 60°C, thereby cooling the film.
[0065] When producing a film with a thickness of about 30 to 50 μm under the above conditions, a film conveying speed of 5 to 9 m / min is appropriate. In addition, from the viewpoint of removing foreign matter, it is preferable to install a screen mesh inside the extruder.
[0066] The temperature of the metal roll surface can be adjusted, for example, by circulating a cooling medium such as cooling water inside the metal roll.
[0067] During cooling, it is more preferable to place a rubber touch roll opposite the metal roll and pinch the laminate of the resin composition for the surface layer and the resin composition for the back layer in a molten state extruded from the outlet of the T-die between the metal roll (cast roll) and the touch roll, from the viewpoint of transferring the smooth surface of the metal roll to the film. The surface temperature of the rubber touch roll is preferably 0 to 70°C, more preferably 0 to 30°C, from the viewpoint of suppressing the transfer of the surface shape of the rubber roll.
[0068] From the viewpoint of smoothing the surface of the laminate film, particularly the outer surface of the backing layer, it is desirable that the surface roughness of the metal roll be small, and it is also desirable that the surface roughness of the touch roll be small. This is because the surface roughness of the metal roll and the touch roll affects the surface properties of the laminate film. The arithmetic mean roughness Ra of the surface of the metal roll, measured in accordance with JIS B0601:2001, is preferably 100 nm or less, more preferably 80 nm or less, even more preferably 60 nm or less, even more preferably 40 nm or less, and even more preferably 20 nm or less, and can be, for example, 10 to 100 nm. The arithmetic mean roughness Ra of the surface of the touch roll, measured in accordance with JIS B0601:2001, is preferably 150 nm or less, more preferably 120 nm or less, and can be, for example, 100 to 150 nm.
[0069] (4. Film Laminated with Substrate) A substrate may be laminated to the laminate film according to one embodiment of the present invention. One embodiment of the present invention is a film in which a substrate is laminated on the front layer and / or back layer of the laminate film. If the average value of the total thickness of the film laminated with the substrate is 50 to 1000 μm, this is preferred from the viewpoints of workability and cost in bonding to automobile interior parts.
[0070] Examples of the substrate include an anchor layer, a decorative layer, a protective layer, an adhesive layer, a printed layer, a metal vapor deposition layer, etc. The substrate may be used as a single layer or as a laminate of two or more types.
[0071] In a preferred embodiment, a decorative film is provided in which the laminate film is laminated as the outermost layer with the surface layer (film containing vinylidene fluoride resin) facing outwards.
[0072] In one embodiment, the decorative film includes the laminate film and a decorative layer that is laminated directly or indirectly on the back surface side of the laminate film and has a design. The decorative layer may be a decorative layer that has a design imparted by one or more methods selected from printing, vapor deposition, painting, lamination, and coloring. Here, "laminate" refers to a sheet-like decorative layer such as a resin sheet on which a design is printed.
[0073] Examples of methods for laminating a substrate to the laminate film according to one embodiment of the present invention include adhesive lamination and thermal lamination. Other known lamination methods can also be used. Furthermore, the laminate film can be used for heat molding. Examples of heat molding methods include vacuum molding, pressure molding, and vacuum pressure molding, in which a substrate is attached to one or both sides of the laminate film.
[0074] Examples of methods for applying decorative film to surfaces of articles such as automotive interior parts include film insert molding, in-mold molding, and vacuum lamination molding (including vacuum and pressure forming such as TOM molding). Film insert molding, in particular, involves a process of preforming the decorative film by heating it, allowing the decorative film to conform to parts with more complex shapes than in-mold molding and vacuum lamination molding. As a result, film insert molding can achieve a good surface coating.
[0075] The present invention will be described in detail below based on examples and comparative examples.
