Separator of lithium-ion battery, and preparation method therefor and use thereof

The electrospinning separator prepared by modifying fluorinated polyolefin polymer uses the hydrofluoric acid absorption function to remove hydrofluoric acid in the electrolyte, solving the problem of transition metal dissolution caused by the decomposition of lithium hexafluorophosphate in lithium-ion batteries, and improving the battery performance. Cycling stability and performance.

WO2024217474A1PCT designated stage expired Publication Date: 2024-10-24SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/088428
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Lithium hexafluorophosphate in lithium-ion batteries decomposes under high temperature or water-containing conditions to produce hydrofluoric acid, which causes the dissolution of transition metals and increases the internal resistance of the battery, affecting cycle performance.

Method used

Lithium-ion battery separators are prepared by electrospinning using modified fluorinated polyolefin polymers, which contain groups with hydrofluoric acid absorption functions to remove hydrofluoric acid in the electrolyte and reduce the dissolution of transition metal ions.

Benefits of technology

It improves the cycle stability and battery performance of lithium-ion batteries, reduces the amount of transition metal dissolution, and enhances the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024088428_24102024_PF_FP_ABST
    Figure CN2024088428_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium batteries. Provided are a separator of a lithium-ion battery, and a preparation method therefor and the use thereof. The separator comprises a modified fluorinated polyolefin polymer, which is obtained by means of a polymerization reaction between a fluorinated polyolefin and a modified monomer, wherein the modified monomer comprises at least one of imidazole and a derivative thereof, and a pyridine olefin substitute and a derivative thereof. The modified polymer raw material used in the separator comprises a fluorinated polyolefin main chain and a side chain with a clearing function, and is prepared into the separator by means of electrostatic spinning, and the separator has the effects of absorbing and clearing hydrofluoric acid; and a lithium-ion battery comprising the separator has a lower transition-metal dissolution amount and better cycle performance, and thus has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium-ion battery separator and its preparation method and application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application with application number CN202310413325.1 filed with the Patent Office of China on April 17, 2023, entitled “A lithium-ion battery separator, its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present disclosure relates to the technical field of lithium-ion batteries, and in particular to a lithium-ion battery separator and a preparation method and application thereof. Background Art

[0004] As an efficient electrochemical energy storage device, lithium-ion batteries have attracted extensive attention from academia and industry due to their high energy density and low redox potential. To date, the electrolyte of lithium-ion batteries is mainly composed of lithium hexafluorophosphate (LiPF6) and alkyl carbonate solvents; however, lithium hexafluorophosphate will decompose at high temperature or in the presence of water to produce hydrofluoric acid (HF) and hexafluorophosphate (PF5 - ), which leads to the dissolution of transition metals (such as nickel, cobalt, manganese, etc.) in the positive electrode material; and the transition metal elements dissolve in the electrolyte, migrate and deposit to the negative electrode of the battery, resulting in serious gas production and increased internal resistance of the battery; in addition, metal deposition promotes the continuous destruction and regeneration of the negative electrode SEI film, consumes a large amount of active lithium and causes the battery cycle performance to decline.

[0005] In the prior art, there are a variety of technical means to solve or prevent the adverse consequences caused by the decomposition of lithium hexafluorophosphate. For example, coating or element doping of the positive electrode material is an effective means to prevent the dissolution of transition metals, but this method cannot reduce the impact of hydrofluoric acid on other structures or components of the battery. In addition, the use of other lithium salts instead of lithium hexafluorophosphate can fundamentally reduce the generation and diffusion of hydrofluoric acid, but there are problems such as poor solubility in solvents and low ionic conductivity. Existing literature has proved that the application of materials with the function of removing hydrofluoric acid can effectively improve the cycle performance of the battery. Introducing electrolyte additives with hydrofluoric acid absorption function is a common means, but the use of additives may cause adverse consequences such as decreased electrolyte conductivity and increased battery internal resistance.

[0006] Application Contents

[0007] The first purpose of the present disclosure is to provide a lithium-ion battery separator. In order to address the potential negative impact of the decomposition of lithium hexafluorophosphate electrolyte, the molecular structure of the separator disclosed herein contains groups with hydrofluoric acid absorption function, thereby removing the hydrofluoric acid generated in the battery electrolyte, thereby reducing the dissolution of transition metal ions and improving the battery cycle stability.

[0008] The second purpose of the present disclosure is to provide a method for preparing the lithium-ion battery separator, which uses an electrospinning method to produce a separator with small pore size, high porosity and strong affinity with the electrolyte.

