Mgagsb thermoelectric material, preparation method therefor, and use thereof
By optimizing the formation energy and preparation process of MgAgSb thermoelectric materials, the problem of insufficient performance of magnesium silver antimony and magnesium bismuth antimony based thermoelectric materials has been solved, achieving efficient thermoelectric performance improvement and cost reduction, and promoting the commercialization of all magnesium based thermoelectric devices. application.
Patent Information
- Application Number
- PCT/CN2023/088954
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Existing thermoelectric materials, especially bismuth telluride-based materials, are high in cost and have low power generation efficiency at temperatures above 300°C, which limits the further large-scale use and performance improvement of thermoelectric devices, and magnesium silver antimony and magnesium bismuth antimony based materials Thermoelectric materials have insufficient performance when constructing all-magnesium-based thermoelectric components, which affects commercial applications.
The formation energy of MgAgSb thermoelectric materials was optimized through first-principles calculations, and a synchronous transmission high-energy ball mill and an annealing process of 310±2°C were used to prepare pure-phase MgAgSb materials, improve their carrier mobility and power factor, and combine hard High-quality alloy ball milling and thermocouples monitor temperature to enhance the thermoelectric properties of materials.
Achieved high thermoelectric figure of merit of MgAgSb thermoelectric materials at room temperature and high temperature, significantly improved carrier mobility and power factor, broke the performance bottleneck of magnesium silver antimony based thermoelectric materials, reduced costs, and has great potential for commercial application, surpassing tellurium Performance of bismuth based thermoelectric devices.
Smart Images

Figure CN2023088954_24102024_PF_FP_ABST
Abstract
Description
A MgAgSb thermoelectric material and its preparation method and application Technical Field
[0001] The present invention belongs to the technical field of thermoelectric materials, and in particular relates to a MgAgSb thermoelectric material and a preparation method and application thereof. Background Art
[0002] Thermoelectric materials can convert heat into electricity. Thermoelectric components fabricated from them are characterized by light weight, compact size, pollution-free operation, simple structure, noiselessness, long service life, and suitability for use in extreme environments such as the deep sea and space. These materials are crucial for addressing current energy crises and environmental pollution challenges, and are receiving significant attention worldwide.
[0003] The world's current energy structure is still dominated by fossil fuels. Nearly 60% of the energy generated by fossil fuel combustion is lost as waste heat, with more than half of this waste heat occurring below 300°C. Furthermore, computer chips and 5G optical communication modules operate at temperatures between 60°C and 110°C, driving the demand for cooling systems to higher temperatures. Therefore, the development and application of near-room temperature (<300°C) thermoelectric materials and components for power generation and cooling have become crucial.
[0004] In recent years, with the continuous discovery of new thermoelectric materials and the development of device construction technology, the performance of thermoelectric materials and thermoelectric components has been gradually improved. At present, thermoelectric components can be commercialized to a certain extent, among which bismuth telluride-based thermoelectric devices are particularly outstanding. However, since bismuth telluride materials contain some scarce and toxic elements, the preparation cost is high, and the power generation efficiency is low within 300°C, which greatly limits the further large-scale use of this material in thermoelectric devices. Therefore, the development of new thermoelectric materials with excellent performance and the construction of corresponding high-performance thermoelectric devices are strategic needs for the development of the entire thermoelectric field, and are also the core issue in breaking through the current performance bottleneck of thermoelectric devices.
[0005] Since their discovery, magnesium-silver-antimony (Mg-Ag-Sb) and magnesium-bismuth-antimony (Mg-Bi-Sb) alloys have become a research hotspot in the field of thermoelectric materials. Through in-depth research and various approaches, researchers have significantly improved the thermoelectric figure of merit (M2M) of n-type Mg-Bi-Sb-based thermoelectric materials, reaching a room-temperature M2M of 0.9. However, compared to n-type Mg-Bi-Sb-based thermoelectric materials, p-type Mg-silver-antimony thermoelectric materials have not achieved a breakthrough in room-temperature M2M since 2014, when they were reported to reach 0.9 and a peak of 1.4. Furthermore, reports of fully magnesium-based thermoelectric components constructed from Mg-silver-antimony and Mg-bismuth-antimony alloys remain rare.
