Method for preparing semiconductor structure, and semiconductor structure
By treating the first epitaxial layer with a halogen compound, the problem of interface roughness caused by element segregation in the semiconductor superlattice structure is solved, and the carrier mobility and structural quality are improved.
Patent Information
- Application Number
- PCT/CN2023/092455
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-05-06
- Publication Date
- 2024-10-24
AI Technical Summary
During the formation of the semiconductor superlattice structure, due to the segregation properties of the elements in the first epitaxial layer, atoms diffuse outward, increasing the interface thickness, roughening the surface, and reducing carrier mobility.
The surface of the first epitaxial layer is treated with a halogen compound of the first element to remove the diffused atoms of the second element and supplement the first element on the surface, thereby thinning the interface transition layer, improving its steepness, and forming a smoother interface. .
It effectively reduces the thickness and steepness of the interface transition layer, increases carrier mobility, and maintains the growth rate and stress state of the superlattice structure.
Smart Images

Figure CN2023092455_24102024_PF_FP_ABST
Abstract
Description
Semiconductor structure preparation method and semiconductor structure
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on April 18, 2023, with application number 202310413590X and invention name “Method for preparing semiconductor structure and semiconductor structure”, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a semiconductor structure and a semiconductor structure. Background Art
[0004] The statements herein merely provide background information related to the present application and do not necessarily constitute exemplary techniques.
[0005] With the development of semiconductor technology, multi-period superlattice structures have been widely studied and applied in advanced semiconductor process nodes and 3D dynamic random access memory (DRAM). An epitaxial period of a superlattice structure is usually composed of a first epitaxial layer and a second epitaxial layer. However, due to the segregation properties of certain elements in the first epitaxial layer, during the formation of the superlattice structure, the atoms corresponding to these elements will diffuse outward at the interface between the first epitaxial layer and the second epitaxial layer, thereby increasing the interface thickness between the first epitaxial layer and the second epitaxial layer. This will cause the surface of the second epitaxial layer to become rough, and a large number of scattering centers will appear at the interface, resulting in a decrease in carrier mobility.
[0006] Summary of the Invention
[0007] According to various embodiments of the present application, a method for manufacturing a semiconductor structure and a semiconductor structure are provided.
[0008] A method for preparing a semiconductor structure, comprising:
[0009] providing a substrate;
[0010] Performing at least one epitaxial growth cycle to form a first epitaxial layer and a second epitaxial layer stacked sequentially from bottom to top on the substrate; the epitaxial growth cycle includes:
[0011] forming the first epitaxial layer on the substrate, wherein the first epitaxial layer includes a compound of a first element and a second element having segregation characteristics;
[0012] performing surface treatment on the upper surface of the first epitaxial layer using a halogen compound of the first element;
[0013] The second epitaxial layer is formed on the surface-treated first epitaxial layer, wherein the second epitaxial layer includes the first element.
[0014] In one embodiment, the first element includes silicon, the second element includes germanium or phosphorus; the first epitaxial layer includes a silicon germanium layer, a silicon phosphide layer or a phosphorus silicon germanium layer, and the second epitaxial layer includes a silicon layer; the halogen compound of the first element includes SiCl2H2 or SiCl2.
[0015] In one embodiment, the upper surface of the first epitaxial layer is surface-treated with a halogen compound of the first element under a preset protective atmosphere; the surface treatment temperature is 700° C. to 1200° C.; and the surface treatment time is 0.1s to 120s.
[0016] In one embodiment, the preset protective atmosphere includes a reducing atmosphere or a vacuum atmosphere.
[0017] In one embodiment, a plurality of epitaxial growth cycles are performed to form the first epitaxial layer and the second epitaxial layer stacked sequentially from bottom to top on the substrate.
[0018] In one embodiment, the number of epitaxial cycles performed is 1 to 200.
[0019] In one embodiment, before performing at least one epitaxial cycle, the method further includes:
[0020] The substrate is pre-treated.
