Epoxy resin composition

The epoxy resin composition, enhanced with a core shell rubber, addresses the issue of residual stress and cracking in semiconductor encapsulation and vehicle parts by achieving excellent toughness and strength, ensuring durability under high-speed rotation conditions.

WO2024214972A1PCT designated stage expired Publication Date: 2024-10-17KCC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003346
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-03-18
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Epoxy resin compositions used in semiconductor encapsulation and vehicle parts face issues with residual stress due to differences in linear expansion coefficients and curing shrinkage, leading to interfacial peeling and cracking, especially under high-speed rotation conditions, where conventional stress relievers like carboxylic acid anhydrides and silicone oils fail to provide adequate toughness without compromising mold workability or strength.

Method used

An epoxy resin composition incorporating a core shell rubber (CSR) with a rubbery core and polymer-acrylate shell, which enhances toughness, flexural strength, and elastic modulus, while maintaining flowability and adhesion, thereby preventing cracking and peeling during high-speed rotation.

Benefits of technology

The epoxy resin composition achieves a toughness range of 25 to 100 kgf.mm, flexural strength of 9 to 17 kgf/mm², and elastic modulus of 1,500 to 2,400 kgf/mm², ensuring the material's durability and resistance to cracking, even under high-speed rotation, without compromising mold workability or strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024003346-APPB-IMG-000001
    Figure PCTKR2024003346-APPB-IMG-000001
  • Figure PCTKR2024003346-APPB-IMG-000002
    Figure PCTKR2024003346-APPB-IMG-000002
Patent Text Reader

Abstract

The present invention relates to an epoxy resin composition for molding and a vehicle part molded using same.
Need to check novelty before this filing date? Find Prior Art

Description

epoxy resin composition

[0001] The present invention relates to an epoxy resin composition and a vehicle part molded using the same.

[0002]

[0003] As semiconductor applications rapidly expand, particularly in the automotive industry, demands for semiconductor performance are increasing, and the level of reliability assessment required to meet these demands is also increasing. In response to these industrial demands, semiconductor component materials are also undergoing various developments. For example, Japanese Patent Application Laid-Open No. 2017-197620 relates to an epoxy resin composition for semiconductor encapsulation, comprising an epoxy resin, a phenolic resin curing agent, and a filler. The composition discloses a technique for improving electrical connection reliability by controlling the content of the filler and the thermoelastic modulus of the cured epoxy resin composition.

[0004] Epoxy resin compositions are excellent materials for encapsulating semiconductor devices due to their high mechanical strength, heat resistance, electrical insulation, and adhesiveness. However, there are problems in that residual stress occurs inside the encapsulating material due to differences in coefficients of linear expansion with respect to semiconductor materials or devices, curing shrinkage, or under high-temperature conditions such as reflow, resulting in interfacial peeling and cracking at the interface with the substrate or the device to be encapsulated.

[0005] Meanwhile, epoxy resin compositions can be used as molding materials for automotive components, and for example, can be used to fill or secure rotor core magnets. Molding materials for such automotive components must be able to withstand deformation or breakage due to high-speed rotation that occurs during vehicle operation. When conventional thermosetting resins are used to secure rotor core magnets, the thermosetting resin can break due to strong centrifugal force during high-speed rotation of the rotor core (over 20,000 rpm), resulting in magnet detachment.

[0006] To address these issues, technologies for applying various stress-relieving agents to epoxy resin compositions for molding are being developed. While carboxylic anhydride-based stress-relieving agents can provide a stress-reducing effect within the composition, they are difficult to disperse within the resin composition and can impair the mold workability of the resin composition. Meanwhile, silicone oils, another stress-relieving agent, can cause flow marks on the surface of the molding material as usage increases, affecting its appearance. Therefore, their usage is limited. Furthermore, silicone resins are expensive and do not offer a significant stress-reducing effect. Furthermore, while silicone powders exhibit excellent stress-reducing effects, they can lower the strength of the resin composition, potentially causing the molding material to break.

[0007] Accordingly, there is a need for development of an epoxy resin composition for molding that has excellent toughness and does not break the thermosetting resin even at high speed rotation.

[0008]

[0009] The present invention provides an epoxy resin composition for molding having excellent toughness. In addition, the present invention provides a vehicle part molded using the epoxy resin composition for molding.

[0010]

[0011] The present invention provides an epoxy resin composition comprising an epoxy resin, a curing agent, a filler, and a core shell rubber (CSR), and having a toughness of 25 to 100 kgf.mm, a flexural strength of 9 to 17 kgf / mm2, and a flexural modulus of 1,500 to 2,400 kgf / mm2.

