Resin composition for thermosetting photo-alignment films
Copolymerizing a monomer with a formaldehyde-trapping effect and using a composition with photoalignable and N-hydroxymethyl or N-alkoxymethyl groups in the cured film composition addresses the toxicity of formaldehyde in photoalignment films, reducing formaldehyde concentration and maintaining performance.
Patent Information
- Application Number
- PCT/JP2024/014880
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
The use of compounds with N-methylol and N-alkoxymethyl groups in photoalignment films poses challenges due to the generation of formaldehyde, which is toxic and carcinogenic, requiring methods to reduce formaldehyde concentration and prevent its increase over time in both liquid and cured film compositions.
A monomer with a specific formaldehyde-trapping effect is copolymerized with a monomer source of formaldehyde, and a composition including a compound with a photoalignable group, a polymer with structural units having N-hydroxymethyl or N-alkoxymethyl groups, and a crosslinking catalyst is used to form a cured film that reduces formaldehyde concentration and prevents its increase.
The approach effectively reduces formaldehyde concentration in liquid and cured film compositions, ensuring safety and maintaining the performance of the alignment material without increasing formaldehyde levels over time.
Smart Images

Figure JP2024014880_17102024_PF_FP_ABST
Abstract
Description
Resin composition for thermosetting photo-alignment film
[0001] The present invention relates to a thermosetting resin composition for a photoalignment film (also referred to as a composition for forming a cured film), an alignment material, and a retardation material.
[0002] In the case of a 3D display using circularly polarized glasses, a retardation material is usually disposed on a display element that forms an image, such as a liquid crystal panel. This retardation material has two types of retardation regions with different retardation characteristics, each of which is regularly arranged in a plurality of regions, forming a patterned retardation material. In the following description, such a retardation material that is patterned so as to arrange a plurality of retardation regions with different retardation characteristics is referred to as a patterned retardation material.
[0003] A patterned retardation material can be produced by optically patterning a retardation material made of polymerizable liquid crystal, as disclosed in, for example, Patent Document 1. Optical patterning of a retardation material made of polymerizable liquid crystal utilizes photo-alignment technology known for forming alignment materials for liquid crystal panels. That is, a coating film made of a photo-alignable material is provided on a substrate, and two types of polarized light with different polarization directions are irradiated onto the coating. A photo-alignment film is then obtained as an alignment material in which two types of liquid crystal alignment regions with different liquid crystal alignment control directions are formed. A solution-like retardation material containing polymerizable liquid crystal is applied onto this photo-alignment film to achieve alignment of the polymerizable liquid crystal. The aligned polymerizable liquid crystal is then cured to form a patterned retardation material.
[0004] The anti-reflection film of an organic EL display is composed of a linear polarizer and a quarter-wave retardation plate. External light directed toward the panel surface of the image display panel is converted into linearly polarized light by the linear polarizer, and then converted into circularly polarized light by the subsequent quarter-wave retardation plate. This circularly polarized external light is reflected by the surface of the image display panel, but the direction of rotation of the polarization plane is reversed upon reflection. As a result, this reflected light is converted by the quarter-wave retardation plate into linearly polarized light in the direction that is blocked by the linear polarizer, in the opposite direction to when it arrived, and is then blocked by the subsequent linear polarizer, resulting in significant suppression of external emission.
[0005] Regarding this quarter-wave retardation plate, Patent Document 2 proposes a method of constructing this optical film with reverse dispersion characteristics by combining a half-wave plate and a quarter-wave plate to form a quarter-wave retardation plate. In this method, an optical film with reverse dispersion characteristics can be constructed using a liquid crystal material with positive dispersion characteristics in a wide wavelength band used for displaying color images.
[0006] In recent years, liquid crystal materials applicable to the retardation layer have been proposed that have reverse dispersion characteristics (Patent Documents 3 and 4). With such liquid crystal materials with reverse dispersion characteristics, instead of combining a half-wave plate and a quarter-wave plate to form a quarter-wave retardation plate using two retardation layers, the retardation layer can be formed as a single layer to ensure reverse dispersion characteristics, thereby enabling an optical film that can ensure a desired retardation over a wide wavelength band to be realized with a simple configuration.
[0007] An alignment layer is used to align liquid crystals. Known methods for forming alignment layers include rubbing and photo-alignment. Photo-alignment is advantageous in that it does not generate static electricity or dust, which are problems with rubbing, and allows for quantitative control of the alignment process.
[0008] In forming an alignment material using a photoalignment method, acrylic resins and polyimide resins having photodimerization moieties such as cinnamoyl groups and chalcone groups in the side chains are known as photoalignment materials. These resins have been reported to exhibit the ability to control the alignment of liquid crystals (hereinafter also referred to as liquid crystal alignment) when irradiated with polarized UV light (see Patent Documents 5 to 7).
[0009] Furthermore, there are also examples in which a thermal crosslinking system is introduced into a photoalignment agent using a cinnamoyl moiety in order to improve alignment sensitivity and impart solvent resistance (see Patent Documents 8 and 9).
[0010] Incidentally, Patent Document 10 describes a thermosetting liquid crystal alignment material using a resin composition having an N-alkoxymethyl group as a highly sensitive photoalignment agent.
[0011] However, because compounds containing N-methylol groups are obtained by forming N-methylol groups through the reaction of amino groups with formaldehyde, they often contain trace amounts of formaldehyde in principle. As of April 2023, formaldehyde is designated as a deleterious substance under the Poisonous and Deleterious Substances Control Act and is highly toxic to living organisms. It has also been shown by the International Agency for Research on Cancer to be carcinogenic. Furthermore, formaldehyde is released into the air from compounds used in building materials and furniture, causing sick building syndrome, which has become a problem. Therefore, when using compounds containing at least one of an N-methylol group and an N-alkoxymethyl group in products, it is necessary to reduce the formaldehyde concentration in the composition and, particularly in the case of molded products and paints, to ensure the safety of manufacturers and consumers who use the products.
[0012] Japanese Patent Application Publication No. 2005-49865 Japanese Patent Application Publication No. 10-68816 U.S. Patent No. 8,119,026 Japanese Patent Application Publication No. 2009-179563 Japanese Patent No. 3,611,342 Japanese Patent Application Publication No. 2009-058584 Japanese Patent Publication No. 2001-517719 International Patent Application Publication No. WO2011 / 126022 International Patent Application Publication No. WO2014 / 010688 WO2010 / 150748
[0013] When a thermal crosslinking system is introduced into a cured film, there is a concern about the generation of formaldehyde. For example, in cured film-forming compositions using crosslinking agents containing N-methylol groups or N-alkoxymethyl groups, a simple method for suppressing the generation of formaldehyde is desired.
[0014] Furthermore, formaldehyde scavengers sold for the purpose of reducing formaldehyde in liquid compositions are recommended to be added to the composition in amounts ranging from a few percent to a maximum of about 20%, which may significantly impair the functionality of the composition itself.Furthermore, even when multiple components are added, the risk of affecting the inherent performance of the composition increases as the number of added components increases.
[0015] Therefore, there is a need for a method that can sufficiently reduce the amount of formaldehyde contained in a cured film-forming composition even when a very small amount of formaldehyde scavenger is added. There is also a need for a method that can sufficiently reduce the amount of formaldehyde in a liquid composition by adding a formaldehyde scavenger, and a method that does not increase formaldehyde over time. Furthermore, there is a need for a method that can sufficiently reduce formaldehyde in liquid compositions, particularly liquid compositions that contain a compound having at least one of an N-methylol group and an N-alkoxymethyl group.
[0016] The present invention was made based on the above findings and investigation results. That is, an object of the present invention is to provide a method for reducing formaldehyde in a liquid composition and a method for producing a liquid composition using said method.
[0017] As a result of extensive research into achieving the above-mentioned object, the present inventors have discovered that by including a step of copolymerizing a monomer having a partial structure with a specific formaldehyde-trapping effect with a monomer that is a formaldehyde-generating source, it is possible to sufficiently reduce the formaldehyde concentration in a liquid composition even at a small copolymerization ratio, and to suppress an increase in formaldehyde over time, and have completed the present invention, which has the following gist:
[0018] That is, the present invention includes the following: [1] A cured film-forming composition comprising: (A) a compound having a photoalignable group, (B) a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit having a partial structure represented by the following formula (1), and (D) a crosslinking catalyst: (In formula (1), Q 1 represents an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or a phenyl group; Q 2 is O, S or NQ 3 represents Q 3represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the dashed line represents a bond.) [2] The cured film-forming composition according to the above [1], wherein the photo-alignable group of the component (A) is a functional group having a structure that undergoes photodimerization or photoisomerization. [3] The cured film-forming composition according to the above [1], wherein the photo-alignable group of the component (A) is a cinnamoyl group. [4] The cured film-forming composition according to the above [1], wherein the photo-alignable group of the component (A) is a group having an azobenzene structure. [5] The cured film-forming composition according to the above [1], which contains an ammonium salt as the component (C). [6] The cured film-forming composition according to the above [5], wherein the ammonium salt is ammonium acetate. [7] An alignment material obtained using the cured film-forming composition according to any one of the above [1] to [6]. [8] A retardation material formed using a cured film obtained from the cured film-forming composition according to any one of the above [1] to [6].
[0019] According to the present invention, it is possible to sufficiently reduce the formaldehyde concentration in the liquid composition and to suppress an increase in formaldehyde over time.
[0020] The present invention will be described in detail below. Note that the following explanation of the constituent elements is an example for explaining the present invention, and the present invention is not limited to these contents.
[0021] <Cured Film-Forming Composition> The cured film-forming composition of the present invention is a cured film-forming composition comprising (A) a compound having a photoalignable group, (B) a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit having a partial structure represented by formula (1), and (D) a crosslinking catalyst. Each component will be described in detail below.
[0022] [Component (A)] The component (A) in the cured film-forming composition of the present invention is a compound having a photoalignable group, more specifically, a low molecular weight compound or polymer having a photoalignable group and a thermally crosslinkable group. That is, the component (A) is a component that imparts photoalignment properties to a cured film obtained from the cured film-forming composition of the present invention, and in this specification, the component (A) is also referred to as a photoalignment component.
[0023] <Low Molecular Weight Compound Having a Photo-Alignment Group and a Thermally Crosslinkable Group> In the cured film-forming composition of the present invention, the low molecular weight compound of component (A) is a compound having a photo-alignment group, and may be a compound further having one group selected from the group consisting of a hydroxy group, a carboxy group, an amide group, an amino group, and an alkoxysilyl group. In the present invention, the photo-alignment group generally refers to a functional group that exhibits the property of being aligned by light irradiation, and typically refers to a functional group at a structural site that undergoes photodimerization or photoisomerization. Other photo-alignment groups include, for example, functional groups that undergo a photo-Fries rearrangement reaction (e.g., benzoic acid ester compounds) and groups that undergo a photodecomposition reaction (e.g., cyclobutane rings).
[0024] The photodimerizable structural moiety that the low molecular weight compound of component (A) can have as a photoalignment group is a moiety that forms a dimer upon irradiation with light, and specific examples thereof include a cinnamoyl group, a chalcone group, a coumarin group, an anthracene group, etc. Among these, a cinnamoyl group is preferred because of its high transparency in the visible light region and its high photodimerization reactivity.
[0025] Furthermore, the photoisomerizable structural moiety that the low molecular weight compound of component (A) can have as a photoalignment group refers to a structural moiety that changes between a cis form and a trans form upon irradiation with light, and specific examples thereof include moieties consisting of an azobenzene structure, a stilbene structure, etc. Among these, an azobenzene structure is preferred due to its high reactivity.
[0026] The low molecular weight compound having a photoalignable group and one group selected from the group consisting of a hydroxy group, a carboxy group, an amide group, an amino group, and an alkoxysilyl group is, for example, a compound represented by the following formula:
[0027]
[0028] In the above formula, A 1 and A 2 each independently represents a hydrogen atom or a methyl group.
[0029] X 11represents a structure in which 1 to 3 substituents selected from alkylene groups having 1 to 18 carbon atoms, phenylene groups, biphenylene groups, and combinations thereof are bonded via one or more bonds selected from a single bond, an ether bond, an ester bond, an amide bond, a urea bond, a urethane bond, an amino bond, a carbonyl bond, and combinations thereof, and the structure may be such that a plurality of the substituents are linked via the bonds.
[0030] X 12 represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, a phenyl group, a biphenyl group, or a cyclohexyl group. In this case, the alkyl group having 1 to 18 carbon atoms, the phenyl group, the biphenyl group, and the cyclohexyl group may be bonded to two or more groups via a single bond, an ether bond, an ester bond, an amide bond, or a urea bond.
[0031] X 13 represents a hydroxy group, a mercapto group, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a phenoxy group, a biphenyloxy group, or a phenyl group.
[0032] X 14 represents a single bond, an alkylene group having 1 to 20 carbon atoms, a divalent aromatic ring group, or a divalent aliphatic ring group. Here, the alkylene group having 1 to 20 carbon atoms may be branched or linear.
[0033] X 15 represents a hydroxy group, a carboxy group, an amide group, an amino group, or an alkoxysilyl group, provided that X 14 When is a single bond, X 15 is a hydroxy group or an amino group.
[0034] X represents a single bond, an oxygen atom, or a sulfur atom. 14 is a single bond, then X is also a single bond.
[0035] When these substituents contain a benzene ring, a hydrogen atom on the benzene ring may be substituted with one or more identical or different substituents selected from an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group, and a cyano group.
[0036] In the above formula, R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 and R 18 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group, or a cyano group.
