Composite film, optical member, preparation method therefor, and electronic device

By using an alternating structure of deposited layers of crystal phases such as Ti, Cr, W, V and Zr and strengthening phases of Cu and/or Ag and Si3N4 layers in the composite film, the problems of poor hardness and wear resistance of the existing coating are solved. , a composite film that achieves high strength and high wear resistance, suitable for electronic equipment such as smart terminals.

WO2024217063A1PCT designated stage expired Publication Date: 2024-10-24BYD CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/143499
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2023-12-29
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing composite structural coating has low wear resistance, hardness and corrosion resistance in the field of non-metallic cover plates. The nanocomposite coating is too thick, resulting in poor toughness. The carbon-doped TiAlN nano-multilayer hard film has a complicated structure and preparation The process is cumbersome and it is difficult to obtain optimized modulation period and modulation ratio.

Method used

A multi-layered composite film structure is adopted, in which the deposition layer and the Si3N4 layer are alternately formed. The deposition layer is composed of crystal phases such as Ti, Cr, W, V and Zr and the strengthening phase of Cu and/or Ag. Cu or Ag is completely integrated with the crystal phase. Not solid solution, the Si3N4 layer is adsorbed on the surface of the growing grains, hindering the growth of the grains, reducing the internal stress of the coating and improving the hardness and toughness.

Benefits of technology

Significantly improves the hardness, wear resistance and toughness of the coating, forming a composite film with high strength and wear resistance, which is suitable for protective windows and lenses of electronic equipment such as smart terminals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023143499_24102024_PF_FP_ABST
    Figure CN2023143499_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A composite film, an optical member, a preparation method therefor, and an electronic device. The composite film comprises multiple stacked composite layers, and each composite layer comprises: a deposition layer and a Si3N4 layer on the deposition layer, wherein the composition of the deposition layer contains a crystal phase and a strengthening phase; the crystal phase is An, A being selected from one or more of Ti, Cr, W, V and Zr; the strengthening phase is X, X being selected from Cu and / or Ag.
Need to check novelty before this filing date? Find Prior Art

Description

Composite film, optical component and preparation method thereof, and electronic device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims the benefit of priority to Chinese patent application No. 202310462804.2, filed on April 21, 2023, and incorporates the entirety of the patent application herein. Technical Field

[0003] The present disclosure relates to the field of wear-resistant materials, and in particular to a composite film, an optical component and a preparation method thereof, and an electronic device. Background Art

[0004] Currently, coating processes are often used in smart terminals, especially mobile phones, tablets, laptops, projectors, instrument protection windows and special lenses to improve product characteristics in order to achieve special optical functions and decorative effects.

[0005] Some composite structural coatings in the prior art are used in the field of non-metallic cover plates and have certain limitations in use. In addition, the wear resistance, hardness and corrosion resistance of the single CrSiCN structural layer are relatively low. The coating thickness of some nano-composite coatings is relatively thick, resulting in poor toughness and increasing the brittle fracture tendency of the film. Some carbon-doped TiAlN nano-multilayer hard film coatings include a base layer, a transition layer, a functional layer and a coating layer. The structure is complex and the preparation process is cumbersome. It is difficult to accurately obtain the optimized modulation period and modulation ratio. Although some coatings have high wear resistance and toughness, they do not have the coating hardness of the nanocrystalline-amorphous multiphase composite structure.

[0006] At present, the coatings disclosed in the prior art have insufficient hardness and poor wear resistance. Therefore, there is an urgent need to research coatings or composite film materials with higher performance.

[0007] Summary of the Invention

[0008] The purpose of the present disclosure is to overcome the problems of poor coating hardness and wear resistance in the prior art and to provide a composite film, an optical component, a preparation method thereof, and an electronic device.

[0009] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides a composite film, wherein the composite film includes a multi-layer stacked composite layer, and the composite layer includes: a deposited layer and a Si3N4 layer on the deposited layer, wherein the composition of the deposited layer includes a crystalline phase and a strengthening phase, the crystalline phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; the strengthening phase is X, X is selected from Cu and / or Ag.