[0012]

[0013] The present invention provides an epoxy resin composition for molding, which has excellent toughness. The epoxy resin composition according to the present invention can be used as a molding material for automotive parts. In particular, the epoxy resin composition according to the present invention has excellent toughness, making it applicable for filling or fixing rotor core magnets.

[0014]

[0015] The present invention will be described in detail below. However, the scope of the present invention is not limited solely to the details described below, and each component may be modified or selectively mixed as needed. Therefore, it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are encompassed.

[0016] As used herein, “viscosity” is measured by a conventional method known in the art, and can be measured, for example, using a Brookfield viscometer. Functional values ​​such as “hydroxyl value” are measured by a conventional method known in the art, and can be measured, for example, by a titration method. “Particle size (D50)” is measured by a conventional method known in the art, and can be measured, for example, by laser light scattering (LLS). “Glass transition temperature” is measured by a conventional method known in the art, and can be measured, for example, by thermomechanical analysis (TMA) or differential scanning calorimetry (DSC). “Softening point” is measured by a conventional method known in the art, for example, by a dropping point system calorimetry DP70 from Mettler Toledo.

[0017]

[0018] Epoxy resin composition

[0019] An epoxy resin composition according to the present invention comprises an epoxy resin, a curing agent, a filler, and a core shell rubber (CSR).

[0020] The toughness of the epoxy resin composition according to the present invention is 25 to 100 kgf.mm, for example, 40 to 80 kgf.mm, or as another example, 50 to 70 kgf.mm. For example, the toughness can be measured according to ASTM D790, and can be determined by the area of ​​the triangle of the maximum load (stress (kgf)) and maximum displacement (strain (mm)) graph that occur during a three-point curvature test. The maximum load is the maximum load applied at the moment when the specimen breaks during the three-point curvature test, and the maximum displacement is the maximum distance that the specimen bends just before breaking during the three-point curvature test. If the toughness is less than the above-mentioned range, cracks may occur in the epoxy molding compound (EMC) due to strong centrifugal force during high-speed rotation, and as a result, when it is used to fill or fix a core magnet (rotor core magnet), the magnet may be detached. In order to manufacture an epoxy resin composition having properties exceeding the aforementioned range, the type and content of the filler must be controlled. For this purpose, if a filler made of fiber material such as glass fiber is used, the filling properties, adhesion, and workability may be reduced.

[0021] The flexural strength of the epoxy resin composition according to the present invention is 9 to 17 kgf / mm2, for example, 10 to 16 kgf / mm2, and as another example, 11 to 15 kgf / mm2. For example, the flexural strength can be measured according to ASTM D790, and can be determined as the force at the breaking point (maximum load) when a force is applied to the center point at a set speed. If the flexural strength is less than the above-mentioned range, the resin may break, and in order to manufacture an epoxy resin composition having a flexural strength exceeding the above-mentioned range, the type and content of the filler must be adjusted, in which case flowability, filling property, etc. may be reduced.

[0022] The flexural modulus of the epoxy resin composition according to the present invention is 1,500 to 2,400 kgf / ㎟, for example, 1,600 to 2,300 kgf / ㎟, or as another example, 1,650 to 2,000 kgf / ㎟. For example, the flexural modulus can be measured according to ASTM D790, and can be determined by the slope of the maximum load (stress (kgf)) and maximum displacement (strain (mm)) graph that occurs during a three-point curvature test. If the flexural modulus is less than the above-mentioned range, ductility may increase, which may cause problems in workability after molding, and if it exceeds the above-mentioned range, brittle characteristics may increase, which may cause easy breakage.

[0023] The glass transition temperature of the epoxy resin composition according to the present invention may be 150 to 250°C, for example, 170 to 220°C.

[0024] The epoxy resin composition of the present invention can be manufactured in a powder form, a granule form, or a sheet form, depending on the mode of use.

[0025]

[0026] epoxy resin

[0027] In the present invention, epoxy resin is used as a main resin, and after reacting with a curing agent and curing, forms a three-dimensional network structure, thereby imparting strong and solid adhesion properties and heat resistance to an adherend.

[0028] As the epoxy resin, an epoxy resin commonly used in the relevant technical field can be used, and for example, one containing two or more epoxy groups in its molecular structure can be used. Non-limiting examples of epoxy resins that can be used include bisphenol A type epoxy resin, alicyclic epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, non-condensed ring type polycyclic structure epoxy resin, bisphenol fluorene modified epoxy, etc., and one or more of these can be included.