[0037] Specific examples of the low molecular weight compound having a photoalignable group and a hydroxy group, which is the component (A), include the compounds represented by the above formulas [A11] to [A15], and compounds other than those represented by the formulas, such as 4-(8-hydroxyoctyloxy)cinnamic acid methyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid methyl ester, 4-(4-hydroxybutyloxy)cinnamic acid methyl ester, 4-(3-hydroxypropyloxy)cinnamic acid methyl ester, 4-(2-hydroxyethyloxy)cinnamic acid methyl ester, 4-hydroxymethyloxycinnamic acid methyl ester, cinnamic acid methyl ester, 4-hydroxycinnamic acid methyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid ethyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid ethyl ester, 4-(4-hydroxybutyloxy)cinnamic acid ethyl ester, 4-(3-hydroxypropyloxy)cinnamic acid ethyl ester, 4-(2-hydroxyethyloxy)cinnamic acid ethyl ester, 4-hydroxymethyloxycinnamic acid ethyl ester, 4-hydroxycinnamic acid ethyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid phenyl Ester, 4-(6-hydroxyhexyloxy)cinnamic acid phenyl ester, 4-(4-hydroxybutyloxy)cinnamic acid phenyl ester, 4-(3-hydroxypropyloxy)cinnamic acid phenyl ester, 4-(2-hydroxyethyloxy)cinnamic acid phenyl ester, 4-hydroxymethyloxycinnamic acid phenyl ester, 4-hydroxycinnamic acid phenyl ester, 4-(8-hydroxyoctyloxy)cinnamic acid biphenyl ester, 4-(6-hydroxyhexyloxy)cinnamic acid biphenyl ester, 4-(4-hydroxy butyloxy)cinnamic acid biphenyl ester, 4-(3-hydroxypropyloxy)cinnamic acid biphenyl ester, 4-(2-hydroxyethyloxy)cinnamic acid biphenyl ester, 4-hydroxymethyloxycinnamic acid biphenyl ester, 4-hydroxycinnamic acid biphenyl ester, cinnamic acid 8-hydroxyoctyl ester, cinnamic acid 6-hydroxyhexyl ester, cinnamic acid 4-hydroxybutyl ester, cinnamic acid 3-hydroxypropyl ester, cinnamic acid 2-hydroxyethyl ester, cinnamic acid hydroxymethyl ester,4-(8-hydroxyoctyloxy)azobenzene, 4-(6-hydroxyhexyloxy)azobenzene, 4-(4-hydroxybutyloxy)azobenzene, 4-(3-hydroxypropyloxy)azobenzene, 4-(2-hydroxyethyloxy)azobenzene, 4-hydroxymethyloxyazobenzene, 4-hydroxyazobenzene, 4-(8-hydroxyoctyloxy)chalcone, 4-(6-hydroxyhexyloxy)chalcone, 4-(4-hydroxybutyloxy)chalcone, 4-(3-hydroxypropyloxy)chalcone , 4-(2-hydroxyethyloxy)chalcone, 4-hydroxymethyloxychalcone, 4-hydroxychalcone, 4'-(8-hydroxyoctyloxy)chalcone, 4'-(6-hydroxyhexyloxy)chalcone, 4'-(4-hydroxybutyloxy)chalcone, 4'-(3-hydroxypropyloxy)chalcone, 4'-(2-hydroxyethyloxy)chalcone, 4'-hydroxymethyloxychalcone, 4'-hydroxychalcone, 7-(8-hydroxyoctyloxy)coumarin, 7-(6-hydroxyhexyloxy)coumarin , 7-(4-hydroxybutyloxy)coumarin, 7-(3-hydroxypropyloxy)coumarin, 7-(2-hydroxyethyloxy)coumarin, 7-hydroxymethyloxycoumarin, 7-hydroxycoumarin, 6-(8-hydroxyoctyloxy)coumarin, 6-(6-hydroxyhexyloxy)coumarin, 6-(4-hydroxybutyloxy)coumarin, 6-(3-hydroxypropyloxy)coumarin, 6-(2-hydroxyethyloxy)coumarin, 6-hydroxymethyloxycoumarin, 6-hydroxycoumarin, 4-[4-(8 4-[4-(6-hydroxyoctyloxy)benzoyl]cinnamic acid methyl ester, 4-[4-(6-hydroxyhexyloxy)benzoyl]cinnamic acid methyl ester, 4-[4-(4-hydroxybutyloxy)benzoyl]cinnamic acid methyl ester, 4-[4-(3-hydroxypropyloxy)benzoyl]cinnamic acid methyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid methyl ester, 4-[4-hydroxymethyloxybenzoyl]cinnamic acid methyl ester, 4-[4-hydroxybenzoyl]cinnamic acid methyl ester,4-[4-(8-hydroxyoctyloxy)benzoyl]cinnamic acid ethyl ester, 4-[4-(6-hydroxyhexyloxy)benzoyl]cinnamic acid ethyl ester, 4-[4-(4-hydroxybutyloxy)benzoyl]cinnamic acid ethyl ester, 4-[4-(3-hydroxypropyloxy)benzoyl]cinnamic acid ethyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid ethyl ester, 4-[4-hydroxymethyloxybenzoyl]cinnamic acid ethyl ester, 4-[4-hydroxybenzoyl]cinnamic acid cinnamic acid ethyl ester, 4-[4-(8-hydroxyoctyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-(6-hydroxyhexyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-(4-hydroxybutyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-(3-hydroxypropyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-hydroxymethyl 4-[4-(4-hydroxypropyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-hydroxymethyloxy)benzoyl]cinnamic acid tert-butyl ester, 4-[4-(8-hydroxyoctyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-(6-hydroxyhexyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-(4-hydroxybutyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-(3-hydroxypropyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid phenyl ester, 4-[4-hydroxymethyloxybenzoyl ]cinnamic acid phenyl ester, 4-[4-hydroxybenzoyl]cinnamic acid phenyl ester, 4-[4-(8-hydroxyoctyloxy)benzoyl]cinnamic acid biphenyl ester, 4-[4-(6-hydroxyhexyloxy)benzoyl]cinnamic acid biphenyl ester, 4-[4-(4-hydroxybutyloxy)benzoyl]cinnamic acid biphenyl ester, 4-[4-(3-hydroxypropyloxy)benzoyl]cinnamic acid biphenyl ester, 4-[4-(2-hydroxyethyloxy)benzoyl]cinnamic acid biphenyl ester,4-[4-hydroxymethyloxybenzoyl]cinnamic acid biphenyl ester, 4-[4-hydroxybenzoyl]cinnamic acid biphenyl ester, 4-benzoylcinnamic acid 8-hydroxyoctyl ester, 4-benzoylcinnamic acid 6-hydroxyhexyl ester, 4-benzoylcinnamic acid 4-hydroxybutyl ester, 4-benzoylcinnamic acid 3-hydroxypropyl ester, 4-benzoylcinnamic acid 2-hydroxyethyl ester, 4-benzoylcinnamic acid hydroxymethyl ester, 4-[4-(8-hydroxyoctyloxy)benzoyl]chalcone, 4-[4-(6-hydroxyhexyloxy)benzoyl]chalcone, 4-[4-(4-hydroxybutyloxy)benzoyl]chalcone, 4-[4-( 4-[4-(3-hydroxypropyloxy)benzoyl]chalcone, 4-[4-(2-hydroxyethyloxy)benzoyl]chalcone, 4-(4-hydroxymethyloxybenzoyl)chalcone, 4-(4-hydroxybenzoyl)chalcone, 4'-[4-(8-hydroxyoctyloxy)benzoyl]chalcone, 4'-[4-(6-hydroxyhexyloxy)benzoyl]chalcone, 4'-[4-(4-hydroxybutyloxy)benzoyl]chalcone, 4'-[4-(3-hydroxypropyloxy)benzoyl]chalcone, 4'-[4-(2-hydroxyethyloxy)benzoyl]chalcone, 4'-(4-hydroxymethyloxybenzoyl)chalcone, 4'-(4-hydroxybenzoyl)chalcone, and the like.
[0038] Specific examples of the low molecular weight compound having a photoalignable group and a carboxy group, which is component (A), include cinnamic acid, ferulic acid, 4-methoxycinnamic acid, 4-propoxycinnamic acid, 3,4-dimethoxycinnamic acid, coumarin-3-carboxylic acid, and 4-(N,N-dimethylamino)cinnamic acid.
[0039] Specific examples of the component (A), a low molecular weight compound having a photoalignable group and an amide group, include cinnamic acid amide, 4-methylcinnamic acid amide, 4-ethylcinnamic acid amide, 4-methoxycinnamic acid amide, and 4-ethoxycinnamic acid amide.
[0040] Specific examples of the component (A), a low molecular weight compound having a photoalignable group and an amino group, include 4-aminocinnamic acid methyl ester, 4-aminocinnamic acid ethyl ester, 3-aminocinnamic acid methyl ester, and 3-aminocinnamic acid ethyl ester.
[0041] Specific examples of the low molecular weight compound having a photoalignable group and an alkoxysilyl group, which is the component (A), include 4-(3-trimethoxysilylpropyloxy)cinnamic acid methyl ester, 4-(3-triethoxysilylpropyloxy)cinnamic acid methyl ester, 4-(3-trimethoxysilylpropyloxy)cinnamic acid ethyl ester, 4-(3-triethoxysilylpropyloxy)cinnamic acid ethyl ester, 4-(3-trimethoxysilylhexyloxy)cinnamic acid methyl ester, 4-(3-triethoxysilylhexyloxy)cinnamic acid methyl ester, 4-(3-trimethoxysilylhexyloxy)cinnamic acid ethyl ester, and 4-(3-triethoxysilylhexyloxy)cinnamic acid ethyl ester.
[0042] The low molecular weight compound of the component (A) is preferably a compound in which a polymerizable group is bonded via a spacer to a group in which a photoalignable moiety and a thermally reactive moiety are bonded, as represented by the following formula (a-1):
[0043]
[0044] (In the formula, R 101 represents a hydroxy group, an amino group, a hydroxyphenoxy group, a carboxyphenoxy group, an aminophenoxy group, an aminocarbonylphenoxy group, a phenylamino group, a hydroxyphenylamino group, a carboxyphenylamino group, an aminophenylamino group, a hydroxyalkylamino group, or a bis(hydroxyalkyl)amino group; X 101 represents a phenylene group which may be substituted with any substituent, and the hydrogen atoms on the benzene ring in the definitions of these substituents may be substituted with a substituent.
[0045] In the case where a hydrogen atom on the benzene ring may be substituted with a substituent, examples of the substituent include alkyl groups such as a methyl group, an ethyl group, a propyl group, a butyl group, and an isobutyl group; haloalkyl groups such as a trifluoromethyl group; alkoxy groups such as a methoxy group and an ethoxy group; halogen atoms such as an iodine atom, a bromine atom, a chlorine atom, and a fluorine atom; a cyano group; and a nitro group.
[0046] The above R 101 Among these, a hydroxy group and an amino group are preferred, and a hydroxy group is particularly preferred.
[0047] The spacer is a divalent group selected from a linear alkylene group, a branched alkylene group, a cyclic alkylene group, and a phenylene group, or a group formed by bonding multiple such divalent groups. In this case, examples of the bond between the divalent groups constituting the spacer, the bond between the spacer and the group represented by formula (a-1), and the bond between the spacer and the polymerizable group include a single bond, an ester bond, an amide bond, a urea bond, and an ether bond. When there are multiple divalent groups, the divalent groups may be the same or different, and when there are multiple bonds, the bonds may be the same or different.
[0048] Specific examples of such a low molecular weight compound in which a polymerizable group is bonded to a group in which a photoalignment moiety and a thermally reactive moiety are bonded, which is component (A), include 4-(6-methacryloxyhexyl-1-oxy)cinnamic acid, 4-(6-acryloxyhexyl-1-oxy)cinnamic acid, 4-(3-methacryloxypropyl-1-oxy)cinnamic acid, 4-(4-(3-methacryloxypropyl-1-oxy)acryloxy)benzoic acid, 4-(4-(6-methacryloxyhexyl-1-oxy)benzoyloxy)cinnamic acid, 4-(6-methacryloxyhexyl-1-oxy)cinnamamide, 4-(6-methacryloxyhexyl-1-oxy)-N-(4-cyanophenyl)cinnamamide, and 4-(6-methacryloxyhexyl-1-oxy)-N-bishydroxyethylcinnamamide.
[0049] The low molecular weight photo-alignment component (A) can be exemplified by the above specific examples, but is not limited to these.
[0050] As described above, in the present invention, a low molecular weight compound can be used as component (A). Component (A) may also be a mixture of one or more low molecular weight compounds.
[0051] <Polymer Having Photoalignment Group and Thermally Crosslinkable Group> In the cured film-forming composition of the present invention, the polymer of component (A) is a polymer having a photoalignment group, i.e., a polymer having a functional group of a structural moiety that is photodimerizable or photoisomerizable as the photoalignment group, and is particularly preferably an acrylic copolymer having at least a photodimerization moiety. Furthermore, it is desirable that the polymer be an acrylic copolymer having, in addition to the photodimerization moiety, one group selected from the group consisting of a hydroxy group, a carboxy group, an amide group, an amino group, and an alkoxysilyl group (hereinafter, these groups are also referred to as the thermally crosslinkable moiety).
[0052] In the present invention, the acrylic copolymer refers to a copolymer obtained by polymerizing a monomer having an unsaturated double bond, such as an acrylic acid ester, a methacrylic acid ester, or styrene.
[0053] The acrylic copolymer (hereinafter also referred to as the specific copolymer) having a photodimerization moiety and a thermal crosslinking moiety of the component (A) may be any acrylic copolymer having such a structure, and there are no particular limitations on the types of the main chain skeleton and side chains of the polymer constituting the acrylic copolymer.