[0006] Currently, thermoelectric devices widely used in automotive air-conditioning seats, environmentally friendly refrigerators, high-power chips, etc. still use traditional bismuth telluride-based thermoelectric materials. However, compared with magnesium-silver-antimony and magnesium-bismuth-antimony-based thermoelectric materials, bismuth telluride-based thermoelectric materials are too expensive, and the prices of raw materials such as tellurium and bismuth are much higher than those of raw materials such as magnesium-silver-antimony. Before the discovery of high-performance magnesium-based thermoelectric materials, bismuth telluride-based thermoelectric materials were an irreplaceable choice for the application of thermoelectric cooling and power generation devices. With continuous research, the performance of magnesium-based thermoelectric materials is gradually improving. At room temperature, the performance is comparable to that of bismuth telluride-based thermoelectric materials, and at high temperature, it surpasses bismuth telluride. This provides a basis and possibility for the application of magnesium-based thermoelectric materials in thermoelectric power generation and cooling devices.
[0007] However, to integrate new thermoelectric materials into devices, good thermoelectric properties alone are far from enough. They also need to be constructed into thermoelectric components with excellent performance before they can be further assembled into thermoelectric power generation and cooling systems. To date, all-magnesium-based thermoelectric components constructed from magnesium-silver-antimony and magnesium-bismuth-antimony-based thermoelectric materials have far from adequate power generation and cooling performance. This is mainly due to the low performance of the p-type magnesium-silver-antimony-based thermoelectric materials used, which has hampered the commercial application of all-magnesium-based thermoelectric devices.
[0008] The inventor of this application previously disclosed a thermoelectric material in US Pat. No. 20160326615A1, which was prepared by processing raw material powders using ball milling and hot pressing processes to prepare a thermoelectric material including MgAgSb, MgAg 0.97 Sb 0.99 As well as materials that replace Mg, Ag and Sb with other elements, in order to obtain thermoelectric figure of merit zT suitable for thermoelectric applications. According to the patent, some impurity phase peaks were found in the XRD spectrum of MgAgSb. Phase analysis identified that they may be Sb and Ag-Sb related impurity phases. Therefore, in order to eliminate impurities and obtain pure phase samples, according to the chemical formula MgAg 0.97 Sb 0.99 By removing some Ag and Sb, the pure phase sample MgAg was obtained. 0.97 Sb 0.99 , and then Mg, Ag and Sb were further substituted based on this composition.
[0009] According to the records of US20160326615A1, the material prepared according to the disclosed method, the thermoelectric figure of merit zT of the material with the stoichiometric composition of MgAgSb at 300K is about 0.5; MgAg 0.97 Sb 0.99The zT value of the composition reaches about 0.7 at 300K and about 1.2 at 450K. The grain size in the SEM image is less than 200nm, and the crystallite size in the TEM image is 10-20nm, showing a mosaic microstructure. 0.97 Sb 0.99 All materials showed an improvement in thermoelectric figure of merit, among which nickel-doped MgAg 0.965 Ni 0.005 Sb 0.99 It has the highest zT value, achieving a zT of about 1 at 325K and a peak zT of about 1.4 at 450K.
[0010] On the basis of the above work, the inventors of the present application have been committed to further improving the performance of MgAgSb-based thermoelectric materials for near-room temperature refrigeration and power generation applications for many years.
[0011] Summary of the Invention
[0012] The purpose of the present invention is to further improve the performance of MgAgSb thermoelectric materials by calculating the principle, adjusting the preparation process and adjusting the material composition, so as to save material costs, improve economic benefits and promote the commercial application of thermoelectric components prepared from magnesium-silver-antimony and magnesium-bismuth-antimony based thermoelectric materials.
[0013] Based on the previous research results, the inventors have studied the 0.97 Sb 0.99 The formation energy of two magnesium-silver-antimony-based thermoelectric materials was calculated using first-principles methods. The calculation process included: (1) using the finite displacement method to calculate the dynamic matrix and thus complete the phonon spectrum calculation, using a supercell size of 2×2×1; (2) constructing the atomic vacancies in the system with the virtual crystal approximation, and using the AkaiKKR software package to complete the formation energy calculation. The software uses the Green's function method to solve the Kohn-Sham equation; the calculation uses the scalar mode to solve the Dirac equation to obtain the core state and valence state of the electron; the exchange potential is simulated using the MJW (Moruzzi, Janak and Williams) method; the experimentally measured lattice parameters are used in the calculation of the formation energy, and the atomic positions are obtained according to the symmetry.
