Method for extracting mg and al by using LF refining slag

By reacting LF refining slag with FeSi powder in a vacuum chamber to generate and recover Mg and Al, it solves the low reuse rate of LF refining slag and the high energy consumption and pollution problems in the traditional Mg and Al production process, and achieves high additional value for resource recovery and economic benefits.

WO2024216882A1PCT designated stage expired Publication Date: 2024-10-24ANSTEEL BEIJING RES INST CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/124860
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2023-10-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

In the existing technology, the reuse rate of LF refining slag is low, resulting in resource waste and environmental pollution. At the same time, the traditional thermal reduction method to produce Mg and Al consumes high energy and costs, and causes serious environmental pollution.

Method used

Using LF refining slag as raw material, it reacts with FeSi powder as a reducing agent in a vacuum chamber to generate gaseous Mg and Al, which are recovered through cooling to realize the extraction and reuse of high value-added Mg and Al, avoiding the traditional process high energy consumption and environmental pollution.

Benefits of technology

It achieves efficient recycling of LF refining slag, saves energy, reduces production costs, avoids waste of resources and environmental pollution, provides high economic benefits of Mg and Al, and provides a new direction for the large-scale utilization of LF refining steel slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023124860_24102024_PF_FP_ABST
    Figure CN2023124860_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention is a method for extracting Mg and Al by using LF refining slag. The method comprises the following steps: a, pouring the poured LF refining slag into a slag tank from a steel ladle, placing the slag tank in a vacuum chamber, adding a reducing agent to the LF refining slag and mixing same to obtain a mixed reaction material; and b, after vacuumizing, heating the mixed reaction material in the slag tank to perform a reaction, and respectively condensing and recovering generated gaseous Mg and Al at a cooling end outside the vacuum chamber to obtain solid Mg and Al. In the method of the present invention, the LF refining slag is used as the raw material, and the residual heat thereof is effectively used to produce Mg and Al with high added values, such that not only is the green treatment problem of LF refining slag solved, and the defects of a traditional thermal reduction method for producing Mg are avoided, but the recovered Mg and Al can be applied to steelmaking production again, thereby solving the problem of large-scale utilization of LF refining steel slag and also obtaining relatively high economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

A method for extracting Mg and Al using LF refined slag Technical Field

[0001] The invention belongs to the technical field of steelmaking slag utilization, and particularly relates to a method for extracting Mg and Al by utilizing LF refined slag. Background Art

[0002] The ladle top slag after LF refining has the characteristics of high basicity, good metallurgical properties, reasonable composition and fast slagging. Except for some furnace slags with high sulfur content, the sulfur in most furnace slags is not saturated and can be returned to the refining process for secondary or even tertiary use.

[0003] While scholars both domestically and internationally have conducted extensive research on the recycling and reuse of LF refined slag, no steel company has yet fully recycled it, resulting in a recycling rate of less than 20%. Unrecyclable LF slag is ultimately dumped into slag pots and transported to slag yards, where it is ultimately disposed of along with converter or electric furnace slag. Because slag contains phosphorus, its blending potential is limited, making it virtually unsuitable for sintering. After metallic Fe is recovered, the slag is stored in piles, occupying and polluting land. Large quantities of slag are either discarded or used as raw material to produce low-value-added products such as cement. The significant dust generation from pulverization during storage poses a threat to environmental protection and wastes resources. This creates significant environmental challenges and becomes a major obstacle to social progress and economic development.

[0004] Therefore, it is necessary to provide a high-value-added energy-saving and emission-reduction method for recycling LF refined slag to solve the shortcomings of low reuse rate of LF refined slag, easy dust generation during stacking, great environmental pollution and low value-added utilization, and realize high-value-added recycling of LF refined slag, and ultimately achieve the goal of circular production and zero emissions.