[0009] The third object of the present disclosure is to provide a use of the lithium-ion battery separator in the lithium battery field.

[0010] In order to achieve the above-mentioned purpose of the present disclosure, the following technical solutions are adopted:

[0011] A lithium-ion battery separator comprises a modified fluoropolyolefin polymer, wherein the polymer is obtained by polymerization of a fluoropolyolefin and a modified monomer; wherein the modified monomer comprises at least one of olefin-substituted imidazole and its derivatives, and olefin-substituted pyridine and its derivatives.

[0012] Furthermore, the fluorinated polyolefin includes at least one of polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene, polyvinyl fluoride, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer and tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether.

[0013] Furthermore, the number average molecular weight of the fluorinated polyolefin is 300,000 to 700,000.

[0014] Furthermore, the modified monomer includes at least one of vinyl imidazole, 2-methyl vinyl imidazole, allyl imidazole, 2-methyl allyl imidazole, 2-vinyl pyridine, 3-vinyl pyridine, 2-methyl vinyl pyridine, allyl pyridine or 4-vinyl pyridine.

[0015] Furthermore, the mass ratio of the fluorinated polyolefin to the modified monomer is (2-5):1.

[0016] The preparation method of the lithium-ion battery separator comprises the following steps: step 1, mixing a solution of fluoropolyolefin, a modified monomer, a catalyst and a ligand compound, and obtaining a modified fluoropolyolefin polymer by heating and polymerization reaction; step 2, preparing a separator by electrostatic spinning the modified fluoropolyolefin polymer.

[0017] Furthermore, in step 1, the solvent of the fluorinated polyolefin solution includes at least one of toluene, o-xylene, chloroform, dichloromethane, carbon tetrachloride, N-methylpyrrolidone, dimethyl sulfoxide or N,N-dimethylformamide; the catalyst includes at least one of cuprous chloride, cuprous bromide, ruthenium chloride, ruthenium bromide or ferrous chloride; the ligand compound includes at least one of 1,1,4,7,10,10-hexamethyltrimethyltetramine, tris(N,N-dimethylaminoethyl)amine or 4,4-dimethyl-2,2-bipyridine, 2,2,2-bipyridine, 4,4-di-tert-butyl-2,2-bipyridine or 4,4-di(5-nonyl)-2,2-bipyridine;

[0018] Furthermore, in step 1, the mass fraction of the fluorinated polyolefin solution is 5% to 20%; the mass of the catalyst is 0.5% to 3% of the fluorinated polyolefin; and the mass ratio of the ligand compound to the catalyst is (4 to 6):1.

[0019] Furthermore, in step 1, the polymerization reaction temperature is 60° C. to 120° C., and the polymerization reaction time is 24 h to 72 h.

[0020] Furthermore, in step 2, the modified fluorinated polyolefin polymer is fully mixed with a second solvent to obtain a spinning solution and used for the electrospinning; wherein the second solvent comprises at least one of toluene, p-xylene, o-xylene, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, carbon tetrachloride or cyclohexane;

[0021] Furthermore, the mass concentration of the modified fluorinated polyolefin polymer in the spinning solution is 2% to 10%.

[0022] Furthermore, in step 2, when the electrospinning is performed, the temperature of the spinning solution is 30° C. to 60° C., and the voltage of the electrospinning is 15 kV to 30 kV.

[0023] The uses of the lithium-ion battery separator in the field of lithium-ion batteries include but are not limited to lithium-ion batteries containing the lithium-ion battery separator, electrical appliances containing the lithium-ion battery separator, etc.

[0024] Furthermore, the use can be a lithium-ion battery, including a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; wherein the active material in the positive electrode sheet includes at least one of lithium manganese oxide, lithium nickel manganese oxide, lithium iron manganese phosphate or lithium nickel cobalt manganese oxide, and the material of the negative electrode sheet includes at least one of graphite, silicon carbon or silicon oxide materials.

[0025] Compared with the prior art, the beneficial effects of the present disclosure are as follows: the present disclosure provides an electrospinning membrane with hydrofluoric acid absorption and scavenging functions, and its preparation method and application. The polymer used in the membrane contains a fluorinated polyolefin main chain and a side chain with scavenging function; the lithium-ion battery containing the membrane has lower transition metal dissolution and better cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] FIG1 provides a comparison chart of the cycle performance in Experimental Example 2. DETAILED DESCRIPTION

[0028] The present disclosure is carried out through the following specific implementation methods: A lithium-ion battery separator includes a modified fluoropolyolefin polymer, and the polymer is obtained by polymerization reaction of a fluoropolyolefin and a modified monomer; wherein the modified monomer includes at least one of imidazole and its derivatives, pyridine olefin substituents and their derivatives.