[0014] The first-principles calculations above show that the phonon spectrum of α-MgAgSb has a small amount of imaginary frequency, indicating that its structural dynamics energy is higher, while MgAg 0.97 Sb 0.99 The system has no imaginary frequency, indicating that the formation of Ag and Sb vacancies enhances the stability of the system, as shown in Figures 18 and 19. The formation energy calculation shown in Figure 20 shows that the MgAgSb material is better than MgAg 0.97 Sb 0.99The formation energy of the material is 228Ry higher, which further indicates that MgAgSb material is less likely to form a pure alloy phase from the perspective of structural dynamics.
[0015] A first aspect of the present invention provides a method for preparing a MgAgSb thermoelectric material, the method comprising:
[0016] (1) placing the raw materials in a stoichiometric ratio according to the chemical formula MgAg into a ball mill, and using a synchronous transmission high-energy ball mill to obtain a uniform powder;
[0017] (2) adding Sb according to the chemical formula MgAgSb to the powder obtained in step (1), and continuing to ball mill using a synchronous transmission high-energy ball mill to obtain a mixture powder;
[0018] (3) sintering the mixture powder obtained in step (2) into a bulk material;
[0019] (4) Annealing the bulk material obtained in step (3) at a temperature of 310±2°C for 12 to 30 hours.
[0020] After extensive experimental research, the inventors of the present invention have found that, compared with the traditional belt-driven ball milling method, the operation of the synchronous transmission high-energy ball mill described in steps (1) and (2) is more stable and efficient, which is conducive to the formation of the pure alloy phase of MgAgSb; combined with the annealing treatment at the critical phase transition temperature of 310±2°C in step (4), a pure phase MgAgSb material with larger grains and fewer defects is obtained. Based on the above findings, the present invention has achieved a major breakthrough in the performance of p-type magnesium-silver-antimony-based thermoelectric materials: since the report in 2014 that the room temperature thermoelectric figure of merit of p-type magnesium-silver-antimony thermoelectric materials reached 0.9 and the peak value after doping reached 1.4, there has been no breakthrough to date; however, the present invention has obtained a pure phase MgAgSb material that has not been obtained in previous studies by adopting the above preparation process, and its carrier mobility in the undoped state can reach 93.3 cm 2 V -1 s -1 , the power factor can reach 25μW cm -1 K -2 The room temperature thermoelectric figure of merit zT is 0.97, and zT reaches 1.6 at 250℃ (the traditionally reported room temperature zT of laboratory spark plasma sintered samples is 0.7, and zT is 1.2 at 250℃).
[0021] According to a preferred embodiment of the present invention, carbide balls are used in the ball milling process described in steps (1) and (2). The inventors have found that for MgAgSb materials, the use of carbide balls made of materials such as tungsten steel for ball milling can further improve the thermoelectric properties of the material compared to the use of traditional stainless steel balls. It is believed that this may be because the use of a synchronous transmission high-energy ball mill and carbide balls improves the ball milling energy and ball milling stability while avoiding cold welding of the material on the wall of the ball mill during the high-energy mechanical alloying process.
[0022] According to the preparation method provided by the present invention, the ball milling time in steps (1) and (2) can be independently 8 to 12 hours.
[0023] In a preferred embodiment, the mass of the cemented carbide ball is 2 to 30 grams, preferably 8 to 15 grams; the radius of the cemented carbide ball can be 2 to 20 mm, preferably 8 to 15 mm.
[0024] According to the preparation method provided by the present invention, the sintering conditions in step (3) may include: heating to 275-290° C. at a rate of 20-80° C. / min under a pressure of 10-100 MPa, and keeping the temperature for 1-30 minutes.
[0025] According to a preferred embodiment of the present invention, the annealing process in step (4) may include: heating the bulk material to a temperature of 310±2°C at a rate of 2-10°C / min, keeping the temperature at this temperature for 20-25 hours, and then cooling to room temperature.
