Organic light-emitting display panel
By adopting a double-layer electron blocking layer structure in an organic light-emitting display panel, the problem of large changes in pixel capacitance is solved, capacitance stability and luminous efficiency are improved, device life is extended, and low-brightness display effects are improved.
Patent Information
- Application Number
- PCT/CN2023/096604
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-05-26
- Publication Date
- 2024-10-24
AI Technical Summary
In organic light-emitting display panels, the capacitance of pixels changes greatly, resulting in poor stability of the display panel. Especially after long-term use, the capacitance becomes smaller, affecting luminous efficiency and display effects.
Adopting a double-layer electron blocking layer structure, in which the hole mobility of the first electron blocking layer is greater than that of the second electron blocking layer, the capacitance stability and carrier balance of the device are adjusted, and the driving is optimized by adjusting the thickness and material selection of the blocking layer voltage and luminous efficiency.
It significantly reduces the capacitance change amplitude of the pixel, improves the capacitance stability and luminous efficiency, extends the device life, and improves the display effect at low brightness.
Smart Images

Figure CN2023096604_24102024_PF_FP_ABST
Abstract
Description
Organic light-emitting display panels Technical Field
[0001] The present application relates to the field of display, and in particular to an organic light-emitting display panel. Background Art
[0002] Organic Light-Emitting Diode (OLED) has the characteristics of self-luminescence, fast response, wide viewing angle, etc. It has a very broad application prospect and has gradually replaced liquid crystal display in the display field.
[0003] In an OLED display panel, a pixel generally contains three sub-pixels: blue, green, and red. The three sub-pixels are driven separately by the backplane driving circuit to display different pictures. The three sub-pixels can emit light of different colors because different organic materials are used. Due to the use of different organic materials, the three sub-pixels have different electrical properties (for example, resistance, capacitance, turn-on voltage, etc.). The difference in electrical properties of sub-pixels often causes a series of display problems in the display panel. One of the more significant differences is reflected in the change in the capacitance of the three sub-pixels before and after they work. Generally speaking, after the OLED device has aged for a period of time, the pixel capacitance will become smaller. Technical issues
[0004] In view of this, the present application provides an organic light emitting display panel capable of reducing the capacitance variation amplitude of pixels. Technical Solutions
[0005] The present application provides an organic light-emitting display panel, comprising a substrate, a first electrode disposed on one side of the substrate, a hole injection layer disposed on a side of the first electrode away from the substrate, a hole transport layer disposed on a side of the hole injection layer away from the substrate, a first electron blocking layer disposed on a side of the hole transport layer away from the substrate, a second electron blocking layer disposed on a side of the first electron blocking layer away from the substrate, a light-emitting layer disposed on a side of the second electron blocking layer away from the substrate, an electron transport layer disposed on a side of the light-emitting layer away from the substrate, an electron injection layer disposed on a side of the electron transport layer away from the substrate, and a second electrode disposed on a side of the electron injection layer away from the substrate. The hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer.
[0006] Optionally, the first triplet excited state energy level of the first electron blocking layer is greater than the first triplet excited state energy level of the second electron blocking layer, and the first triplet excited state energy level of the second electron blocking layer is greater than the first triplet excited state energy level of the light-emitting layer.
[0007] Optionally, a difference between a first triplet excited state energy level of the first electron blocking layer and a first triplet excited state energy level of the second electron blocking layer is greater than or equal to 0.1 eV;
[0008] A difference between a first triplet excited state energy level of the second electron blocking layer and a first triplet excited state energy level of the light emitting layer is greater than or equal to 0.1 eV.
[0009] Optionally, the difference between the highest occupied orbital energy levels of the first electron blocking layer and the second electron blocking layer is less than or equal to 0.2 eV, and the difference between the highest occupied orbital energy levels of the second electron blocking layer and the light-emitting layer is less than or equal to 0.2 eV.
[0010] Optionally, the highest occupied orbital energy level of the first electron block is in the range of -5.4 eV to -5.6 eV, and the highest occupied orbital energy level of the second electron block is in the range of -5.5 eV to -5.7 eV.
[0011] Optionally, the highest occupied orbital energy level of the hole transport layer is greater than or equal to the highest occupied orbital energy level of the first electron blocking layer.
[0012] Optionally, the difference between the highest occupied orbital energy level of the hole transport layer and the highest occupied orbital energy level of the first electron blocking layer is less than or equal to the difference between the highest occupied orbital energy level of the first electron blocking layer and the highest occupied orbital energy level of the second electron blocking layer.
[0013] Optionally, the difference between the highest occupied orbital energy limits of the hole transport layer and the first electron blocking layer is less than or equal to 0.2 eV.
[0014] Optionally, the carrier tolerance of the first electron blocking layer is smaller than the carrier tolerance of the second electron blocking layer.
[0015] Optionally, the thickness of the first electron blocking layer is greater than the thickness of the second electron blocking layer.
[0016] Optionally, when the luminance of the light-emitting layer decreases to 95% of the initial luminance, the first variation range of the capacitance between the first electrode and the second electrode is less than or equal to 5%.
[0017] Wherein, ω1 is the first change amplitude of the capacitance between the first electrode and the second electrode, a is the initial value of the capacitance between the first electrode and the second electrode, and b is the measured capacitance between the first electrode and the second electrode when the luminescence brightness of the light-emitting layer decreases to 95% of the initial brightness.