[0010] A second aspect of the present disclosure provides an optical component, wherein the optical component includes a substrate and the composite film disposed on a surface of the substrate, wherein the substrate includes one or more of metal, glass, ceramic, and sapphire.

[0011] A third aspect of the present disclosure provides a method for preparing an optical component, comprising:

[0012] A substrate is provided, and at least one composite layer is deposited on the surface of the substrate, wherein the composite layer includes a deposited layer and a Si3N4 layer stacked in sequence, wherein the deposited layer comprises a crystalline phase and a strengthening phase, the crystalline phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; and the strengthening phase is X, X is selected from Cu and / or Ag.

[0013] A fourth aspect of the present disclosure provides an electronic device, wherein the electronic device comprises the composite film or the optical component or the optical component obtained by the preparation method.

[0014] Through the above technical solution, the composite film obtained in this application selects Cu or Ag that is completely insoluble in AN to be added to the AN coating. The addition of Cu or Ag not only greatly reduces the internal stress of the coating and improves the hardness and fracture toughness of the coating, but also the solid solution strengthening and fine grain strengthening of Cu or Ag atoms bring about a significant improvement in wear resistance, toughness and hardness. At the same time, Si3N4 is adsorbed on the surface of the growing AN particles due to its low activity, hindering the grain growth, and the film layer is further strengthened. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] FIG1 is a schematic diagram of a laminated composite film whose substrate is an Al alloy;

[0016] FIG2 is a schematic diagram of a stacked layer of a composite film whose substrate is not an Al alloy. DETAILED DESCRIPTION

[0017] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0018] A first aspect of the present disclosure provides a composite film, wherein the composite film includes a multi-layer stacked composite layer, the composite layer including: a deposited layer and a Si3N4 layer on the deposited layer, wherein the composition of the deposited layer includes a crystalline phase and a strengthening phase, the crystalline phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; the strengthening phase is X, X is selected from Cu and / or Ag.

[0019] In the present disclosure, the composite film obtained in this application includes a deposited layer composed of a crystalline phase and a strengthening phase, wherein the Cu or Ag in the strengthening phase is completely insoluble in the AN in the crystalline phase. The addition of Cu or Ag to the AN coating not only greatly reduces the internal stress of the coating, but also improves the hardness and fracture toughness of the coating. The solid solution strengthening and fine grain strengthening of Cu or Ag atoms greatly improve the wear resistance, toughness and hardness of the composite film. At the same time, due to the low activity of Si3N4, it is adsorbed on the surface of the growing AN particles, hindering the grain growth, and the film layer is further strengthened. The deposited layer and the Si3N4 layer on the deposited layer greatly improve the wear resistance, toughness and hardness of the composite film.

[0020] In the present disclosure, the composite film may include a multi-layer composite layer, and the deposited layer and the Si3N4 layer alternately form a stacked structure of multi-layer composite layers. By stacking single layers, a composite film structure with a desensitization layer can be formed, which greatly improves the wear resistance, toughness and hardness, and further strengthens the film layer.

[0021] In some specific embodiments of the present disclosure, in the composite film, the thickness ratio of the deposited layer to the Si3N4 layer is 1:3 to 3:1. For example, the thickness ratio of the deposited layer to the Si3N4 layer can be 1:3, 1:2, 1:1, 2:1, 3:1, etc. In some embodiments, the thickness ratio of the deposited layer to the Si3N4 layer is 1:(1-3). In one embodiment, the thickness ratio of the deposited layer to the Si3N4 layer is 1:2. In this thickness ratio range of the composite film, a larger Si3N4 layer content will reduce the material's sensitivity to wear, but too much will reduce the strengthening effect of the deposited layer. Therefore, when the thickness ratio of the deposited layer to the Si3N4 layer is 1:3 to 3:1, the composite film has high hardness and good high wear resistance.