[0029] The epoxy resin may be one having an epoxy equivalent weight (EEW) of 50 to 350 g / eq, for example, 150 to 250 g / eq, a viscosity (150°C) of 1 to 20 poise, for example, 2 to 10 poise, and a softening point of 60 to 80°C, for example, 65 to 70°C. An epoxy resin satisfying the above-described properties has relatively low viscosity characteristics, so that even when a high content of filler is included, flowability can be secured and mixing is easy. If the softening point of the epoxy resin exceeds the above-described range, the high viscosity may cause insufficient flowability, which may result in underfilling and undermolding problems, and if it is below the above-described range, bleed, flush, etc. may occur, which may deteriorate workability.

[0030] Based on the total weight of the epoxy resin composition, the content of the epoxy resin may be 5 to 30 wt%, for example, 10 to 20 wt%. If the content of the epoxy resin is less than the above-mentioned range, adhesion, flowability, and moldability may be reduced, and if it exceeds the above-mentioned range, the reliability of the molding material may be deteriorated due to an increase in moisture absorption, and the strength may be reduced due to a relative decrease in the filler content.

[0031]

[0032] hardener

[0033] The epoxy resin composition according to the present invention includes a curing agent. The curing agent reacts with the epoxy resin to promote curing of the composition.

[0034] The curing agent may be any curing agent known in the art that undergoes a curing reaction with an epoxy resin. For example, the curing agent may be a phenol-based compound having two or more phenolic hydroxyl groups in one molecule. For example, the curing agent may include at least one selected from the group consisting of a phenol novolac resin, a cresol novolac resin, a phenol aralkyl resin, and a polyfunctional phenol compound.

[0035] The curing agent may be one having a hydroxyl equivalent of 50 to 300 g / eq, for example, 80 to 150 g / eq, a viscosity (150°C) of 0.1 to 30 poise, for example, 1 to 10 poise, an electrical conductivity of 15 μS / cm or less, for example, 9 μS / cm or less, a volatile content of 1% or less, for example, 0.2% or less, and a softening point of 70 to 90°C, for example, 75 to 88°C. If the hydroxyl equivalent of the curing agent exceeds the above-mentioned range, the glass transition temperature may be lowered, and if the viscosity exceeds the above-mentioned range, the hardness of the cured epoxy material may be lowered. In addition, if the electrical conductivity of the curing agent exceeds the above-mentioned range, heat dissipation may be lowered, voids may occur, and if the softening point exceeds the above-mentioned range, rigidity may be increased, which may cause breakage.

[0036] Based on the total weight of the epoxy resin composition, the content of the curing agent may be 1 to 30 wt%, for example, 5 to 15 wt%. If the content of the curing agent is less than the above-mentioned range, curability and moldability may be reduced, and if it exceeds the above-mentioned range, the reliability of the molding material may be deteriorated and the strength may be reduced due to increased moisture absorption.

[0037]

[0038] filler

[0039] The epoxy resin composition according to the present invention includes a filler. The filler serves to improve the strength and flowability of the epoxy resin composition.

[0040] As the filler, any filler commonly used in the relevant technical field can be used without limitation. For example, inorganic fillers such as silica, silica nitride, alumina, aluminum nitride, and boron nitride can be used, and these can be used alone or in combination of two or more. The shape of the filler is not particularly limited, and both angular and spherical shapes can be used.

[0041] The above filler may include two types of fillers having different particle sizes. For example, the filler may include a first filler having an average particle size (D50) of 3 to 14 μm, for example, 7 to 14 μm, and a second filler having an average particle size (D50) of 14.5 to 30 μm, for example, 14.5 to 21.5 μm.

[0042] Based on the total weight of the epoxy resin composition, the content of the filler may be 40 to 90 wt%, for example, 50 to 90 wt%. If the content of the filler is less than the above-mentioned range, the moisture absorption in the cured product of the epoxy resin composition may increase, which may lower the reliability of the molding material. If the content of the filler exceeds the above-mentioned range, the fluidity may decrease, resulting in poor moldability.

[0043]

[0044] Core shell rubber (CSR)

[0045] The epoxy resin composition according to the present invention comprises a core-shell rubber (CSR). The CSR of the present invention functions as a stress reliever, maintaining strength while reducing modulus, thereby improving the toughness, flexural strength, and bending strength of the thermosetting resin, thereby exhibiting excellent effects in preventing breakage.