[0018] Optionally, after the light-emitting layer operates for 120 hours, a change in the second capacitance between the first electrode and the second electrode is less than or equal to 10%.
[0019] Wherein, ω2 is the variation amplitude of the second capacitance between the first electrode and the second electrode, c is the initial value of the capacitance between the first electrode and the second electrode, and d is the measured capacitance between the first electrode and the second electrode when the light-emitting layer operates for 120 hours.
[0020] Optionally, the light-emitting layer generates a green light source.
[0021] Optionally, the hole mobility of the first electron blocking layer is greater than or equal to 10 -5 cm 2 V -1 s -1 , the hole carrier mobility of the second electron blocking layer is greater than or equal to 10 -6 cm 2 V -1 s -1 .
[0022] Optionally, the materials of the first electron blocking layer and the second electron blocking layer are independently selected from one of the following compounds.
[0023] Optionally, the material of the first electron blocking layer is TCTA, TAPC or BCzPh, and the material of the second electron blocking layer is CBPE or 4CzPBP.
[0024] The present application also provides an organic light-emitting display panel, comprising:
[0025] substrate;
[0026] A first electrode is provided on one side of the substrate;
[0027] a hole injection layer, disposed on a side of the first electrode away from the substrate;
[0028] a hole transport layer, disposed on a side of the hole injection layer away from the substrate;
[0029] a first electron blocking layer, disposed on a side of the hole transport layer away from the substrate;
[0030] a second electron blocking layer, disposed on a side of the first electron blocking layer away from the substrate;
[0031] a light-emitting layer, disposed on a side of the second electron blocking layer away from the substrate;
[0032] an electron transport layer, disposed on a side of the light-emitting layer away from the substrate;
[0033] an electron injection layer, disposed on a side of the electron transport layer away from the substrate;
[0034] a second electrode, disposed on a side of the electron injection layer away from the substrate;
[0035] wherein the hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer,
[0036] The materials of the first electron blocking layer and the second electron blocking layer are independently selected from one of the following compounds:
[0037] When the luminance of the light-emitting layer decreases to 95% of the initial luminance, a first variation range of the capacitance between the first electrode and the second electrode is less than or equal to 5%.
[0038] wherein ω1 is a first variation amplitude of the capacitance between the first electrode and the second electrode, a is an initial value of the capacitance between the first electrode and the second electrode, and b is a measured capacitance between the first electrode and the second electrode when the luminance of the light-emitting layer decreases to 95% of the initial luminance; or
[0039] After the light-emitting layer operates for 120 hours, the change in the second capacitance between the first electrode and the second electrode is less than or equal to 10%.
[0040] Wherein, ω2 is the variation amplitude of the second capacitance between the first electrode and the second electrode, c is the initial value of the capacitance between the first electrode and the second electrode, and d is the measured capacitance between the first electrode and the second electrode when the light-emitting layer operates for 120 hours. Beneficial effects
[0041] The present application provides an organic light-emitting display panel, which includes a substrate, a first electrode, a hole injection layer, a hole transport layer, a first electron blocking layer, a second electron blocking layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a second electrode, which are stacked in sequence. The hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer. By providing a double-layer electron blocking layer in the device, the present application improves the capacitance stability of the pixel and improves the carrier balance, thereby ensuring the luminous efficiency of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions in this application, the following is a brief introduction to the drawings required for use in the description of the implementation methods. Obviously, the drawings described below are only some implementation methods of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0043] FIG1 is a structural diagram of an organic light emitting display panel provided in one embodiment of the present application.
[0044] FIG. 2( a ) to FIG. 2 ( c ) are comparison diagrams of capacitance curves before and after aging of Examples 1, 4, and 6 of the present application. Modes for Carrying Out the Invention
[0045] The following will be combined with the drawings in the embodiment of this application to clearly and completely describe the technical solutions in this application. Obviously, the embodiment described is only a part of the embodiment of this application, not all the embodiments. Based on the embodiment of this application, all other embodiments obtained by those skilled in the art without making creative efforts are within the scope of protection of this application.
[0046] In the present application, unless otherwise expressly specified and limited, the first feature "above" or "below" the second feature may include the first and second features directly, or may include the first and second features not being directly connected but being in contact through another feature between them. Moreover, the first feature "above", "above" and "above" the second feature include the first feature being directly above and obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature "below", "below" and "below" the second feature include the first feature being directly below and obliquely below the second feature, or simply means that the first feature is lower in level than the second feature. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.
[0047] The present application provides an organic light-emitting display panel, comprising a substrate, a first electrode, a hole injection layer, a hole transport layer, a first electron blocking layer, a second electron blocking layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a second electrode, which are sequentially stacked. The hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer.
[0048] This application reduces carrier damage to the interface between the electron blocking layer and the light-emitting layer by providing a double electron blocking layer in the device, thereby improving the capacitance stability of the pixel. By adjusting the thickness ratio of the first electron blocking layer to the second electron blocking layer, the driving voltage, luminous efficiency, and lifespan of the device can be adjusted. In addition, by placing the first electron blocking layer with higher hole mobility on the side of the second electron blocking layer with lower hole mobility away from the light-emitting layer, the carrier balance can be improved, ensuring the luminous efficiency of the device.