[0026] The inventors discovered that in conventional annealing processes for preparing MgAgSb-based materials, the furnace temperature is simply set at approximately 300°C without monitoring or considering the material's own temperature. This may be a significant factor in the failure to obtain pure-phase MgAgSb materials and the resulting small grain size. Therefore, the present invention innovatively employs a thermocouple in contact with the material to monitor the material's temperature. This temperature is then used to control the heat supply within the furnace, maintaining the bulk material temperature at 310±2°C during annealing.
[0027] A second aspect of the present invention provides a magnesium-silver-antimony-based thermoelectric material, which is a MgAgSb thermoelectric material prepared by the above-mentioned preparation method, wherein the magnesium-silver-antimony-based thermoelectric material is a pure-phase MgAgSb material.
[0028] According to the magnesium-silver-antimony-based thermoelectric material provided by the present invention, the thermoelectric figure of merit zT of the pure phase MgAgSb material is 0.97-1.6 at 25° C.-250° C.
[0029] According to the magnesium-silver-antimony-based thermoelectric material provided by the present invention, the carrier mobility of the pure phase MgAgSb material is about 93.3 cm 2 V -1 s -1 .
[0030] Preferably, the power factor of the pure phase MgAgSb material is about 25 μW cm -1 K -2 .
[0031] The third aspect of the present invention provides the use of the MgAgSb thermoelectric material or the MgAgSb thermoelectric material prepared according to the method of the present invention in thermoelectric components for thermoelectric power generation and refrigerators.
[0032] According to the application provided by the present invention, the thermoelectric component is preferably a fully magnesium-based thermoelectric component, which includes a p-type magnesium-silver-antimony thermoelectric material and an n-type magnesium-bismuth-antimony-based thermoelectric material, wherein the p-type magnesium-silver-antimony thermoelectric material is the magnesium-silver-antimony-based thermoelectric material provided by the present invention or the magnesium-silver-antimony-based thermoelectric material prepared according to the preparation method of the present invention.
[0033] The thermoelectric component prepared by the present invention, which is composed of a p-type magnesium-silver-antimony thermoelectric material and an n-type magnesium-bismuth-antimony-based thermoelectric material, can achieve the cooling performance of existing bismuth telluride-based thermoelectric components, far surpassing the power generation performance of existing bismuth telluride-based thermoelectric components, while achieving a significant reduction in cost.
[0034] BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings, in which:
[0036] FIG1 is a diagram showing the grain size of the MgAgSb material obtained in step (3) of Example 1 of the present invention before annealing.
[0037] FIG2 is a diagram showing the grain size of the MgAgSb material after annealing in step (4) of Example 1 of the present invention.
[0038] FIG3 is a comparison photograph of the Hi-Energy / Mill 8000D synchronous drive high energy ball mill (a) used in Example 1 of the present invention and the SPEX 8000D Mixer / Mill belt drive ball mill (b) used in Comparative Example 1.
[0039] FIG4 is an X-ray diffraction (XRD) comparison chart of the MgAgSb mixture powder prepared in step (2) of Example 1 of the present invention and the MgAgSb mixture powder prepared in Comparative Example 1 and the MgAgSb standard peak.
[0040] FIG5 is a graph comparing the yields of the MgAgSb mixture powder prepared by a synchronous drive high-energy ball mill in Example 1 of the present invention and the MgAgSb mixture powder prepared by a belt drive ball mill in Comparative Example 1.
[0041] Figure 6 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 Comparison of carrier concentration and mobility of the material and the MgAgSb material prepared in Example 1 before and after annealing.
[0042] Figure 7 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The conductivity comparison chart of the material and the MgAgSb material prepared in Example 1 before and after annealing.
[0043] Figure 8 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The relationship between the lower Seebeck coefficient and temperature of the MgAgSb material prepared in the material and Example 1 before and after annealing.
[0044] Figure 9 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 Comparison of the thermal conductivity and lattice thermal conductivity of the material and the MgAgSb material prepared in Example 1 before and after annealing as a function of temperature.
[0045] Figure 10 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 Comparison of the change of thermoelectric figure of merit zT of the material and the MgAgSb material prepared in Example 1 with temperature before and after annealing.
[0046] FIG11 is a comparison diagram of the thermoelectric figure of merit zT of the MgAgSb material of the present invention and two MgAgSb samples reported in the literature as a function of temperature.
[0047] FIG12 is a comparison diagram of the electrical conductivity and Seebeck coefficient of the MgAgSb material in Comparative Example 3 after annealing at different temperatures.