[0054] Examples of the photodimerization moiety include a cinnamoyl group, a chalcone group, a coumarin group, and an anthracene group. Among these, a cinnamoyl group is preferred because of its high transparency in the visible light region and high photodimerization reactivity. More preferred cinnamoyl groups and substituents containing a cinnamoyl structure include structures represented by the following formula [1] or formula [2]. In this specification, a cinnamoyl group in which the benzene ring is a naphthalene ring is also included in the "cinnamoyl group" and "substituent containing a cinnamoyl structure."
[0055]
[0056] In the above formula [1], X 1represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a phenyl group, or a biphenyl group, in which case the hydrogen atoms on the phenyl group and the biphenyl group may be substituted with either a halogen atom or a cyano group.
[0057] In the above formula [2], X 2 represents a hydrogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, a phenyl group, a biphenyl group, or a cyclohexyl group. In this case, a plurality of alkyl groups having 1 to 18 carbon atoms, phenyl groups, biphenyl groups, and cyclohexyl groups may be bonded via one or more bonds selected from a single bond, an ether bond, an ester bond, an amide bond, a urea bond, a urethane bond, an amino bond, a carbonyl bond, or a combination thereof.
[0058] In the above formulas [1] and [2], A represents any one of formulas [A1], [A2], [A3], [A4], [A5] and [A6].
[0059] In the above formula [A1], formula [A2], formula [A3], formula [A4], formula [A5] and formula [A6], R 31 , R 32 , R 33 , R 34 , R 35 , R 36 , R 37 and R 38 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a halogen atom, a trifluoromethyl group, or a cyano group.
[0060] The thermal crosslinking moiety is a moiety that bonds with the crosslinking agent (B) by heating, and specific examples thereof include a hydroxy group, a carboxy group, an amide group, an amino group, and an alkoxysilyl group.
[0061] The acrylic copolymer of component (A) preferably has a weight-average molecular weight of 3,000 to 200,000. If the weight-average molecular weight is too high, exceeding 200,000, the solubility in solvents may decrease, leading to poor handling, whereas if the weight-average molecular weight is too low, less than 3,000, the copolymer may not cure sufficiently during heat curing, resulting in poor solvent resistance and poor heat resistance.
[0062] The acrylic copolymer having a photodimerization moiety and a thermal crosslinking moiety, component (A), can be synthesized simply by copolymerizing a monomer having a photodimerization moiety with a monomer having a thermal crosslinking moiety.
[0063] Examples of the monomer having a photodimerization moiety include monomers having a cinnamoyl group, a chalcone group, a coumarin group, an anthracene group, etc. Among these, monomers having a cinnamoyl group are particularly preferred because of their high transparency in the visible light region and high photodimerization reactivity.
[0064] Among these, monomers having a cinnamoyl group or a substituent containing a cinnamoyl structure represented by the above formula [1] or formula [2] are more preferred. Specific examples of such monomers include monomers represented by the following formula [3] or formula [4]:
[0065]
[0066] In the above formula [3], X 1 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a phenyl group, or a biphenyl group. In this case, the hydrogen atoms on the phenyl group and the biphenyl group may be substituted with either a halogen atom or a cyano group. 1 and L 2 each independently represents a single bond, an ether bond, an ester bond, an amide bond, a urea bond or a urethane bond.
[0067] In the above formula [4], X 2 represents a hydrogen atom, a cyano group, an alkyl group having 1 to 18 carbon atoms, a phenyl group, a biphenyl group, or a cyclohexyl group. In this case, a plurality of alkyl groups having 1 to 18 carbon atoms, phenyl groups, biphenyl groups, and cyclohexyl groups may be bonded via one or more bonds selected from a single bond, an ether bond, an ester bond, an amide bond, a urea bond, a urethane bond, an amino bond, a carbonyl bond, or a combination thereof.
[0068] In the above formula [3] and formula [4], X 3 and X 5each independently represents a single bond, an alkylene group having 1 to 20 carbon atoms, a divalent aromatic ring, or a divalent aliphatic ring. Here, the alkylene group having 1 to 20 carbon atoms may be branched or linear.
[0069] In the above formula [3] and formula [4], X 4 represents a polymerizable group. Specific examples of the polymerizable group include an acryloyl group, a methacryloyl group, a styrene group, a maleimide group, an acrylamide group, and a methacrylamide group.
[0070] In the above formulas [3] and [4], A represents any one of formulas [A1], [A2], [A3], [A4], [A5] and [A6] as described above.
[0071] Examples of the monomer having a thermal crosslinking moiety include monomers having a hydroxy group such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 2,3-dihydroxypropyl acrylate, 2,3-dihydroxypropyl methacrylate, diethylene glycol monoacrylate, diethylene glycol monomethacrylate, caprolactone 2-(acryloyloxy)ethyl ester, caprolactone 2-(methacryloyloxy)ethyl ester, poly(ethylene glycol) ethyl ether acrylate, poly(ethylene glycol) ethyl ether methacrylate, 5-acryloyloxy-6-hydroxynorbornene-2-carboxylic-6-lactone, and 5-methacryloyloxy-6-hydroxynorbornene-2-carboxylic-6-lactone; acrylic acid, methacrylic acid, crotonic acid, mono-(2-(acryloyloxy)ethyl ester), methyl acrylate, ... monomers having a phenolic hydroxy group such as hydroxystyrene, N-(hydroxyphenyl)methacrylamide, N-(hydroxyphenyl)acrylamide, N-(hydroxyphenyl)maleimide, N-(hydroxyphenyl)maleimide; monomers having an amide group such as acrylamide and methacrylamide; monomers having an alkoxysilyl group such as methacryloyloxypropyltrimethoxysilane, methacryloyloxypropyltriethoxysilane, acryloyloxypropyltrimethoxysilane and acryloyloxypropyltriethoxysilane; and monomers having an amino group such as dimethylaminoethyl methacrylate, diethylamino methacrylate and tert-butylaminoethyl methacrylate.
[0072] The amounts of the monomer having a photodimerization moiety and the monomer having a thermal crosslinking moiety used to obtain the specific copolymer are preferably 40% by mass to 95% by mass, and 5% by mass to 60% by mass, based on the total amount of all monomers used to obtain the specific copolymer. By setting the content of the monomer having a photodimerization moiety to 40% by mass or more, high sensitivity and good liquid crystal alignment properties can be imparted. On the other hand, by setting the content to 95% by mass or less, sufficient thermosetting properties can be imparted, and high sensitivity and good liquid crystal alignment properties can be maintained.
[0073] In addition, in the cured film-forming composition of the present invention, when obtaining the specific copolymer, a monomer having a photodimerization moiety and a thermal crosslinking moiety (hereinafter, these may also be referred to as specific functional groups) and a monomer copolymerizable therewith (hereinafter, also referred to as a monomer having a non-reactive functional group) may be used in combination.
[0074] Specific examples of such monomers include acrylic acid ester compounds, methacrylic acid ester compounds, maleimide compounds, acrylamide compounds, acrylonitrile, maleic anhydride, styrene compounds, vinyl compounds, etc. Specific examples of the above-mentioned monomers are listed below, but the present invention is not limited to these.
[0075] Examples of the acrylic acid ester compounds include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, benzyl acrylate, naphthyl acrylate, anthryl acrylate, anthrylmethyl acrylate, phenyl acrylate, glycidyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-propyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecyl acrylate, and 8-ethyl-8-tricyclodecyl acrylate.
[0076] Examples of the methacrylic acid ester compounds include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthryl methacrylate, anthrylmethyl methacrylate, phenyl methacrylate, glycidyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, γ-butyrolactone methacrylate, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecyl methacrylate, and 8-ethyl-8-tricyclodecyl methacrylate.
[0077] Examples of the vinyl compound include methyl vinyl ether, benzyl vinyl ether, vinyl naphthalene, vinyl carbazole, allyl glycidyl ether, 3-ethenyl-7-oxabicyclo[4.1.0]heptane, 1,2-epoxy-5-hexene, and 1,7-octadiene monoepoxide.
[0078] Examples of the styrene compound include styrene, methylstyrene, chlorostyrene, and bromostyrene.
[0079] Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide.
[0080] The method for obtaining the specific copolymer used in the cured film-forming composition of the present invention is not particularly limited, and examples thereof include a method of polymerizing a monomer having a specific functional group (a monomer having a photodimerization moiety and a monomer having a thermal crosslinking moiety), optionally a monomer having a non-reactive functional group, a polymerization initiator, and the like in a solvent in which these monomers coexist at a temperature of 50°C to 110°C. The solvent used in this case is not particularly limited as long as it dissolves the monomer having the specific functional group, the optional monomer having a non-reactive functional group, the polymerization initiator, and the like. Specific examples include the solvents described below in the section on solvents.
[0081] The specific copolymer thus obtained is usually in the form of a solution dissolved in a solvent, and can be used as is as the polymer solution of component (A) in the present invention.
[0082] In addition, the solution of the specific copolymer obtained as described above can be reprecipitated by adding diethyl ether, water, or the like under stirring, and the resulting precipitate can be filtered and washed, and then dried at room temperature or by heating under normal pressure or reduced pressure to obtain a powder of the specific copolymer.By such an operation, the polymerization initiator and unreacted monomers coexisting with the specific copolymer can be removed, and as a result, a powder of the purified specific copolymer can be obtained.If the specific copolymer cannot be sufficiently purified by one operation, the obtained powder can be redissolved in a solvent and the above operation can be repeated.
[0083] In the cured film-forming composition of the present invention, the powder of the specific copolymer may be used as it is as the polymer of component (A), or the powder may be redissolved in, for example, a solvent described below and used in the form of a solution.
[0084] Furthermore, as the polymer of component (A), a polymer obtained by reacting a polymer having an epoxy group in the side chain with a cinnamic acid derivative can also be used.
[0085] The polymer having an epoxy group in the side chain may be, for example, a polymer of a polymerizable unsaturated compound having an epoxy group or a copolymer of a polymerizable unsaturated compound having an epoxy group and another polymerizable unsaturated compound.
[0086] Specific examples of the polymerizable unsaturated compound having an epoxy group include glycidyl acrylate, glycidyl methacrylate, α-ethyl glycidyl acrylate, α-n-propyl glycidyl acrylate, α-n-butyl glycidyl acrylate, 3,4-epoxybutyl acrylate, 3,4-epoxybutyl methacrylate, 6,7-epoxyheptyl acrylate, 6,7-epoxyheptyl methacrylate, α-ethyl 6,7-epoxyheptyl acrylate, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, and p-vinylbenzyl glycidyl ether.
[0087] Examples of other polymerizable unsaturated compounds include (meth)acrylic acid alkyl esters, (meth)acrylic acid cyclic alkyl esters, methacrylic acid aryl esters, acrylic acid aryl esters, unsaturated dicarboxylic acid diesters, bicyclounsaturated compounds, maleimide compounds, unsaturated aromatic compounds, conjugated diene compounds, unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, unsaturated dicarboxylic acid anhydrides, and other polymerizable unsaturated compounds.
[0088] Specific examples of these include alkyl methacrylates such as hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, diethylene glycol monomethacrylate, 2,3-dihydroxypropyl methacrylate, 2-methacryloxyethyl glycoside, 4-hydroxyphenyl methacrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, 2-ethylhexyl methacrylate, isodecyl methacrylate, n-lauryl methacrylate, tridecyl methacrylate, and n-stearyl methacrylate; alkyl acrylates such as methyl acrylate and isopropyl acrylate; and cyclic alkyl methacrylates such as cyclohexyl methacrylate, 2-methylcyclohexyl methacrylate, tricyclo[5.2.1.0]methacrylate. 2,6 ] decan-8-yl methacrylate, tricyclo[5.2.1.0 2,6 ] decan-8-yloxyethyl methacrylate, isobornyl methacrylate, cholestanyl methacrylate, etc.; acrylic acid cyclic alkyl esters such as cyclohexyl acrylate, 2-methylcyclohexyl acrylate, tricyclo[5.2.1.0 2,6 ] decan-8-yl acrylate, tricyclo[5.2.1.0 2,6 ] decan-8-yloxyethyl acrylate, isobornyl acrylate, cholestanyl acrylate, etc.; methacrylic acid aryl esters such as phenyl methacrylate, benzyl methacrylate, etc.; acrylic acid aryl esters such as phenyl acrylate, benzyl acrylate, etc.; unsaturated dicarboxylic acid diesters such as diethyl maleate, diethyl fumarate, diethyl itaconate, etc.;
[0089] Examples of bicyclo unsaturated compounds include bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-methoxybicyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dimethoxybicyclo[2.2.1]hept-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5 , 6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-di(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-di(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, etc.; maleimide compounds, such as N-phenylmaleimide, N- Cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimidobenzoate, N-succinimidyl-4-maleimidobutyrate, N-succinimidyl-6-maleimidocaproate, N-succinimidyl-3-maleimidopropionate, N-(9-acridinyl)maleimide, and the like; unsaturated aromatic compounds, such as styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, and the like; conjugated diene compounds, such as 1,3-butadiene, Examples of unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid; examples of unsaturated dicarboxylic acids include maleic acid, fumaric acid, citraconic acid, mesaconic acid, and itaconic acid; examples of unsaturated dicarboxylic acid anhydrides include the anhydrides of the above-mentioned unsaturated dicarboxylic acids; and examples of polymerizable unsaturated compounds other than those mentioned above include acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, and vinyl acetate.
[0090] The copolymerization ratio of the polymerizable unsaturated compound having an epoxy group in the polymer having an epoxy group in the side chain is preferably 30% by mass or more, more preferably 50% by mass or more.
[0091] The synthesis of a polymer having an epoxy group in the side chain can be carried out by a known radical polymerization method, preferably in a solvent in the presence of a suitable polymerization initiator.