[0046] The above core may be a core having rubber elasticity but insoluble in epoxy resin, and may include, for example, butadienes such as polybutadiene, isoprene, and chloroprene, butadiene copolymers such as butadiene-styrene, (meth)acrylates such as butyl (meth)acrylate, 2-ethylhexyl acrylate, and lauryl methacrylate, or silicone rubber, and may include these alone or in combination of two or more.

[0047] The above shell serves to improve the affinity between the epoxy resin and the components constituting the core, and may be formed in a form in which it is graft polymerized (bonded) to the core. In order to be stably dispersed in the epoxy resin composition, the shell may be one having swelling properties, compatibility, or affinity with the epoxy resin. For example, the shell may include a (meth)acrylate polymer such as polymethyl(meth)acrylate (PMMA), an acrylate copolymer with styrene, etc., and may include these alone or in combination of two or more. The (co)polymer constituting the shell may be surface-treated with an organic or inorganic functional group to improve dispersibility. Non-limiting examples of the organic or inorganic functional groups include organic functional groups such as a hydroxyl group, a methyl group, an ethyl group, and the like, and inorganic functional groups such as a silane group.

[0048] For example, the core shell rubber (CSR) has a core made of a material having rubber elasticity such as silicone rubber, and a shell made of an organic component such as polymethyl(meth)acrylate (PMMA). The shell has excellent compatibility, thereby improving the affinity between the epoxy resin and the components constituting the core, and can be formed in a form in which it is graft-polymerized (bonded) to the core, thereby improving the bonding strength with the resin and thus improving the dispersibility. The silicone rubber of the core can impart flexibility to the epoxy resin composition, thereby lowering the modulus and thereby improving the toughness.

[0049] The particle size (D50) of the core-shell rubber (CSR) may be 45 μm or less, for example, 1 to 25 μm. When a core-shell rubber (CSR) having a particle size (D50) within the aforementioned range is applied, the dispersibility is improved and the modulus of the epoxy resin composition is lowered, thereby improving the toughness. When the particle size exceeds the aforementioned range, the dispersibility is reduced, and cracks or peeling may occur as force is concentrated on the part where the particles are aggregated. In addition, the low-stress characteristics may not be sufficiently expressed due to the aggregated particles, and mechanical properties such as strength may be reduced.

[0050] The glass transition temperature of the core shell rubber (CSR) may be -200 to -50°C, for example, -140 to -120°C. If the glass transition temperature of the core shell rubber (CSR) is below the above-mentioned range, the flexural strength of the epoxy resin composition may be poor, and if it exceeds the above-mentioned range, the flexural modulus of the epoxy resin composition may be poor. As a result, the toughness of the epoxy resin composition may be reduced, which may cause cracks to occur in the epoxy molding compound (EMC), and when it is used to fill or fix a core magnet (Rotor core magnet), the magnet may be detached.

[0051] Based on the total weight of the epoxy resin composition, the content of the core shell rubber (CSR) may be 0.01 to 10 wt%, for example, 1 to 5 wt%. If the content of the core shell rubber (CSR) is less than the above-mentioned range, the low-stress effect and the toughness strengthening effect may not be sufficiently expressed, and if it exceeds the above-mentioned range, mechanical properties such as strength may decrease, or thermal characteristics such as glass transition temperature and thermal expansion coefficient may become inferior.

[0052]

[0053] additives

[0054] The epoxy resin composition according to the present invention may further include additives commonly used in the relevant technical field, such as an adhesion enhancer, a release agent, a catalyst, a colorant, a flame retardant, etc., as needed.

[0055] As an adhesion enhancer to improve the bonding between organic and inorganic materials and the adhesion to a metal substrate, epoxy silane, amino silane, mercapto silane, acrylic silane, vinyl silane, etc. can be used, and as a release agent to improve the releasability between the epoxy molding compound (EMC) and the external mold, long-chain fatty acids, metal salts of long-chain fatty acids, paraffin wax, carnauba wax, polyethylene wax, etc. can be used. In addition, imidazole compounds, amine compounds, organic phosphine compounds, etc. can be used as a curing accelerator to improve the curing speed and workability. In addition, additives such as a coloring agent (e.g., carbon black, Bengala, etc.) and a flame retardant (e.g., metal hydroxide, etc.) to provide color to the resin composition can be further included.

[0056] The above additives may be added within a content range known in the relevant technical field, and for example, may be included in an amount of 0.01 to 10 wt%, respectively, based on the total weight of the epoxy resin composition, but is not limited thereto.

