Wadding and use thereof
By using a combined design of mesh-like open fiber structures and crimped fibers in the wadding, the problem of filler migration during washing is solved, achieving a lightweight, warm and fluffy effect, and is suitable for a variety of uses such as clothing and beds. supplies.
Patent Information
- Application Number
- PCT/CN2024/087857
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
Existing chemical fiber filler flakes tend to shift during the washing process, resulting in a decrease in warmth retention and bulkiness, and it is difficult to achieve the requirements of lightweight and low weight.
A mesh-like open fiber structure is distributed on both sides of the filler made of fiber, and the design of the crimped fibers entangles the fibers with the structure, reducing the free deflection of the filler and ensuring fluffiness and warmth.
It achieves the maintenance of the stability and fluffiness of the filling during the washing process, reduces the weight of the flakes, improves the warmth retention effect, and ensures lightweight characteristics.
Smart Images

Figure CN2024087857_24102024_PF_FP_ABST
Abstract
Description
Flakes and their uses Technical Field
[0001] The invention relates to a flake and application thereof, in particular to a flake which has small washing deviation and is light, warm and fluffy and application thereof. Background Art
[0002] As living standards continue to improve, people's demands for warmth are also increasing. While natural fillings offer excellent warmth and bulk, they also have drawbacks such as odor and caking. Replacing natural fillings with synthetic fiber fillings has become a trend. Developing lightweight, warm, and fluffy synthetic fiber fillings with minimal wash drift is urgently needed.
[0003] To this end, researchers have conducted a lot of exploration and efforts. For example, Japanese Patent Document Tokkai 2018500472 discloses a fiber ball filler and a product containing the aforementioned fiber ball filler. Specifically, the filler includes a non-woven fabric containing a fiber mixture, wherein synthetic fibers account for 40 to 95% by weight of the fiber mixture, and bonding fibers with a bonding temperature lower than the softening temperature of the aforementioned synthetic fibers account for 5 to 40% by weight. The aforementioned synthetic fibers have a fineness of 0.5 to 7.0 denier and a length of 18 to 51 mm, and the bonding fibers have a fineness of 1.0 to 5.0 denier and a length of 18 to 71 mm. m; The non-woven fabric mentioned above structurally includes 50 to 95 weight percent of a plurality of fiber balls, and 5 to 50 weight percent of a plurality of non-woven fabrics adjacent to one or more fiber balls mentioned above but not including one or more fiber balls mentioned above or any part thereof. The non-woven fabric and the fiber balls are bonded together by adhesive fibers to form a filler. This structure improves the washing deviation of the fiber balls to a certain extent, but the use of adhesive fibers reduces the feel of the flakes. Moreover, under the same conditions, the non-woven fabric has a larger gram weight, which increases the overall gram weight of the flakes, affecting the lightweight and warmth retention of the flakes.
[0004] For example, Chinese patent document CN101892599B discloses a forming device and method for fixing down flakes on a warp knitted net. Specifically, down is fed into the warp knitted net in the form of flakes to form down flakes laid on the warp knitted net. The down flakes laid on the warp knitted net are entangled and consolidated on the warp knitted net by high-pressure water jets. The weight of the warp knitted net is 2 to 20 g / m2. 2 Although the high-pressure water jet consolidation method can fix the down and solve the problem of washing deviation, this consolidation method will also cause the fluffiness of the down to drop significantly.
[0005] Summary of the Invention
[0006] The object of the present invention is to provide a flocculent sheet which has little washing deviation and is light, warm and fluffy, and its use.
[0007] In order to achieve the above object, the present invention is constituted as follows:
[0008] The flakes of the present invention include a filler and fiber structures distributed on both sides of the filler. The filler is composed of fibers, including crimped fibers A with a crimp number of 4 to 25 per 25 mm. Among the fiber structures on both sides of the filler, at least one side of the fiber structure is a mesh-shaped open fiber structure, and the open area of the mesh-shaped open fiber structure accounts for more than 60% of its total area.