[0048] FIG13 is a comparison diagram of the power factors of the MgAgSb material in Comparative Example 3 after annealing at different temperatures.
[0049] FIG14 is a graph showing the thermoelectric power generation efficiency of the all-magnesium-based device prepared in Example 2 of the present invention as a function of the hot end temperature.
[0050] FIG15 is a graph showing the variation of thermoelectric power generation efficiency of existing all-magnesium-based devices with hot-end temperature as reported in the literature.
[0051] FIG16 is a graph showing the change in cooling temperature difference of the all-magnesium-based device as a function of the hot end temperature, obtained in Example 2 of the present invention.
[0052] FIG17 is a graph showing the change in cooling temperature difference of existing all-Mg-based devices with the hot end temperature as reported in the literature.
[0053] Figure 18 shows the MgAg prepared in Comparative Example 2 obtained by first principles calculation. 0.97 Sb 0.99 Phonon spectrum of the material.
[0054] FIG19 is a phonon spectrum of the MgAgSb material prepared in Example 1 obtained by first-principles calculation.
[0055] Figure 20 shows the MgAg prepared in Comparative Example 2 obtained by first principles calculation. 0.97 Sb 0.99 The material forms an energy comparison diagram with the MgAgSb material prepared in Example 1.
[0056] Best Mode for Carrying Out the Invention
[0057] The present invention will be further described below with reference to the following examples. The examples are merely illustrative and are not intended to limit the scope of the present invention in any way.
[0058] Example 1
[0059] Preparation of MgAgSb thermoelectric material of the present invention
[0060] (1) Mg chips and Ag blocks were weighed in a glove box according to the chemical formula MgAg, with a total weight of 5.2 g. They were placed in a stainless steel ball mill containing two carbide balls (each with a mass of 10 g and a radius of 10.5 mm). The Mg chips and Ag blocks were then placed in a high-energy ball mill (model: Hi-Energy / Mill 8000D, transmission mode: synchronous transmission, working mode: three-position ∞-type swing vibration, speed: 875 times / min) and ball milled for 10 h to obtain MgAg alloy powder.
[0061] (2) According to the chemical formula MgAgSb, Sb blocks were added to the MgAg alloy powder obtained in step (1), and the mixture powder was obtained by continuing ball milling for 10 hours.
[0062] (3) The mixed powder and the electrode material Ag powder were placed in batches into a graphite mold with a diameter of 12.7 mm and flattened layer by layer to form a sandwich-like Ag / MgAgSb / Ag structure. The structure was then sintered into a cylindrical block material by spark plasma sintering. The sintering process was as follows: heating to 285°C at a rate of 50°C / min, holding for 5 minutes, and sintering at a pressure of 80 MPa. After sintering, a block material with a thickness of 3 mm and a diameter of 12.7 mm was obtained, of which the electrode layer thickness was 0.1 mm.
[0063] (4) The obtained sample was placed in a quartz tube, evacuated to 0.5 Pa, melted and sealed under a high-temperature flame gun, and then the quartz tube containing the sample was placed in a muffle furnace and heated at a rate of 5°C / min until the temperature of the bulk material reached 310°C, and maintained at this temperature for 24 hours, and then cooled to room temperature with the furnace.
[0064] In order to characterize the effect of the annealing process on the grain size, backscattered electron diffraction (EBSD) analysis was performed on the MgAgSb material before and after annealing. Figure 1 is a grain size diagram of the MgAgSb material obtained in step (3) before annealing, showing that the average grain size is about 200nm. Figure 2 is a grain size diagram of the MgAgSb material after annealing in step (4), showing that the average grain size is about 2μm. By comparing Figure 1 and Figure 2, it can be seen that the annealing process of the present invention causes the MgAgSb grains originally about 200nm in size to grow into large grains of about 2μm in size. Thanks to the reduction of the influence of grain boundaries, its thermal conductivity will be reduced, and as shown in the carrier mobility test below, its carrier mobility will also increase significantly.
[0065] Comparative Example 1
[0066] In this comparative example, MgAgSb mixture powder was prepared in a manner similar to steps (1) and (2) of Example 1, except that a conventional SPEX 8000D Mixer / Mill belt-driven ball mill and conventional stainless steel balls were used for ball milling.