[0021] In one embodiment, the pre-processing of the substrate includes:
[0022] Pre-treating the substrate with hydrofluoric acid; and / or
[0023] The substrate is subjected to a reduction treatment at a preset temperature and a preset reducing atmosphere.
[0024] In one embodiment, the preset temperature is 700°C to 1200°C.
[0025] A semiconductor structure comprising:
[0026] substrate;
[0027] A first epitaxial layer and a second epitaxial layer are sequentially stacked on the substrate; wherein the first epitaxial layer includes a compound of a first element and a second element having segregation characteristics; and the second epitaxial layer includes the first element;
[0028] An interface transition layer is located between the adjacent first epitaxial layer and the second epitaxial layer.
[0029] In one embodiment, the first element includes silicon, the second element includes germanium or phosphorus; the first epitaxial layer includes a silicon germanium layer, a silicon phosphide layer or a phosphorus silicon germanium layer, and the second epitaxial layer includes a silicon layer; the halogen compound of the first element includes SiCl2H2 or SiCl2.
[0030] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the following briefly introduces the drawings required for use in the embodiments or the conventional technology descriptions. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] FIG1 is a flow chart of a method for preparing a semiconductor structure provided in one embodiment;
[0033] FIG2 is a schematic cross-sectional view of a structure obtained in step S101 of a method for preparing a semiconductor structure provided in one embodiment;
[0034] FIG3 is a schematic cross-sectional view of a structure obtained in step S102 of a method for preparing a semiconductor structure provided in one embodiment;
[0035] FIG4 is a schematic cross-sectional view of a structure obtained in step S1021 of a method for preparing a semiconductor structure provided in one embodiment;
[0036] FIG5 is a schematic cross-sectional view of a structure obtained in step S1022 of a method for preparing a semiconductor structure provided in one embodiment;
[0037] FIG6 is a schematic cross-sectional view of a structure obtained in step S1023 of a method for preparing a semiconductor structure provided in one embodiment;
[0038] FIG7 is a comparison diagram of high-resolution transmission electron microscopy of a superlattice structure without surface treatment and a superlattice structure with surface treatment in one embodiment, as well as a comparison diagram after image processing. DETAILED DESCRIPTION
[0039] To facilitate understanding of the present application, the present application will be described more fully below with reference to the accompanying drawings. The accompanying drawings provide embodiments of the present application. However, the present application may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to make the disclosure of the present application more thorough and comprehensive.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.
[0041] It should be understood that when an element or layer is referred to as being "on," "adjacent to," "connected to," or "coupled to" another element or layer, it can be directly on, adjacent to, connected to, or coupled to the other element or layer, or there can be intervening elements or layers. Conversely, when an element is referred to as being "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" another element or layer, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, doping types, and / or portions, these elements, components, regions, layers, doping types, and / or portions should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, doping type, or portion from another element, component, region, layer, doping type, or portion. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.
[0042] Spatially relative terms such as "under," "beneath," "beneath," "under," "on the surface of," "above," and the like, may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the drawings is turned over, an element or feature described as "under" or "under" or "beneath" the other elements would be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include alternative orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.
[0043] As used herein, the singular forms "a," "an," and "the" may also include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include," "comprising," "having," and the like specify the presence of stated features, integers, steps, operations, components, parts, or combinations thereof, but do not preclude the presence or addition of one or more other features, integers, steps, operations, components, parts, or combinations thereof. Also, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.
[0044] Embodiments of the invention are described herein with reference to cross-sectional views which are schematic illustrations of preferred embodiments (and intermediate structures) of the present application, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Accordingly, embodiments of the present application should not be limited to the specific shapes of the regions shown herein, but rather include deviations in shapes due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges, rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation occurs. Accordingly, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the present application.
[0045] With the development of semiconductor technology, multi-period superlattice structures have been widely studied and applied in advanced semiconductor process nodes and 3D dynamic random access memory (DRAM). An epitaxial period of a superlattice structure is usually composed of a first epitaxial layer and a second epitaxial layer. However, due to the segregation properties of certain elements in the first epitaxial layer, during the formation of the superlattice structure, the atoms corresponding to these elements will diffuse outward at the interface between the first epitaxial layer and the second epitaxial layer, thereby increasing the interface thickness between the first epitaxial layer and the second epitaxial layer. This will cause the surface of the second epitaxial layer to become rough, and a large number of scattering centers will appear at the interface, resulting in a decrease in carrier mobility.