[0076] (1. Preparation of Pellet-Shaped Resin Composition) <Vinylidene Fluoride Resin> The following materials were prepared as vinylidene fluoride resins (PVDF): Kynar 740 (trade name, manufactured by Arkema) (a homopolymer of vinylidene fluoride produced using a propylene glycol-based emulsifier as a polymerization aid, melting point 168°C) (abbreviation: K740) Kynar 1000HD (trade name, manufactured by Arkema) (a homopolymer of vinylidene fluoride produced using a fluorine-based emulsifier as a polymerization aid, melting point 168°C) (abbreviation: 1000HD)
[0077] The content of the propylene glycol unit in the compound having the propylene glycol unit (parts by mass, indicated as "PG content" in the tables) relative to 100 parts by mass of the vinylidene fluoride unit content of the vinylidene fluoride resin was measured using a nuclear magnetic resonance (NMR) spectrometer under the conditions described above. The results are shown in Tables 1 to 4. Since no compound having a propylene glycol unit was detected in 1000HD, it is indicated as "-" in the tables.
[0078] <Methacrylate Resin> The following materials were prepared as methacrylate resins: "Sumipex MGSS" (polymethyl methacrylate with a Tg of 101°C) (abbreviation: MGSS) manufactured by Sumitomo Chemical Co., Ltd.
[0079] <Antioxidant> The following materials were prepared as antioxidants. - Phosphite ester-based antioxidant manufactured by BASF Japan Ltd.: trade name Irgafos168 (tris(2,4-di-tert-butylphenyl)phosphite) (abbreviation: Irgafos168) - Phosphite ester-based antioxidant manufactured by ADEKA Corporation: trade name Adekastab PEP-8 (3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane) (abbreviation: PEP-8) - Phosphite ester-based antioxidant manufactured by ADEKA Corporation: trade name Adekastab PEP-36 (3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane) (abbreviation: PEP-36) Phosphite ester antioxidant manufactured by ADEKA Corporation: trade name Adekastab HP-10 (2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocin) (abbreviation: HP-10) Phenolic antioxidant manufactured by BASF Japan Ltd.: trade name Irganox 1010 (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)) (abbreviation: Irganox 1010) Phenolic antioxidant manufactured by BASF Japan Ltd.: trade name Irganox 1076 (octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) (abbreviation: Irganox 1076)
[0080] In each Example, Comparative Example, and Reference Example, the materials were kneaded with the compositions shown in Tables 1 to 4 using a φ30 mm twin-screw extruder, and the extruded resin composition was cut with a pelletizer to obtain pellets (each having a size of 28 mm) according to each Example, Comparative Example, and Reference Example. 3 As the vinylidene fluoride resin, K740 was used in the examples and comparative examples, and 1000HD was used in the reference example.
[0081] (2. Evaluation of Properties of Pellet-Shaped Resin Compositions) The yellowness index (YI) of the pellets obtained above according to each of the Examples, Comparative Examples, and Reference Examples (referred to in the tables as "Yellowness index (YI) (A) of pellets before heating") was measured in accordance with ASTM E313 using a colorimetric color difference meter ZE6000 manufactured by Nippon Denshoku Industries Co., Ltd. The pellets obtained above according to each of the Examples, Comparative Examples, and Reference Examples were dry-heated (80°C x 48 hours) in a dehumidifying dryer DFB-25Z manufactured by Kawata Corporation, and the yellowness index (YI) (B) of the pellets after cooling to room temperature was measured in the same manner (referred to in the tables as "Yellowness index (YI) (B) of pellets after heating"). The results are shown in Tables 1 to 4. Tables 1 to 4 also show the difference ΔYI between (A) and (B) above.
[0082]
[0083]
[0084]
[0085]
[0086] As can be seen from Tables 1 to 4, vinylidene fluoride produced using a propylene glycol-based emulsifier contains residual compounds having propylene glycol units, and the pellet-shaped resin compositions of Comparative Examples 1-1 and 1-2 produced by kneading these compounds have a high yellowness. Furthermore, heating the pellet-shaped resin compositions of Comparative Examples 1-1 and 1-2 caused further yellowing. Furthermore, Comparative Examples 1-3 and 1-4 showed that adding a phenolic antioxidant had little effect on suppressing yellowing.
[0087] In contrast, in Examples 1-1 to 1-10, in which a phosphite-based antioxidant was added, yellowing was significantly suppressed, and yellowing hardly progressed even when heated. Thus, it was demonstrated that adding a phosphite-based antioxidant is effective in suppressing yellowing of resin compositions containing a vinylidene fluoride resin, a methacrylic acid ester resin, and a compound having a propylene glycol unit. Note that, since the vinylidene fluoride resins used in Reference Examples 1-1 to 1-3 were produced using a fluorine-based emulsifier (i.e., the resin compositions did not contain a compound having a propylene glycol unit), yellowing was not observed.
