Method for manufacturing a blisk for a turbine engine with orbital-friction-welded blades

The method addresses the challenge of achieving a healthy weld junction in bladed disks by determining the radial height of the weld based on geometric and orbital friction welding parameters, ensuring structural integrity and reducing environmental impact through optimized design and manufacturing.

WO2024218270A1PCT designated stage expired Publication Date: 2024-10-24SAFRAN AERO BOOSTERS SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/060661
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing bladed disks for turbomachines using orbital friction welding face challenges in achieving a healthy and contaminant-free weld junction, particularly in controlling the radial height of the junction and ensuring structural integrity, which can lead to material health issues and structural defects.

Method used

A method that determines the radial height of the weld junction based on the maximum thickness of the weld, considering geometric parameters of the blades and stubs, as well as orbital friction welding parameters like eccentricity, frequency, and forging pressure, to ensure optimal positioning and minimize the risk of crack propagation, thereby improving the structural and dimensional quality of the bladed disk.

Benefits of technology

This approach allows for precise determination of the weld junction height, reducing the risk of structural defects, improving the dimensional quality of the bladed disk, and enabling cost and time savings by optimizing the design phase, thus enhancing the performance and environmental impact of aircraft engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024060661_24102024_PF_FP_ABST
    Figure EP2024060661_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a blisk (2) for a turbine engine, comprising a plurality of blades (4) joined by orbital-friction welding to stubs (6) on the disk, at a radial junction height h between the blades and the stubs, characterised in that the radial junction height h, measured from an inter-blade surface (8) of the disc, is greater than or equal to a radial height hsc of a critical threshold (SC), plus one half of a maximum thickness of the weld emax. The invention relates to a method for manufacturing a blisk, wherein emax is determined by a geometric parameter z of the section of the blades and stubs at the junction, where z is an average of the mean radii zi sweeping across the section at any point i of the periphery of said section.
Need to check novelty before this filing date? Find Prior Art

Description

METHOD FOR MANUFACTURING A BLADED DISC FOR A TURBOMACHINE WITH ORBITAL FRICTION WELDED BLADES

[0001] The invention relates to a method of manufacturing a bladed disc for a turbomachine, and more particularly to a method of manufacturing a bladed disc by orbital friction welding of blades to a turbomachine rotor disc. The invention also relates to a turbomachine bladed disc obtained by means of the method. Prior art

[0002] Climate change is a major concern for many legislative and regulatory bodies around the world. Indeed, various carbon emission restrictions have been, are being, or will be adopted by various states. In particular, an ambitious standard applies to both new aircraft types and those already in operation, requiring the implementation of technological solutions to comply with current regulations. Civil aviation has been mobilizing for several years now to contribute to the fight against climate change.

[0003] Technological research efforts have already led to very significant improvements in the environmental performance of aircraft. The Applicant takes into consideration the impact factors in all phases of design and development to obtain less energy-intensive, more environmentally friendly aeronautical components and products whose integration and use in civil aviation have moderate environmental consequences with the aim of improving the energy efficiency of aircraft.

[0004] Consequently, the Applicant is constantly working to reduce its negative climate impact by using methods and operating virtuous development and manufacturing processes and minimizing greenhouse gas emissions to the minimum possible in order to reduce the environmental footprint of its activity.

[0005] This sustained research and development work focuses on new generations of aircraft engines, the weight reduction of aircraft, particularly through the materials used and lighter on-board equipment, the development of the use of electrical technologies to ensure propulsion, and, as an essential complement to technological progress, aeronautical biofuels.

[0006] To this end, the invention is the result of technological research aimed at significantly improving aircraft performance and, in this sense, contributes to reducing the environmental impact of aircraft.

[0007] In this context, the invention relates to an orbital friction welding method for producing a bladed disc (commonly referred to as "blisk") or a bladed drum (commonly referred to as "blum") for a turbomachine compressor.

[0008] Orbital friction welding is a welding process in which the parts to be joined are brought into contact under stress and welded by a circular motion generally defined by an eccentric, and accompanied by a uniform tangential speed, so as to generate friction and homogeneous heating at a weld junction between the two parts.

[0009] Linear friction welding is also known to be used, a welding process in which the necessary heat is created by a back-and-forth movement of the interfaces to be welded. However, orbital friction welding has several advantages over linear friction, for example, the relative movement between the two interfaces is continuous thanks to the circular friction movement, which provides better thermal homogeneity. Unlike linear movement for which the relative speed of the two parts becomes zero at each half-oscillation period. In addition, the cycle time of orbital welding is considerably lower than that of linear friction welding (respectively approximately 2 minutes compared to approximately 5 minutes).

[0010] Published patent document EP 1 495 829 A1 discloses a method for manufacturing combined profiled blades and discs, in which each of the blades has a stub to be welded to the disc by linear friction. The document proposes a stub design comprising a ratio of the widest part to the narrowest part of said stub which is less than 2 to minimize its camber.