[0009] The flakes of the present invention include a filler and fiber structures distributed on both sides of the filler. At least one side of the fiber structure is a mesh-like open fiber structure. Under the same conditions, the flakes can be made lighter by reducing their grammage. Furthermore, the fibers forming the filler have a certain degree of curl, which allows them to be entangled with the fiber structure, eliminating the need for special processing such as hydroentanglement. While maintaining fluffiness, the free displacement of the filler is reduced. The flakes of the present invention can be used to make clothing, bedding, outdoor products, decorative materials, and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a schematic diagram of the thermal insulation sheet of the present invention, wherein 1 is a fiber structure with a mesh-like opening structure, 2 is a filler, and 3 is a curled fiber on the surface of the filler. DETAILED DESCRIPTION
[0011] The flake of the present invention comprises a filler and fiber structures disposed on both sides of the filler. The filler is located between the fiber structures, and the fiber structures are disposed on both sides of the outer surface of the flake. Without the fiber structures, the filler, when used alone, would freely move between the outer and inner layers of fabric. This would cause significant shifting and clumping of the filler, particularly after washing, resulting in poor thermal insulation. Therefore, it is crucial for the present invention to provide fiber structures on both sides of the filler to form the flake.
[0012] To maintain the bulk of the filling, the present invention utilizes the fiber crimp morphology to entangle the filling with the fiber structure, thereby preventing shifting during washing. When the crimped fibers have fewer than 4 crimps / 25mm, fiber entanglement is minimal, but shifting during washing is not effectively prevented. When the crimped fibers have more than 25 crimps / 25mm, the filling becomes dense, resulting in poor bulk and reduced warmth retention. Therefore, the present invention requires that the fibers forming the filling contain crimped fibers A with a crimp count of 4 to 25 crimps / 25mm. More preferably, the crimp count of crimped fibers A is 8 to 20 crimps / 25mm. In the present invention, the filler can be a blend of fibers with different crimp morphologies. It can be a blend of low-crimp fibers (less than 4 crimps / 25mm) and crimped fibers A (4-25 crimps / 25mm). It can also be a blend of high-crimp fibers (over 25 crimps / 25mm) and crimped fibers A (4-25 crimps / 25mm). It can also be composed entirely of crimped fibers A (4-25 crimps / 25mm). Preferably, the filler is composed entirely of crimped fibers A (4-25 crimps / 25mm). When low-crimp fibers or high-crimp fibers are included, the content of crimped fibers A (4-25 crimps / 25mm) is required to be at least 10% by weight. When the filler is composed entirely of crimped fibers A (4-25 crimps / 25mm), the crimp numbers of the fibers may vary, as long as the crimp number is within the above range.
[0013] The flakes of the present invention include a filler and a fiber structure distributed on both sides of the filler, and the fiber structure on at least one side has a mesh opening structure, which is called a mesh opening fiber structure. The mesh opening fiber structure here can be a single-layer fiber structure with a mesh opening structure, or a multi-layer fiber structure with a mesh opening structure. The fiber structures on both sides of the filler can all be mesh opening fiber structures, or one side can be a mesh opening fiber structure and the other side can be a non-mesh opening fiber structure. In this case, compared with a flake with non-mesh opening structures on both sides of the filler, when the total weight of the flakes is constant, the amount of filling cotton used increases and the warmth retention can also be improved. The size and shape of a single mesh opening can be the same or different. Considering the aesthetics and the convenience of weaving, it is preferred that the openings are of the same size and shape. In addition, the opening area of the mesh opening fiber structure not only affects the gram weight of the flakes, but also affects the entanglement of the fiber structure and the filler. When the open area of a reticulated open fiber structure accounts for less than 60% of its total area, the probability of entanglement between the crimped fibers and the fiber structure is low, the wash drift rate increases, and the basis weight is relatively high. Therefore, the present invention requires that the open area of the reticulated open fiber structure account for at least 60% of its total area, and more preferably, the open area ratio is 80% to 95%.