[0049] The specific implementation of this application is described below with reference to the accompanying drawings.
[0050] Referring to FIG. 1 , an organic light-emitting display panel 100 according to one embodiment of the present application includes an anode 10, a hole injection layer 20, a hole transport layer 30, an electron blocking layer 40, a light-emitting layer 50, a hole blocking layer 60, an electron transport layer 70, an optical coupling layer 80, and a cathode 90, which are stacked in sequence. The organic light-emitting device in the organic light-emitting display panel 100 in this embodiment is an upright OLED device. It will be appreciated that the organic light-emitting device in the organic light-emitting display panel 100 in other embodiments of the present application may also be an inverted OLED device.
[0051] The anode 10 and the cathode 90 are independently selected from a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode. The material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide. The composite electrode of metal and metal oxide is selected from one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS. The material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba.
[0052] The hole injection layer 20 is a layer for injecting holes from the anode 10, and the material of the hole injection layer 20 is preferably a compound capable of transporting holes. Specific examples of the hole injection material include metal porphyrins, oligothiophenes, arylamine-based organic materials, hexanitrile hexaazatriphenylene-based organic materials, quinacridone-based organic materials, perylene-based organic materials, anthraquinone, and polyaniline-based and polythiophene-based conductive polymers, but are not limited thereto.
[0053] The hole transport layer 30 receives holes from the hole injection layer 20 and transports the holes to the light-emitting layer 50. Suitable hole transport materials include those that can receive holes from the anode 10 or the hole injection layer 20, move the holes to the light-emitting layer 50, and have high hole mobility. Specific examples of hole transport materials include, but are not limited to, arylamine-based organic materials, conductive polymers, and block copolymers having both conjugated and non-conjugated portions.
[0054] The electron blocking layer 40 has the function of transporting holes and blocking electrons from reaching the hole transport layer 30, thereby increasing the probability of recombination between electrons and holes in the light-emitting layer 50. The electron blocking layer 40 includes a first electron blocking layer 41, a second electron blocking layer 42, and a third electron blocking layer 43. The light-emitting layer 50 includes a green light-emitting layer 51, a red light-emitting layer 52, and a blue light-emitting layer 53. The green light-emitting layer 51, the red light-emitting layer 52, and the blue light-emitting layer 53 are arranged side by side on the electron blocking layer 40. The first electron blocking layer 41 and the second electron blocking layer 42 are stacked and arranged between the green light-emitting layer 51 and the anode 10. The first electron blocking layer 41 is arranged between the second electron blocking layer 42 and the anode 10. The third electron blocking layer 43 is arranged between the red light-emitting layer 52, the blue light-emitting layer 53, and the anode 10. That is, a double-layer electron blocking layer is provided in the green pixel, and a single-layer blocking layer is provided in the red and blue pixels. Furthermore, the hole mobility of the first electron blocking layer 41 is greater than the hole mobility of the second electron blocking layer 42 .
[0055] In the prior art, organic light-emitting display panels usually use a single-layer electron blocking layer. The hole carriers injected by the anode are all accumulated at the interface between the electron blocking layer and the light-emitting layer, causing greater damage to the interface between the electron blocking layer and the light-emitting layer, resulting in poor performance of the device in the capacitance reliability analysis experiment, that is, poor device stability. Among them, after the same usage time, the capacitance of the blue pixel and the red pixel changes less than the initial value, while the capacitance of the green pixel changes more than the initial value. After working for a long time, the threshold voltage at which the green pixel in the product is lit will become lower than that of the blue and red pixels, causing the product to have a greening problem at low brightness (low grayscale). In this embodiment, by using a double-layer electron blocking layer 40 in the green pixel, the hole carriers injected by the anode 10 are dispersed at the interface between the first electron blocking layer 41 and the second electron blocking layer 42 and the interface between the second electron blocking layer 42 and the light-emitting layer 50, reducing the hole carrier concentration, reducing interface damage, and improving capacitance stability. By improving the capacitance stability of the green pixel, the green light emission of the display panel at low voltage is improved.
[0056] It can be understood that in this embodiment, a double-layer electron blocking layer is only used in the green pixel, but in other embodiments of the present application, a double-layer electron blocking layer can also be used in the red pixel or the green pixel, or a double-layer electron blocking layer can be used in two or three of the red pixel, green pixel and blue pixel to improve their capacitance stability.
[0057] On this basis, the function of the first electron blocking layer 41 is to adjust the driving voltage, and the function of the second electron blocking layer 42 is to adjust the device luminous efficiency and device life. Specifically, since the hole transport rate of the first electron blocking layer 41 is high, by increasing the proportion of the first electron blocking layer 41, the driving voltage can be reduced, while the hole transport rate of the second electron blocking layer 42 is low. By increasing the proportion of the second electron blocking layer 42, the injection of hole carriers into the light-emitting layer 50 can be restricted, thereby improving the carrier balance and improving the luminous efficiency. Thus, by keeping the total thickness of the first electron blocking layer 41 and the second electron blocking layer 42 unchanged, by adjusting the relative thickness of the first electron blocking layer 41 and the second electron blocking layer 42, both the driving voltage and the luminous efficiency can be adjusted. However, if the mobility of the second electron blocking layer 42 is too fast, it will affect the carrier balance in the electron blocking layer 40 and affect the luminous efficiency of the device. Therefore, the first electron blocking layer 41 with higher hole mobility is placed on the side of the second electron blocking layer 42 with lower hole mobility away from the light-emitting layer 50.