[0011] However, the stump design proposed by the document has room for improvement, as it cannot be applied to orbital welding. Indeed, such a stump does not allow for a healthy, contaminant-free orbital welded joint to be obtained.

[0012] Published patent document EP 2 535 516 A1 discloses a method of orbital friction welding of blades to a turbomachine rotor in which, once a material consumption is reached in a welding zone between the blade and the disc, the orbital movement is stopped at a reference position, and a forging force is exerted on the blade against the rotor in order to form the weld.

[0013] However, the orbital welding process disclosed in the document has room for improvement. This may require better control of the position of the blade welding zone relative to the rotor disc, so as to avoid structural defects while ensuring material health in the welding zone.

[0014] The invention aims to solve at least one of the problems posed by the prior art. More specifically, the invention aims to propose a solution making it possible to accurately determine the radial height of an orbital friction welded junction of a blade to a rotor disk stub.

[0015] The invention is the result of technological research aimed at very significantly improving the performance of aircraft and, in this sense, contributes to reducing the environmental impact of aircraft. For this purpose, the present invention relates to a method for manufacturing a bladed disc comprising blades joined by orbital friction welding to stubs on the disc and extending radially outwardly, said method comprising a step of determining the radial junction height h between the blades and the stubs, remarkable in that the radial junction height h is determined as a function of a maximum thickness of the weld e max , said radial junction height being all the greater as the maximum thickness of the weld max is large, said maximum thickness of the weld maxbeing determined by a geometric parameterz of the section of the blades and the stubs at the junction, wherez is an average of the mean radiiz i scanning said section at any point on the periphery of said section, the maximum thickness of the weld max determined being all the smaller as the geometric parameter is small.

[0016] According to an advantageous embodiment of the invention, the maximum thickness of the weld max is also determined by at least one of the following orbital friction welding parameters: eccentricity; frequency; and forging pressure.

[0017] According to an advantageous embodiment of the invention, the maximum thickness of the weld max is also determined by at least one of the following orbital friction welding parameters: eccentricity; frequency; and forging pressure.

[0018] According to an advantageous embodiment of the invention, the material consumption rate is measured during a parameterization orbital friction welding carried out with the same parameters as the orbital friction welding of the blades.

[0019] Preferably, the measurement of the material consumption rate is measured by means of data acquisition on a machine performing orbital friction welding.

[0020] According to an advantageous embodiment of the invention, the material consumption rate is determined on the basis of the following orbital friction welding parameters: eccentricity; frequency; and forging pressure.

[0021] According to an advantageous embodiment of the invention, the radial junction height h, measured from an inter-blade surface of the disc, is greater than or equal to a radial height h SCof a critical threshold, increased by half of a tolerance interval IT determined according to the maximum thickness of the weld max .

[0022] Advantageously, the critical threshold corresponds to a limit of non-propagation towards the disc of a crack initiated in the blade. The radial height h SC of the critical threshold is determined either by means of crack propagation calculations or by considering that said radial height h SC is greater than or equal to twice a fillet radius of the stubs with said inter-blade surface.

[0023] The determined tolerance interval IT corresponds to an area in which the junction is included, it is an area allowing the presence of the junction, in particular in the case where the blade and the disc each comprise a different alloy from a base material.

[0024] According to an advantageous embodiment of the invention, the tolerance interval IT is greater than or equal to the maximum thickness of the weld. max .

[0025] According to an advantageous embodiment of the invention, the tolerance interval IT is determined as a function of an obliqueness tolerance of the junction relative to the inter-blade surface of the disc.

[0026] The invention also relates to a bladed disk for a turbomachine, comprising a plurality of blades joined by orbital friction welding to stubs on the disk, at a radial junction heighthbetween the blades and the stubs, remarkable in that the radial junction heighth, measured from an inter-blade surface of the disk, is greater than or equal to a radial heighth SC of a critical threshold, increased by half of a maximum thickness of the weld max .

[0027] According to an advantageous embodiment of the invention, the bladed disc corresponds to a moving wheel intended to be arranged upstream of a flow separation nozzle in an axial turbomachine.

[0028] Advantageously, the bladed disc is manufactured according to the method for manufacturing a bladed disc according to the invention.

[0029] The measures of the invention are particularly advantageous in that the radial height of the weld plane determined by the method from the design of the bladed disc makes it possible to dimension the blade and the stub so as to ensure an optimal radial position of the welded joint. Thus, stress constraints exerted on the joint can be anticipated prior to the manufacture of the bladed disc, so as to improve the structural and dimensional quality of the joint and of the manufactured disc.