[0014] When the mesh opening fiber structure has a single mesh opening area of less than 1mm 2 When the interwoven parts are more, under the same conditions, the weight of the fiber structure tends to increase, and it may affect the feel. When the mesh opening fiber structure has a single mesh opening area greater than 100mm 2 When the fiber structure has a fixed effect on the filler, it may affect the washing deviation of the flakes. Therefore, as a preference, the area of a single mesh opening in the mesh open fiber structure of the present invention is 1 to 100 mm. 2 , more preferably 15 to 50 mm 2 .
[0015] In the present invention, the weight of the mesh open fiber structure is less than 2g / m 2 If the fiber structure is easily broken by the centrifugal force during washing, the washing durability of the flakes tends to decrease; and the weight of the mesh open fiber structure is greater than 15g / m 2 If the weight of the wadding is the same, the amount of filler used will be reduced, and the hand feel, bulkiness and thermal insulation effect of the wadding will tend to decline. Therefore, as a preferred method, the weight of the mesh open fiber structure of the present invention is 2 to 15 g / m 2 , more preferably 2 to 8 g / m 2 .
[0016] The mesh-like open fiber structure of the present invention is not particularly limited in form and can be a knitted fabric, a woven fabric, etc., preferably a knitted fabric, more preferably a warp knitted fabric. The structure of the warp knitted fabric is not particularly limited as long as it can form a mesh-like open structure, such as a warp knitted fabric. In the present invention, the mesh size of 1 to 100 mm is most preferably 2 , forged mesh with a porosity of more than 60%.
[0017] The fiber raw material for forming the mesh-like open fiber structure in the present invention is also very important. It can be filament or staple yarn, preferably filament. Among them, the filament can be multifilament or monofilament, preferably multifilament. The fineness of the yarn used in the fiber structure is preferably 10-70D. Generally, the outer side of the flakes is mostly made of lighter and thinner fabrics. In order to avoid the foreign body feeling affecting the feel and appearance of the finished product, the fineness is more preferably 10-30D. The above-mentioned filament multifilament can be fully drawn yarn FDY or false twisted yarn DTY. Considering that the flakes will subsequently undergo washing, ironing and other procedures, in order to ensure dimensional stability, FDY is preferred.
[0018] The fiber structure of the non-net-shaped open structure of the present invention is not particularly limited in form and can be knitted fabric, woven fabric, non-woven fabric, etc. In order to ensure that the feel and appearance are not affected, the weight is preferably 2 to 15 g / m 2.
[0019] The filler of the present invention contains crimped fibers. If the crimped fibers are too short, their ability to entangle with the mesh structure tends to decrease. On the other hand, if the crimped fibers are too long, they tend to entangle with themselves, which may also affect their ability to entangle with the mesh structure. Therefore, in order to allow as many crimped fibers as possible to pass through the openings of the fiber structure, the crimped fibers of the present invention preferably have a length of 10 to 70 mm, more preferably 20 to 50 mm.
[0020] The filler in the present invention is not particularly limited and can be chemical fiber fillers such as pearl cotton, opened cotton, and imitation down cotton, or natural fillers such as wool and cotton. However, considering the cost and the curl morphology of the fibers, chemical fiber fillers are more preferred. Pearl cotton, also known as granular cotton, is formed from small balls of curled short fibers through a ball forming machine. It is relatively compact, has less surface hairiness, and has low bulk. Open cotton is formed from curled short fibers through a specific opening process, has more surface hairiness, and is more fluffy. Imitation down cotton is obtained by combing, forming, and hot-melting ultrafine staple fibers, three-dimensional hollow curly short fibers, etc., and has less surface hairiness. Considering the surface hairiness and bulkiness, the filler in the present invention is most preferably opened cotton.
[0021] In the present invention, the materials of the fibers forming the filler and the fibers forming the fiber structure are not particularly limited, and may be polyester fibers, polyamide fibers, or polyolefin fibers, etc. It is preferred that the fibers forming the filler and the fibers forming the fiber structure are made of the same material, since flakes of the same material do not require additional special treatment when recycled and can be directly recycled. The same material here refers to the same chemical composition of the fibers, such as all being ordinary fibers or all being modified fibers, and does not include a mixture of ordinary fibers and modified fibers or a mixture of ordinary melting point fibers and low melting point fibers. Polyamide 6 and polyamide 66 are not fibers of the same material. Taking into account the maturity of the recycling system, etc., the fiber raw material used in the present invention is more preferably polyethylene terephthalate fiber (PET) or polyamide 6 fiber.