[0046] For example, for the traditional silicon / silicon germanium superlattice structure, due to the segregation property of germanium atoms, during the formation of the silicon germanium layer, germanium atoms will diffuse into the silicon layer at the silicon / silicon germanium interface, thereby increasing the thickness of the interface transition layer from silicon germanium to silicon, causing the surface of the silicon layer to become rough, thereby reducing the carrier mobility.
[0047] Referring to FIG. 1 , the present application provides a method for preparing a semiconductor structure, comprising the following steps:
[0048] S101: providing a substrate;
[0049] S102: Perform at least one epitaxial growth cycle to form a first epitaxial layer and a second epitaxial layer stacked sequentially from bottom to top on the substrate. The epitaxial growth cycle includes:
[0050] S1021: forming a first epitaxial layer on a substrate, wherein the first epitaxial layer includes a compound of a first element and a second element having segregation characteristics;
[0051] S1022: performing surface treatment on the upper surface of the first epitaxial layer using a halogen compound of the first element;
[0052] S1023: forming a second epitaxial layer on the upper surface of the surface-treated first epitaxial layer, wherein the second epitaxial layer includes the first element.
[0053] In step S101 , referring to step S101 in FIG. 1 and FIG. 2 , a substrate 10 is provided.
[0054] The material of the substrate 10 may be any suitable substrate 10 material known in the art, for example, at least one of the following materials: silicon (Si), germanium (Ge), red phosphorus, silicon germanium (SiGe), silicon carbide (SiC), carbon silicon germanium (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP), or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI), and germanium on insulator (GeOI), or double-side polished silicon wafers (DSP), or ceramic substrates such as alumina, quartz or glass substrates, etc., which are not limited in this embodiment.
[0055] Optionally, the substrate 10 may include a first element, which may refer to the most important element in the substrate 10 . For example, when the material of the substrate 10 is silicon, the first element may be silicon.
[0056] In step S102 , referring to step S102 in FIG. 1 and FIG. 3 , at least one epitaxial cycle is performed to form a first epitaxial layer 201 and a second epitaxial layer 202 stacked sequentially from bottom to top on the substrate 10 .
[0057] As shown in FIG3 , at least one epitaxial growth cycle is performed to ultimately form a superlattice structure 20 on a substrate 10. The superlattice structure 20 refers to a multilayer film structure in which thin layers of two different components are alternately grown and maintain a strict periodic pattern. It can be understood as a specific form of layered fine composite material. In other words, the superlattice structure 20 can include a first epitaxial layer 201 and a second epitaxial layer 202 stacked sequentially from bottom to top. The primary semiconductor properties of the first epitaxial layer 201 and the second epitaxial layer 202, such as the band gap or doping level, can be independently controlled, and the number of layers in the first epitaxial layer 201 and the second epitaxial layer 202 can also be manually controlled during growth.
[0058] Among them, the epitaxial cycle includes:
[0059] S1021: forming a first epitaxial layer on a substrate, wherein the first epitaxial layer includes a compound of a first element and a second element having segregation characteristics.
[0060] As shown in FIG4 , the second element can be determined after the first element is determined. For example, if the first element is silicon, the second element can be phosphorus (P), germanium (Ge), and the like. In actual application scenarios, the types of the first and second elements can be determined by comprehensively considering the actual process requirements and cost, and this embodiment does not limit this. To facilitate understanding of this solution, FIG4 is a schematic diagram of forming the first epitaxial layer 201 in the first epitaxial cycle.
[0061] S1022: performing surface treatment on the upper surface of the first epitaxial layer using a halogen compound of the first element.