[0022] In some specific embodiments of the present disclosure, the total thickness of the composite film is 540-3000 nm. For example, the total thickness of the composite film can be 540 nm, 600 nm, 700 nm, 900 nm, 1000 nm, 1200 nm, 1500 nm, 1800 nm, 2000 nm, 2500 nm, 3000 nm, etc. In some embodiments, the total thickness of the composite film is 800-2000 nm; wherein the thickness of each layer of the composite film can be the same or different. Within the above thickness range, the composite film has high strength and high wear resistance.

[0023] In some specific embodiments of the present disclosure, in the composite layer, the thickness of the Si3N4 layer is 20-500nm, for example, the thickness of the Si3N4 layer can be 20nm, 30nm, 50nm, 80nm, 100nm, 300nm, 500nm, etc. In some embodiments, the thickness of the Si3N4 layer is 20-250nm; the thickness of the deposited layer is 20-600nm, for example, the thickness of the deposited layer can be 20nm, 40nm, 50nm, 80nm, 100nm, 150nm, 200nm, 250nm, 300nm, 500nm, 600nm, etc. In some embodiments, the thickness of the deposited layer is 50-300nm. When the thickness of the Si3N4 layer and the deposited layer is within the above thickness range, the composite laminate has high strength and high wear resistance.

[0024] In some specific embodiments of the present disclosure, the composite film comprises 6-30 composite layers, for example, 6, 8, 10, 12, 15, 17, 20, 25, 30, etc. In some embodiments, the composite film comprises 6-18 composite layers. When the number of layers is within the range of 6-30 or 6-18, the internal stress caused by the excessive number of layers and the reduction in wear resistance can be reduced.

[0025] In some specific embodiments of the present disclosure, the A is Ti, the crystal phase is TiN, and the strengthening phase is Cu.

[0026] In some specific embodiments of the present disclosure, the composite film has a nanohardness of 17-23 GPa and a pencil hardness of 7-9 H. By selecting Cu or Ag, which is completely insoluble in AN, and adding them to the AN coating, the addition of Cu or Ag not only significantly reduces the internal stress of the coating and improves the hardness and fracture toughness of the coating, but also significantly improves the wear resistance, toughness, and hardness through solid solution strengthening and grain refinement of the Cu or Ag atoms. Simultaneously, due to its low mobility, Si3N4 adsorbs on the surface of growing AN particles, hindering grain growth and further strengthening the film layer, thereby increasing the nanohardness of the composite film and achieving a pencil hardness of up to 9 H.

[0027] A second aspect of the present disclosure provides an optical component, wherein the optical component includes a substrate and the composite film disposed on a surface of the substrate, wherein the substrate includes one or more of metal, glass, ceramic, and sapphire.

[0028] In some specific embodiments of the present disclosure, the bottommost deposition layer in the composite film is located on the surface of the substrate. As shown in FIG1 , a deposition layer and a Si3N4 layer on the deposition layer are sequentially deposited on the surface of the substrate, and multiple layers are alternately stacked.

[0029] In some specific embodiments of the present disclosure, as shown in FIG2 , when the substrate is an aluminum alloy, the optical component may further include an Al coating, the Al coating being located between the substrate and the lowest deposition layer in the composite film, wherein the thickness of the Al coating is 50-200 nm, for example, the thickness of the Al coating may be 50 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, and the like. In some embodiments, the thickness of the Al coating is 50-100 nm. In the present disclosure, when the electronic device is an aluminum alloy product, it is necessary to plate a base layer of Al on the surface of the substrate to enhance the bonding force between the coating and the substrate, so that the coating and the substrate can be firmly bonded, and pure Al has good plasticity. As a base layer and distributed in the strengthening coating in the form of fine particles, it can reduce the internal stress and friction coefficient of the coating, while giving the coating a high hardness.