[0058] Optionally, the hole mobility of the first electron blocking layer 41 is greater than or equal to 10 -5 cm 2 V -1 s -1 , the hole carrier mobility of the second electron blocking layer 42 is greater than or equal to 10 -6 cm 2 V -1 s -1 If the hole mobility of the first electron blocking layer 41 and the second electron blocking layer 42 is too low, the device voltage will be too high, resulting in the product power consumption not meeting the standard.
[0059] Optionally, the light-emitting layer 50 includes a host material and a guest material. To prevent triplet (T-state) excitons generated in the host material in the light-emitting layer 50 from overflowing to the electron blocking layer 40, the first electron blocking layer 41, the second electron blocking layer 42, and the first triplet excited state T1 energy level of the host material are gradually reduced.
[0060] Optionally, the first triplet excited state energy level difference between the first electron blocking layer 41 and the second electron blocking layer 42 is greater than or equal to 0.1 eV, and the first triplet excited state energy level difference between the second electron blocking layer 42 and the host material is greater than or equal to 0.1 eV. If the first triplet excited state energy level difference between the first electron blocking layer 41 and the second electron blocking layer 42 is less than 0.1 eV, the effect of preventing T-state exciton overflow may be insufficient.
[0061] Optionally, the first triplet excited state energy level of the host material is greater than or equal to 2.6 eV, the first triplet excited state energy level of the second electron blocking layer 42 is greater than or equal to 2.7 eV, and the first triplet excited state energy level of the first electron blocking layer 41 is greater than or equal to 2.8 eV. The T1 energy level of the green guest material (Dopant) is approximately 2.4-2.5 eV, so the green guest material can have a lower limit of 2.6 eV.
[0062] Optionally, to facilitate carrier transport, the highest occupied molecular orbital (HOMO) energy levels of the first electron blocking layer 41, the second electron blocking layer 42, and the host material decrease. The HOMO energy difference between the first electron blocking layer 41 and the second electron blocking layer 42 is less than or equal to 0.2 eV, the HOMO energy difference between the second electron blocking layer 42 and the host material is less than or equal to 0.2 eV, the HOMO energy level range of the first electron blocking layer is between -5.4 eV and -5.6 eV, and the HOMO energy level range of the second electron blocking layer is between -5.5 eV and -5.7 eV.
[0063] Optionally, the highest occupied orbital energy level of the hole transport layer 30 is greater than or equal to the highest occupied orbital energy level of the first electron blocking layer 41. To facilitate carrier transport, the highest occupied orbital (HOMO) energy levels of the hole transport layer 30, the first electron blocking layer 41, the second electron blocking layer 42, and the host material decrease in sequence. In practical applications, the difference between the highest occupied orbital energy level of the hole transport layer 30 and the highest occupied orbital energy level of the first electron blocking layer 41 is less than or equal to the difference between the highest occupied orbital energy level of the first electron blocking layer 41 and the highest occupied orbital energy level of the second electron blocking layer 42. The difference between the highest occupied orbital energy peaks of the hole transport layer 30 and the first electron blocking layer 41 is less than or equal to 0.2 eV.
[0064] Optionally, the carrier tolerance of the first electron blocking layer 41 is less than the carrier tolerance of the second electron blocking layer 42. The so-called "carrier tolerance" refers to the stability of the electron blocking layer relative to the carriers. The stronger the carrier tolerance of the electron blocking layer, the smaller the performance change under the impact of the carriers. If the carrier tolerance is strong, when used in a device, the amplitude of the capacitance change of the device will be small as the device increases with the use time. That is, after the same aging time, the smaller the amplitude of the capacitance change of the device, the higher the carrier stability of the electron blocking layer. Holes are injected from the anode 10, and most of them accumulate at the interface between the electron blocking layer 40 and the light-emitting layer 50. By making the second electron blocking layer 42 with good carrier tolerance directly contact the light-emitting layer 50, the damage to the light-emitting layer 50 is reduced, the decrease in capacitance is alleviated, and the device life is improved.
[0065] Optionally, the thickness of the first electron blocking layer 41 is greater than the thickness of the second electron blocking layer 42. The present application does not limit the preferred range and ratio of the thickness of the first electron blocking layer 41 to the thickness of the second electron blocking layer 42. Different preferred ranges and ratios of thickness can be set for different material combinations. For example, considering mass production, the thickness of the second electron blocking layer 42 does not exceed 200 angstroms. In addition, the second electron blocking layer 42 generally has a lower hole mobility. If the second electron blocking layer 42 is thicker than the first electron blocking layer 41, a voltage surge may occur. Therefore, the thickness of the first electron blocking layer 41 is set to be greater than the thickness of the second electron blocking layer 42 to avoid excessive driving voltage.
[0066] Optionally, the materials of the first electron blocking layer 41 and the second electron blocking layer 42 are independently selected from one of the following compounds.