[0092] Commercially available products may be used as the polymer having an epoxy group in the side chain. Examples of such commercially available products include EHPE3150 and EHPE3150CE (manufactured by Daicel Corporation), UG-4010, UG-4035, UG-4040, and UG-4070 (ARUFON series manufactured by Toagosei Co., Ltd.), ECN-1299 (manufactured by Asahi Kasei Corporation), DEN431 and DEN438 (manufactured by The Dow Chemical Company), and jE Examples of suitable inks include R-152 (manufactured by Mitsubishi Chemical Corporation), Epicron N-660, N-665, N-670, N-673, N-695, N-740, N-770, and N-775 (all manufactured by DIC Corporation (formerly Dainippon Ink and Chemicals, Inc.)), and EOCN-1020, EOCN-102S, and EOCN-104S (all manufactured by Nippon Kayaku Co., Ltd.).
[0093] Examples of the cinnamic acid derivative include cinnamic acid derivatives having a carboxy group, such as those represented by the following formulas (1-1) to (1-5): (In the formula, R 1 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, etc.)
[0094] Further, as the cinnamic acid derivative having a carboxy group, in the monomer represented by the above formula [3], X 1 Compounds in which is a hydrogen atom are also preferably used.
[0095] The compounds represented by the above formulas (1-1) to (1-5) can be synthesized by appropriately combining standard methods in organic chemistry.
[0096] The reaction product of the polymer having an epoxy group in the side chain and a cinnamic acid derivative can be synthesized by reacting the polymer having an epoxy group as described above with a cinnamic acid derivative, preferably in the presence of a catalyst, preferably in a suitable organic solvent.
[0097] The proportion of the cinnamic acid derivative used in the reaction is preferably 0.01 to 1.5 mol, more preferably 0.05 to 1.3 mol, and even more preferably 0.1 to 1.1 mol, per 1 mol of epoxy groups contained in the polymer having epoxy groups.
[0098] The catalyst that can be used here may be a compound known as a so-called curing accelerator that accelerates the reaction between an organic base or an epoxy compound and an acid anhydride.
[0099] Examples of the organic base include primary or secondary organic amines such as ethylamine, diethylamine, piperazine, piperidine, pyrrolidine, and pyrrole; tertiary organic amines such as triethylamine, tri-n-propylamine, tri-n-butylamine, pyridine, 4-dimethylaminopyridine, and diazabicycloundecene; and quaternary organic amines such as tetramethylammonium hydroxide. Of these organic bases, tertiary organic amines such as triethylamine, tri-n-propylamine, tri-n-butylamine, tri-n-pentylamine, pyridine, and 4-dimethylaminopyridine; and quaternary organic amines such as tetramethylammonium hydroxide are preferred.
[0100] Examples of the curing accelerator include tertiary amines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, cyclohexyldimethylamine, and triethanolamine; 2-methylimidazole, 2-n-heptylimidazole, 2-n-undecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, and 1,2-dimethylimidazole. azole, 2-ethyl-4-methylimidazole, 1-(2-cyanoethyl)-2-methylimidazole, 1-(2-cyanoethyl)-2-n-undecylimidazole, 1-(2-cyanoethyl)-2-phenylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-di(hydroxymethyl)imidazole, 1-(2-cyanoethyl)-2-phenyl-4, 5-Di[(2'-cyanoethoxy)methyl]imidazole, 1-(2-cyanoethyl)-2-n-undecylimidazolium trimellitate, 1-(2-cyanoethyl)-2-phenylimidazolium trimellitate, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-(2'-n-undecylimidazolyl)ethyl-s imidazole compounds such as 2-methylimidazole, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]ethyl-s-triazine, an isocyanuric acid adduct of 2-methylimidazole, an isocyanuric acid adduct of 2-phenylimidazole, and an isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine; organic phosphorus compounds such as diphenylphosphine, triphenylphosphine, and triphenyl phosphite;
[0101] quaternary phosphonium salts such as benzyltriphenylphosphonium chloride, tetra-n-butylphosphonium bromide, methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, n-butyltriphenylphosphonium bromide, tetraphenylphosphonium bromide, ethyltriphenylphosphonium iodide, ethyltriphenylphosphonium acetate, tetra-n-butylphosphonium o,o-diethylphosphorodithionate, tetra-n-butylphosphonium benzotriazolate, tetra-n-butylphosphonium tetrafluoroborate, tetra-n-butylphosphonium tetraphenylborate, and tetraphenylphosphonium tetraphenylborate; diazabicycloalkenes such as 1,8-diazabicyclo[5.4.0]undecene-7 and organic acid salts thereof; quaternary ammonium salts such as tetraethylammonium bromide, tetra-n-butylammonium bromide, tetraethylammonium chloride, and tetra-n-butylammonium chloride; boron compounds such as boron trifluoride and triphenyl borate; metal halide compounds such as zinc chloride and stannic chloride; high-melting point dispersion-type latent curing accelerators such as amine addition-type accelerators such as dicyandiamide and adducts of amines and epoxy resins; microcapsule-type latent curing accelerators in which the surface of the curing accelerators such as the imidazole compounds, organic phosphorus compounds, and quaternary phosphonium salts is coated with a polymer; amine salt-type latent curing accelerators; and latent curing accelerators such as high-temperature dissociation-type thermal cationic polymerization-type latent curing accelerators such as Lewis acid salts and Bronsted acid salts.
[0102] Of these, preferred are quaternary phosphonium salts such as benzyltriphenylphosphonium chloride, tetra-n-butylphosphonium bromide, methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, n-butyltriphenylphosphonium bromide, tetraphenylphosphonium bromide, ethyltriphenylphosphonium iodide, ethyltriphenylphosphonium acetate, tetra-n-butylphosphonium o,o-diethylphosphorodithionate, tetra-n-butylphosphonium benzotriazolate, tetra-n-butylphosphonium tetrafluoroborate, tetra-n-butylphosphonium tetraphenylborate, and tetraphenylphosphonium tetraphenylborate; and quaternary ammonium salts such as tetraethylammonium bromide, tetra-n-butylammonium bromide, tetraethylammonium chloride, and tetra-n-butylammonium chloride.
[0103] The catalyst is preferably used in an amount of 100 parts by mass or less, more preferably 0.01 to 100 parts by mass, and even more preferably 0.1 to 20 parts by mass, per 100 parts by mass of the polymer having an epoxy group.
[0104] Examples of the organic solvent include hydrocarbon compounds, ether compounds, ester compounds, ketone compounds, amide compounds, and alcohol compounds. Of these, ether compounds, ester compounds, ketone compounds, and alcohol compounds are preferred from the viewpoints of solubility of the raw materials and the product and ease of product purification. The solvent is used in an amount such that the solids concentration (the proportion of the mass of components other than the solvent in the reaction solution to the total mass of the solution) is preferably 0.1 mass% or more, more preferably 5 to 50 mass%.
[0105] The reaction temperature is preferably 0 to 200° C., more preferably 50 to 150° C. The reaction time is preferably 0.1 to 50 hours, more preferably 0.5 to 20 hours.
[0106] In this way, a solution containing a reaction product of the polymer having an epoxy group and the cinnamic acid derivative is obtained. This solution may be used as it is for the preparation of a cured film-forming composition, or the polymer contained in the solution may be isolated and then used for the preparation of a cured film-forming composition, or the isolated polymer may be purified and then used for the preparation of a cured film-forming composition.
[0107] In this embodiment, the acrylic copolymer of component (A) may be a mixture of multiple specific copolymers.
[0108] As described above, in the present invention, a high molecular weight specific copolymer can be used as component (A), and component (A) may also be a mixture of one or more specific copolymers.
[0109] [Component (B)] The component (B) contained in the cured film-forming composition of the present embodiment is a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit having a partial structure represented by the above formula (1), and more specifically, is a polymer obtained by copolymerizing a monomer having an N-alkoxymethyl group or an N-hydroxymethyl group and a monomer having a group represented by the above formula (1) (hereinafter, also referred to as specific copolymer 2).
[0110] Preferred examples of the monomer having an N-alkoxymethyl group or an N-hydroxymethyl group include compounds represented by the following formula (X1): (In the formula, R 31 represents a hydrogen atom or a methyl group, R 32 represents a hydrogen atom or a linear or branched alkyl group having 1 to 10 carbon atoms)
[0111] Specific examples of the compound represented by formula (X1) include acrylamide compounds or methacrylamide compounds substituted with a hydroxymethyl group or an alkoxymethyl group, such as N-hydroxymethyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide, where (meth)acrylamide refers to both methacrylamide and acrylamide.
[0112] In the above formula (1), Q 1 The alkyl group having 1 to 6 carbon atoms represented by is preferably an alkyl group having 1 to 5 carbon atoms. Examples of such an alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl-n-pentyl group, a 4-methyl-n-pentyl group, a 5-methyl-n-pentyl group, a 6-methyl-n-pentyl group, a 7-methyl-n-pentyl group, a 8-methyl-n-pentyl group, a 9-methyl-n-pentyl group, a 10-methyl-n-pentyl group, a 11-methyl-n-pentyl group, a 12-methyl-n-pentyl group, a 13-methyl-n-pentyl group, a 14-methyl-n-pentyl group, a 15-methyl-n-pentyl group, a 16-methyl-n-pentyl group, a 17-methyl-n-pentyl group, a 18-methyl-n-pentyl group, a 19-methyl-n-pentyl group, a 20-methyl-n-pentyl group, a 21-methyl-n-pentyl group, a 22-methyl-n-pentyl group, a 23-methyl-n-pentyl group, a 24-methyl-n-pentyl group, a 25-methyl-n-pentyl group, a 26-methyl-n-pentyl group, a Examples of such alkyl groups include butyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. Among these, methyl, ethyl, n-propyl, n-butyl, and isobutyl groups are preferred.
[0113] In the above formula (1), Q 1The alkoxy group having 1 to 6 carbon atoms represented by is preferably an alkoxy group having 1 to 5 carbon atoms. Examples of such an alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentyloxy group, a 2-methyl-n-pentyloxy group, a 3-methyl-n-pentyloxy group, a 4-methyl-n-pentyloxy group, a 5-methyl-n-pentyloxy group, a 6-methyl-n-pentyloxy group, a 7-methyl-n-pentyloxy group, a 8-methyl-n-pentyloxy group, a 9-methyl-n-pentyloxy group, a 10-methyl-n-pentyloxy group, a 11-methyl-n-pentyloxy group, a 12-methyl-n-pentyloxy group, a 13-methyl-n-pentyloxy group, a 14-methyl-n-pentyloxy group, a 15-methyl-n-pentyloxy group, a 16-methyl-n-pentyloxy group, a 17-methyl-n-pentyloxy group, a 18-methyl-n-pentyloxy group, a 19-methyl-n-pentyloxy group, a 20-methyl-n-pentyloxy group, a 21-methyl-n-pentyloxy group, a 22-methyl-n-pentyloxy group, a 23-methyl-n-pentyloxy Examples of such an alkyl group include butyloxy, 1,1-dimethyl-n-butoxy, 1,2-dimethyl-n-butoxy, 1,3-dimethyl-n-butoxy, 2,2-dimethyl-n-butoxy, 2,3-dimethyl-n-butoxy, 3,3-dimethyl-n-butoxy, 1-ethyl-n-butoxy, 2-ethyl-n-butoxy, 1,1,2-trimethyl-n-propoxy, 1,2,2-trimethyl-n-propoxy, 1-ethyl-1-methyl-n-propoxy, 1-ethyl-2-methyl-n-propoxy, cyclopropoxy, cyclobutoxy, cyclopentyloxy, and cyclohexyloxy. Among these, methoxy, ethoxy, and n-propoxy are preferred.
[0114] In the above formula (1), Q 2 is O, S or NQ 3 represents Q 3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 3 The alkyl group having 1 to 4 carbon atoms represented by Q 1 Among the specific examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I), those having 1 to 4 carbon atoms are preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred, with a methyl group being more preferred.
[0115] Examples of the monomer having a group represented by formula (1) include acetoacetoxyethyl acrylate and acetoacetoxyethyl methacrylate.
[0116] The amounts of the monomer having an N-hydroxymethyl group or an N-alkoxymethyl group and the monomer having a group represented by formula (1) used to obtain a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit having a partial structure represented by formula (1) are, based on the total amount of all monomers used to obtain specific copolymer 2, preferably 10 mol% to 99.9 mol% of the monomer having an N-hydroxymethyl group or an N-alkoxymethyl group, more preferably 30 mol% to 99 mol%, and even more preferably 50 mol% to 95 mol%, and preferably 0.1 mol% to 90 mol% of the monomer having a group represented by formula (1), more preferably 1 mol% to 70 mol%, and even more preferably 5 mol% to 50 mol%.
[0117] When obtaining a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit represented by the above formula (1), a monomer having a non-reactive functional group, as exemplified in the section on component (A), can be used. When the total amount of the monomer having an N-hydroxymethyl group or an N-alkoxymethyl group and the monomer having a group represented by formula (1) is less than 100 mol%, the amount of the monomer having a non-reactive functional group used is the remaining portion.
[0118] The weight average molecular weight of the polymer that is component (B) of such a polymer is preferably from 1,000 to 500,000, more preferably from 2,000 to 200,000, still more preferably from 3,000 to 150,000, and particularly preferably from 3,000 to 70,000.
[0119] These polymers of component (B) can be used alone or in combination of two or more.
[0120] In the cured film-forming composition of the present embodiment, the content of the polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group as component (B) and a structural unit having a partial structure represented by formula (1) above is preferably 10 parts by mass to 3,000 parts by mass, and more preferably 20 parts by mass to 2,500 parts by mass, based on 100 parts by mass of the compound as component (A).
[0121] [Component (C)] The cured film-forming composition of the present embodiment may further contain an ammonium salt as component (C). By containing an ammonium salt, the reaction of capturing formaldehyde can be promoted, and the amount of formaldehyde contained in the cured film-forming composition can be significantly reduced. Examples of the ammonium salt as component (C) include ammonium chloride, ammonium bromide, ammonium fluoride, ammonium iodide, ammonium acetate, ammonium carbonate, ammonium formate, ammonium phosphate, and ammonium borate. Among these, ammonium acetate is preferred in terms of availability.