[0030] A third aspect of the present disclosure provides a method for preparing an optical component, comprising:

[0031] A substrate is provided, and at least one composite layer is deposited on the surface of the substrate, wherein the composite layer includes a deposited layer and a Si3N4 layer stacked in sequence, wherein the deposited layer comprises a crystalline phase and a strengthening phase, the crystalline phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; and the strengthening phase is X, X is selected from Cu and / or Ag.

[0032] In some specific embodiments of the present disclosure, the surface of the substrate further has an Al coating layer obtained by deposition.

[0033] In some specific embodiments of the present disclosure, the substrate includes one or more of metal, glass, ceramic, and sapphire.

[0034] In some specific embodiments of the present disclosure, the deposition may be performed by sputtering in an N2 and Ar atmosphere, and the sputtering process is performed in an N2 300 sccm and Ar 200 sccm atmosphere.

[0035] In some specific embodiments of the present disclosure, the sputtering temperature is 25-60°C.

[0036] In some specific embodiments of the present disclosure, the sputtering is performed using an AX alloy target.

[0037] In some specific embodiments of the present disclosure, the AX alloy target is selected from A 90 X 10 Target or A 80 X 20 In some embodiments, the AX alloy target is selected from Ti 90 Cu 10 Target or Ti 80 Cu 20Target material. Selecting this ratio of target material allows the strengthening phase to strengthen the crystalline phase, but too high a crystalline phase content will inhibit the growth of the crystalline phase, resulting in reduced strength and wear resistance of the composite film.

[0038] In some specific embodiments of the present disclosure, the method for preparing an optical component specifically includes:

[0039] (1) sputtering the substrate using an AX alloy target to obtain a deposited layer;

[0040] (2) sputtering the deposited layer using a Si target to obtain a Si3N4 layer;

[0041] (3) repeating steps (1) and (2) several times to form a multilayer composite layer to obtain the optical component;

[0042] In some specific embodiments of the present disclosure, when the substrate is an aluminum alloy, the method for preparing the optical component specifically includes:

[0043] (1) sputtering an aluminum alloy substrate using an Al target to obtain a deposited Al coating;

[0044] (2) sputtering the deposited Al coating using an AX alloy target to obtain a deposited layer;

[0045] (3) sputtering the deposited layer using a Si target to obtain a Si3N4 layer;

[0046] (4) Repeat steps (2) and (3) several times to form a multi-layer composite layer to obtain the optical component.

[0047] A fourth aspect of the present disclosure provides an electronic device, wherein the electronic device comprises the composite film or the optical component or the optical component obtained by the preparation method.

[0048] The present disclosure will be described in detail below through examples.

[0049] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents and instruments used, if no manufacturer is specified, are commercially available conventional products.

[0050] Example 1

[0051] (1) Polishing and cleaning of substrate surface

[0052] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0053] (2) Deposition of Al coating

[0054] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0055] (3) Sedimentary layer

[0056] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0057] (4) Si3N4 layer

[0058] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0059] (5) repeating steps (3) and (4) seven times to form a multilayer stack to obtain the composite film;

[0060] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0061] Example 2

[0062] (1) Polishing and cleaning of substrate surface

[0063] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0064] (2) Deposition of Al coating

[0065] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0066] (3) Sedimentary layer

[0067] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 20 nm. The alloy target power supply was then turned off.

[0068] (4) Si3N4 layer

[0069] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, deposition thickness 40nm.

[0070] (5) repeating steps (3) and (4) eight times to form a multilayer stack to obtain the composite film;

[0071] The total thickness of the composite film is 540 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0072] Example 3

[0073] (1) Polishing and cleaning of substrate surface

[0074] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0075] (2) Deposition of Al coating

[0076] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0077] (3) Sedimentary layer

[0078] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0079] (4) Si3N4 layer

[0080] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, deposition thickness 150nm.

[0081] (5) repeating steps (3) and (4) five times to form a multilayer stack to obtain the composite film;

[0082] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:3.