[0067] Optionally, the material of the first blocking layer includes TCTA, TAPC, or BCzPh, and the material of the second blocking layer includes CBPE or 4CzPBP. Specifically, the material of the first electron blocking layer 41 can be TCTA, TAPC, or BCzPh, and the material of the second electron blocking layer 42 can be CBPE or 4CzPBP. The first electron blocking layer 41 and the second electron blocking layer 42 can also include other functional materials in addition to the above-mentioned electron blocking materials. Compared with TCTA, TAPC, and BCzPh, CBPE and 4CzPBP have higher luminous efficiency and smaller capacitance variation (derived from carrier tolerance), and therefore, are more suitable as the second electron blocking layer 42.
[0068] The light-emitting material of the light-emitting layer 50 is a material capable of emitting light in the visible light region by receiving holes and electrons from the hole transport layer 30 and the electron transport layer 70, respectively, and combining the holes and electrons. Specific examples thereof include: 8-hydroxy-quinoline aluminum complex (Alq3); carbazole-based compounds; diphenylethylene compounds; BAlq; 10-hydroxybenzoquinoline-metal compounds; benzo-based azoles, benzothiazole-based and benzimidazole-based compounds; poly(p-phenylenevinylene) (PPV)-based polymers; spiro compounds; polyfluorenes; rubrene, and the like, but are not limited thereto.
[0069] The light-emitting layer 50 may include a host material and a dopant material. The host material includes fused aromatic ring derivatives, heterocyclic compounds, and the like. Specifically, fused aromatic ring derivatives include anthracene derivatives, pyrene derivatives, naphthalene derivatives, pentacene derivatives, phenanthrene compounds, fluoranthene compounds, and the like. Heterocyclic compounds include carbazole derivatives, dibenzofuran derivatives, ladder-type furan compounds, pyrimidine derivatives, and the like. However, the materials are not limited thereto.
[0070] Dopant materials, i.e., guest materials include aromatic amine derivatives, styrylamine compounds, boron complexes, fluoranthene compounds, metal complexes, etc. Specifically, aromatic amine derivatives are fused aromatic ring derivatives having substituted or unsubstituted arylamino groups, and include pyrene, anthracene, diindenophenone, ... Styrylamine compounds are compounds in which a substituted or unsubstituted arylamine is substituted with at least one arylvinyl group, and one, two, or more substituents selected from aryl, silyl, alkyl, cycloalkyl, and arylamino groups are substituted or unsubstituted. Specifically, examples include styrylamine, styryldiamine, styryltriamine, and styryltetramine, but are not limited thereto. Furthermore, metal complexes include, but are not limited to, iridium complexes and platinum complexes.
[0071] Optionally, the luminescence mechanism of the blue light-emitting layer 53 is efficient blue emission induced by triplet-triplet annihilation (TTA).
[0072] The hole-blocking layer 60, in a broad sense, functions as an electron transport layer. The hole-blocking layer 60 transports electrons while preventing holes from reaching the electron transport layer, thereby increasing the probability of recombination between electrons and holes in the light-emitting layer 50. The material for the hole-blocking layer 60 can be any of the materials for the electron transport layer described below, as needed.
[0073] The electron transport layer 70 receives electrons from the electron injection layer and transports them to the light-emitting layer 50. Suitable electron transport materials include those that can advantageously receive electrons from the cathode 90 and move them to the light-emitting layer 50, and have high electron mobility. Specific examples include, but are not limited to, Al complexes of 8-hydroxyquinoline; complexes containing Alq3; organic free radical compounds; and hydroxyflavone-metal complexes.
[0074] The optical coupling layer 80 can further extract the light emitted by the light emitting layer 50 to improve the luminous efficiency of the light emitting layer 50. The material of the optical coupling layer 80 can be, for example, an organic material.
[0075] It can be understood that the organic light-emitting display panel 100 of the present application can omit some unnecessary film layers as needed, such as the hole injection layer 20, the hole transport layer 30, the hole blocking layer 60, and the optical coupling layer 80, and can also add film layers such as the electron transport layer as needed.
[0076] The organic light-emitting display panel 100 of the present application may only include an anode 10 , an electron blocking layer 40 , a light-emitting layer 50 , and a cathode 90 , which are stacked in sequence.
[0077] The present invention will be described below with reference to specific embodiments, but the present invention is not limited to the following embodiments. It should be understood that the appended claims summarize the scope of the present invention. Under the guidance of the concept of the present invention, those skilled in the art should realize that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.
[0078] The inventors selected five different electron blocking materials for research, namely, CBPE, 4CzPBP, TCTA, TAPC and BCzPh, and prepared the green electroluminescent top light-emitting devices in Comparative Examples 1 to 5 using these five materials.
[0079] Comparative Example 1
[0080] A green electroluminescent top-emitting device was prepared with the following structure: from bottom to top: a glass substrate; an anode 10 made of indium tin oxide (ITO) with a thickness of 195 nm; a hole transport layer 30 made of NPB with a thickness of 120 nm; an electron blocking layer 40 made of TCTA with a thickness of 40 nm; a light-emitting layer 50 made of mCBP as a host material and doped with Ir(ppy)3 at a doping concentration of 6 wt% and a thickness of 40 nm; an electron transport layer 70 made of TPBi with a thickness of 35 nm; and a cathode 90 made of a Mg:Ag (mass ratio 1:10) mixed electrode with a thickness of 12 nm. During device preparation, the organic material was deposited at a rate of 1 A / s, and the metal material was deposited at a rate of 2 A / s.