[0122] When the cured film-forming composition of the present embodiment contains an ammonium salt as the component (C), the content thereof is preferably 0.001 to 100 parts by mass, and more preferably 0.01 to 60 parts by mass, based on 100 parts by mass of the compound as the component (A).
[0123] [Component (D)] The cured film-forming composition that forms a cured film on the surface of the optical film of the present invention contains a crosslinking catalyst as component (D) in addition to the above-mentioned components (A), (B), and, if necessary, (C). Examples of the crosslinking catalyst as component (D) include acids and thermal acid generators. This component (D) is effective in accelerating the thermal curing reaction in the formation of a cured film using the cured film-forming composition that forms a cured film on the surface of the optical film of the present invention.
[0124] When an acid or thermal acid generator is used as component (D), component (D) is not particularly limited as long as it is a sulfonic acid group-containing compound, hydrochloric acid or a salt thereof, or a compound that thermally decomposes during pre-bake or post-bake to generate an acid, i.e., a compound that thermally decomposes at a temperature of 60°C to 250°C to generate an acid.
[0125] Examples of such compounds include sulfonic acids such as hydrochloric acid, methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, octanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, camphorsulfonic acid, trifluoromethanesulfonic acid, p-phenolsulfonic acid, 2-naphthalenesulfonic acid, mesitylenesulfonic acid, p-xylene-2-sulfonic acid, m-xylene-2-sulfonic acid, 4-ethylbenzenesulfonic acid, 1H,1H,2H,2H-perfluorooctanesulfonic acid, perfluoro(2-ethoxyethane)sulfonic acid, pentafluoroethanesulfonic acid, nonafluorobutane-1-sulfonic acid, dodecylbenzenesulfonic acid, 1,2-ethanedisulfonic acid, and methanesulfonic anhydride, as well as hydrates and salts thereof.
[0126] Examples of the compound that generates an acid when heated include bis(tosyloxy)ethane, bis(tosyloxy)propane, bis(tosyloxy)butane, p-nitrobenzyl tosylate, o-nitrobenzyl tosylate, 1,2,3-phenylene tris(methylsulfonate), p-toluenesulfonic acid pyridinium salt, p-toluenesulfonic acid morphonium salt, p-toluenesulfonic acid ethyl ester, p-toluenesulfonic acid propyl ester, p-toluenesulfonic acid butyl ester, p-toluenesulfonic acid isobutyl ester, p-toluenesulfonic acid methyl ester, p-toluenesulfonic acid phenethyl ester, cyanomethyl p-toluenesulfonate, 2,2,2-trifluoroethyl p-toluenesulfonate, 2-hydroxybutyl p-tosylate, N-ethyl-4-toluenesulfonamide, and the compounds represented by the following formulae [TAG-1] to [TAG-41].
[0127]
[0128]
[0129]
[0130]
[0131]
[0132]
[0133]
[0134] The component (D) is commercially available, and examples thereof include TA-100, TA-100FG, IK-1, and IK-1FG (all manufactured by San-Apro Ltd.), San-Aid (registered trademark) SI-B2A, San-Aid (registered trademark) SI-B7, San-Aid (registered trademark) SI-B3A, San-Aid (registered trademark) SI-B3, San-Aid (registered trademark) SI-B5, San-Aid (registered trademark) SI-B4, San-Aid (registered trademark) SI-150, San-Aid (registered trademark) SI-110, San-Aid (registered trademark) SI-60, San-Aid (registered trademark) SI-80, and San-Aid (registered trademark) SI-100 (all manufactured by Sanshin Chemical Industry Co., Ltd.).
[0135] The content of component (D) in the cured film-forming composition of the present invention is 0.01 to 500 parts by mass, preferably 0.01 to 400 parts by mass, more preferably 0.05 to 300 parts by mass, and even more preferably 0.1 to 200 parts by mass, per 100 parts by mass of the photoalignment component (A). By ensuring that the content of component (D) is 0.01 parts by mass or more, sufficient thermosetting properties and solvent resistance can be imparted, and high sensitivity to light exposure can also be imparted. Furthermore, by ensuring that the content is 500 parts by mass or less, the storage stability of the cured film-forming composition can be improved.
[0136] [Component (E)] The cured film-forming composition of the present embodiment may contain a hydrophilic polymer as component (E). The polymer as component (E) may be a polymer having one or more substituents selected from a hydroxy group, a carboxy group, and an amino group (hereinafter also referred to as a specific polymer).
[0137] In the cured film-forming composition of the present embodiment, the specific polymer (E) is preferably a highly hydrophilic polymer having high hydrophilicity so as to be more hydrophilic than the component (A). The specific polymer is preferably a polymer having a hydrophilic group such as a hydroxy group, a carboxy group, or an amino group, and more specifically, a polymer having one or more substituents selected from a hydroxy group, a carboxy group, and an amino group.
[0138] Examples of the polymer that is component (E) include acrylic polymers, urethane-modified acrylic polymers, polyamic acids, polyimides, polyvinyl alcohols, polyesters, polyester polycarboxylic acids, polyether polyols, polyester polyols, polycarbonate polyols, polycaprolactone polyols, polyalkyleneimines, polyallylamine, polymers having a linear or branched structure such as celluloses (cellulose or derivatives thereof), phenol novolac resins, and melamine formaldehyde resins, and cyclic polymers such as cyclodextrins. Of these, the acrylic polymers that can be used include polymers obtained by polymerizing monomers having an unsaturated double bond, such as acrylic acid esters, methacrylic acid esters, and styrene.
[0139] The specific polymer that is component (E) is preferably a hydroxyalkyl cyclodextrin, a cellulose, an acrylic polymer having at least one of a polyethylene glycol ester group and a hydroxyalkyl ester group having 2 to 5 carbon atoms, and at least one of a carboxy group and a phenolic hydroxy group, an acrylic polymer having an aminoalkyl group on the side chain, an acrylic polymer having a hydroxyalkyl group on the side chain such as polyhydroxyethyl methacrylate, a polyether polyol, a polyester polyol, a polycarbonate polyol, or a polycaprolactone polyol.
[0140] The acrylic polymer having at least one of a polyethylene glycol ester group and a hydroxyalkyl ester group having 2 to 5 carbon atoms, and at least one of a carboxy group and a phenolic hydroxy group, which is a preferred example of the specific polymer of component (E), is not particularly limited as long as it is an acrylic polymer having such a structure, and there are no particular limitations on the types of the main chain skeleton and side chains of the polymer constituting the acrylic polymer.
[0141] A preferred structural unit having at least one of a polyethylene glycol ester group and a hydroxyalkyl ester group having 2 to 5 carbon atoms is represented by the following formula [E1]. A preferred structural unit having at least one of a carboxy group and a phenolic hydroxy group is represented by the following formula [E2]. In the above formula [E1] and formula [E2], X 3 and X 4 each independently represents a hydrogen atom or a methyl group; Y 1 is H-(OCH 2 CH 2 ) n - group (wherein the value of n is 2 to 50, preferably 2 to 10) or a hydroxyalkyl group having 2 to 5 carbon atoms; Y 2 represents a group having a carboxy group or a phenolic hydroxy group.
[0142] The acrylic polymer, an example of component (E), preferably has a weight-average molecular weight of 3,000 to 200,000, more preferably 4,000 to 150,000, and even more preferably 5,000 to 100,000. If the weight-average molecular weight is too high (exceeding 200,000), solubility in solvents may decrease, resulting in poor handling. If the weight-average molecular weight is too low (less than 3,000), the polymer may not cure sufficiently during thermal curing, resulting in poor solvent resistance and heat resistance. The weight-average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard. The same applies hereinafter in this specification.
[0143] A simple method for synthesizing an acrylic polymer, which is an example of component (E), is to copolymerize a monomer having at least one of a polyethylene glycol ester group and a hydroxyalkyl ester group having 2 to 5 carbon atoms (hereinafter also referred to as an e1 monomer) with a monomer having at least one of a carboxy group and a phenolic hydroxy group (hereinafter also referred to as an e2 monomer).
[0144] The monomer having the polyethylene glycol ester group is, for example, H—(OCH 2 CH 2 ) n The value of n is 2 to 50, preferably 2 to 10.
[0145] Examples of the monomer having a hydroxyalkyl ester group having 2 to 5 carbon atoms include 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, and N-hydroxyethyl acrylamide.
[0146] Examples of the monomer having a carboxy group include acrylic acid, methacrylic acid, and vinylbenzoic acid. Examples of the monomer having a phenolic hydroxy group include p-hydroxystyrene, m-hydroxystyrene, and o-hydroxystyrene.
[0147] Furthermore, in the present embodiment, when synthesizing an acrylic polymer, which is an example of component (E), a monomer other than the e1 monomer and the e2 monomer, specifically a monomer having neither a hydroxy group nor a carboxy group, can be used in combination, as long as the effects of the present invention are not impaired.
[0148] Examples of such monomers include acrylic acid ester compounds such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, and tert-butyl acrylate; methacrylic acid ester compounds such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and tert-butyl methacrylate; maleimide compounds such as maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; acrylamide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.
[0149] The amounts of e1 monomer and e2 monomer used to obtain the acrylic polymer, which is an example of component (E), are preferably 2 mol % to 95 mol % of e1 monomer and 5 mol % to 98 mol % of e2 monomer, based on the total amount of all monomers used to obtain the acrylic polymer, which is component (E).
[0150] When a monomer having only a carboxy group is used as the e2 monomer, it is preferable that the e1 monomer accounts for 60 mol% to 95 mol% and the e2 monomer accounts for 5 mol% to 40 mol% based on the total amount of all monomers used to obtain the acrylic polymer (component (E)). On the other hand, when a monomer having only a phenolic hydroxy group is used as the e2 monomer, it is preferable that the e1 monomer accounts for 2 mol% to 80 mol% and the e2 monomer accounts for 20 mol% to 98 mol%. If the amount of e2 monomer is too small, the liquid crystal alignment property is likely to be insufficient, and if it is too large, the compatibility with component (A) is likely to be reduced.
[0151] The method for obtaining the acrylic polymer, an example of component (E), is not particularly limited, but for example, it can be obtained by a polymerization reaction at a temperature of 50°C to 110°C in a solvent containing e1 monomer, e2 monomer, and optionally monomers other than e1 monomer and e2 monomer, a polymerization initiator, etc. The solvent used in this case is not particularly limited as long as it dissolves e1 monomer, e2 monomer, and optionally monomers other than e1 monomer and e2 monomer, the polymerization initiator, etc. Specific examples are described in the section <Solvent> below.
[0152] The acrylic polymer having an aminoalkyl group on the side chain, which is a preferred example of the specific polymer of component (E), is, for example, a polymer of an aminoalkyl ester monomer such as aminoethyl acrylate, aminoethyl methacrylate, aminopropyl acrylate, or aminopropyl methacrylate, or a copolymer of the aminoalkyl ester monomer with one or more monomers selected from the group consisting of the e1 monomer, the e2 monomer, and monomers other than these monomers, for example, monomers having neither a hydroxy group nor a carboxy group.
[0153] Examples of the acrylic polymer having a hydroxyalkyl group on the side chain, which is a preferred example of the specific polymer of component (E), include a polymer of a hydroxyalkyl ester monomer such as hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxypentyl acrylate, and hydroxypentyl methacrylate, or a copolymer of the hydroxyalkyl ester monomer with one or more monomers selected from the group consisting of the e1 monomer, the e2 monomer, and monomers other than these monomers, for example, monomers having neither a hydroxy group nor a carboxy group.
[0154] The acrylic polymer, which is an example of component (E), obtained by the above method is usually in the form of a solution dissolved in a solvent.
[0155] Alternatively, the solution of the acrylic polymer (an example of component (E)) obtained by the above method can be reprecipitated by adding it to diethyl ether, water, or the like under stirring, and the resulting precipitate can be filtered and washed, and then dried at room temperature or by heating under normal or reduced pressure to obtain a powder of the acrylic polymer (an example of component (E)). This procedure can remove the polymerization initiator and unreacted monomers coexisting with the acrylic polymer (an example of component (E)), resulting in a purified powder of the acrylic polymer (an example of component (E)). If sufficient purification cannot be achieved by a single procedure, the obtained powder can be redissolved in a solvent, and the above procedure can be repeated.
[0156] Preferred examples of the specific polymer of component (E) include polyether polyols, such as polyethylene glycol, polypropylene glycol, and propylene glycol, as well as polyhydric alcohols such as bisphenol A, triethylene glycol, and sorbitol, which are either adducted or condensed with propylene oxide, polyethylene glycol, or polypropylene glycol. Specific examples of polyether polyols include ADEKA ADEKA Polyether P series, G series, EDP series, BPX series, FC series, and CM series manufactured by ADEKA; NOF Corp.'s UNIOX (registered trademark) HC-40, HC-60, ST-30E, ST-40E, G-450, and G-750; UNIOL (registered trademark) TG-330, TG-1000, TG-3000, TG-4000, HS-1600D, DA-400, DA-700, and DB-400; and NONION (registered trademark) LT-221, ST-221, and OT-221.