[0067] Table 1 shows a parameter comparison of the ball milling technology used in Example 1 of the present invention and the ball milling technology used in Comparative Example 1.
[0068] Table 1
[0069] Figure 3 compares the Hi-Energy / Mill 8000D synchronous drive high-energy ball mill (a) used in Example 1 of the present invention and the SPEX 8000D Mixer / Mill belt drive ball mill (b) used in Comparative Example 1. The photos of the two drive systems show that the belt drive system is prone to problems such as belt loosening and poor contact during operation, leading to speed reduction. The synchronous drive system, on the other hand, effectively solves this problem, ensuring that the ball mill maintains a stable speed over extended periods of operation.
[0070] FIG4 is a comparison of X-ray diffraction (XRD) patterns of the MgAgSb mixture powder prepared in step (2) of Example 1 and the MgAgSb mixture powder prepared in Comparative Example 1, relative to the standard peaks of MgAgSb. FIG4 shows that, within the same 10-hour ball milling time, the XRD pattern of the MgAgSb mixture powder prepared in step (2) of Example 1 is very close to the standard peaks, with virtually no impurities present. However, the XRD pattern of the MgAgSb mixture powder prepared in Comparative Example 1 contains numerous impurity peaks that are not attributable to MgAgSb, indicating that the purity of the prepared material is low.
[0071] Figure 5 compares the yields of the MgAgSb mixture powder prepared using a synchronous drive high-energy ball mill in Example 1 and the MgAgSb mixture powder prepared using a belt drive ball mill in Comparative Example 1. As can be seen from Figure 5 , the yield of the MgAgSb mixture powder prepared using the synchronous drive high-energy ball mill is much higher than that prepared using the belt drive ball mill.
[0072] Comparative Example 2
[0073] In this comparative example, the same method as in Example 1 was used to prepare MgAg 0.97 Sb 0.99 The thermoelectric material is used to compare its performance with the MgAgSb thermoelectric material prepared in Example 1.
[0074] Comparative Example 3
[0075] In this comparative example, MgAgSb mixture powder was prepared in a manner similar to that of Example 1, except that in step (4), no annealing, annealing at 250°C for 24 hours, and annealing at 300°C for 24 hours were used instead of annealing at 310°C for 24 hours in Example 1.
[0076] Performance Testing
[0077] 1. Carrier concentration and mobility test: PPMS is used to test the Hall coefficient of the sample under the condition of reversible magnetic field (±2T). The carrier concentration and Hall mobility are respectively calculated by formula n H =1 / eR H and μ H =σ / (en H ) is calculated. Figure 6 is the MgAg prepared in Example 2 0.97 Sb 0.99 As can be seen from Figure 6, the MgAgSb material prepared in Example 1 is better than the MgAgSb material prepared in Comparative Example 2. 0.97 Sb 0.99 The material fills the vacancy defects inside, and the mobility increases from 67.8
[0078] cm 2 V -1 s -1 Increased to 80.8cm 2 V -1 s -1 By further annealing to grow the grains, the mobility of the MgAgSb material prepared in Example 1 increased to 93.3 cm 2 V -1 s -1 .
[0079] 2. Conductivity test: The samples were cut into rectangular blocks with a size of 2 mm × 3 mm × 11 mm, and the conductivity and Seebeck coefficient of the samples were tested using a Linseis LSR-3 instrument. 0.97 Sb 0.99 The conductivity of the material is compared with that of the MgAgSb material prepared in Example 1 and before and after annealing. As can be seen from Figure 7, the room temperature conductivity of the material is improved from that of the MgAgSb prepared in Comparative Example 2 to that of the MgAgSb prepared in Example 1. 0.97 Sb 0.99 290Scm of material -1 Increased to 356Scm -1 By further annealing to grow the grains, the room temperature conductivity of the MgAgSb material prepared in Example 1 increased to 452 Scm -1 .
[0080] Figure 8 is the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The relationship between the Seebeck coefficient and temperature of the MgAgSb material prepared in Example 1 before and after annealing. As can be seen from Figure 8, the MgAg prepared in Comparative Example 2 0.97 Sb 0.99 The material and the MgAgSb material prepared in Example 1 have no significant change in Seebeck coefficient before and after annealing, which further proves that the improvement in mobility leads to the improvement in the electrical properties of the MgAgSb material.