[0081] Comparative Example 2
[0082] The difference between Comparative Example 2 and Comparative Example 1 is that the material of the electron blocking layer 40 is TAPC.
[0083] Comparative Example 3
[0084] The difference between Comparative Example 3 and Comparative Example 1 is that the material of the electron blocking layer 40 is BCzPh.
[0085] Comparative Example 4
[0086] The difference between Comparative Example 4 and Comparative Example 1 is that the material of the electron blocking layer 40 is CBPE.
[0087] Comparative Example 5
[0088] The difference between Comparative Example 5 and Comparative Example 1 is that the material of the electron blocking layer 40 is 4CzPBP.
[0089] For comparative examples 1 to 5, the voltage @J10, CE, CIEx, LT95 @ 50 mA / cm2 and capacitance change amplitude were measured respectively.
[0090] Voltage @J10 indicates that the current density reaches 10mAcm 2 The voltage at this time is measured by a Keithley 2400 digital source meter.
[0091] CIEx stands for color coordinates. The CIEx test is used to verify that the device in the present embodiment is green and to allow comparison of all devices under the same color. CIEx is measured using a PR 655 spectrometer.
[0092] CE (Current efficiency) represents current efficiency. It is calculated using a formula after the test computer collects current information from a Keithley 2400 SourceMeter instrument and optical information from a PR 655 spectrometer.
[0093] LT95@50mA / cm 2 Detect when the current density reaches 50mA / cm 2 , the time it takes for the initial brightness of the light-emitting device to decay to 95%.
[0094] The capacitance was measured using a Zurich Instruments impedance analyzer.
[0095] The key indicator of capacitance change is the peak capacitance change before and after the OLED device is operated. The capacitance difference before and after operation can be characterized by two test conditions:
[0096] 1. The first method is to measure the initial capacitance and pass the current density of 50mA / cm 2 (J50) current, under normal temperature conditions, after the brightness decays to 95% of the initial brightness, the capacitance after the test is compared with the initial capacitance to obtain the difference before and after;
[0097] 2. The second method is to measure the initial capacitance and pass the current density of 10mA / cm 2 (J10) current, work at 85℃ for 120 hours, take out the capacitance after test, compare it with the initial capacitance, and get the difference before and after.
[0098] The steps for testing J50 capacitors at room temperature include:
[0099] Initial capacitance test: Use an impedance analyzer to perform an initial capacitance test on the device.
[0100] Normal temperature operation: At normal temperature, a current density of 50mA / cm is applied to the above device. 2of current.
[0101] After-value capacitance test: When the brightness of the above device decays to 95% of the initial brightness, take it out and perform after-value capacitance test on the device again using an impedance analyzer.
[0102] Define the initial peak capacitance of the device as a, the peak capacitance after working at room temperature J50 as b, and the change range is 1.
[0103] The steps for high temperature J10 capacitor testing include:
[0104] Initial capacitance test: Use an impedance analyzer to perform an initial capacitance test on the device.
[0105] High temperature operation: At a temperature of 85°C, a current density of 10 mA / cm is applied to the above device. 2 of current.
[0106] After-value capacitance test: After the above device has been operated continuously for 120 hours under the conditions, it is taken out and the after-value capacitance test of the device is performed again using an impedance analyzer.
[0107] Define the initial peak capacitance of the device as c, and the peak capacitance after 120hr of high temperature J10 operation as d, and its change range is 2,
[0108] Capacitance test method:
[0109] The capacitance test frequencies in this proposal are 60Hz, 120Hz, 1KHz and 10KHz respectively.
[0110] Table 1 Performance test data of comparative examples 1 to 5
[0111] The experimental results in Table 1 show that when used alone as electron-blocking layers, the capacitance of each of the five electron-blocking materials exhibited significant changes before and after aging. Of these, the capacitance changes before and after aging for CBPE and 4CzPBP were relatively small. Therefore, CBPE and 4CzPBP are considered suitable for use as the second electron-blocking layer, while TCTA, TAPC, and BCzPh are suitable for use as the first electron-blocking layer. Next, the inventors fabricated green electroluminescent devices of Examples 1 to 12 using these five materials as electron-blocking layer materials.
[0112] Example 1
[0113] A green electroluminescent top-emitting device with the following structure was prepared: from bottom to top: a glass substrate; an anode 10 made of indium tin oxide (ITO) with a thickness of 195 nm; a hole transport layer made of NPB with a thickness of 120 nm; a first electron blocking layer made of TCTA with a thickness of 350 angstroms; a second electron blocking layer made of CBPE with a thickness of 50 angstroms; a light-emitting layer made of mCBP as a host material and doped with Ir(ppy)3 at a doping concentration of 6 wt% and a thickness of 40 nm; an electron transport layer made of TPBi with a thickness of 35 nm; and a cathode made of a Mg:Ag (mass ratio 1:10) mixed electrode with a thickness of 12 nm. During device preparation, the organic material was deposited at a rate of 1 A / s, and the metal material was deposited at a rate of 2 A / s.
[0114] Example 2
[0115] The difference between Example 2 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TCTA, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is CBPE, and the thickness is 100 angstroms.
[0116] Example 3
[0117] The difference between Example 3 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TCTA, and the thickness is 350 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 50 angstroms.