[0062] As shown in FIG5 , halogen elements include fluorine, chlorine, bromine, iodine, etc., which are the most typical non-metallic elements. The halogen compound 30 of the first element refers to a class of compounds containing the first element and the halogen element. Taking silicon as the first element as an example, the halogen compound of silicon can include silicon tetrafluoride (SiF4), silicon dichloride (SiCl2), silicon dichloride (SiH2Cl2), etc. To facilitate understanding of this solution, FIG5 is a schematic diagram of the surface treatment of the first epitaxial layer 201 in the first epitaxial cycle.
[0063] S1023: forming a second epitaxial layer on the surface-treated first epitaxial layer, wherein the second epitaxial layer includes the first element.
[0064] As shown in Figure 6, to facilitate understanding of this solution, Figure 6 is a schematic diagram of the formation of the second epitaxial layer 202 in the first epitaxial cycle. The remaining epitaxial cycles can be grown according to the patterns shown in Figures 4-6. For example, in the second epitaxial cycle, the first epitaxial layer 201 of the second epitaxial cycle is formed on top of the second epitaxial layer 202 of the first epitaxial cycle, and so on, ultimately forming the first epitaxial layer 201 and the second epitaxial layer 202 alternately stacked from bottom to top. Optionally, the number of epitaxial cycles can range from 1 to 300.
[0065] As shown in Figure 6, when the second epitaxial layer 202 is formed on the upper surface of the first epitaxial layer 201, because the first epitaxial layer 201 and the second epitaxial layer 202 are composed of different elements, an interface transition layer 203 is formed at the interface between the first epitaxial layer 201 and the second epitaxial layer 202. At the same time, because the second element has a segregation property, after the second epitaxial layer 202 is formed, the atoms corresponding to the second element diffuse on the surface of the first epitaxial layer 201, resulting in a relatively thick interface transition layer 203.
[0066] By treating the upper surface of the first epitaxial layer 201 with a halogen compound 30 of the first element, the thickness of the interface transition layer 203 can be reduced. This is because, on the one hand, the halogen compound 30 of the first element reacts with atoms corresponding to the second element diffused from the upper surface of the first epitaxial layer 201, thereby removing some of the diffused atoms corresponding to the second element. On the other hand, because these halogen compounds contain the first element, they can compensate for the first element on the upper surface of the first epitaxial layer 201. Consequently, when the first epitaxial layer 201 and the second epitaxial layer 202 contact to form the interface transition layer 203, the thickness of the interface transition layer 203 can be reduced and the steepness of the interface transition layer 203 can be improved, thereby preventing a decrease in carrier mobility.
[0067] In addition, after the first epitaxial layer 201 is treated with the halogen compound 30 of the first element, the growth rate of the entire superlattice structure 20 is not affected, and the stress state inside the first epitaxial layer 201 is not affected.
[0068] The method for preparing the semiconductor structure includes: providing a substrate; performing at least one epitaxial growth cycle to form a first epitaxial layer and a second epitaxial layer stacked sequentially from bottom to top on the substrate; the epitaxial growth cycle includes: forming a first epitaxial layer on the substrate, the first epitaxial layer including a compound of a first element and a second element having segregation characteristics; surface treating the upper surface of the first epitaxial layer with a halogen compound of the first element; and forming a second epitaxial layer on the upper surface of the surface-treated first epitaxial layer, the second epitaxial layer including the first element. Because the upper surface of the first epitaxial layer is surface treated with the halogen compound of the first element, the halogen compound of the first element can simultaneously remove the diffused second element and replenish the first element. Thus, when the first epitaxial layer and the second epitaxial layer contact to form an interface transition layer, the thickness of the interface transition layer can be reduced and the steepness of the interface transition layer can be improved, thereby preventing a decrease in carrier mobility.
[0069] Optionally, after surface treatment with the halogen compound 30 of the first element, the thickness of the interface transition layer 203 between the first epitaxial layer 201 and the second epitaxial layer 202 is 0.2 nm-0.8 nm.