[0157] A preferred example of the specific polymer of component (E) is a polyester polyol, which may be a product obtained by reacting a polycarboxylic acid such as succinic acid, glutaric acid, adipic acid, sebacic acid, phthalic acid, terephthalic acid, or isophthalic acid with a diol such as ethylene glycol, propylene glycol, butylene glycol, polyethylene glycol, or polypropylene glycol. Specific examples of polyester polyols include Polylite (registered trademark) OD-X-286, OD-X-102, OD-X-355, OD-X-2330, OD-X-240, OD-X-668, OD-X-2108, OD-X-2376, OD-X-2044, OD-X-688, OD-X-2068, OD-X-2547, OD-X-2420, and OD-X-25 manufactured by DIC. 23, OD-X-2555, OD-X-2560, Kuraray polyols P-510, P-1010, P-2010, P-3010, P-4010, P-5010, P-6010, F-510, F-1010, F-2010, F-3010, P-1011, P-2011, P-2013, P-2030, N-2010, PNNA-2016, and Kawasaki Kasei Chemicals Ltd. MAXIMOL RDK-133, RFK-505, SDK-145, RMK-342.
[0158] A preferred example of the specific polymer (E) is polycaprolactone polyol, which is obtained by ring-opening polymerization of ε-caprolactam using a polyhydric alcohol such as trimethylolpropane or ethylene glycol as an initiator. Specific examples of polycaprolactone polyols include Polylite (registered trademark) OD-X-2155, OD-X-640, and OD-X-2568 manufactured by DIC, and Placcel (registered trademark) 205, L205AL, 205U, 208, 210, 212, L212AL, 220, 230, 240, 303, 305, 308, 312, and 320 manufactured by Daicel Chemical Industries, Ltd.
[0159] A preferred example of the specific polymer of component (E), polycarbonate polyol, is one obtained by reacting a polyhydric alcohol such as trimethylolpropane or ethylene glycol with diethyl carbonate, diphenyl carbonate, ethylene carbonate, etc. Specific examples of polycarbonate polyols include PLACCEL (registered trademark) CD205, CD205PL, CD210, CD220, C-590, C-1050, C-2050, C-2090, C-3090, etc., manufactured by Daicel Chemical Industries, Ltd.
[0160] Preferred examples of the specific polymer of component (E) include cellulose, such as hydroxyalkyl celluloses, hydroxyethyl cellulose, hydroxypropyl cellulose, and the like; hydroxyalkyl alkyl celluloses, such as hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl ethyl cellulose, and the like; and cellulose, among which hydroxyalkyl celluloses, such as hydroxyethyl cellulose, hydroxypropyl cellulose, and the like, are preferred.
[0161] Cyclodextrins, which are a preferred example of the specific polymer of component (E), include cyclodextrins such as α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin; methylated cyclodextrins such as methyl-α-cyclodextrin, methyl-β-cyclodextrin, and methyl-γ-cyclodextrin; hydroxymethyl-α-cyclodextrin, hydroxymethyl-β-cyclodextrin, hydroxymethyl-γ-cyclodextrin, 2-hydroxyethyl-α-cyclodextrin, 2-hydroxyethyl-β ... and hydroxyalkyl cyclodextrins such as 2-hydroxypropyl-α-cyclodextrin, 2-hydroxypropyl-β-cyclodextrin, 2-hydroxypropyl-γ-cyclodextrin, 3-hydroxypropyl-α-cyclodextrin, 3-hydroxypropyl-β-cyclodextrin, 3-hydroxypropyl-γ-cyclodextrin, 2,3-dihydroxypropyl-α-cyclodextrin, 2,3-dihydroxypropyl-β-cyclodextrin, and 2,3-dihydroxypropyl-γ-cyclodextrin.
[0162] A preferred example of the specific polymer of component (E), the phenol novolak resin, is, for example, a phenol-formaldehyde polycondensate.
[0163] In the cured film-forming composition of the present embodiment, the polymer of component (E) may be used in the form of a powder, or in the form of a solution obtained by redissolving a purified powder in a solvent described below.
[0164] In the cured film-forming composition of the present embodiment, the polymer of component (E) may be a mixture of multiple types of polymers of component (E).
[0165] When the resin composition for forming a retardation material of the present invention contains the component (E), the content thereof is preferably 10 parts by mass to 1000 parts by mass, more preferably 30 parts by mass to 500 parts by mass, based on 100 parts by mass of the photo-alignment component of the component (A).
[0166] [Component (F)] The cured film-forming composition of the present invention may also contain, as component (F), a component that improves the adhesiveness of the cured film to be formed (hereinafter also referred to as an adhesion-improving component).
[0167] The adhesion improving component (F) can link the polymerizable functional group of the polymerizable liquid crystal with the crosslinking reaction site of the alignment material by a covalent bond so as to improve the adhesion between the alignment material obtained from the cured film-forming composition of the present invention and the polymerizable liquid crystal layer. As a result, the retardation material of the present embodiment obtained by laminating the cured polymerizable liquid crystal on the alignment material of the present embodiment can maintain strong adhesion even under high temperature and high humidity conditions and can exhibit high durability against peeling, etc.
[0168] The component (F) is preferably a monomer or polymer having a group selected from a hydroxy group and an N-alkoxymethyl group, and a polymerizable group. Examples of such component (F) include a compound having a hydroxy group and a (meth)acrylic group, a compound having an N-alkoxymethyl group and a (meth)acrylic group, and a polymer having an N-alkoxymethyl group and a (meth)acrylic group. Specific examples of each are shown below.
[0169] An example of component (F) is a polyfunctional acrylate containing a hydroxy group (hereinafter also referred to as a hydroxy group-containing polyfunctional acrylate). Examples of the hydroxy group-containing polyfunctional acrylate that is an example of component (F) include pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol pentaacrylate. Commercially available products include KAYARAD PET-30 (manufactured by Nippon Kayaku Co., Ltd.).
[0170] Examples of component (F) include compounds having one acrylic group and one or more hydroxy groups, such as 10-hydroxydecyl acrylate, 10-hydroxydecyl methacrylate, and 12-hydroxydodecyl methacrylate.
[0171] Furthermore, examples of the compound of component (F) include compounds having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule.
[0172] Examples of the polymerizable group containing a C═C double bond include an acrylic group, a methacrylic group, a vinyl group, an allyl group, and a maleimide group.
[0173] As a preferred example of the compound having at least one polymerizable group containing a C═C double bond and at least one N-alkoxymethyl group in one molecule, there can be mentioned a compound represented by the following formula (X1): (In the formula, R 31 represents a hydrogen atom or a methyl group, R 32 represents a hydrogen atom or a linear or branched alkyl group having 1 to 10 carbon atoms)
[0174] Specific examples of the compound represented by formula (X1) include acrylamide compounds or methacrylamide compounds substituted with a hydroxymethyl group or an alkoxymethyl group, such as N-hydroxymethyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide, where (meth)acrylamide refers to both methacrylamide and acrylamide.
[0175] Preferred examples of the compound having a polymerizable group containing a C═C double bond and an N-alkoxymethyl group as component (F) include the following compounds.
[0176] The content of the (F) component in the liquid crystal aligning agent according to an embodiment of the present invention is preferably 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, relative to 100 parts by mass of the alignment component (A).
[0177] [Other Additives] The cured film-forming composition of the present invention may contain other additives as long as the effects of the present invention are not impaired. Examples of other additives include a sensitizer. The sensitizer is effective in accelerating the photoreaction when forming a cured film on the surface of the optical film of the present invention.
[0178] Examples of the sensitizer include derivatives of benzophenone, anthracene, anthraquinone, thioxanthone, etc., and nitrophenyl compounds, etc. Among these, N,N-diethylaminobenzophenone, which is a benzophenone derivative, and 2-nitrofluorene, 2-nitrofluorenone, 5-nitroacenaphthene, 4-nitrobiphenyl, 4-nitrocinnamic acid, 4-nitrostilbene, 4-nitrobenzophenone, and 5-nitroindole, which are nitrophenyl compounds, are particularly preferred.
[0179] These sensitizers are not particularly limited to those mentioned above, and these can be used alone or in combination of two or more compounds.
[0180] In an embodiment of the present invention, the proportion of the sensitizer used is preferably 0.1 to 20 parts by mass, and more preferably 0.2 to 10 parts by mass, per 100 parts by mass of component (A). If this proportion is too small, the effect as a sensitizer may not be fully obtained, whereas if it is too large, the transmittance of the formed cured film may decrease or the coating film may become rough.
[0181] The cured film-forming composition according to an embodiment of the present invention may contain other additives such as a silane coupling agent, a surfactant, a rheology modifier, a pigment, a dye, a storage stabilizer, an antifoaming agent, and an antioxidant, as long as the effects of the present invention are not impaired.
[0182] [Solvent] The cured film-forming composition according to an embodiment of the present invention is often used in the form of a solution in a solvent. The solvent used in this case dissolves the components (A), (B), and (D), and optionally the components (C), (E), and (F), and other additives. The type and structure of the solvent are not particularly limited as long as it has the ability to dissolve the components.
[0183] Specific examples of the solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether, propylene glycol propyl ether acetate, cyclopentyl methyl ether, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-butanone, and 3-methyl-2-pentanone. , 2-pentanone, 2-heptanone, γ-butyrolactone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, n-propyl acetate, isopropyl acetate, isopropanol, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.
[0184] The solvent is commercially available, and examples thereof include Neoethanol (registered trademark) PM, Neoethanol (registered trademark) MIP, Neoethanol (registered trademark) IPM, Neoethanol (registered trademark) IPE, Neoethanol (registered trademark) PHI, Neoethanol (registered trademark) MHI, Neoethanol (registered trademark) PIP, Neoethanol (registered trademark) HIMTE, Neoethanol (registered trademark) PHM, Neoethanol (registered trademark) IPME, and Neoethanol (registered trademark) P-7 (all manufactured by Taishin Chemical Co., Ltd.).
[0185] These solvents can be used alone or in combination of two or more. Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, cyclohexanone, 2-heptanone, propylene glycol propyl ether, propylene glycol propyl ether acetate, ethyl acetate, ethyl lactate, butyl lactate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, and Neoethanol (registered trademark) IPM are more preferred because of their excellent film-forming properties and high safety.
[0186] <Preparation of Cured Film-Forming Composition> As described above, the composition that forms the cured film on the surface of the optical film of the present invention is a composition in which a photoalignment component (A), a polymer (B) having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group and a structural unit having a partial structure represented by formula (1) above, and a crosslinking catalyst (D) are dissolved in a solvent. If desired, the composition may further contain an ammonium salt (C), a hydrophilic polymer (E), and an adhesion-improving component (F). Other additives may also be added as long as they do not impair the effects of the present invention.
[0187] Preferred examples of the resin composition for forming a retardation material of the present invention are as follows: [1]: A resin composition for forming a retardation material, comprising (A) a photoalignment component, 10 parts by mass to 2,000 parts by mass of (B) component based on 100 parts by mass of the component (A), and 0.01 parts by mass to 200 parts by mass of (D) crosslinking catalyst relative to 100 parts by mass of the component (A).
[0188] [2]: A resin composition for forming a retardation material, comprising: (A) a photoalignment component; 10 parts by mass to 2,000 parts by mass of (B) component based on 100 parts by mass of the (A) component; 0.001 parts by mass to 100 parts by mass of (C) ammonium salt based on 100 parts by mass of the (A) component; and 0.01 parts by mass to 200 parts by mass of (D) crosslinking catalyst relative to 100 parts by mass of the (A) component.
[0189] [3]: A resin composition for forming a retardation material, comprising: (A) a photo-alignment component, 10 parts by mass to 2000 parts by mass of the (B) component based on 100 parts by mass of the (A) component, 0.001 parts by mass to 100 parts by mass of the (C) ammonium salt based on 100 parts by mass of the (A) component, 0.01 parts by mass to 200 parts by mass of the (D) crosslinking catalyst based on 100 parts by mass of the (A) component, and 10 parts by mass to 1000 parts by mass of the (E) base polymer based on 100 parts by mass of the (A) component. [3-2]: A resin composition for forming a retardation material, comprising: (A) a photo-alignment component, 10 parts by mass to 2000 parts by mass of the (B) component based on 100 parts by mass of the (A) component, 0.01 parts by mass to 200 parts by mass of the (D) crosslinking catalyst based on 100 parts by mass of the (A) component, and 10 parts by mass to 1000 parts by mass of the (E) base polymer based on 100 parts by mass of the (A) component.
[0190] [4]: A resin composition for forming a retardation material, comprising: (A) a photoalignment component; 10 parts by mass to 2000 parts by mass of a (B) component based on 100 parts by mass of the (A) component; 0.001 parts by mass to 100 parts by mass of a (C) ammonium salt based on 100 parts by mass of the (A) component; 0.01 parts by mass to 200 parts by mass of a (D) crosslinking catalyst relative to 100 parts by mass of the (A) component; and 1 part by mass to 200 parts by mass of a (F) component based on 100 parts by mass of the (A) component.
[0191] [5]: A resin composition for forming a retardation material, comprising: (A) a photoalignment component; 10 parts by mass to 2000 parts by mass of a (B) component based on 100 parts by mass of the (A) component; 0.001 parts by mass to 100 parts by mass of a (C) ammonium salt based on 100 parts by mass of the (A) component; 0.01 parts by mass to 200 parts by mass of a (D) crosslinking catalyst relative to 100 parts by mass of the (A) component; 10 parts by mass to 1000 parts by mass of an (E) base polymer based on 100 parts by mass of the (A) component; and 1 part by mass to 200 parts by mass of a (F) component based on 100 parts by mass of the (A) component. [5-2]: A resin composition for forming a retardation material, comprising: (A) a photoalignment component; 10 parts by mass to 2,000 parts by mass of a (B) component based on 100 parts by mass of the (A) component; 0.01 parts by mass to 200 parts by mass of a (D) crosslinking catalyst relative to 100 parts by mass of the (A) component; 10 parts by mass to 1,000 parts by mass of an (E) base polymer based on 100 parts by mass of the (A) component; and 1 part by mass to 200 parts by mass of a (F) component based on 100 parts by mass of the (A) component.