[0118] Example 4
[0119] The difference between Example 4 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TCTA, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 100 angstroms.
[0120] Example 5
[0121] The difference between Example 5 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TAPC, with a thickness of 350 angstroms; the material of the second electron blocking layer 42 is CBPE, with a thickness of 50 angstroms.
[0122] Example 6
[0123] The difference between Example 6 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TAPC, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is CBPE, and the thickness is 100 angstroms.
[0124] Example 7
[0125] The difference between Example 7 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TAPC, and the thickness is 350 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 50 angstroms.
[0126] Example 8
[0127] The difference between Example 8 and Comparative Example 1 is that the material of the first electron blocking layer 41 is TAPC, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 100 angstroms.
[0128] Example 9
[0129] The difference between Example 9 and Comparative Example 1 is that the material of the first electron blocking layer 41 is BCzPh, and the thickness is 350 angstroms; the material of the second electron blocking layer 42 is CBPE, and the thickness is 50 angstroms.
[0130] Example 10
[0131] The difference between Example 10 and Comparative Example 1 is that the material of the first electron blocking layer 41 is BCzPh, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is CBPE, and the thickness is 100 angstroms.
[0132] Example 11
[0133] The difference between Example 11 and Comparative Example 1 is that the material of the first electron blocking layer 41 is BCzPh, and the thickness is 350 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 50 angstroms.
[0134] Example 12
[0135] The difference between Example 12 and Comparative Example 1 is that the material of the first electron blocking layer 41 is BCzPh, and the thickness is 300 angstroms; the material of the second electron blocking layer 42 is 4CzPBP, and the thickness is 100 angstroms.
[0136] Table 2 Performance test data of Examples 1 to 12
[0137] From the comparison between Table 1 and Table 2, it can be seen that compared with the comparative examples 1 to 5 with a single electron blocking layer, the voltage @ J10 of the examples 1 to 12 using the double electron blocking layer 40 is significantly reduced, and the LT95 @ 50 mA / cm 2 The results show that the double-layer barrier layer can significantly improve the driving voltage, improve the device life, and improve the capacitance stability.
[0138] In addition, please refer to Figures 2(a) to 2(c). In these Figures, the solid black line represents the capacitance curve before aging, and the dashed black line represents the capacitance curve after aging. Figures 2(a) to 2(c) show that the capacitance of Example 6, which uses a double-layer electron blocking layer, decreases much more slowly than that of Examples 1 and 4, demonstrating its capacitance stabilization effect.
[0139] The above provides a detailed introduction to the implementation methods of this application. Specific examples are used herein to illustrate the principles and implementation methods of this application. The above description of the implementation methods is intended only to help understand this application. At the same time, those skilled in the art may vary the specific implementation methods and application scopes based on the concepts of this application. In summary, the contents of this specification should not be construed as limiting this application.
Claims
1. An organic light emitting display panel, comprising: substrate; A first electrode is arranged on one side of the substrate; A hole injection layer is arranged on a side of the first electrode away from the substrate; A hole transport layer, disposed on a side of the hole injection layer away from the substrate; A first electron blocking layer is disposed on a side of the hole transport layer away from the substrate; A second electron blocking layer is disposed on a side of the first electron blocking layer away from the substrate; A light-emitting layer is disposed on a side of the second electron blocking layer away from the substrate; An electron transport layer is arranged on a side of the light-emitting layer away from the substrate; An electron injection layer, disposed on a side of the electron transport layer away from the substrate; A second electrode is disposed on a side of the electron injection layer away from the substrate; Among them, the hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer.
2. The organic light emitting display panel according to claim 1, wherein: The first triplet excited state energy level of the first electron blocking layer is greater than the first triplet excited state energy level of the second electron blocking layer, and the first triplet excited state energy level of the second electron blocking layer is greater than the first triplet excited state energy level of the light emitting layer.
3. The organic light emitting display panel according to claim 2, wherein: The difference between the first triplet excited state energy level of the first electron blocking layer and the first triplet excited state energy level of the second electron blocking layer is greater than or equal to 0.1 eV; A difference between a first triplet excited state energy level of the second electron blocking layer and a first triplet excited state energy level of the light emitting layer is greater than or equal to 0.1 eV.
4. The organic light emitting display panel according to claim 1, wherein: The difference between the highest occupied orbital energy levels of the first electron blocking layer and the second electron blocking layer is less than or equal to 0.2 eV, and the difference between the highest occupied orbital energy levels of the second electron blocking layer and the light-emitting layer is less than or equal to 0.2 eV.
5. The organic light emitting display panel according to claim 4, wherein: The highest occupied orbital energy level of the first electron block is in the range of -5.4 eV to -5.6 eV, and the highest occupied orbital energy level of the second electron block is in the range of -5.5 eV to -5.7 eV.
6. The organic light emitting display panel according to claim 1, wherein: A highest occupied orbital energy level of the hole transport layer is greater than or equal to a highest occupied orbital energy level of the first electron blocking layer.
7. The organic light emitting display panel according to claim 6, wherein: The difference between the highest occupied orbital energy level of the hole transport layer and the highest occupied orbital energy level of the first electron blocking layer is less than or equal to the difference between the highest occupied orbital energy level of the first electron blocking layer and the highest occupied orbital energy level of the second electron blocking layer.