[0005] Summary of the Invention

[0006] The present invention is based on the inventors' discovery and understanding of the following facts and problems: In the related art, the research methods for recycling LF refined slag all have some defects, which are mainly manifested in: (1) Refining hot slag circulation process. Many steel companies have implemented heat recovery experiments on residual steel slag after refining, but due to the limitations of factory buildings, lifting equipment, product outlines and production organization, the hot slag circulation ratio is low; (2) After the refined slag is cooled and crushed, its heat cannot be fully utilized for solid reuse. The slag formation speed of the next cycle using cold slag is slow, which is not conducive to energy saving and consumption reduction; (3) The LF refined slag thermal oxidation method for desulfurization technology is difficult to implement due to the limitation of production space, and high-temperature gas with a temperature of 1300-1450°C is difficult to ensure; (4) The solid-state hydrothermal leaching method for desulfurization wastes a large amount of cooling water and steel slag heat during the treatment process, and also causes secondary pollution.

[0007] The main industrial magnesium smelting methods include electrolysis, carbothermal reduction, the Pidgeon process, and the Magnetherm semi-continuous magnesium smelting process. Carbothermal reduction was only used in factories in the 1930s and 1940s. Currently, electrolysis and the Pidgeon process are the only mainstream industrial methods worldwide. Before the mid-1990s, electrolysis accounted for over 80% of global magnesium production, while the Pidgeon and Magnetherm processes accounted for only about 20%. Since the early 2000s, the Magnetherm process has been largely discontinued, and electrolysis has also declined significantly, leaving the Pidgeon process alone with over 80% of global production.

[0008] Thermal reduction is one of the methods for producing metallic Mg. It mainly uses dolomite, magnesite, etc. as raw materials. MgO is sintered in the middle section of the kiln, and then a reducing agent is added to heat and reduce it to metallic magnesium in a reduction furnace. The Pijiang process is widely used at home and abroad to refine magnesium. That is, calcined dolomite (MgO, Cao) is used as raw material, ferrosilicon is used as a reducing agent, and they are mixed in a certain proportion and ground into fine powder. The powder is pressed into agglomerates and loaded into a reduction tank. The magnesium vapor is heated and crystallized in a reduction furnace to obtain magnesium vapor. The solid magnesium is condensed and crystallized, and then melted into magnesium ingots. The advantage of this method is simplicity. The disadvantage is that the raw materials are heated after mixing in a cold state, and the production process consumes a lot of energy. The calcination of dolomite and the thermal reduction of magnesium refining processes are both carried out at high temperatures, last for a long time, and require a large amount of fuel. Moreover, the two processes are carried out separately, which further increases the fuel consumption and processing costs of the production process.

[0009] Whether it is the Pidgeon process or the French Magnetherm semi-continuous magnesium smelting process, both use ferrosilicon, especially ferrosilicon with a silicon content of more than 75% (usually 75 # Ferrosilicon) is used as a reducing agent, and ore containing MgO is used as a raw material for magnesium smelting. It is then ground, mixed, and pressed into balls with a mineralizer (CaF2) in a certain proportion. The balls are then placed in a reduction tank, where they are subjected to high temperature and high vacuum (1200°C, 13Pa) to react and form Mg vapor, which is then crystallized to form metallic Mg. The role of the mineralizer (CaF2) is to lower the temperature at which the liquid phase appears and accelerate the reaction rate.

[0010] Under high temperature and vacuum conditions, the chemical reaction of Si reducing MgO is shown in formula (1). 2MgO+Si=SiO2+2Mg(gas) (1)