[0022] The flakes of the present invention can be used to make clothing, bedding, outdoor supplies, decorative materials and the like.
[0023] The present invention will be further described below with reference to the following embodiments and comparative examples.
[0024] The determination methods of the various parameters involved in the present invention are as follows:
[0025] (1) Fiber curl
[0026] 0.01 g of filler was taken out from the flakes, and all single fibers were decomposed. Referring to the JIS L 1015:2021 standard, the curl number of all the decomposed single fibers was measured using a fiber curl elasticity tester (XCP-1AN, Shanghai Xinxian Instrument Co., Ltd.).
[0027] (2) Length of curly fibers
[0028] Based on the curl obtained in (1) above, the fibers were divided into three categories: low-curl fibers with fewer than 4 curls / 25 mm, curly fibers A with 4 to 25 curls / 25 mm, and high-curl fibers with more than 25 curls / 25 mm. Twenty fibers of each type were selected as test specimens. The lengths of the individual fibers were then measured using the following method: glycerin was applied to the specimens, they were straightened, and the lengths were measured using a ruler (10 cm range). A total of 20 sets of data were obtained, and the average value was taken as the length of the curly fiber.
[0029] (3) Content of curly fiber A
[0030] Based on the degree of crimp obtained in (1) above, fibers are classified into three categories: low-crimp fibers with fewer than 4 crimps / 25 mm, crimped fibers A with 4 to 25 crimps / 25 mm, and high-crimp fibers with more than 25 crimps / 25 mm. The three types of fibers are weighed separately, with the weight of the low-crimped fibers being a, the weight of the crimped fibers A being b, and the weight of the high-crimped fibers being c. The crimped fiber A content is calculated using the following formula: crimped fiber A content (%) = [b / (a+b+c)] * 100.
[0031] (4) Area of a single mesh opening
[0032] a. Sample and equipment preparation
[0033] Cut three 5cm*5cm pieces of fiber structure with a mesh opening structure as samples. First, take one of the samples and observe and photograph it through light using a digital microscope (KEYENCE VHX-2000). The magnification should be selected based on whether a clear image can be obtained, such as 30x.
[0034] b. Measurement
[0035] Then, 10 mesh openings were randomly selected from the above-mentioned images, and the images were processed using the processing software provided by the digital microscope to automatically calculate the area of each mesh opening, thereby obtaining 10 sets of data. The results were averaged from the 10 sets of data.
[0036] Repeat the above steps to measure the remaining two samples, and take the average value of the three samples as the final result.
[0037] (5) Opening area ratio
[0038] a. Preparation of samples and equipment
[0039] Refer to the test method "(4) Area of a single mesh opening a. Sample and equipment preparation".
[0040] b. Measurement
[0041] The image is processed using the processing software provided by the digital microscope to automatically calculate the total area S of the image and the area S' of all mesh openings in the image.
[0042] c. Calculation
[0043] Calculated according to the following formula: Opening area ratio (%) = [S' / S] * 100.
[0044] The same method was used to measure and calculate the opening area ratios on the remaining two samples, and the final result was the average of the three samples.
[0045] (6) Fineness
[0046] First, cut a 5cm*5cm piece of flocculent material as the sample flocculent material. When sampling, be sure to cut from a flat piece without any bonding points. Then disassemble the mesh structure from the sample flocculent material. Then, disassemble 10 single yarns from the mesh structure and test according to the single yarn method of GB / T 14343-2008. The average value of the 10 single yarns is taken as the final result.