[0083] Example 4

[0084] (1) Polishing and cleaning of substrate surface

[0085] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0086] (2) Deposition of Al coating

[0087] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0088] (3) Sedimentary layer

[0089] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0090] (4) Si3N4 layer

[0091] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0092] (5) repeating steps (3) and (4) twice to form a multilayer stack to obtain the composite film;

[0093] The total thickness of the composite film is 450 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0094] Example 5

[0095] (1) Polishing and cleaning of substrate surface

[0096] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0097] (2) Deposition of Al coating

[0098] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0099] (3) Sedimentary layer

[0100] The TiCu alloy targets with different composition ratios were sputtered. 80 Cu 20 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0101] (4) Si3N4 layer

[0102] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0103] (5) repeating steps (3) and (4) seven times to form a multilayer stack to obtain the composite film;

[0104] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0105] Example 6

[0106] (1) Polishing and cleaning of substrate surface

[0107] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0108] (2) Deposition of Al coating

[0109] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0110] (3) Sedimentary layer

[0111] The ZrCu alloy targets with different composition ratios were sputtered. 80 Cu 20 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a ZrN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0112] (4) Si3N4 layer

[0113] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0114] (5) repeating steps (3) and (4) seven times to form a multilayer stack to obtain the composite film;

[0115] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0116] Example 7

[0117] (1) Polishing and cleaning of substrate surface

[0118] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0119] (2) Deposition of Al coating

[0120] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0121] (3) Sedimentary layer

[0122] The TiAg alloy targets with different composition ratios were sputtered. 80 Ag 20 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Ag film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0123] (4) Si3N4 layer

[0124] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0125] (5) repeating steps (3) and (4) seven times to form a multilayer stack to obtain the composite film;

[0126] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0127] Example 8

[0128] (1) Polishing and cleaning of substrate surface

[0129] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0130] (2) Deposition of Al coating

[0131] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0132] (3) Sedimentary layer

[0133] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 150 nm. The alloy target power supply was then turned off.

[0134] (4) Si3N4 layer

[0135] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, deposition thickness 50nm.

[0136] (5) repeating steps (3) and (4) seven times to form a multilayer stack to obtain the composite film;

[0137] The total thickness of the composite film is 1600 nm, and the thickness ratio of the deposited layer to the Si3N4 layer is 3:1.

[0138] Example 9

[0139] (1) Polishing and cleaning of substrate surface

[0140] The glass substrate was cleaned with a degreaser in an ultrasonic chamber, rinsed with deionized water, and dried with N2 gas; finally, the dried substrate was placed on a vacuum sputtering fixture.

[0141] (2) Sedimentary layer

[0142] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0143] (3) Si3N4 layer

[0144] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0145] (4) repeating steps (2) and (3) seven times to form a multilayer stack to obtain the composite film;

[0146] The total thickness of the composite film is 1200 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0147] Comparative Example 1

[0148] (1) Polishing and cleaning of substrate surface

[0149] The surface of the Al alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0150] (2) Deposition of Al coating

[0151] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0152] (3) Sedimentary layer

[0153] A pure Ti target was used for sputtering. Ar was introduced at a flow rate of 300 sccm and N2 at a flow rate of 200 sccm. The alloy target power was turned on to deposit a TiN film with a thickness of 50 nm. The alloy target power was then turned off.

[0154] (4) Si3N4 layer

[0155] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0156] (5) Repeat steps (3) and (4) 7 times, and the total thickness of the composite film is 1200 nm; the thickness ratio of the deposited layer and the Si3N4 layer is 1:2.

[0157] Comparative Example 2

[0158] (1) Polishing and cleaning of substrate surface

[0159] The surface of the Al alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0160] (2) Deposition of Al coating

[0161] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0162] (3) Sedimentary layer

[0163] Using Ti 90 Cu 10The alloy target was sputtered. Ar was introduced at a flow rate of 300 sccm and N2 at a flow rate of 200 sccm. The power supply to the alloy target was turned on to deposit a TiN film with a thickness of 20 nm. The power supply to the alloy target was then turned off.