[0011] The disadvantages of traditional thermal reduction method for producing Mg are: 1) dolomite, magnesite and other raw materials are used in production, and the mining process damages the natural ecological environment; 2) dolomite, magnesite and other raw materials need to be burned into MgO in the middle section of the kiln. The calcination is carried out at high temperature, which takes a long time and consumes a lot of fuel. The fuel consumption and processing cost of the production process are high; 3) the thermal reduction magnesium production process requires the raw materials to be mixed from room temperature and then heated in a cold state to the high temperature of 1200-1250℃ required for the reaction. It takes a long time and also consumes a lot of fuel. It is carried out separately from process 1), which further increases the fuel consumption and processing cost of the production process; 4) the Pijiang method uses external heating, and the heat is gradually transferred from the outside of the reactor to the inside. The production cycle is long, the heat loss is large, and the thermal energy utilization rate is low. Analysis shows that the thermal energy utilization rate of the typical process is only about 20%; 5) the production process is seriously polluted by smoke and dust, the working environment is poor, and the surrounding ecological environment is deteriorated; 6) CaF2 needs to be added during production, which pollutes the environment.

[0012] Aluminum and its alloys are among the most widely used and economically viable materials. Due to its high reactivity, aluminum can currently only be produced on a large scale through electrolysis. However, this process is energy-intensive and costly, leading researchers to explore various economical methods for aluminum production.

[0013] The present invention aims to address, at least to a certain extent, one of the technical problems in the related art. To this end, embodiments of the present invention provide a method for extracting Mg and Al from LF refined slag. This method uses LF refined slag as a raw material and effectively utilizes its residual heat to produce high-value-added Mg and Al. This method not only addresses the green treatment of LF refined slag but also avoids the shortcomings of traditional thermal reduction methods for producing Mg. The recovered Mg and Al can be reused in steelmaking, achieving high economic benefits while addressing the challenge of large-scale utilization of LF refined slag.

[0014] The method for extracting Mg and Al using LF refined slag according to an embodiment of the present invention comprises the following steps:

[0015] a. Pour the cast LF refined slag from the ladle into a slag pot, place it in a vacuum chamber, add a reducing agent to the LF refined slag and mix it to obtain a mixed reaction material;

[0016] b. After the vacuum is drawn, the mixed reaction materials in the slag pot are heated to react, and the generated gaseous Mg and Al are condensed and recovered at the cooling end outside the vacuum chamber.

[0017] The advantages and technical effects of the method for extracting Mg and Al using LF refined slag in the embodiment of the present invention are as follows: 1. In the method of the embodiment of the present invention, LF refined slag after casting is used as raw material, which has low cost, almost zero, and high residual temperature of LF refined slag. Steel slag contains a large amount of sensible heat. LF refined slag is used to preheat the reducing agent and provide part of the energy required for the reaction of MgO and Al2O3 in the slag. After adding some additional heat, the reduction reaction can be met. The heat is fully and effectively utilized, saving a lot of energy; 2. In the method of the embodiment of the present invention, LF refined slag after casting is used as raw material to extract Mg and Al. LF refined slag is an industrial solid waste. Using it to replace industrial raw materials such as dolomite, magnesite and bauxite realizes waste utilization and saves non-renewable mineral resources. 3. The method of the embodiment of the present invention effectively solves the problem of recycling and reuse of LF refined steel slag, realizes green treatment, and avoids the technical defects of traditional production of Mg and Al. The recovered Mg and Al can be reused in steelmaking production, achieving higher economic benefits and providing a new direction for the large-scale utilization of LF refined steel slag. 4. The method of the embodiment of the present invention has a simple process, low cost, energy saving and environmental protection, is easy to be applied in large-scale industry, and has broad prospects.

[0018] In some embodiments, in step a, the temperature of the LF refined slag is not less than 1200°C.

[0019] In some embodiments, in step a, the reducing agent is FeSi powder.

[0020] In some embodiments, the Si content in the FeSi powder is 72 wt%-78 wt%.

[0021] In some embodiments, in step a, the FeSi powder is added in an amount of 20 wt% to 30 wt% of the LF refined slag.

[0022] In some embodiments, in step a, the reducing agent is added to the LF refined slag in batches.

[0023] In some embodiments, in step b, the vacuum degree of the vacuum chamber is 5-20 Pa.

[0024] In some embodiments, in step b, the reaction temperature is 1300-1500°C.