[0070] In one embodiment, the first element includes silicon, the second element includes germanium or phosphorus; the first epitaxial layer 201 includes a silicon germanium layer, a silicon phosphide layer or a phosphorus silicon germanium layer, and the second epitaxial layer 202 includes a silicon layer; the halogen compound 30 of the first element includes SiCl2H2 or SiCl2.
[0071] For example, the first element is silicon, the second element is germanium, and the halogen compound 30 of the first element is SiCl2H2 or SiCl2. In this case, the substrate 10 can be a silicon substrate, the first epitaxial layer 201 is a silicon germanium layer, and the second epitaxial layer 202 is a silicon layer. When forming the first epitaxial layer 201, the silicon germanium (SiGe) grown by using a silicon germanium precursor is used. 1-x Ge x ,) layer thickness can be 1nm-200nm. Thereafter, the valve of the silicon germanium precursor is quickly closed, and a silicon halogen compound such as SiCl2H2 or SiCl2 is introduced into the growth chamber for surface treatment. The surface treatment time can be 0.1s to 120s. Finally, when forming the second epitaxial layer 202, the thickness of the silicon layer grown using the silicon precursor can be 1nm-500nm, thereby completing the growth of one epitaxial cycle. The above-mentioned process of forming epitaxial cycles can be continuously repeated to form at least one epitaxial cycle, thereby forming a superlattice structure 20.
[0072] FIG7 is a comparison of the cross-sectional structures of the interface transition layer 203 without the silicon halogen compound treatment and the interface transition layer 203 with the silicon halogen compound treatment during an epitaxial growth cycle, wherein FIG7(a) is an HRTEM image of the superlattice structure without the surface treatment, FIG7(b) is an HRTEM image of the superlattice structure without the surface treatment after image processing, FIG7(c) is an HRTEM image of the superlattice structure with the surface treatment, and FIG7(d) is an HRTEM image of the superlattice structure with the surface treatment after image processing. The distance between the two dotted lines in FIG7(a) and FIG7(b) represents the thickness of the interface transition layer 203 without the silicon halogen compound treatment, and the distance between the two dotted lines in FIG7(c) and FIG7(d) represents the thickness of the interface transition layer 203 without the silicon halogen compound treatment. As can be seen from FIG7 , after treatment with the silicon halogen compound, the thickness of the interface transition layer 203 between the silicon layer and the silicon germanium layer is significantly reduced (the thickness of the interface transition layer 203 after surface treatment is approximately 0.5 nm), and the steepness of the interface transition layer 203 is also significantly improved, thereby further preventing a decrease in carrier mobility.
[0073] In one embodiment, the upper surface of the first epitaxial layer 201 is surface-treated using a halogen compound 30 of a first element under a preset protective atmosphere; the surface treatment temperature is 700° C. to 1200° C.; and the surface treatment time is 0.1s to 120s.
[0074] The preset protective atmosphere can be the atmosphere condition when forming the first epitaxial layer 201. Still taking the first epitaxial layer 201 as a silicon germanium layer as an example, when forming the first epitaxial layer 201, the silicon germanium (Si 1-x Ge x , 0<x<1) layer, thereafter, the upper surface of the first epitaxial layer 201 can be processed by simply closing the precursor valve and opening the valve for the silicon halogen compound. During this process, there is no need to switch the gas atmosphere. In other words, the first preset protective atmosphere can also be the gas atmosphere used during the formation of the first epitaxial layer 201.
[0075] In addition, the surface treatment temperature may also be the temperature condition when forming the first epitaxial layer 201. Still taking the first epitaxial layer 201 as a silicon germanium layer as an example, when forming the first epitaxial layer 201, the silicon germanium (Si 1-x Ge x, 0<x<1) layer, then, by simply closing the precursor valve and opening the valve for the silicon halogen compound, the upper surface of the first epitaxial layer 201 can be treated. During this process, the temperature conditions do not need to be changed. In other words, the surface treatment temperature can also be the temperature conditions used when forming the first epitaxial layer 201.
[0076] In one embodiment, the preset protective atmosphere includes a reducing atmosphere or a vacuum atmosphere. For example, the preset protective atmosphere can be a pure hydrogen atmosphere, or a mixed atmosphere of hydrogen and an inert gas, or an ultra-high vacuum atmosphere.