[0047] (7) Fiber material
[0048] The filling and fiber structure in the flakes are separated. The filling and fiber structure are scanned separately using Fourier transform infrared spectroscopy, and the types of their respective fiber raw materials are analyzed based on the infrared characteristic peaks. For example, at 1720 cm -1 There are characteristic peaks of carbonyl at 1265cm -1 If there is an ester characteristic peak at 1640cm -1 There are characteristic peaks of amide groups at 1560 cm -1 If there are characteristic peaks of -NH- and -CH- at the same position, it is judged to be polyamide fiber. If all fiber characteristic peaks are consistent, it can be considered that they are made of the same material.
[0049] Remove the filling and observe its appearance. If it is a ball-shaped fiber aggregate, it is pearl cotton. If it is a loose, irregular mixture of many fibers, it is open cotton. If it is a sheet-like, bonded mass, it is imitation down cotton or spray-bonded cotton. Observe the fibers under a microscope and if the surface has scales and feels rough, it is wool.
[0050] (8) Weight
[0051] First, cut a 5cm*5cm piece of flocculent cloth as the sample flocculent cloth. When sampling, be sure to cut the flocculent cloth on a flat surface without any sticking points. Then disassemble the mesh structure from the sample flocculent cloth and weigh it M. According to the following formula, calculate the gram weight of the sample cloth. Measure the gram weight of the remaining two pieces of sample cloth in the same way, and take the average value as the final result. Gram weight (g / m 2 )=M / (0.05*0.05)
[0052] (9) Washing deviation rate
[0053] The wash drift rate was evaluated using a cushion.
[0054] a. Cushion preparation
[0055] Prepare a flocculent sheet of 40cm×40cm in size, with a density of 206*162 pieces / inch and a gram weight of 45.5g / m 2 Plain woven fabric is used as the surface fabric, with a density of 204*58 threads / inch and a weight of 37.0g / m 2 Use plain woven fabric as the inner layer. Sew the outer layer, wadding, and inner layer together horizontally, with a line every 10 cm, to obtain a 40 cm x 40 cm cushion.
[0056] b. Washing
[0057] Refer to ISO 6330:2012(E) Standard for household washing and drying programs for textile testing. For the washing machine, select "Type A", the washing program "4M", the number of washes is 5, and the drying program after washing is "A-Line Drying".
[0058] c. Observation and analysis
[0059] After washing, remove the top and backing fabrics of the cushion, leaving only the flocculent fabric. Place the cushion flat on a transparent plate. Illuminate the flocculent fabric with a D65 light source vertically from below the plate. Take a photo from above the flocculent fabric (the camera is parallel to the flocculent fabric). Print the photo. Cut out the padded and unpadded areas and weigh them separately. The weight of the padded area (W1) and the weight of the unpadded area (W2) are calculated.
[0060] d. Calculate the post-wash offset rate = W1 / (W1+W2)×100.
[0061] Repeat the above steps for a total of 5 samples and take the average of the 5 results as the final result. A larger wash drift rate indicates more filler drift and poorer wash durability.
[0062] (10) Appearance evaluation
[0063] Observe the appearance of the unwashed cushion described in the preceding paragraph (9) under a D65 light source. If the fiber structure is not visible, it indicates no effect ("○"); if the fiber structure is slightly visible, it indicates a slight effect ("△"); if the fiber structure is clearly visible, it indicates a serious effect ("×").
[0064] (11) Feel
[0065] Ten people evaluated the hand feel of the unwashed cushions mentioned in the previous section (9) and divided them into four grades: excellent, good, fair, and poor. If more than eight people rated the hand feel good, it was considered excellent; if 7-8 people rated it good; if 6-7 people rated it fair; and if 5 or fewer people rated it poor.
[0066] (12) Insulation rate
[0067] The test sample is the seat cushion prepared in step (9) above. The test is carried out according to the KES method, with the heating plate temperature ΔT = 20°C and the wind speed 0.19 m / s. The larger the thermal insulation value, the better the thermal insulation performance.