[0025] In some embodiments, in step b, the reaction time is 1-3 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] FIG1 is a process flow chart of extracting Mg and Al using LF refined slag according to an embodiment of the present invention. DETAILED DESCRIPTION

[0027] The following describes in detail embodiments of the present invention. The embodiments are exemplary and intended to explain the present invention, but are not to be construed as limiting the present invention.

[0028] a. Pour the cast LF refined slag from the ladle into a slag pot, place it in a vacuum chamber, add a reducing agent to the LF refined slag and mix it to obtain a mixed reaction material;

[0029] b. After the vacuum is drawn, the mixed reaction materials in the slag pot are heated to react, and the generated gaseous Mg and Al are condensed and recovered at the cooling end outside the vacuum chamber.

[0030] In the method for extracting Mg and Al using LF refined slag according to the embodiment of the present invention, the cast LF refined slag is used as the raw material, which has low cost, almost zero. In addition, the residual temperature of the LF refined slag is high, and the steel slag contains a large amount of sensible heat. The LF refined slag is used to preheat the reducing agent and provide part of the energy required for the reaction of MgO and Al2O3 in the slag. After adding some additional heat, the reduction reaction can be satisfied. The heat is fully and effectively utilized, saving a lot of energy. In the method according to the embodiment of the present invention, the cast LF refined slag is used as the raw material to extract Mg and Al. The LF refined slag is industrial solid waste. It is used to replace the industrial raw materials dolomite, magnesite and aluminum ore, realizing waste utilization and saving non-renewable mineral resources. The method according to the embodiment of the present invention effectively solves the problem of recycling and reuse of LF refined steel slag, realizes green treatment, and avoids the technical defects of traditional production of Mg and Al. The recovered Mg and Al can be reused in steelmaking production, achieving high economic benefits and providing a new direction for the large-scale utilization of LF refined steel slag. The method according to the embodiment of the present invention has a simple process, low cost, energy saving and environmental protection, is easy to be applied in large-scale industry, and has broad prospects.

[0031] In some embodiments, in step a, the temperature of the LF refined slag is not less than 1200° C. In the method of the embodiment of the present invention, the temperature of the LF refined slag after pouring substantially reaches above 1200° C., containing a large amount of sensible heat. The waste heat of the LF refined slag can be used to preheat the reducing agent and also provide most of the energy required for the MgO and Al2O3 reactions. This fully utilizes the heat of the LF refined slag, saves a lot of energy, and is energy-saving and environmentally friendly.

[0032] In some embodiments, in step a, the reducing agent is FeSi powder. Preferably, the FeSi powder has a Si content of 72-78 wt%. Further preferably, the FeSi powder is added in an amount of 20-30 wt% relative to the LF refined slag. Preferably, the reducing agent is added to the LF refined slag in batches. In the methods of the embodiments of the present invention, the amount of reducing agent is optimized to further improve the heat utilization rate of the LF refined slag and the extraction recovery rate of Mg and Al.

[0033] In some embodiments, in step b, the vacuum degree of the vacuum chamber is 5-20 Pa, the reaction temperature is 1300-1500° C., and the reaction time is 1-3 hours. In the method of the present invention, the LF refined slag and the reducing agent react in a vacuum environment, which can fully utilize the waste heat of the LF refined slag. Only additional heat is required to achieve the full energy required for the reduction reaction, thereby realizing the extraction of Mg and Al using LF refined slag as a raw material.

[0034] The present invention is described in detail below with reference to the embodiments.

[0035] A steel plant has 260t LF, the amount of LF refining slag is 3t / furnace, and the temperature of the LF refining slag returned to the ladle after pouring is 1200-1250℃.

[0036] Example 1

[0037] (1) Reducing agent ingredients: FeSi powder with a Si content of 75 wt% is added. The amount of FeSi powder is 20 wt% of the amount of LF refined slag, and the addition amount is 600 kg;

[0038] (2) Pour the cast LF refined slag from the ladle into the slag pot and transport it to the vacuum chamber. Use the slag pot as the reaction container, the LF refined slag temperature is 1220℃, and the prepared FeSi powder is added to the LF refined slag in batches, and then mixed evenly.