[0057]

[0058] Semiconductor devices and automotive components

[0059] The present invention provides a vehicle component molded using the aforementioned epoxy resin composition. For example, the aforementioned epoxy resin composition can be used as a molding material to secure and seal components within a vehicle component requiring excellent vibration resistance, heat resistance, dimensional stability, and deformation resistance.

[0060] For example, a permanent magnet can be inserted into a hollow space formed within a rotor core, and the epoxy resin composition of the present invention can be filled between the hollow space and the permanent magnet to fix the permanent magnet within the rotor core.

[0061]

[0062] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are intended only to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0063]

[0064] [Experimental Example 1-9]

[0065] Each epoxy resin composition for each experimental example was prepared by mixing each component according to the composition described in Table 1 below. The physical properties of each resin composition were measured using the following method, and the results are described in Table 1 below.

[0066]

[0067] Sample manufacturing

[0068] A mixture of the epoxy resin composition manufactured in each experimental example was molded at 175°C for 120 seconds using a transfer molding method to manufacture a specimen for evaluating physical properties.

[0069]

[0070] toughness

[0071] It was measured according to ASTM D790, and 4 specimens of 125 mm x 12.5 mm x 6 mmT were prepared, and the area of ​​the triangle of the maximum load (stress (kgf)) and maximum displacement (strain (mm)) graph that occurs during the UTM (Universal test machine) 3-point bending test was calculated to evaluate the toughness (Support span distance: 100 mm, Crosshead speed: 2.8 mm / min). The maximum load is the maximum load applied at the moment the specimen breaks during the 3-point bending test, and the maximum displacement is the maximum distance the specimen bends just before breaking during the 3-point bending test.

[0072]

[0073] Flexural strength

[0074] According to ASTM D790, the flexural strength was evaluated by measuring the force at the breaking point (maximum load) when force was applied to the center point at a given speed.

[0075]

[0076] Flexural modulus

[0077] It was measured according to ASTM D790, and the flexural modulus was evaluated by measuring the slope of the maximum load (stress (kgf)) and maximum displacement (strain (mm)) graph that occurred during the three-point curvature test.

[0078]

[0079]

[0080] Epoxy resin: O-cresol novolac type, epoxy equivalent 200 g / eq, viscosity (150 ℃) 7 poise, softening point 67 ℃

[0081] Hardener: phenol resin, hydroxyl equivalent 120 g / eq, viscosity (150 ℃) 6 poise, electrical conductivity 5 ㎲ / ㎝, volatile matter 0.1%, softening point 83 ℃

[0082] Filler: Mixture of spherical and angular silica with an average particle size (D50) of 19.9 ㎛

[0083] CSR-A: Silicone core, polymethyl(meth)acrylate (PMMA) shell, particle size (D50) 10 μm, Tg -130 ℃

[0084] CSR-B: Silicon core, PMMA shell, particle size (D50) 20 μm, Tg -45 ℃

[0085] CSR-C: Silicon core, PMMA shell, particle size (D50) 50 μm, Tg -65 ℃

[0086] Silicone powder: particle size (D50) 5 ㎛

[0087] Silane: Epoxy silane (Boiling point 190 ℃)

[0088] Wax: polyethylene wax (acid value 15-30 mgKOH / g)

[0089] Colorant: carbon black with an average particle size of 20 nm

[0090] Catalyst: Imidazole series (2MZ, Shikoku Chemical)

[0091] Flame retardant: Mg-based inorganic flame retardant

[0092]

[0093] [Physical property evaluation]

[0094] The physical properties of the epoxy resin composition manufactured in each experimental example were measured as follows, and the results are shown in Table 2 below.

[0095]

[0096] Spiral flow

[0097] Flowability was measured using a transfer molding press (175°C, 70 kgf / cm2) using an evaluation mold according to EMMI-1-66. It is desirable to secure a flowability of 30 inches or more so that the EMC can flow to the slot area where the magnet is inserted in the rotor core and fill the space.

[0098]

[0099] G / T

[0100] After setting the temperature (175°C) to the same temperature as the mold press using a hot plate, the time from the melting point to the gelation point of each specimen was measured. To ensure the time required for the EMC to fill the slot area, it is desirable to secure a gel time of 15 seconds or more.