[0077] In one embodiment, as shown in FIG. 3 , multiple epitaxial cycles are performed to form a first epitaxial layer 201 and a second epitaxial layer 202 stacked sequentially from bottom to top on the substrate 10 .
[0078] For 3D DRAM and similar semiconductor devices, the substrate 10 is usually a silicon substrate 10, the first epitaxial layer 201 is a silicon germanium layer or a silicon phosphide layer, and the second epitaxial layer 202 is a silicon layer to form a superlattice structure 20. In order to ensure the performance and process feasibility requirements of the above-mentioned semiconductor devices, the thickness of the silicon germanium layer or silicon phosphide layer used as the first epitaxial layer 201 usually needs to reach a certain level (for example, >60nm), and the number of epitaxial periods of the superlattice structure 20 formed by the first epitaxial layer 201 and the second epitaxial layer 202 is as large as possible. That is, for the above-mentioned semiconductor devices, the thicker the superlattice structure 20 is, the better.
[0079] In one embodiment, the number of epitaxial cycles performed is 1-200.
[0080] In one embodiment, before performing at least one epitaxial growth cycle, the method for preparing a semiconductor structure further includes: pre-treating the substrate 10 .
[0081] In one embodiment, pre-treating the substrate 10 includes: pre-treating the substrate 10 with hydrofluoric acid, and / or performing a reduction treatment on the substrate 10 at a preset temperature and in a preset reducing atmosphere.
[0082] In one embodiment, the preset temperature is 700° C. to 1200° C. For example, the preset reducing atmosphere may be a pure hydrogen atmosphere, or a mixed atmosphere of hydrogen and an inert gas.
[0083] Furthermore, the preset protective atmosphere and the preset reducing atmosphere can be the same, for example, both can be reducing atmospheres. Thus, during at least one epitaxial growth cycle, there is no need to switch gas atmospheres, thereby avoiding cumbersome process operations and further saving costs.
[0084] Furthermore, during the execution of at least one epitaxial cycle, the temperature can be kept at a preset temperature, thereby eliminating the need to frequently switch temperature ranges, thereby avoiding cumbersome process operations and further saving costs.
[0085] On the other hand, the present application also provides a semiconductor structure, as shown in Figure 3, the semiconductor structure includes a substrate 10, a first epitaxial layer 201 and a second epitaxial layer 202 stacked in sequence on the substrate 10, and an interface transition layer 203; wherein, the first epitaxial layer 201 includes a compound of a first element and a second element having segregation characteristics; the second epitaxial layer 202 includes the first element; and the interface transition layer 203 is located between the adjacent first epitaxial layer 201 and the second epitaxial layer 202.
[0086] The material of the substrate 10 may be any suitable substrate material known in the art, for example, at least one of the following materials: silicon (Si), germanium (Ge), red phosphorus, silicon germanium (SiGe), silicon carbide (SiC), carbon silicon germanium (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP), or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI), and germanium on insulator (GeOI), or double-side polished silicon wafers (DSP), or ceramic substrates such as alumina, quartz or glass substrates, etc., which are not limited in this embodiment.
[0087] Optionally, the substrate 10 may include a first element, which may refer to the most important element in the substrate 10 . For example, when the material of the substrate 10 is silicon, the first element may be silicon.
[0088] As shown in Figure 3, the first epitaxial layer 201 and the second epitaxial layer 202 stacked from bottom to top can form a superlattice structure 20. Superlattice structure 20 refers to a multilayer film structure composed of thin layers of two different components grown alternately and maintaining a strict periodic pattern. It can be understood as a specific form of layered fine composite material. The primary semiconductor properties of the first epitaxial layer 201 and the second epitaxial layer 202, such as band gap or doping level, can be independently controlled, and the number of layers in the first epitaxial layer 201 and the second epitaxial layer 202 can also be manually controlled during growth.