[0029] It should be noted that the “imidazole and its derivatives containing olefin substitution” in the present disclosure means: on the basis of imidazole and its derivatives, they include at least one olefin substituent. Those skilled in the art can directly purchase them as needed, or use imidazole and its derivatives as raw materials for substitution synthesis; similarly, the “pyridine and its derivatives containing olefin substitution” means: on the basis of pyridine and its derivatives, they include at least one olefin substituent. Those skilled in the art can directly purchase them as needed, or use pyridine and its derivatives as raw materials for substitution synthesis.

[0030] The preparation method of the lithium-ion battery separator comprises the following steps: step 1, mixing the solution of the fluoropolyolefin, the modified monomer, the catalyst and the ligand compound, and obtaining the modified fluoropolyolefin polymer by heating and polymerization reaction; step 2, preparing the lithium-ion battery separator by electrostatic spinning the modified fluoropolyolefin polymer.

[0031] As one embodiment, the process of step 1 specifically includes: 1) mixing the fluoropolyolefin and a solvent, stirring thoroughly at 30°C to 80°C until completely dissolved, and then cooling to room temperature to obtain a solution of the fluoropolyolefin; 2) thoroughly mixing the fluoropolyolefin solution, the modified monomer, and the catalyst under an inert environment, and then adding the ligand compound to carry out a heating polymerization reaction; 3) purifying the reaction mixture to obtain the modified fluoropolyolefin polymer. As another embodiment, the purification process includes: pouring the mixture into methanol, filtering after settling, and then redissolving the filtered product in NMP solution; repeating the above steps three times, and then sequentially settling the filtered product in methanol, filtering, and drying the final filtered product to obtain the modified fluoropolyolefin polymer.

[0032] As an embodiment, the number average molecular weight of the fluorinated polyolefin includes but is not limited to 30, 35, 40, 45, 50, 55, 60, 65, and 70 (unit: 10,000).

[0033] As an embodiment, the mass ratio of the fluorinated polyolefin to the modified monomer includes but is not limited to 2:1, 3:1, 4:1, and 5:1.

[0034] As an embodiment, the mass fraction of the fluoropolyolefin solution (based on solute) includes but is not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%.

[0035] As an embodiment, the mass of the catalyst is 0.5%, 1%, 1.5%, 2%, 2.5%, or 3% of the mass of the fluorinated polyolefin; as an embodiment, the mass of the catalyst is 1% of the mass of the fluorinated polyolefin.

[0036] As an embodiment, the mass ratio of the ligand compound to the catalyst includes but is not limited to 4:1, 4.5:1, 5:1, 5.5:1, and 6:1.

[0037] As an embodiment, the temperature of the polymerization reaction includes but is not limited to 60, 70, 80, 90, 100, 110, 120 (unit: ° C), and the time of the polymerization reaction includes but is not limited to 24, 30, 36, 48, 60, 72 (unit: h).

[0038] As an embodiment, when performing the electrospinning, the temperature of the spinning solution includes but is not limited to 30, 35, 40, 45, 50, 55, 60 (unit: ° C), and the voltage of the electrospinning includes but is not limited to 15, 20, 25, 30 (unit: kV).

[0039] Example 1

[0040] (1) Graft modification of PVDF

[0041] 5 g of PVDF and 50 mL of NMP were added to a three-necked flask and dissolved at 80 ° C. After the PVDF was completely dissolved, the temperature was lowered to room temperature; 2.5 g of 1-vinylimidazole and 0.05 g of CuCl were added to the three-necked flask, argon was introduced into the apparatus and stirring was continued for 30 min, 0.25 g of 1,1,4,7,10,10-hexamethyltrimethyltetramine was added, and then the temperature was raised to 120 ° C. and the reaction was reacted for 48 h before terminating the reaction; the reaction solution was poured into methanol for sedimentation, filtered, and dried to obtain the grafted product of this embodiment.