[0068] Example 01:
[0069] The weight of the polyamide FDY is 2.5g / m 2 The warp knitted mesh fabrics 1 and 2 are used as the fiber structures of the upper and lower surfaces respectively. The warp knitted mesh fabrics 1 and 2 are made of warp satin fabric, and the mesh opening shape is a quadrilateral with a side length of 5 mm and an opening area of about 25 mm. 2 The open area accounts for 87%. The filling material is a blend of open cotton, consisting of a 35:65 ratio of regular round-section polyester crimped fiber A-1 (8 crimps / 25mm) and hollow polyester crimped fiber A-2 (18 crimps / 25mm). The regular round-section polyester crimped fiber A-1 has a single filament fineness of 5D and a length of 32mm; the hollow polyester crimped fiber A-2 has a hollowness of 25%, a single filament fineness of 3.3D, and a length of 38mm.
[0070] Feed the warp knitted mesh cloth 2 into the lower feeding port of the flake processing equipment, and evenly spread the loose cotton (spreading weight is 60g / m 2 ), feeding the warp knitted mesh fabric 1 into the upper feeding port at a conveying speed of 5 m / min, and rolling it after being squeezed by a pressure roller to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0071] Example 02:
[0072] A fluff sheet of the present invention was obtained by mixing open cotton fibers, consisting of a mixture of ordinary round-cross-section polyester crimped fibers A-1 with 8 crimps / 25 mm and hollow polyester crimped fibers A-2 with 4 crimps / 25 mm in a ratio of 35:65, with the remaining preparation being the same as in Example 01. Specific parameters are shown in Table 1.
[0073] Example 03:
[0074] The hollow polyester crimped fiber A-2 was replaced with a hollow polyester crimped fiber A-2 having 25 crimps / 25 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0075] Example 04:
[0076] The material is made of 30D / 12f polyamide FDY with a gram weight of 5.5g / m 2 The warp knitted mesh fabrics 1 and 2 are used as the fiber structures of the upper and lower layers respectively. The warp knitted mesh fabrics 1 and 2 are made of warp satin fabric, and the mesh opening shape is a quadrilateral with a side length of 5 mm and an opening area of about 25 mm. 2 , the opening area accounts for 85%.
[0077] A filler consisting of a mixture of ordinary round-section low-crimp polyester fiber with 3 crimps / 25 mm and hollow polyester crimped fiber A-2 with 18 crimps / 25 mm in a ratio of 5:95 was used. The remaining conditions were the same as in Example 01 to produce the flocculent sheet of the present invention. Specific parameters are shown in Table 1.
[0078] Example 05:
[0079] The weight of the selected warp knitted mesh fabrics 1 and 2 is 6.7g / m 2 , opening area is 0.8mm 2 , the opening area accounts for 65%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0080] Example 06:
[0081] The weight of the warp knitted mesh fabrics 1 and 2 is 4.3 g / m 2 , opening area is 4mm 2 , the opening area accounts for 78%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0082] Example 07:
[0083] The weight of the selected warp knitted mesh fabrics 1 and 2 is 3.2g / m 2 , opening area is 16mm 2, the opening area accounts for 83%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0084] Example 08:
[0085] The weight of the warp knitted mesh fabrics 1 and 2 is 2.3g / m 2 、Opening area is 64mm 2 , the opening area accounts for 89%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0086] Example 09:
[0087] The weight of the warp knitted mesh fabrics 1 and 2 is 2.0 g / m 2 、Opening area is 100mm 2 , the opening area accounts for 91%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0088] Example 10:
[0089] The yarns used for the warp knitted mesh fabrics 1 and 2 are 8D polyamide FDY (monofilament) with a gram weight of 1.3 g / m 2 The rest of the process is the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0090] Example 11:
[0091] The yarn of the warp knitted mesh fabrics 1 and 2 is 75D / 36f polyamide FDY with a gram weight of 15.0g / m 2 , the opening area accounts for 85%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 1.