8. The organic light emitting display panel according to claim 6, wherein: The difference between the highest occupied orbital energy limits of the hole transport layer and the first electron blocking layer is less than or equal to 0.2 eV.
9. The organic light emitting display panel according to claim 1, wherein: The carrier tolerance of the first electron blocking layer is smaller than the carrier tolerance of the second electron blocking layer.
10. The organic light emitting display panel according to claim 1, wherein: The thickness of the first electron blocking layer is greater than the thickness of the second electron blocking layer.
11. The organic light emitting display panel according to claim 1, wherein: When the luminance of the luminous layer decreases to 95% of the initial luminance, a first variation amplitude of the capacitance between the first electrode and the second electrode is less than or equal to 5%. Among them, ω1 is the first change amplitude of the capacitance between the first electrode and the second electrode, a is the initial value of the capacitance between the first electrode and the second electrode, and b is the measured capacitance between the first electrode and the second electrode when the luminescence brightness of the light-emitting layer decreases to 95% of the initial brightness.
12. The organic light emitting display panel according to claim 1, wherein: After the light-emitting layer operates for 120 hours, the variation of the second capacitance between the first electrode and the second electrode is less than or equal to 10%. Wherein, ω2 is the variation amplitude of the second capacitance between the first electrode and the second electrode, c is the initial value of the capacitance between the first electrode and the second electrode, and d is the measured capacitance between the first electrode and the second electrode when the light-emitting layer works for 120 hours.
13. The organic light emitting display panel according to claim 1, wherein: The light emitting layer generates a green light source.
14. The organic light emitting display panel according to claim 1, wherein: The hole mobility of the first electron blocking layer is greater than or equal to 10 -5 cm 2 V -1 s -1 , the hole carrier mobility of the second electron blocking layer is greater than or equal to 10 -6 cm 2 V -1 s -1 .
15. The organic light emitting display panel according to claim 1, wherein: The materials of the first electron blocking layer and the second electron blocking layer are independently selected from one of the following compounds:
16. The organic light emitting display panel according to claim 15, wherein: The material of the first electron blocking layer is TCTA, TAPC or BCzPh, and the material of the second electron blocking layer is CBPE or 4CzPBP.
17. An organic light emitting display panel, comprising: substrate; A first electrode is arranged on one side of the substrate; A hole injection layer is arranged on a side of the first electrode away from the substrate; A hole transport layer, disposed on a side of the hole injection layer away from the substrate; A first electron blocking layer is disposed on a side of the hole transport layer away from the substrate; A second electron blocking layer is disposed on a side of the first electron blocking layer away from the substrate; A light-emitting layer is disposed on a side of the second electron blocking layer away from the substrate; An electron transport layer is arranged on a side of the light-emitting layer away from the substrate; An electron injection layer, disposed on a side of the electron transport layer away from the substrate; A second electrode is disposed on a side of the electron injection layer away from the substrate; wherein the hole mobility of the first electron blocking layer is greater than the hole mobility of the second electron blocking layer, the highest occupied orbital energy level of the first electron blocking layer is greater than the highest occupied orbital energy level of the second electron blocking layer, and the highest occupied orbital energy level of the second electron blocking layer is greater than the highest occupied orbital energy level of the light-emitting layer, The materials of the first electron blocking layer and the second electron blocking layer are independently selected from one of the following compounds: When the luminance of the luminous layer decreases to 95% of the initial luminance, a first variation amplitude of the capacitance between the first electrode and the second electrode is less than or equal to 5%. Wherein, ω1 is a first variation amplitude of the capacitance between the first electrode and the second electrode, a is an initial value of the capacitance between the first electrode and the second electrode, and b is a measured capacitance between the first electrode and the second electrode when the luminance of the luminous layer decreases to 95% of the initial luminance; or After the light-emitting layer operates for 120 hours, the variation of the second capacitance between the first electrode and the second electrode is less than or equal to 10%. Wherein, ω2 is the variation amplitude of the second capacitance between the first electrode and the second electrode, c is the initial value of the capacitance between the first electrode and the second electrode, and d is the measured capacitance between the first electrode and the second electrode when the light-emitting layer works for 120 hours.
18. The organic light emitting display panel according to claim 17, wherein: The first triplet excited state energy level of the first electron blocking layer is greater than the first triplet excited state energy level of the second electron blocking layer, and the first triplet excited state energy level of the second electron blocking layer is greater than the first triplet excited state energy level of the light emitting layer.
19. The organic light emitting display panel according to claim 18, wherein: The difference between the first triplet excited state energy level of the first electron blocking layer and the first triplet excited state energy level of the second electron blocking layer is greater than or equal to 0.1 eV; A difference between a first triplet excited state energy level of the second electron blocking layer and a first triplet excited state energy level of the light emitting layer is greater than or equal to 0.1 eV.
20. The organic light emitting display panel according to claim 17, wherein: The difference between the highest occupied orbital energy levels of the first electron blocking layer and the second electron blocking layer is less than or equal to 0.2 eV, and the difference between the highest occupied orbital energy levels of the second electron blocking layer and the light-emitting layer is less than or equal to 0.2 eV.
Citation Information
Patent Citations
Display panel and display device
CN113437231A
Light-emitting device, display panel and display device
CN115867063A
Organic light emitting element and light source device
JP2017054870A