[0088] (3. Production of Laminated Film) <<For Surface Layer>> The aforementioned K740 and 1000HD were prepared as vinylidene fluoride resins (PVDF). The aforementioned MGSS was prepared as methacrylate resins. The aforementioned Irgafos168, PEP-8, PEP-36, and HP-10 were prepared as phosphite antioxidants. <<For Back Layer>> <Methacrylate Resin> The following materials were prepared as methacrylate resins: - "Hypet HBS000" manufactured by Mitsubishi Chemical Corporation (a methacrylate resin with a Tg of 97°C that contains a crosslinked rubber component of butyl acrylate (n-BA) and butyl methacrylate (BMA)) (abbreviation: HBS000) <Vinylidene Fluoride Resin> The following materials were prepared as vinylidene fluoride resins (PVDF). Kynar 720 (trade name: Arkema) (a homopolymer of vinylidene fluoride produced using a propylene glycol-based emulsifier as a polymerization aid, melting point: 168°C) (abbreviation: K720) <UV absorber> The following material was prepared as the UV absorber: Tinuvin (registered trademark) 234, a benzotriazole-based UV absorber manufactured by BASF The content of the UV absorber was 3.2 parts by mass relative to 100 parts by mass of the mixed resin of vinylidene fluoride-based resin and methacrylate ester-based resin in the back surface layer.
[0089] (4. Preparation of Laminated Film) In each of the Examples, Comparative Examples, and Reference Examples, materials were kneaded using a φ30 mm twin-screw extruder with the compositions shown in Tables 5 to 7, and the extruded resin composition was cut using a pelletizer to obtain pellets (each having a size of 28 mm) for the surface layer and the back layer of each of the Examples, Comparative Examples, and Reference Examples. 3 As the vinylidene fluoride resin for the surface layer, K740 was used in the examples and comparative examples, and 1000HD was used in the reference example.
[0090] Using two φ40 mm single-screw extruders and a feed block die-type multi-layer extruder equipped with a feed block and a T-die at the tip, the surface layer pellets and the back layer pellets were melt-extruded. The film-like resin composition extruded from the T-die at a temperature of 240 ° C was conveyed at a conveying speed of 6.7 m / min and cooled by sandwiching it between a metal roll (surface temperature: about 20 ° C) and a rubber touch roll (surface temperature: about 40 ° C) through which cooling water flows, to obtain a laminated film corresponding to each test number. Here, the arithmetic mean roughness Ra of the surface of the metal roll was measured in accordance with JIS B0601:2001 using a contact surface roughness meter (Mitutoyo Corporation "SJ210") and found to be 0.013 μm. The arithmetic mean roughness Ra of the surface of the touch roll was measured in accordance with JIS B0601:2001 using a contact type surface roughness meter ("SJ210" manufactured by Mitutoyo Corporation) and was found to be 0.116 μm.
[0091] (5. Evaluation of Film Properties) <5-1. Average Thickness> For each laminate film (widthwise length 400 mm) produced under the above conditions, a cross section was observed at a magnification of 2000x using a confocal laser microscope ("VK-X100" manufactured by Keyence Corporation), and the thicknesses of the surface layer and back layer were measured based on the distance between two points. Measurements were performed at nine points at 50 mm intervals in the film width direction (TD) at any one point in the machine direction (MD), and the average value was taken as the measured value. In each of the Examples, Comparative Examples, and Reference Examples, the average thickness of the surface layer was 17 μm, and the average thickness of the back layer was 33 μm.
[0092] <5-2. Haze> The haze value of each laminate film produced under the above conditions was measured at 25°C using a haze meter ("NDH7000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7136: 2000. The results are shown in Tables 5 to 7.
[0093] <5-3. Total Light Transmittance> For each laminate film produced under the above conditions, the total light transmittance at 25°C was determined using a haze meter ("NDH7000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7361-1: 1997. The results are shown in Tables 5 to 7.