[0192] The blending ratios, preparation methods, etc., when the composition that forms the cured film on the surface of the optical film of the present invention is used as a solution are described in detail below. The solid content of the composition that forms the cured film on the surface of the optical film of the present invention is not particularly limited as long as each component is uniformly dissolved in the solvent, but is 1% by mass to 80% by mass, preferably 2% by mass to 60% by mass, and more preferably 3% by mass to 40% by mass. Here, the solid content refers to all components of the cured film-forming composition excluding the solvent.
[0193] The method for preparing the composition for forming the cured film on the surface of the optical film of the present invention is not particularly limited. Examples of the preparation method include a method of mixing a solution of the component (B) dissolved in a solvent with the component (A), and optionally the components (C), (D), and further optionally the components (E) and (F) in predetermined proportions to prepare a homogeneous solution, or a method of further adding and mixing other additives as necessary at an appropriate stage of this preparation method.
[0194] In preparing the composition for forming the cured film on the surface of the optical film of the present invention, as described above, a solution of specific copolymer 2 (component (B)) obtained by polymerization in a solvent can be used as is. In this case, for example, component (A), and optionally component (C), and further components (D), (E), etc. are added to a solution of component (B) obtained by copolymerizing the aforementioned monomer having an N-hydroxymethyl group or an N-alkoxymethyl group, a monomer having a group represented by formula (1), and optionally other monomers, to prepare a homogeneous solution. At this time, additional solvent may be added for the purpose of adjusting the concentration. In this case, the solvent used in the production process of component (B) and the solvent used to adjust the concentration of the cured film-forming composition may be the same or different.
[0195] The prepared solution of the cured film-forming composition is preferably filtered using a filter having a pore size of about 0.2 μm before use in forming the cured film.
[0196] <Cured Film, Alignment Material, and Retardation Material> The cured film-forming composition of the present embodiment can be obtained by applying a solution of the cured film-forming composition to a substrate (e.g., a silicon / silicon dioxide-coated substrate, a silicon nitride substrate, a substrate coated with a metal such as aluminum, molybdenum, or chromium, a glass substrate, a quartz substrate, or an ITO substrate) or a film (e.g., a resin film such as a triacetyl cellulose (TAC) film, a cycloolefin polymer film, a polyethylene terephthalate film, or an acrylic film) by bar coating, spin coating, flow coating, roll coating, slit coating, spin coating followed by slit coating, inkjet coating, printing, or the like to form a coating film, and then heating and drying the coating on a hot plate, in an oven, or the like to form a cured film.
[0197] The heating and drying conditions are such that when a cured film is used as a liquid crystal alignment film, the curing reaction proceeds to such an extent that the components of the liquid crystal alignment film are not eluted into the polymerizable liquid crystal solution to be applied thereon, and for example, a heating temperature and a heating time appropriately selected from the ranges of 50°C to 200°C and 0.4 to 60 minutes are used. The heating temperature and heating time are preferably 60°C to 160°C and 0.5 to 10 minutes.
[0198] The thickness of the cured film on the surface of the optical film of the present invention is, for example, 0.05 μm to 5 μm, and can be appropriately selected in consideration of the step and optical and electrical properties of the resin film used as the substrate.
[0199] The optical film of the present invention produced in this manner can be irradiated with polarized UV light to cause the cured film formed on the substrate to function as a liquid crystal alignment film, i.e., as a component for aligning compounds having liquid crystallinity, including polymerizable liquid crystals, and the optical film can be used as an alignment material.
[0200] The polarized UV irradiation method generally uses ultraviolet to visible light with a wavelength of 150 nm to 450 nm, and is carried out by irradiating linearly polarized light from a vertical or oblique direction at room temperature or in a heated state.
[0201] In the alignment material of the present invention, the cured film that becomes the liquid crystal alignment film has solvent resistance and heat resistance, so that a retardation material made of a polymerizable liquid crystal solution is applied onto this alignment material, and then heated to the phase transition temperature of the liquid crystal to turn the retardation material into a liquid crystal state and align it on the alignment material. Then, the retardation material in the desired alignment state is cured as it is, and a retardation material having a layer with optical anisotropy can be formed.
[0202] As the retardation material, for example, the liquid crystal monomer having polymerizable group and the composition containing it are used.And, in the present invention, when the substrate on which the alignment material is formed is a film, the retardation material of the present invention is useful as a retardation film.The retardation material that forms such a retardation material is in a liquid crystal state, and on the alignment material, there are some that take the alignment state such as horizontal alignment, cholesteric alignment, vertical alignment, hybrid alignment, etc., and can be used according to the retardation properties that are required.
[0203] Furthermore, when producing a patterned retardation material for use in a 3D display, the cured film on the surface of the optical film of the present invention is exposed to polarized UV light through a line-and-space pattern mask at an angle of, for example, +45 degrees from a predetermined reference, and then the mask is removed and exposed to polarized UV light at a lower exposure dose at an angle of -45 degrees. This converts the cured film on the film surface into a liquid crystal alignment film in which two types of liquid crystal alignment domains with different liquid crystal alignment control directions are formed, and the optical film can be used as an alignment material. A retardation material made of a polymerizable liquid crystal solution is then applied to the alignment material, and the retardation material is then placed in a liquid crystal state by heating to the liquid crystal phase transition temperature. The polymerizable liquid crystal in the liquid crystal state is oriented on the alignment material in which the two types of liquid crystal alignment domains are formed, forming alignment states corresponding to each of the liquid crystal alignment domains. The retardation material in this alignment state is then cured as is to fix the above-mentioned alignment state, thereby obtaining a patterned retardation material in which two types of retardation domains with different retardation characteristics are regularly arranged.
[0204] The optical film of the present invention can also be used as a liquid crystal alignment film for a liquid crystal display element. For example, the optical film of the present embodiment formed as described above can be used to laminate two optical films together via a spacer so that the alignment materials of the two films face each other, and then a liquid crystal can be injected between the substrates to produce a liquid crystal display element in which the liquid crystal is aligned. Therefore, the optical film of the present invention can be suitably used for producing various retardation materials (retardation films), liquid crystal display elements, etc.
[0205] EXAMPLES The present invention will be specifically described below with reference to examples of the present invention, but the present invention should not be construed as being limited to these examples.
[0206] [Abbreviations used in Examples] The meanings of the abbreviations used in the following examples are as follows: <Raw Materials> BMAA: N-butoxymethylacrylamide AAEM: (2-acetoacetoxy)ethyl methacrylate (monomer having a group represented by formula (1)) 4HBA: 4-hydroxybutyl acrylate (corresponding to e1 monomer) MMA: methyl methacrylate (corresponding to e2 monomer) AIBN: α,α'-azobisisobutyronitrile MAIB: 2,2'-azobis(isobutyrate) dimethyl
[0207] MCA:
[0208] M6CA:
[0209] <C component> AcNH 4 : Ammonium acetate
[0210] <Component D: Crosslinking catalyst> PTSA: p-toluenesulfonic acid monohydrate CSA: (±)-10-camphorsulfonic acid PPTS: pyridinium p-toluenesulfonate
[0211] <Component E> PEPO: Polylite (registered trademark) 8651 (manufactured by DIC Corporation, polyester polyol) RMK: Maximol (registered trademark) RMK-342 (manufactured by Kawasaki Chemical Industries, Ltd., polyester polyol) HPC: NISSO HPC-SSL (manufactured by Nippon Soda Co., Ltd., hydroxypropyl cellulose)
[0212] <Component F> HDC-DA: 10HDA: 10-hydroxydecyl acrylate 10HDMA: 10-hydroxydecyl methacrylate 12HDDMA: 12-hydroxydodecyl methacrylate PET30: KAYARAD PET-30 (manufactured by Nippon Kayaku Co., Ltd., a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate)
[0213] <Other additives> MEK-ST-L: organosilica sol MEK-ST-L (manufactured by Nissan Chemical Industries, Ltd.) (30% by mass MEK dispersion)
[0214] <Solvents> PM: Propylene glycol monomethyl ether IPM: Neoethanol (registered trademark) IPM (manufactured by Taishin Chemical Co., Ltd.) EA: Ethyl acetate BA: Butyl acetate CPN: Cyclopentanone MEK: Methyl ethyl ketone
[0215] <Measurement of weight average molecular weight> Apparatus: GPC apparatus (HLC-8320) manufactured by Tosoh Corporation Column: TSKgel (registered trademark) α-4000 and TSKgel (registered trademark) α-3000 manufactured by Tosoh Corporation Column oven: 40°C Flow rate: 1 mL / min Eluent: N,N-dimethylformamide Standard: polystyrene
[0216] Synthesis of Component B Synthesis Example 1 BMAA (50.0 g, 318 mmol), AAEM (3.58 g, 16.7 mmol), α-thioglycerol (0.362 g, 3.35 mmol) as a chain transfer agent, and MAIB (0.154 g, 0.669 mmol) as a polymerization catalyst were dissolved in PM (36.0 g), and this solution was then added dropwise over 60 minutes to a flask containing PM (90.1 g) maintained at 70°C. After completion of the dropwise addition, the mixture was allowed to react overnight, yielding a solution (PB-1) (solids concentration 30% by mass) of an acrylic copolymer (BMAA / AAEM = 95 / 5 (molar ratio)). The weight-average molecular weight Mw of the resulting acrylic copolymer was 26,000.
[0217] Synthesis Example 2 BMAA (47.0 g, 299 mmol), AAEM (7.11 g, 33.2 mmol), α-thioglycerol (0.359 g, 3.32 mmol) as a chain transfer agent, and MAIB (0.153 g, 0.664 mmol) as a polymerization catalyst were dissolved in PM (36.4 g), and this solution was then added dropwise over 60 minutes to a flask containing PM (91.0 g) maintained at 70°C. After completion of the dropwise addition, the mixture was allowed to react overnight, yielding a solution (PB-2) (solids concentration 30% by mass) of an acrylic copolymer (BMAA / AAEM = 90 / 10 (molar ratio)). The weight-average molecular weight Mw of the resulting acrylic copolymer was 52,300.
[0218] Synthesis Example 3 BMAA (34.0 g, 216 mmol), AAEM (19.8 g, 92.4 mmol), α-thioglycerol (0.334 g, 3.09 mmol) as a chain transfer agent, and MAIB (0.142 g, 0.617 mmol) as a polymerization catalyst were dissolved in PM (36.2 g), and this solution was then added dropwise over 60 minutes to a flask containing PM (90.5 g) maintained at 70°C. After completion of the dropwise addition, the mixture was allowed to react overnight, yielding a solution (PB-3) (solids concentration 30% by mass) of an acrylic copolymer (BMAA / AAEM = 70 / 30 (molar ratio)). The weight-average molecular weight Mw of the resulting acrylic copolymer was 56,000.
[0219] Synthesis Example 4 BMAA (23.0 g, 146 mmol), AAEM (31.3 g, 146 mmol), α-thioglycerol (0.316 g, 2.92 mmol) as a chain transfer agent, and MAIB (0.134 g, 0.582 mmol) as a polymerization catalyst were dissolved in PM (36.5 g), and this solution was then added dropwise over 60 minutes to a flask containing PM (91.3 g) maintained at 70°C. After completion of the dropwise addition, the mixture was allowed to react overnight, yielding a solution (PB-4) (solids concentration 30% by mass) of an acrylic copolymer (BMAA / AAEM = 50 / 50 (molar ratio)). The weight-average molecular weight Mw of the resulting acrylic copolymer was 60,000.
[0220] <Synthesis of Component E> <Synthesis Example 5> 4HBA (197.0 g, 1.37 mol) and MAIB (3.1 g, 13 mmol) as a polymerization catalyst were dissolved in PM (133.4 g), and this solution was then added dropwise over 2 hours to a flask containing PM (166.8 g) maintained at 70°C. After completion of the addition, the mixture was allowed to react for 18 hours to obtain an acrylic polymer solution (PE-1) (solids concentration 40% by mass). The weight average molecular weight Mw of the obtained acrylic polymer was 22,700.
[0221] Synthesis Example 6 4HBA (248.0 g, 1.72 mol), α-thioglycerol (1.9 g, 18 mmol), and MAIB (0.20 g, 0.87 mmol) as a polymerization catalyst were dissolved in PM (166.7 g), and this solution was then added dropwise over 4 hours to a flask containing PM (83.4 g) maintained at 70°C. After completion of the addition, the mixture was allowed to react for 18 hours to obtain an acrylic polymer solution (PE-2) (solids concentration: 50% by mass). The weight-average molecular weight Mw of the resulting acrylic polymer was 24,000.
[0222] Synthesis Example 7 MMA (84.4 g, 843 mmol), 4HBA (13.5 g, 93.6 mmol), and MAIB (2.2 g, 9.6 mmol) as a polymerization catalyst were dissolved in PM (150.1 g), and this solution was then added dropwise over 2 hours to a flask containing PM (250.2 g) maintained at 70°C. After completion of the addition, the mixture was allowed to react for 18 hours to obtain a solution (PE-3) (solids concentration 20% by mass) of an acrylic copolymer (MMA / 4HBA = 90 / 10 (molar ratio)). The weight average molecular weight Mw of the resulting acrylic copolymer was 38,900.
[0223] <Synthesis of Other Additives> <Synthesis Example 8> BMAA (145.5 g, 925.5 mmol) and AIBN (4.6 g, 28 mmol) as a polymerization catalyst were dissolved in PM (150.1 g), and this solution was then added dropwise over 30 minutes to a flask containing PM (200.1 g) maintained at 80°C. After completion of the addition, the mixture was allowed to react for 5 hours to obtain an acrylic polymer solution (PBMAA) (solid content concentration 30% by mass). The weight average molecular weight Mw of the obtained acrylic polymer was 23,000.