[0164] (4) Si3N4 layer

[0165] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, deposition thickness 40nm.

[0166] (5) Repeat steps (3) and (4) 4 times, and the total thickness of the composite film is 300 nm; the thickness ratio of the deposited layer and the Si3N4 layer is 1:2.

[0167] Comparative Example 3

[0168] (1) Polishing and cleaning of substrate surface

[0169] The surface of the aluminum alloy substrate was ground and polished in sequence using water-sandpaper with different roughnesses; then it was cleaned with a degreaser in an ultrasonic container, pickled, rinsed with deionized water, and blown dry with N2 gas; finally, the dried substrate was placed on a vacuum sputtering machine fixture.

[0170] (2) Deposition of Al coating

[0171] Place the aluminum alloy substrate on the fixture of the sputtering machine and evacuate the chamber until the vacuum degree of the coating chamber reaches 3×10 -3 When Pa, Ar is introduced. After the gas stabilizes, the ion source is turned on to perform ion cleaning on the substrate surface for 2-5 minutes; the ion source continues to work, and the sputtering power supply of the Al target is turned on at the same time, with a power of 5kW and a thickness of 50nm, to complete the coating of the first layer of the base layer.

[0172] (3) Sedimentary layer

[0173] The TiCu alloy targets with different composition ratios were sputtered. 90 Cu 10 Alloy target. Ar gas at a flow rate of 300 sccm and N₂ gas at a flow rate of 200 sccm were introduced. The alloy target power supply was turned on to deposit a TiN-Cu film with a thickness of 50 nm. The alloy target power supply was then turned off.

[0174] (4) Si3N4 layer

[0175] Turn on the Si target power supply, power 10kW, N2 flow 300sccm, Ar flow 300sccm, and deposition thickness 100nm.

[0176] The total thickness of the composite film is 150 nm, and the thickness ratio of the deposition layer to the Si3N4 layer is 1:2.

[0177] Test example:

[0178] The above performance tests were performed on the composite membranes of Examples 1-9 and Comparative Examples 1-3. The test results of Examples 1-9 were good, while the vibration wear resistance of the composite membranes of the comparative examples was poor.

[0179] 1. Neutral salt spray test: NaCl%: 5% (pH 6.5-7.2), test environment 35℃.

[0180] 2. Acidic sweat test: Acidic sweat is obtained by adjusting the sweat formula to 2.5g NaCl + 2.19g NH4Cl + 0.63g urea + 1.88g lactic acid + 0.32g acetic acid + 125mL pure water and using sodium hydroxide to adjust the pH value to 4.7.

[0181] 3. Vibration wear resistance: R180 / 530TE30 (equipment frequency: 50±0.5Hz, amplitude 1.65±0.1mm).

[0182] 4. Boiling test: temperature 100℃, time 0.5h, 1h, 2h respectively.

[0183] The performance of the composite films obtained in Examples 1-9 and Comparative Examples 1-3 was tested, and the results are shown in Table 1.

[0184] Table 1

[0185] From the results in Table 1, it can be seen that the composite laminates prepared in Examples 1-9 of the present disclosure have significantly better wear resistance and higher hardness, and are not affected by the substrate.

[0186] In the examples, the ratio of the crystalline phase to the reinforcing phase in the deposited layer is crucial for improving the strength and wear resistance of the laminate. Furthermore, the thickness and number of layers in the composite structure also significantly impact the strength and wear resistance of the composite film. A single layer structure and a thin film layer cannot reduce internal stress in the coating, strengthen the grains, or improve the overall strength of the composite film.