[0092] Example 12:
[0093] The length of the hollow polyester curly fiber A-2 was 10 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0094] Example 13:
[0095] The length of the hollow polyester curly fiber A-2 was 23 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0096] Example 14:
[0097] The length of the hollow polyester curly fiber A-2 was 63 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0098] Example 15:
[0099] The length of the hollow polyester curly fiber A-2 was 75 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0100] Example 16:
[0101] A mixture of conventional round-cross-section polyester crimped fiber A-1 with 8 crimps / 25 mm and hollow polyester crimped fiber A-2 with 18 crimps / 25 mm was prepared in a ratio of 35:65 and pelletized in a pelletizer to form pearl cotton. The remaining steps were the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0102] Example 17:
[0103] A wadding of the present invention was obtained by mixing conventional round-cross-section polyester crimped fibers A-1 with 8 crimps / 25 mm and hollow polyester crimped fibers A-2 with 18 crimps / 25 mm in a ratio of 35:65. The fibers were opened, carded, and web-formed, and then sprayed with a binder to form a wadding. The remaining steps were the same as in Example 01. Specific parameters are shown in Table 2.
[0104] Example 18:
[0105] The 15.0 g / m2 fiber is made of low melting point polyester fiber (melting point 120°C) and three-dimensional hollow crimped ordinary polyester fiber (melting point 260°C, crimp number 8 / 25mm, hollow ratio 8%) in a weight ratio of 30:70. 2 The non-woven fabric (manufactured by Jinan Haoxin Industrial Co., Ltd.) was used as the lower fiber structure, and the rest was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0106] Example 19:
[0107] The length of the hollow polyester curly fiber A-2 was 8 mm, and the rest of the process was the same as in Example 01 to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0108] Example 20:
[0109] The yarn of the warp knitted mesh fabrics 1 and 2 is 30D / 12f polyamide FDY with a gram weight of 16.0g / m 2 , opening area is 25mm 2 , the opening area accounts for 71%, and the rest is the same as in Example 01, to obtain the flakes of the present invention. Specific parameters are shown in Table 2.
[0110] Clothing, bedding, outdoor products or decorative materials are made from the flakes of Examples 1-20.
[0111] Comparative Example 01:
[0112] A mixture of open cotton, consisting of a mixture of 35:65 of regular round-cross-section polyester crimped fibers A-1 (30 crimps / 25 mm) and hollow polyester crimped fibers A-2 (30 crimps / 25 mm), was used as the filling. The remaining conditions were the same as in Example 01 to produce a flocculent sheet. Specific parameters are shown in Table 2.
[0113] Comparative Example 02:
[0114] The 15.0 g / m 2 Non-woven fabrics (manufactured by Jinan Haoxin Industrial Co., Ltd.) were used as the upper and lower fiber structures of the flakes, and the rest was the same as in Example 01 to obtain flakes. Specific parameters are shown in Table 2.
[0115] Table 1
[0116] Table 2
Claims
1. A flake, comprising a filler and a fiber structure distributed on both sides of the filler, characterized in that: The filler is composed of fibers, including curled fibers A with a curl number of 4 to 25 / 25 mm; among the fiber structures on both sides of the filler, at least one side of the fiber structure is a mesh open fiber structure, and the opening area of the mesh open fiber structure accounts for more than 60% of its total area.
2. The flakes according to claim 1, characterized in that: The area of a single mesh opening on the mesh open fiber structure is 1 to 100 mm 2 .
3. The flakes according to claim 1 or 2, characterized in that: The mesh open fiber structure has a gram weight of 2 to 15 g / m 2 .
4. The flakes according to claim 1 or 2, characterized in that: The yarn forming the mesh-like open fiber structure has a fineness of 10 to 70 deniers.
5. The flakes according to claim 1, characterized in that: The length of the curled fibers A in the filler is 10 to 70 mm.
6. The flakes according to claim 5, characterized in that: The filler is one or more of pearl cotton, loose cotton, imitation down cotton and wool.
7. Use of the flakes according to claim 1 in clothing, bedding, outdoor products and decorative materials.
Citation Information
Patent Citations
Cotton padding
CN202173121U
Combined breathable comforter inner
CN203388604U
Water washable bedding
JP1997313323A
Inner cotton
JP2017177532A
Futon and futon packaging
JP3228478U