[0224] Preparation Example 1 PEPO (100 parts by mass) as component (E), MCA (30 parts by mass) as component (A), and PB-1 (190 parts by mass) obtained in Synthesis Example 1 as component (B) were mixed, and PM was added as a solvent and stirred for 2 hours. Dissolution was confirmed visually, yielding a solution. The resulting solution was then filtered through a filter with a pore size of 0.2 μm, yielding a composition (A-1) with a solids concentration of 8.0% by mass.
[0225] Preparation Examples 2 to 15, 17 to 18, 20 to 41, 43 (A-2) to (A-15), (A-17) to (A-18), (A-20) to (A-34), (B-1) to (B-7), and (B-9) were prepared in the same manner as in Preparation Example 1, except that the types and amounts of each component shown in Table 1 below were used.
[0226] Preparation Example 16: PE-2 (100 parts by mass) obtained in Synthesis Example 7 and PE-3 (40 parts by mass) obtained in Synthesis Example 8 were used as the component (E), M6CA (40 parts by mass) was used as the component (A), PB-1 (174 parts by mass) obtained in Synthesis Example 1 was used as the component (B), and AcNH was used as the component (C). 4 (1 part by mass), 10HDA (8 parts by mass) as component (F), and MEK-ST-L (40 parts by mass) as an additive were mixed, to which PM and MEK were added so that the solvent composition was PM:MEK = 97.75:2.05 (mass ratio), and the mixture was stirred for 2 hours. After visually confirming dissolution, a solution was obtained. The resulting solution was then filtered through a glass filter with a pore size of 1.0 μm to prepare composition (A-16) with a solids concentration of 8.0 mass%.
[0227] Preparation Examples 19 and 42 (A-19) and (B-8) were prepared in the same manner as in Preparation Example 16, except that the types and amounts of each component shown in Table 1 below were used.
[0228]
[0229] [Quantification of Formaldehyde Concentration in Composition] Example 1 Formaldehyde in a composition was detected by derivatization using the acetylacetone method. The acetylacetone method involves mixing a sample solution with a reaction solution and labeling it according to the reaction of Scheme 1 below. In this example, the reaction solution used was a mixture of 15 g of ammonium acetate, 600 μL of acetic acid, and 500 μL of acetylacetone diluted to 200 mL with MilliQ ultrapure water, following the general protocol for the acetylacetone method. As a pretreatment step, 700 μL of pure water was added to a microtube, and 300 μL of A-1 prepared in Preparation Example 1 was added. The mixture was stirred for 2 minutes using a mixer rotor, followed by centrifugation to recover the supernatant. 700 μL of the reaction solution and 300 μL of the supernatant were added, reacted at 50°C for 30 minutes, and then allowed to stand at room temperature for 30 minutes to prepare a formaldehyde derivatization solution diluted 11.1 times. This preparation was subjected to liquid chromatography to quantify the formaldehyde derivative, which was a derivatized compound in the formaldehyde-derivatized solution. As a result, the formaldehyde concentration in A-1 was found to be 1.5 ppm.
[0230] Examples 2 to 34 The same procedure as in Example 1 was carried out, except that A-1 was changed to A-2 to A-34, and the formaldehyde concentration was quantified. The results are shown in Table 2 below.
[0231] Comparative Examples 1 to 9 The same procedure as in Example 1 was carried out, except that A-1 was changed to B-1 to B-9, and the formaldehyde concentration was quantified. The results are shown in Table 2 below.
[0232]
[0233] As is clear from the results in Table 2, the amount of formaldehyde could be significantly reduced by copolymerizing a monomer having a group represented by formula (1) with a monomer having an N-hydroxymethyl group or an N-alkoxymethyl group.
[0234] Preparation of Catalyst Solution Preparation Example 44 PTSA (1.0 g) as a catalyst and PM (19.0 g) as a solvent were added, stirred for 1 hour, and visually confirmed to be dissolved. The solution was filtered through a filter with a pore size of 0.2 μm to prepare a catalyst solution (D-1).
[0235] Preparation Example 45: PPTS (1.0 g) as a catalyst and PM (19.0 g) as a solvent were added, stirred for 1 hour, and visually confirmed to be dissolved. The solution was filtered through a filter with a pore size of 0.2 μm to prepare a catalyst solution (D-2).
[0236] Preparation Example 46: CSA (2.0 g) as a catalyst and PM (18.0 g) as a solvent were added, stirred for 1 hour, and visually confirmed to be dissolved. The solution was filtered through a filter with a pore size of 0.2 μm to prepare a catalyst solution (D-3).
[0237] <Preparation of liquid crystal aligning agent> <Example 35> To A-1 (2.00 g) obtained in Preparation Example 1, D-1 (0.12 g) obtained in Preparation Example 44 and EA (0.54 g) as a dilution solvent were added, and the mixture was stirred for 1 minute to obtain liquid crystal aligning agent AL-1.
[0238] <Examples 36 to 45, 52, 55 to 62> The same procedure as in Example 35 was performed, except that A-1 was changed to A-2 to A-11, A-18, A-21 to A-28, to obtain liquid crystal aligning agents AL-2 to 11, AL-18, AL-21 to 28. The blending amounts of the components are shown in Table 3.
[0239] Comparative Examples 10 to 15 The same procedure as in Example 35 was carried out, except that A-1 was changed to B-1 to B-6, to obtain liquid crystal aligning agents BL-1 to BL-6. The blending amounts of the components are shown in Table 3.
[0240] Example 46 To A-12 (2.00 g) obtained in Preparation Example 12, D-2 (0.12 g) obtained in Preparation Example 45 and EA (0.54 g) as a dilution solvent were added, and the mixture was stirred for 1 minute to obtain a liquid crystal aligning agent AL-12. The blending amounts of the components are shown in Table 3.
[0241] Examples 47 to 49 The same procedure as in Example 46 was carried out, except that A-12 was replaced with A-13 to A-15, thereby obtaining liquid crystal aligning agents AL-13 to AL-15. The blending amounts of the components are shown in Table 3.
[0242] Comparative Example 16 The same procedure as in Example 46 was carried out, except that A-12 was changed to B-7, to obtain a liquid crystal aligning agent BL-7. The blending amounts of the components are shown in Table 3.
[0243] Example 50 To A-16 (2.00 g) obtained in Preparation Example 16, D-3 (0.08 g) obtained in Preparation Example 46 and EA (0.5 g) and IPM (1.3 g) as dilution solvents were added, and the mixture was stirred for 24 hours to obtain liquid crystal aligning agent AL-16. The blending amounts of the components etc. are shown in Table 3.
[0244] <Examples 51, 53 to 54, 63 to 68> The same procedure as in Example 50 was performed, except that A-16 was changed to A-17, A-19 to A-20, and A-29 to A-34, thereby obtaining liquid crystal aligning agents AL-17, AL-19 to A-20, and AL-29 to A-34. The blending amounts of the components are shown in Table 3.
[0245] Comparative Examples 17-18 The same procedure as in Example 50 was carried out, except that A-16 was replaced with B-8 and B-9, to obtain liquid crystal aligning agents BL-8 and BL-9. The blending amounts of the components are shown in Table 3.
[0246] <Preparation of polymerizable liquid crystal solution for horizontal alignment> Paliocolor (registered trademark) LC-242 (manufactured by BASF Japan Ltd.) (19.3 g), which is a polymerizable liquid crystal for horizontal alignment, Omnirad (registered trademark) 907 (manufactured by IGM Resins B.V.) (0.6 g) as a photoradical initiator, and BYK (registered trademark)-361N (manufactured by BYK Japan KK) (0.1 g) as a leveling agent were added, and CPN (80 g) was further added as a solvent, followed by stirring for 2 hours and visually confirming that the mixture had dissolved, thereby obtaining a 20 mass % polymerizable liquid crystal solution (LC-1).
[0247] <Formation of Liquid Crystal Alignment Film and Preparation of Retardation Film> <Example 69> The liquid crystal alignment agent (AL-1) obtained in Example 35 was applied to a TAC film substrate using a bar coater to a wet film thickness of 4 μm. The film was dried by heating at 120°C for 1 minute in a hot air circulation oven to form a cured film on the film. Next, linearly polarized light with a wavelength of 313 nm was applied to the surface of this cured film at 10 mJ / cm. 2 A polymerizable liquid crystal solution for horizontal alignment RMS16-089 (manufactured by Merck) was applied to the liquid crystal alignment film using a bar coater to a wet film thickness of 12 μm. After drying by heating in an oven at 72°C for 1 minute, the film was irradiated with unpolarized light at a wavelength of 365 nm at 500 mJ / cm under nitrogen.2 The polymerizable liquid crystal was cured by vertical irradiation with an exposure amount of 10 ...
[0248] <Examples 70 to 78, 86, Comparative Examples 19 to 23> Using (AL-2) to (AL-10), (AL-18), (BL-1) to (BL-5) as liquid crystal aligning agents, retardation films were produced in the same manner as in Example 69.
[0249] Example 79 The liquid crystal aligning agent (AL-11) obtained in Example 45 was applied to a TAC film substrate using a bar coater to a wet film thickness of 4 μm. The film was dried by heating at 120° C. for 2 minutes in a hot air circulation oven to form a cured film on the film. Next, linearly polarized light with a wavelength of 313 nm was applied to the surface of the cured film at 20 mJ / cm. 2 The liquid crystal alignment film was then vertically irradiated with an exposure dose of 400 mJ / cm. The polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to the liquid crystal alignment film to a wet film thickness of 10 μm using a bar coater. The film was then dried by heating in an oven at 100°C for 2 minutes, and then irradiated with unpolarized light at a wavelength of 365 nm at a dose of 400 mJ / cm under nitrogen. 2 The polymerizable liquid crystal was cured by vertical irradiation with an exposure amount of 10 ...
[0250] <Examples 80 to 83, 89 to 96, Comparative Examples 24 to 25> Using (AL-12) to (AL-15), (AL-21) to (AL-28), and (BL-6) to (BL-7) as liquid crystal aligning agents, retardation films were produced in the same manner as in Example 79.
[0251] Example 84 The liquid crystal aligning agent (AL-16) obtained in Example 50 was applied to an acrylic film substrate using a bar coater to a wet film thickness of 10 μm. The film was dried by heating at 90° C. for 1 minute in a hot air circulation oven to form a cured film on the film. Next, linearly polarized light with a wavelength of 313 nm was applied to the surface of the cured film at 20 mJ / cm. 2 The liquid crystal alignment film was then vertically irradiated with an exposure dose of 500 mJ / cm. The polymerizable liquid crystal solution LC-1 for horizontal alignment was applied to the liquid crystal alignment film to a wet film thickness of 8 μm using a bar coater. The film was then dried by heating in an oven at 90°C for 1 minute, and then irradiated with unpolarized light at a wavelength of 365 nm at a dose of 500 mJ / cm under nitrogen.2 The polymerizable liquid crystal was cured by vertical irradiation with an exposure amount of 10 ...
[0252] <Examples 85, 87 to 88, 97 to 102, Comparative Examples 26 to 27> Using (AL-17), (AL-19) to (AL-20), (AL-29) to (AL-34), and (BL-8) to (BL-9) as liquid crystal aligning agents, retardation films were produced in the same manner as in Example 84.
[0253] The retardation films prepared above were evaluated by the following methods. The evaluation results are shown in Table 4.
[0254] The prepared retardation film on the substrate was sandwiched between a pair of polarizing plates, and the state of retardation property expression under crossed Nicols was visually observed. The results were recorded in the "Orientation" column as "○" when the retardation was expressed without defects, and "×" when the retardation was not expressed.
[0255] [Evaluation of Adhesion] Cross-cuts (1 mm x 1 mm x 100 squares) were made using a cutter knife on the surface of the retardation film on the prepared substrate (the surface on which the polymerizable liquid crystal layer was formed), and then cellophane tape (Cellotape (registered trademark), manufactured by Nichiban Co., Ltd., 24 mm wide) was attached. Next, when the cellophane tape was peeled off, the number of squares where the polymerized polymerizable liquid crystal layer remained on the underlying cured film and the underlying film substrate without peeling off was counted. The results were recorded in the "Adhesion" column as "Good" if the entire layer remained, "Good" if only a portion peeled off, and "Poor" if the entire layer peeled off.
[0256]
[0257] As is clear from the results in Table 4, it was found that, with regard to the properties of orientation and adhesion, even when a monomer having a group represented by formula (1) was copolymerized with a monomer having an N-hydroxymethyl group or an N-alkoxymethyl group, the properties were not deteriorated and only the formaldehyde concentration could be reduced.
Claims
1. A composition for forming a cured film, comprising: (A) a compound having a photoalignable group; (B) a polymer having a structural unit having an N-hydroxymethyl group or an N-alkoxymethyl group, and a structural unit having a partial structure represented by the following formula (1); and (D) a crosslinking catalyst. (In formula (1), Q 1 represents an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or a phenyl group; Q 2 is O, S or NQ 3 represents Q 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the dashed line represents a bond.
2. The cured film-forming composition according to claim 1, wherein the photoalignable group of the component (A) is a functional group having a structure that undergoes photodimerization or photoisomerization.
3. A cured film-forming composition according to claim 1 or 2, wherein the photoalignable group of component (A) is a cinnamoyl group.
4. The cured film-forming composition according to claim 1, wherein the photoalignable group of the component (A) is a group having an azobenzene structure.
5. The cured film-forming composition according to claim 1, further comprising an ammonium salt as component (C).
6. The cured film-forming composition according to claim 5, wherein the ammonium salt of component (C) is ammonium acetate.
7. An alignment material obtained by using the cured film-forming composition according to any one of claims 1 to 6.
8. A retardation material formed by using a cured film obtained from the cured film-forming composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Composition forming heat-cured film having photo-alignment properties
WO2011126022A1
Cured-film-forming composition, alignment material, and phase difference material
WO2015129890A1