[0089] The second element can be determined after the first element is determined. For example, if the first element is silicon, the second element can be phosphorus (P), germanium (Ge), etc. In actual application scenarios, the types of the first and second elements can be determined by comprehensively considering the actual process requirements and cost, and this embodiment does not limit this.
[0090] The halogen compound 30 of the first element refers to a compound containing the first element and a halogen element. Halogen elements include fluorine, chlorine, bromine, iodine, and the like, which are the most typical non-metallic elements. For example, if the first element is silicon, halogen compounds of silicon may include silicon tetrafluoride (SiF4), silicon dichloride (SiCl2), silicon dichloride (SiH2Cl2), and the like.
[0091] When the second epitaxial layer 202 is formed on the upper surface of the first epitaxial layer 201, because the first epitaxial layer 201 and the second epitaxial layer 202 are composed of different elements, an interface transition layer 203 is formed at the interface between the first epitaxial layer 201 and the second epitaxial layer 202. Furthermore, because the second element has a segregation property, after the second epitaxial layer 202 is formed, atoms corresponding to the second element diffuse on the surface of the first epitaxial layer 201, resulting in a relatively thick interface transition layer 203.
[0092] By treating the upper surface of the first epitaxial layer 201 with a halogen compound 30 of the first element, the thickness of the interface transition layer 203 can be reduced. This is because, on the one hand, the halogen compound 30 of the first element reacts with atoms corresponding to the second element diffused from the upper surface of the first epitaxial layer 201, thereby removing some of the diffused atoms corresponding to the second element. On the other hand, because these halogen compounds contain the first element, they can compensate for the first element on the upper surface of the first epitaxial layer 201. Consequently, when the first epitaxial layer 201 and the second epitaxial layer 202 contact to form the interface transition layer 203, the thickness of the interface transition layer 203 can be reduced and the steepness of the interface transition layer 203 can be improved, thereby preventing a decrease in carrier mobility.
[0093] In addition, after the first epitaxial layer 201 is treated with the halogen compound 30 of the first element, the growth rate of the entire superlattice structure 20 is not affected, and the stress state inside the first epitaxial layer 201 is not affected.
[0094] The semiconductor structure includes a substrate 10, a first epitaxial layer 201 and a second epitaxial layer 202 sequentially stacked on the substrate 10, and an interface transition layer 203. The first epitaxial layer 201 includes a compound of a first element and a second element having segregation characteristics; the second epitaxial layer 202 includes the first element; and the interface transition layer 203 is located between the adjacent first epitaxial layer 201 and the second epitaxial layer 202. Because the upper surface of the first epitaxial layer 201 is surface-treated with a halogen compound 30 of the first element, the halogen compound 30 of the first element can simultaneously remove diffused second elements and replenish the first element. Therefore, when the first epitaxial layer 201 and the second epitaxial layer 202 contact to form the interface transition layer 203, the thickness of the interface transition layer 203 can be reduced and the steepness of the interface transition layer 203 can be improved, thereby preventing a decrease in carrier mobility.
[0095] In one embodiment, the first element includes silicon, the second element includes germanium or phosphorus; the first epitaxial layer 201 includes a silicon germanium layer, a silicon phosphide layer or a phosphorus silicon germanium layer, and the second epitaxial layer 202 includes a silicon layer; the halogen compound 30 of the first element includes SiCl2H2 or SiCl2.
[0096] As shown in FIG7 , FIG7 is a comparison of the cross-sectional structures of the interface transition layer 203 that has not been treated with a silicon halogen compound and the interface transition layer 203 that has been treated with a silicon halogen compound during an epitaxial growth cycle, wherein FIG7 (a) is a HRTEM image of the superlattice structure that has not been treated with a surface treatment, FIG7 (b) is a HRTEM image of the superlattice structure that has not been treated with a surface treatment after image processing, FIG7 (c) is a HRTEM image of the superlattice structure that has been treated with a surface treatment, and FIG7 (d) is a HRTEM image of the superlattice structure that has been treated with a surface treatment after image processing. The distance between the two dotted lines in FIG7 (a) and FIG7 (b) represents the thickness of the interface transition layer 203 that has not been treated with a silicon halogen compound, and the distance between the two dotted lines in FIG7 (c) and FIG7 (d) represents the thickness of the interface transition layer 203 that has not been treated with a silicon halogen compound. As can be seen from FIG7 , after treatment with the silicon halogen compound, the thickness of the interface transition layer 203 between the silicon layer and the silicon germanium layer is significantly reduced (the thickness of the interface transition layer 203 after surface treatment is approximately 0.5 nm), and the steepness of the interface transition layer 203 is also significantly improved, thereby further preventing a decrease in carrier mobility.