[0187] The composite film includes a deposited layer composed of a crystalline phase and a strengthening phase, wherein Cu or Ag is completely insoluble in AN. The addition of Cu or Ag to the AN coating not only greatly reduces the internal stress of the coating, but also improves the hardness and fracture toughness of the coating. The solid solution strengthening and fine grain strengthening of Cu or Ag atoms greatly improve the wear resistance, toughness and hardness of the composite film. At the same time, due to the low activity of Si3N4, it is adsorbed on the surface of the growing AN particles, hindering the growth of grains, and the film layer is further strengthened. The deposited layer and the Si3N4 layer on the deposited layer greatly improve the wear resistance, toughness and hardness of the composite film.

[0188] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed by the present disclosure and fall within the scope of protection of the present disclosure.

Claims

1. A composite film, wherein The composite film includes a multi-layer stacked composite layer, and the composite layer includes: a deposition layer and a Si3N4 layer on the deposition layer, wherein the composition of the deposition layer includes a crystal phase and a strengthening phase, the crystal phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; the strengthening phase is X, X is selected from Cu and / or Ag.

2. The composite film according to claim 1, wherein In the composite film, the thickness ratio of the deposited layer to the Si3N4 layer is 1:(1-3).

3. The composite film according to claim 1 or 2, wherein The total thickness of the composite film is 540-3000 nm.

4. The composite film according to claim 3, wherein The total thickness of the composite film is 800-2000nm.

5. The composite film according to claim 3 or 4, wherein In the composite layer, the thickness of the Si3N4 layer is 20-500nm, and the thickness of the deposited layer is 20-600nm.

6. The composite film according to claim 5, wherein The thickness of the Si3N4 layer is 20-250nm, and the thickness of the deposited layer is 50-300nm.

7. The composite film according to any one of claims 1 to 6, wherein: The composite film comprises 5-30 composite layers.

8. The composite film according to claim 7, wherein The composite film comprises 6-18 composite layers.

9. The composite film according to any one of claims 1 to 8, wherein The A is Ti, and the strengthening phase is Cu.

10. The composite film according to any one of claims 1 to 9, wherein: The nano hardness of the composite film is 17-23 GPa, and the pencil hardness is 7-9H.

11. An optical component, wherein: The optical component comprises a substrate and a composite film according to any one of claims 1 to 10 disposed on a surface of the substrate, wherein the substrate comprises one or more of metal, glass, ceramic, and sapphire.

12. The optical element according to claim 11, wherein: The lowermost deposited layer in the composite film is located on the surface of the substrate.

13. The optical element according to claim 11 or 12, wherein: When the substrate is an aluminum alloy, the optical component may further include an Al coating layer, wherein the Al coating layer is located between the substrate and the lowermost deposition layer in the composite film.

14. The optical element according to claim 13, wherein: The thickness of the Al coating is 50-200 nm.

15. The optical element according to claim 14, wherein: The thickness of the Al coating is 50-100 nm.

16. A method for preparing an optical component, wherein: include: A substrate is provided, and at least one composite layer is deposited on the surface of the substrate, wherein the composite layer comprises sequentially stacked layer and Si3N4 layer, wherein the composition of the deposited layer includes a crystalline phase and a strengthening phase, the crystalline phase is AN, A is selected from one or more of Ti, Cr, W, V and Zr; the strengthening phase is X, X is selected from Cu and / or Ag.

17. The preparation method according to claim 16, wherein: The surface of the substrate also has an Al coating layer deposited thereon.

18. The preparation method according to claim 16 or 17, wherein: The substrate includes one or more of metal, glass, ceramic, and sapphire.

19. An electronic device, wherein: The electronic device comprises the composite film according to any one of claims 1 to 10, or the optical component according to any one of claims 11 to 15, or the optical component made by the preparation method according to any one of claims 16 to 18.

Citation Information

Patent Citations

  • TiCuN nano composite coating and preparation method thereof

    CN103160783A

  • Method of manufacturing multi-layer thin film, member including the same and electronic product including the same

    CN105229195A

  • Ti-Ag-N nano-composite coating and preparation method thereof

    CN106756821A

  • Transparent substrate with antireflective film

    CN108312655A

  • Noble metal nanoparticle dispersed thin film and its production method