[0042] (2) Electrospinning membrane

[0043] 1 g of the grafted product was dissolved in 10 g of a mixed solvent containing tetrahydrofuran, N-methylpyrrolidone and N,N-dimethylacetamide, wherein the mass ratio of the three solvents was 5:3:2; the mixture was stirred at 45°C for 2 h to obtain an electrospinning solution; and electrospinning was performed under the conditions of a spinning voltage of 20 kV, a solution propulsion speed of 1.0 mL / min, and a receiving distance of 20 cm to obtain the diaphragm of this embodiment.

[0044] Example 2

[0045] The process is basically the same as Example 1, except that the PVDF in step (1) is replaced by PVDF-HFP, and the 1-vinylimidazole is replaced by 2-methylallylimidazole.

[0046] Example 3

[0047] The process is basically the same as Example 1, except that 2.5 g of 1-vinylimidazole in step (1) is replaced by 1 g of 2-vinylpyridine.

[0048] Example 4

[0049] The method is basically the same as Example 1, except that the NMP in step (1) is replaced by DMF, and the 1,1,4,7,10,10-hexamethyltrimethyltetramine is replaced by 4,4-dimethyl-2,2-bipyridine.

[0050] Example 5

[0051] The process is basically the same as Example 1, except that the step (1) of "heating to 120°C and reacting for 48h" is replaced by "heating to 60°C and reacting for 72h".

[0052] Example 6

[0053] The process is basically the same as Example 1, except that the 10 g mixed solvent of tetrahydrofuran, N-methylpyrrolidone and N,N-dimethylacetamide in step (2) is replaced by N-methylpyrrolidone, dimethyl sulfoxide and cyclohexane.

[0054] Example 7

[0055] The method is basically the same as Example 1, except that the step (2) of "stirring at 45°C for 2 h" is replaced by "stirring at 60°C for 1.5 h".

[0056] Example 8

[0057] The process is basically the same as Example 1, except that the spinning voltage of 20 kV in step (2) is replaced by 30 kV.

[0058] Comparative Example

[0059] 1 g of PVDF was dissolved in 10 g of a mixed solvent of tetrahydrofuran, N-methylpyrrolidone, and N,N-dimethylacetamide, with a mass ratio of the three solvents being 5:3:2. The solution was stirred at 45°C for 2 h to obtain an electrospinning solution. Electrospinning was performed under the conditions of a spinning voltage of 20 kV, a solution propulsion speed of 1.0 mL / min, and a receiving distance of 20 cm to obtain a PVDF membrane.

[0060] Test Example 1

[0061] The diaphragms from each example and comparative example were placed in sample bottles containing 30 ml of a 1 mol / L LiPF6 / EC electrolyte solution with an initial acidity of 353 ppm. Three separate tests were conducted on three separate samples of the diaphragms produced in each example (and comparative example). After the sample bottles were stored at 45°C for 7 days, the acidity of each electrolyte was measured. The results are shown in Table 1 below. Compared to the comparative example, the diaphragm system produced in this example can remove HF generated in the electrolyte.

[0062] Table 1

[0063] Test Example 2

[0064] A monolithic battery was assembled using the separators of Example 1 and the comparative example. The positive electrode ratio was lithium nickel manganese oxide: PVDF: SP = 96:2:2; the negative electrode ratio was graphite: SP: CMC: SBR = 96.5:1.5:1.5:1.5; the electrolyte was a 1 mol / L LiPF6 solution, and the solvent was EC + EMC (volume ratio 3:7).

[0065] The two assembled monolithic batteries were subjected to cycling tests using a 0.5C / 1C charge-discharge cycle in a 25°C constant temperature chamber with a voltage range of 3.5-5V. A comparison of the cycling data is shown in Figure 1.

[0066] At the same time, ICP tests were performed on the negative electrode sheets and separators of the two assembled monolithic batteries. The specific test method was: the two monolithic batteries were immersed in aqua regia, diluted, and then tested for the content of each element. The test data are shown in Table 2 below.

[0067] It can be seen from FIG1 and Table 2 that, compared with the ungrafted diaphragm system of the comparative example, the battery cell of the grafted diaphragm system of this embodiment has better cycle performance and lower transition metal dissolution amount, and has excellent technical effects.

[0068] Table 2 Industrial Applicability

[0069] The present disclosure provides a lithium-ion battery separator. To address the potential negative impact of the decomposition of lithium hexafluorophosphate electrolyte, the molecular structure of the separator contains groups with hydrofluoric acid absorption function, thereby removing the hydrofluoric acid generated in the battery electrolyte, thereby reducing the dissolution of transition metal ions and improving the battery cycle stability.