[0097] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features of the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0098] The above embodiments only express several implementation methods of the present application. The descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, and these all fall within the scope of protection of the present application. Therefore, the scope of protection of the patent application shall be based on the attached claims.
Claims
1. A method for preparing a semiconductor structure, comprising: providing a substrate; Performing at least one epitaxial cycle to form a first epitaxial layer and a second epitaxial layer stacked sequentially from bottom to top on the substrate; the epitaxial cycle includes: forming the first epitaxial layer on the substrate, wherein the first epitaxial layer includes a compound of a first element and a second element having a segregation characteristic; Performing surface treatment on the upper surface of the first epitaxial layer using a halogen compound of the first element; The second epitaxial layer is formed on the surface-treated first epitaxial layer, wherein the second epitaxial layer includes the first element.
2. The method for preparing a semiconductor structure according to claim 1, wherein: The first element includes silicon, and the second element includes germanium or phosphorus; the first epitaxial layer includes a silicon germanium layer, a silicon phosphide layer or a phospho-silicon germanium layer, and the second epitaxial layer includes a silicon layer; the halogen compound of the first element includes SiCl2H2 or SiCl2.
3. The method for preparing a semiconductor structure according to claim 1, wherein: The upper surface of the first epitaxial layer is surface treated with the halogen compound of the first element under a preset protective atmosphere; the surface treatment temperature is 700° C. to 1200° C.; and the surface treatment time is 0.1s to 120s.
4. The method for preparing a semiconductor structure according to claim 3, wherein: The preset protective atmosphere includes a reducing atmosphere or a vacuum atmosphere.
5. The method for preparing a semiconductor structure according to claim 1, wherein: A plurality of the epitaxial cycles are performed to form the first epitaxial layer and the second epitaxial layer stacked sequentially from bottom to top on the substrate.
6. The method for preparing a semiconductor structure according to claim 5, wherein: The number of the epitaxial cycles executed is 1 to 200.
7. The method for preparing a semiconductor structure according to any one of claims 1 to 6, wherein: Before performing at least one epitaxial cycle, the method further comprises: The substrate is pre-treated.
8. The method for preparing a semiconductor structure according to claim 7, wherein: The pre-processing of the substrate comprises: Pre-treating the substrate with hydrofluoric acid; and / or The substrate is subjected to reduction treatment at a preset temperature and a preset reducing atmosphere.
9. The method for preparing a semiconductor structure according to claim 8, wherein: The preset temperature is 700°C to 1200°C.
10. A semiconductor structure, wherein: include: substrate; A first epitaxial layer and a second epitaxial layer sequentially stacked on the substrate; wherein the first epitaxial layer comprises a compound of a first element and a second element having a segregation characteristic; and the second epitaxial layer comprises the first element; The interface transition layer is located between the first epitaxial layer and the second epitaxial layer.
11. The semiconductor structure according to claim 10, wherein: The first element includes silicon, and the second element includes germanium or phosphorus; the first epitaxial layer includes a silicon germanium layer, a silicon phosphide layer or a phospho-silicon germanium layer, and the second epitaxial layer includes a silicon layer; the halogen compound of the first element includes SiCl2H2 or SiCl2.
Citation Information
Patent Citations
Super junction device structure and preparation method thereof
CN110137245A
Silicon-based gallium arsenide epitaxial structure, laser and preparation method
CN115938916A
Inverted layer epitaxial liftoff process
US6033995A