[0039] (3) The system is evacuated to a vacuum of 19 Pa (absolute pressure). The reaction materials in the slag pot are heated to 1500°C in the vacuum chamber and kept at this temperature for 1 hour. Under the suction of the vacuum system, the gaseous Mg and Al generated by the reaction condense into solid Mg and Al at the cooling end outside the vacuum chamber for recovery.

[0040] The main components of the LF refined slag before and after the reaction in this embodiment are shown in Table 1. It can be seen from Table 1 that after the reaction, Mg and Al in the LF refined slag are effectively extracted and recovered, and the MgO content in the LF refined slag is as low as 2.3%, and Al2O3 is reduced to 6.2%.

[0041] Table 1

[0042] According to calculation, in the method of this embodiment, the Mg recovery rate is 73%, and the Al recovery rate is 76%.

[0043] Example 2

[0044] (1) Reducing agent ingredients: FeSi powder with a Si content of 78 wt% is added. The amount of FeSi powder is 25 wt% of the amount of LF refined slag, and the addition amount is 750 kg;

[0045] (2) Pour the cast LF refined slag from the ladle into the slag pot and transport it to the vacuum chamber. Use the slag pot as the reaction container, the LF refined slag temperature is 1210℃, and the prepared FeSi powder is added to the LF refined slag in batches, and then mixed evenly.

[0046] (3) The system is evacuated to a vacuum of 15 Pa. The reaction materials in the slag pot are heated to 1400°C within the vacuum chamber and kept at this temperature for 2 hours. Under the suction of the vacuum system, the gaseous magnesium and aluminum generated by the reaction condense into solid Mg and Al at the cooling end outside the vacuum chamber for recovery.

[0047] The main components of the LF refined slag before and after the reaction in this embodiment are shown in Table 2. It can be seen from Table 2 that after the reaction, Mg and Al in the LF refined slag are effectively extracted and recovered, and the MgO content in the LF refined slag is as low as 2%, and Al2O3 is reduced to 8%.

[0048] Table 2

[0049] According to calculation, in the method of this embodiment, the Mg recovery rate is 68%, and the Al recovery rate is 69%.

[0050] Example 3

[0051] (1) Reducing agent ingredients: FeSi powder with a Si content of 72 wt% is added. The amount of FeSi powder is 30 wt% of the amount of LF refined slag, and the addition amount is 900 kg;

[0052] (2) The cast LF refined slag is poured from the ladle into a slag pot and transported to a vacuum chamber. The slag pot is used as a reaction container. The temperature of the LF refined slag is 1210℃. The prepared FeSi powder is added to the LF refined slag in batches and then mixed evenly.

[0053] (3) The system is evacuated to a vacuum of 6 Pa. The reaction materials in the slag pot are heated to 1301°C within the vacuum chamber and kept at this temperature for 3 hours. Under the suction of the vacuum system, the gaseous magnesium and aluminum generated by the reaction condense into solid Mg and Al at the cooling end outside the vacuum chamber for recovery.

[0054] The main components of the LF refined slag before and after the reaction in this example are shown in Table 3. It can be seen from Table 3 that after the reaction, Mg and Al in the LF refined slag are effectively extracted and recovered, and the MgO content in the LF refined slag is as low as 1.5%, and Al2O3 is reduced to 7%.

[0055] Table 3

[0056] According to calculation, in the method of this embodiment, the Mg recovery rate is 78%, and the Al recovery rate is 73%.

[0057] Comparative Example 1

[0058] (1) Reducing agent ingredients: FeSi powder with a Si content of 75 wt% is added. The amount of FeSi powder is 5 wt% of the amount of LF refined slag, and the addition amount is 150 kg;

[0059] (2) The cast LF refined slag is poured from the ladle into a slag pot and transported to a vacuum chamber. The slag pot is used as a reaction container. The temperature of the LF refined slag is 1210℃. The prepared FeSi powder is added to the LF refined slag in batches and then mixed evenly.