Claims

1. A lithium ion battery separator, It is characterized in that The diaphragm includes a modified fluorinated polyolefin polymer, and the polymer is obtained by polymerization of a fluorinated polyolefin and a modified monomer; The modified monomer includes at least one of olefin-substituted imidazole and its derivatives, and olefin-substituted pyridine and its derivatives.

2. The lithium ion battery separator according to claim 1, It is characterized in that The fluorinated polyolefin includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinyl fluoride, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer and tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether.

3. The lithium ion battery separator according to claim 2, It is characterized in that The number average molecular weight of the fluorinated polyolefin is 300,000 to 700,000.

4. The lithium ion battery separator according to claim 1, It is characterized in that The modified monomer includes at least one of vinyl imidazole, 2-methyl vinyl imidazole, allyl imidazole, 2-methyl allyl imidazole, 2-vinyl pyridine, 3-vinyl pyridine, 2-methyl vinyl pyridine, allyl pyridine or 4-vinyl pyridine.

5. The lithium ion battery separator according to claim 1, It is characterized in that The mass ratio of the fluorinated polyolefin to the modified monomer is (2-5):

1.

6. The method for preparing a lithium ion battery separator according to any one of claims 1 to 5, It is characterized in that The steps include: Step 1: mixing a fluorinated polyolefin solution, a modified monomer, a catalyst and a ligand compound, and subjecting the mixture to a heating polymerization reaction to obtain a modified fluorinated polyolefin polymer; Step 2: preparing a diaphragm by electrostatic spinning the modified fluorinated polyolefin polymer.

7. The method for preparing a lithium ion battery separator according to claim 6, It is characterized in that In step 1, the solvent of the fluorinated polyolefin solution includes at least one of toluene, o-xylene, chloroform, dichloromethane, carbon tetrachloride, N-methylpyrrolidone, dimethyl sulfoxide or N,N-dimethylformamide; The catalyst comprises at least one of cuprous chloride, cuprous bromide, ruthenium chloride, ruthenium bromide or ferrous chloride; The ligand compound includes at least one of 1,1,4,7,10,10-hexamethyltrimethyltetramine, tris(N,N-dimethylaminoethyl)amine or 4,4-dimethyl-2,2-bipyridine, 2,2,2-bipyridine, 4,4-di-tert-butyl-2,2-bipyridine or 4,4-di(5-nonyl)-2,2-bipyridine.

8. The method for preparing a lithium ion battery separator according to claim 7, It is characterized in that The mass fraction of the fluorinated polyolefin solution is 5% to 20%.

9. The method for preparing a lithium ion battery separator according to claim 7, It is characterized in that The mass of the catalyst is 0.5% to 3% of the fluorinated polyolefin.

10. The method for preparing a lithium ion battery separator according to claim 7, It is characterized in that The mass ratio of the ligand compound to the catalyst is (4-6):

1.

11. The method for preparing a lithium ion battery separator according to claim 6, It is characterized in that In step 1, the polymerization reaction temperature is 60° C. to 120° C., and the polymerization reaction time is 24 h to 72 h.

12. The method for preparing a lithium ion battery separator according to claim 6, It is characterized in that In step 2, the modified fluorinated polyolefin polymer is fully mixed with a second solvent to obtain a spinning solution and used for the electrospinning; wherein the second solvent includes at least one of toluene, p-xylene, o-xylene, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, carbon tetrachloride or cyclohexane.

13. The method for preparing a lithium ion battery separator according to claim 12, It is characterized in that The mass concentration of the modified fluorinated polyolefin polymer in the spinning solution is 2% to 10%.

14. The method for preparing a lithium ion battery separator according to claim 12, It is characterized in that In step 2, when the electrospinning is performed, the temperature of the spinning solution is 30° C. to 60° C., and the voltage of the electrospinning is 15 kV to 30 kV.

15. Use of the lithium ion battery separator according to any one of claims 1 to 5 in the field of lithium ion batteries.

Citation Information

Patent Citations

  • Preparation method of modified diaphragm for lithium-ion secondary battery as well as product and preparation device thereof

    CN102218871A

  • Lithium ion secondary battery and diaphragm thereof

    CN103943805A

  • Acid-scavenging functional separators for power performance of lithium ion electrochemical cells

    CN109148796A

  • High-temperature-environment-resistant battery diaphragm, preparation method thereof and lithium ion battery

    CN115579579A

  • Lithium ion battery diaphragm as well as preparation method and application thereof

    CN116454537A