[0101]

[0102] Glass transition temperature / coefficient of linear expansion

[0103] Specimens of the same size were molded and measured from room temperature to 300℃ at a heating rate of 10℃ / min using a TMA (Thermo-mechanical Analyzer), and the glass transition temperature was obtained using the onset point technique. Considering the heat generated during high-speed rotation of the rotor core, it is desirable to secure a glass transition temperature of 170℃ or higher. In this case, the shrinkage / expansion due to the temperature rise and cooling process can be minimized, thereby preventing the occurrence of cracks in the EMC.

[0104] In addition, the linear expansion coefficient α1 below the glass transition temperature and the linear expansion coefficient α2 above the glass transition temperature were measured using a TMA (Thermomechanical Analyzer). When a1 is 20 ppm / ℃ or less and a2 is 80 ppm / ℃ or less, peeling and cracking due to shrinkage / expansion can be effectively prevented.

[0105]

[0106] Ag delamination

[0107] TO-247 packages were formed using MGP (Multi-gang pot) equipment with Ag-plated general-purpose lead frames. The formed packages were post-cured and subjected to 260°C IR reflow processes five times. Internal delamination was confirmed using SAT (Scanning Acoustic Tomography), and the results were evaluated as excellent (◎), good (○), average (△), or poor (X).

[0108]

[0109] Magnet detachment / breakage

[0110] After molding the magnet slot of the rotor core using the epoxy resin composition of each experimental example, the maximum load (kgf) applied until the magnet was detached from the slot was measured using a UTM facility. A maximum load of 50 kgf or more was judged as passing, and the EMC area was observed for incomplete filling and breakage, and evaluated as excellent (◎), good (○), average (△), or poor (X).

[0111]

[0112]

[0113] As shown in Table 2 above, the epoxy resin compositions of Experimental Examples 1-3 according to the present invention exhibited excellent physical properties across all measured items. On the other hand, the epoxy resin compositions of Experimental Examples 4 and 5, in which the flexural modulus was outside the range of the present invention, and the epoxy resin compositions of Experimental Examples 6 and 7, in which the toughness and flexural strength were outside the range of the present invention, exhibited generally inferior physical properties compared to Experimental Examples 1-3. In addition, when the epoxy resin compositions of Experimental Example 8, which included silicone powder instead of core-shell rubber, and Experimental Example 9, which did not include core-shell rubber, were used, the magnet was easily detached from the slot. In particular, in the case of the epoxy resin composition of Experimental Example 9, Ag peeling and cracking of the EMC portion were also observed.

[0114]

[0115] The present invention provides an epoxy resin composition for molding having excellent toughness and a vehicle part molded using the epoxy resin composition for molding.

[0116]

[0117]

Claims

1. Contains epoxy resin, hardener, filler and core shell rubber (CSR). An epoxy resin composition having a toughness of 25 to 100 kgf.mm, a flexural strength of 9 to 17 kgf / ㎟, and a flexural modulus of 1,500 to 2,400 kgf / ㎟.

2. An epoxy resin composition according to claim 1, wherein the epoxy resin has an epoxy equivalent weight (EEW) of 50 to 350 g / eq, a viscosity (150°C) of 1 to 20 poise, and a softening point of 60 to 80°C.

3. An epoxy resin composition according to claim 1, wherein the curing agent has a hydroxyl equivalent of 50 to 300 g / eq, a viscosity (150°C) of 0.1 to 30 poise, an electrical conductivity of 15 μs / cm or less, a volatile content of 1% or less, and a softening point of 70 to 90°C.

4. In the first paragraph, the core of the core shell rubber (CSR) includes at least one selected from the group consisting of butadienes, butadiene copolymers, (meth)acrylates, and silicone rubber. An epoxy resin composition comprising a shell comprising at least one selected from the group consisting of (meth)acrylate polymers and styrene and acrylate copolymers.

5. An epoxy resin composition in the first paragraph, wherein the particle size (D50) of the core shell rubber (CSR) is 45 ㎛ or less and the glass transition temperature is -200 to -50 ℃.

6. An epoxy resin composition comprising 5 to 30 wt% of the epoxy resin, 1 to 30 wt% of the hardener, 40 to 90 wt% of the filler, and 0.01 to 10 wt% of the core shell rubber (CSR) based on the total weight of the epoxy resin composition in the first paragraph.

7. A vehicle part molded using an epoxy resin composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Epoxy resin composition and cured product thereof

    JP2013209503A

  • Epoxy resin composition and electric power equipment using the same

    JP2015168701A

  • Epoxy resin composition

    JP2023032370A

  • Partial swivel device for seat of vehicle

    KR1020200133454A

  • Bogie for railway wagons for high-load and high-speed transportation

    KR1020240001295A