[0060] (3) The system is evacuated to a vacuum of 19 Pa. The reaction materials in the slag pot are heated to 1500°C in the vacuum chamber and kept at this temperature for 1 hour. Under the suction of the vacuum system, the gaseous magnesium and aluminum generated by the reaction are condensed into solid Mg and Al at the cooling end outside the vacuum chamber for recovery.

[0061] The main components of the LF refined slag before and after the reaction in this embodiment are shown in Table 4. It can be seen from Table 4 that after the reaction, Mg and Al in the LF refined slag are effectively extracted and recovered, and the MgO content in the LF refined slag is as low as 6.7%, and Al2O3 is reduced to 21%.

[0062] Table 4

[0063] According to calculation, in the method of Comparative Example 1, the Mg recovery rate is 25%, and the Al recovery rate is 23%.

[0064] Comparative Example 2

[0065] The method is the same as that of Example 3, except that the reducing agent is added at 35 wt% of the LF refined slag, and the added amount is 1050 kg of FeSi powder with a Si content of 78 wt%.

[0066] The main components of LF refined slag before and after the reaction are shown in Table 5.

[0067] Table 5

[0068] According to calculation, in the method of Comparative Example 2, the Mg recovery rate is 65%, and the Al recovery rate is 62%.

[0069] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and integrate different embodiments or examples and features of different embodiments or examples described in this specification without contradiction.

[0070] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for extracting Mg and Al using LF refined slag, characterized in that: The steps include: a. Pour the cast LF refined slag from the ladle into a slag pot, place it in a vacuum chamber, add a reducing agent to the LF refined slag and mix to obtain a mixed reaction material; b. After the vacuum is drawn, the mixed reaction materials in the slag pot are heated to react, and the generated gaseous Mg and Al are condensed and recovered at the cooling end outside the vacuum chamber.

2. The method for extracting Mg and Al using LF refined slag according to claim 1, characterized in that: In the step a, the temperature of the LF refined slag is not less than 1200°C.

3. The method for extracting Mg and Al using LF refined slag according to claim 1, characterized in that: In the step a, the reducing agent is FeSi powder.

4. The method for extracting Mg and Al using LF refined slag according to claim 3, characterized in that: The Si content in the FeSi powder is 72wt%-78wt%.

5. The method for extracting Mg and Al using LF refined slag according to claim 3 or 4, characterized in that: In the step a, the FeSi powder is added in an amount of 20wt%-30wt% of the LF refined slag.

6. The method for extracting Mg and Al using LF refined slag according to claim 1, characterized in that: In the step a, the reducing agent is added to the LF refined slag in batches.

7. The method for extracting Mg and Al using LF refined slag according to claim 1, characterized in that: In the step b, the vacuum degree of the vacuum chamber is 5-20Pa.

8. The method for extracting Mg and Al using LF refined slag according to claim 1, characterized in that: In the step b, the reaction temperature is 1300-1500°C.

9. The method for extracting Mg and Al using LF refined slag according to claim 1 or 8, characterized in that: In the step b, the reaction time is 1-3 hours.

Citation Information

Patent Citations

  • Method for preparing high purity silicon aluminum silicon alloy by vacuum carbon thermal reduction

    CN101462723A

  • Method adopting minerals containing magnesium silicate to produce magnesium

    CN103451453A

  • Method for preparing ferro-silicon and magnesium using ferro-nickel slag, preparation apparatus used therefor, and smelting reduction furnace

    CN104245974A

  • System for jointly preparing nickel-iron alloy and metal magnesium from silicon-magnesium type nickel laterite ore

    CN106435217A

  • Method for extracting magnesium from nickel-iron slag

    CN110423900A