[0081] 3. Changes of thermal conductivity and lattice thermal conductivity with temperature: The thermal diffusivity D of the sample was measured using a Linseis LFA 1000 laser thermal conductivity tester, the density ρ of the sample was measured using the Archimedean drainage method, and the heat capacity C of the sample was measured using a DSC 404 high-temperature differential scanning calorimeter. p , then by the formula κ=DρC p The thermal conductivity of the material is calculated. The electronic thermal conductivity of the material is obtained by using the Widmann-Franz law through the electrical conductivity, and then the formula κ L =κ-κ eThe lattice thermal conductivity of the sample was calculated. 0.97 Sb 0.99 Comparison of the thermal conductivity and lattice thermal conductivity of the material and the MgAgSb material prepared in Example 1 before and after annealing as a function of temperature.
[0082] 4. Changes of thermoelectric figure of merit zT with temperature: According to the electrical conductivity, Seebeck coefficient and thermal conductivity of the sample obtained in the previous test, the formula zT=S 2 The thermoelectric figure of merit zT of the sample is calculated by σT / κ. Figure 10 is the MgAg prepared in Example 2. 0.97 Sb 0.99 A comparison of the thermoelectric figure of merit zT of the material and the MgAgSb material prepared in Example 1 before and after annealing as a function of temperature is shown in Figure 10. As can be seen from Figure 10, the thermoelectric figure of merit zT of the sample increases from 0.72 at room temperature, with a maximum of 1.2, for MgAg0.97Sb0.99, to 0.97 at room temperature, with a maximum of 1.6, for MgAgSb after annealing, an overall improvement of 30%.
[0083] FIG11 is a comparison of the thermoelectric figure of merit zT of the MgAgSb material of the present invention and two MgAgSb samples reported in the literature as a function of temperature.
[0084] ref[1]: Zhao, H., et al., High thermoelectric performance of MgAgSb-based materials. Nano Energy, 2014.7: p.97-103;
[0085] ref[2]: Kirkham, MJ, et al., Abinitiodetermination of crystal structures of the thermoelectric material MgAgSb. Physical Review B, 2012.85(14).
[0086] As can be seen from FIG11 , the thermoelectric figure of merit zT of the MgAgSb sample of the present invention is much higher than that of the two MgAgSb samples reported in the literature in the entire test temperature range, which demonstrates the superiority of the material of the present invention in terms of performance.
[0087] 5. Figure 12 compares the conductivity and Seebeck coefficient of the MgAgSb material in Comparative Example 3 after annealing at different temperatures. Figure 13 compares the power factor of the MgAgSb material in Comparative Example 3 after annealing at different temperatures. As can be seen from the figure, the room temperature conductivity of the MgAgSb material does not change significantly after annealing at 250°C and 300°C for one day, while the room temperature conductivity is significantly improved after annealing at 310°C for one day, and the Seebeck coefficient does not change significantly, ultimately resulting in an improvement in the power factor of the sample. This confirms the advantage of annealing at 310°C.
[0088] Example 2
[0089] Preparation of thermoelectric devices
[0090] The MgAgSb material prepared in Example 1 was cut into small pieces measuring 1.3 mm * 1.3 mm * 3 mm, forming magnesium-silver-antimony-based thermoelectric elements. These elements were then assembled with n-type magnesium-bismuth-antimony-based thermoelectric elements measuring 1.3 mm * 1.3 mm * 3 mm via soldering to produce seven pairs of thermoelectric devices.
[0091] The power generation and cooling performance of the thermoelectric device were tested using Mini-PEM. The device achieved a thermoelectric power generation efficiency of 12% at a temperature difference of 300K near room temperature, which is much higher than that of bismuth telluride-based power generation devices. At the same time, its room temperature cooling temperature difference reached 61K, which is comparable to that of bismuth telluride-based cooling devices.
[0092] FIG14 is a graph showing the thermoelectric power generation efficiency of the all-magnesium-based device prepared in this embodiment as a function of the hot end temperature. FIG15 is a graph showing the thermoelectric power generation efficiency of the existing all-magnesium-based device as a function of the hot end temperature reported in ref[3]: P. Ying et al., Robust thermoelectric module based on MgAgSb / Mg3(Sb,Bi)2with an 8.5% conversion efficiency and a 72K maximum cooling. Energy Environ. Sci, 2022.15: p. 2557-2566. By comparing FIG14 and FIG15 , it can be seen that the thermoelectric power generation efficiency of the all-magnesium-based device prepared in this embodiment can reach 12% at a temperature difference of 300K, which is much higher than the thermoelectric power generation efficiency of the existing all-magnesium-based devices reported.