[0094] <5-4. Chemical Resistance> Each laminated film produced under the above conditions was cut into a 10 cm square, and then 0.5 g of a chemical agent (Neutrogena Ultra sheer SPF45) was spread on the surface layer side of the laminated film. The film was left to stand in a thermostatic chamber at 80°C for 2 hours, and then the chemical agent on the surface layer side was wiped off and washed with cotton containing alcohol. The appearance of the surface layer was then visually observed and evaluated according to the following criteria. The results are shown in Tables 5 to 7. A: No traces of chemical agent impregnation or deformation of surface shape. B: At least one of traces of chemical agent impregnation and deformation of surface shape was observed.
[0095] <5-5. Bleeding out of UV absorber> Each laminate film produced under the above conditions was subjected to a temperature cycle test in a thermostatic chamber (-30°C x 7 hours → 23°C x 1 hour → 80°C x 15 hours → 23°C x 1 hour) for 5 cycles. After the 5 cycles, the laminate film was visually observed and evaluated according to the following criteria. The results are shown in Tables 5 to 7. A: No precipitation of either powdery or needle-like solid material (UV absorber) was observed. B: Precipitation of at least one of powdery or needle-like solid material (UV absorber) was observed.
[0096] The laminate film of Comparative Example 2-1 had insufficient chemical resistance due to a low content of vinylidene fluoride resin in the surface layer. The laminate film of Comparative Example 2-2 had cloudiness due to the absence of methacrylate resin in the surface layer. The laminate film of Comparative Example 2-3 had cloudiness due to an excessive content of phosphite ester antioxidant relative to the mixed resin. In contrast, in Examples 2-1 to 2-10, the contents of vinylidene fluoride resin, methacrylate ester resin, and phosphite ester antioxidant were appropriate, so that films with little cloudiness, high transparency, and high chemical resistance could be obtained when formed into films.
[0097]
[0098]
[0099]
[0100] 1 laminated film, 10 surface layer, 20 back layer
Claims
1. A resin composition comprising: 100 parts by mass of a mixed resin of 60 to 95 parts by mass of a vinylidene fluoride resin and 5 to 40 parts by mass of a methacrylic acid ester resin; a compound having a propylene glycol unit; and 0.05 parts by mass or more and 1 part by mass or less of a phosphite ester antioxidant relative to 100 parts by mass of the mixed resin.
2. The resin composition according to claim 1, wherein the content of the propylene glycol unit in the compound having the propylene glycol unit is 0.001 part by mass or more and 0.1 part by mass or less per 100 parts by mass of the vinylidene fluoride unit content of the vinylidene fluoride resin.
3. The resin composition according to claim 1 or 2, wherein the phosphite-based antioxidant is at least one selected from the group consisting of tris(2,4-di-tert-butylphenyl)phosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, 2,4,8,10-tetrakis(1,1-dimethylethyl)-6-[(2-ethylhexyl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane.
4. The resin composition according to claim 1 or 2, wherein the resin composition is in the form of pellets and has a yellowness index of 6.0 or less.
5. A resin composition according to claim 1 or 2, wherein the total content of the vinylidene fluoride resin, the methacrylate ester resin and the phosphite ester antioxidant is 90 mass% or more based on the total amount of the resin composition.
6. A laminated film comprising a surface layer made of the resin composition according to claim 1 or 2, and a back layer made of a resin composition containing a methacrylic acid ester resin and laminated on one side of the surface layer.
7. The laminate film according to claim 6, wherein the haze of the laminate film measured in accordance with JIS K7136:2000 is 3.0% or less.
8. A decorative film comprising: the laminated film according to claim 6; and a decorative layer laminated directly or indirectly on the back layer side of the laminated film and having a design.
Citation Information
Patent Citations
High-resistance modified polyvinylidene fluoride formula
CN102604287A
laminate
JP1986146538A
Matte thermoplastic resin film and matte thermoplastic resin laminate film
JP2018193534A
Vinylidene fluoride resin composition, resin film, back sheet for solar cells, and solar cell module
WO2013008885A1
Vinylidene fluoride polymer composition, polymer film, layered body, and back sheet for solar cell module
WO2016143549A1
Cited By
Resin composition and molded body
WO2026205385A1
Resin composition and molded body
WO2026205386A1