[0093] Figure 16 shows the variation of the cooling temperature difference of the all-magnesium-based device produced in this embodiment with the hot end temperature. Figure 17 shows the variation of the cooling temperature difference of the existing all-magnesium-based device reported in ref [3] with the hot end temperature. Comparing Figures 16 and 17, it can be seen that the cooling temperature difference of the all-magnesium-based device produced in this embodiment can reach 62K at room temperature, which is higher than the 52K room temperature cooling temperature difference of the existing all-magnesium-based device reported.
Claims
1. A method for preparing a MgAgSb thermoelectric material, the preparation method include: (1) placing raw materials in a stoichiometric ratio according to the chemical formula MgAg into a ball mill, and using a synchronous transmission high-energy ball mill to obtain uniform powder; (2) adding Sb according to the chemical formula MgAgSb to the powder obtained in step (1), and continuing to use the synchronous transmission high-energy ball mill to obtain a mixture powder; (3) sintering the mixture powder obtained in step (2) into a bulk material; (4) Annealing the bulk material obtained in step (3) at a temperature of 310±2°C for 12 to 30 hours.
2. The preparation method according to claim 1, in, In the ball milling process described in steps (1) and (2), a hard alloy ball is used for ball milling, for example, a tungsten steel ball is used for ball milling; Preferably, the mass of the cemented carbide ball is 2 to 30 grams, preferably 8 to 15 grams; the radius of the cemented carbide ball is 2 to 20 mm, preferably 8 to 15 mm; 3. The preparation method according to claim 1 or 2, in, The ball milling time in steps (1) and (2) is independently 8 to 12 hours.
4. The preparation method according to any one of claims 1 to 3, in, The sintering conditions in step (3) include: heating to 275-290° C. at a rate of 20-80° C. / min under a pressure of 10-100 MPa, and keeping the temperature for 1-30 min, preferably 2-10 min.
5. The preparation method according to any one of claims 1 to 4, in, The annealing process in step (4) includes: heating the bulk material to a temperature of 310±2°C at a rate of 2-10°C / min, keeping the temperature at this temperature for 20-25 hours, and then cooling to room temperature.
6. The MgAgSb thermoelectric material prepared by the preparation method according to any one of claims 1 to 5, in, The MgAgSb thermoelectric material is a pure phase MgAgSb material.
7. The MgAgSb thermoelectric material according to claim 6, in, At 25° C. to 300° C., the thermoelectric figure of merit zT of the pure phase MgAgSb material is 0.97 to 1.
6.
8. The MgAgSb thermoelectric material according to claim 6 or 7, in, The carrier mobility of the pure phase MgAgSb material is about 93.3 cm 2 V -1 s -1 ; Preferably, the power factor of the pure phase MgAgSb material is about 25 μW cm -1 K -2 .
9. Use of the MgAgSb thermoelectric material according to any one of claims 6 to 8 or the MgAgSb thermoelectric material prepared by the preparation method according to any one of claims 1 to 5 in thermoelectric components for thermoelectric power generation and refrigerators.
10. The use according to claim 9, in, The thermoelectric component is a fully magnesium-based thermoelectric component, which includes a p-type magnesium-silver-antimony thermoelectric material and an n-type magnesium-bismuth-antimony-based thermoelectric material, wherein the p-type magnesium-silver-antimony thermoelectric material is the MgAgSb thermoelectric material described in any one of claims 6 to 8 or the MgAgSb thermoelectric material prepared according to the preparation method described in any one of claims 1 to 5.
Citation Information
Patent Citations
n-type Mg-Sb based room temperature thermoelectric material and preparation method thereof
CN108531795A
High-performance P-type alpha-MgAgSb-based thermoelectric material and preparation method thereof
CN108767103A
Preparation method of room-temperature magnesium-based thermoelectric material and product
CN113073220A
P-type magnesium-silver-antimony thermoelectric material and preparation method and application thereof
CN115835758A
Compound thermoelectric material and manufacturing method thereof
JP2007116156A