[0030] The method for manufacturing the bladed disc of the present invention allows for considerable time and cost savings, since said method makes it possible to avoid prior art techniques in which it is necessary to wait for the first welding tests to make cuts on test pieces aimed at approximately validating the radial position of the welded junction. Indeed, the method according to the invention corresponds to a predictive method for optimizing the height of the junction during the design phase of the blade, and therefore allows this constraint to be integrated directly into the optimization of the shape of the blade.

[0031] It is understood that each detail of an embodiment below may be combined with each other detail of the other embodiments.

[0032] The figure represents a perspective view of a bladed disc according to the invention;

[0033] Diagrammatically illustrates a side view of a blade of the bladed disc thereof which is joined by orbital friction welding to a stub extending radially outwardly from an inter-blade surface of said disc;

[0034] Illustrates a side view of the blade with a misaligned joint exhibiting an skew with a nominal weld joint;

[0035] Illustrates schematically a section of the blade and / or stub at the weld junction visible at;

[0036] Illustrates the junction section of the when determining an average radius A scanning said section from a point A on the periphery of said section;

[0037] Illustrates the junction section of the when determining an average radius B scanning said section from a point B on the periphery of said section;

[0038] Schematically represents a perspective view, during orbital friction welding, of the blade to the disc stub, by means of the joining section illustrated in figures 4 to 6;

[0039] Illustrates a mapping of the amplitude of the average rays i sweeping the junction section at every point of its periphery;

[0040] Illustrates the joint section of the showing three marks for taking measurements of the maximum thickness of the welded joint, with two of these joint sections identical;

[0041] The is a first graph representing the evolution of the estimated thickness of the welded joint compared to actual measurement points of said thickness, following a local width of the junction section of the, and to a first reference positioned at 1 / 4 of a total extent of said section;

[0042] The is a second graph representing the evolution of the estimated thickness of the welded joint compared to actual measurement points, following a local width of the junction section of the, and to a second reference point positioned at half the total extent of said section;

[0043] There is a third graph representing the evolution of the estimated thickness of the welded joint compared to actual measurement points, following a local width of the junction section of the, and to a third mark positioned at 3 / 4 of the total extent of said section. Detailed description of the embodiments

[0044] In the following description, the terms "internal" and "external" refer to a positioning relative to the axis of rotation of an axial turbomachine and / or to a central axis of a bladed rotor disk. The axial direction corresponds to the direction along the axis of rotation of the turbomachine, with lengths being measured axially. Widths are measured circumferentially. The radial direction is perpendicular to the axis of rotation. Upstream and downstream refer to the main flow direction of the flow in the turbomachine.

[0045] The dimensions of the figures are not to scale and in particular the thicknesses or radial dimensions are exaggerated to facilitate reading of the figures.

[0046] The figure represents a perspective view of a bladed disc 2 according to the invention.

[0047] The bladed disc 2 comprises a plurality of blades 4 joined by orbital friction welding to stubs 6 extending radially outwardly from an inter-blade surface 8 of said disc 2. The welding is explained later in this description.

[0048] Advantageously, the weld forms a junction 10 (shown in dotted lines) between each blade 4 and the corresponding stub 6, said junction 10 being arranged at a radial junction height h measured from the inter-blade surface 8 of the bladed disc 2.

[0049] Preferably, the bladed disc 2 is a movable wheel intended to be arranged upstream of an air flow separation nozzle in a turbomachine. For this purpose, the inter-blade surface 8 corresponds to an air guiding surface of a fluid stream along and through a rotor. Alternatively, the bladed disc 2 may correspond to a drum-type rotor belonging to a high-pressure or low-pressure compressor.

[0050] Preferably, the disc 2 is a so-called “bi-material” disc comprising two different titanium alloys. For example, the blades 4 can be made from a Ta6v alloy, and the disc from one of the following alloys: Ti17, Ti575, Ti1023.

[0051] Advantageously, the mixture of the two different titanium alloys (Ta6v and Ti17) presents easier machinability, and makes it possible to achieve a gain in mass compared to a solution based, for example, solely on a Ti17 alloy, this is notably due to a density of Ta6v which is slightly lower than that of Ti17.

[0052] Indeed, the Ti17 alloy was preferentially chosen for the disc part for its good HCF (High Cycle Fatigue) and LFC (Low Cycle Fatigue) fatigue characteristics. A Ti17 disc will also display a greater margin in burst speed than a Ta6v disc. For the blades, the Ta6v alloy was chosen because it provides the blades with a higher elongation at break (better impact resistance), and better crack propagation behavior which results in better durability in low energy impacts.

[0053] The junction 10 thus corresponds to the limit separating the two different titanium alloys. For this purpose, the lower the radial height h of the junction 10, the greater the radial extent of the blade 4, which will allow the blade 4 to better resist impacts with debris, given that the characteristics of the titanium alloy forming the blade 4 are chosen to resist impacts (low and high energy) more than those of the alloy forming the disc. However, the junction 10 must be arranged above a critical threshold delimiting a critical zone (this will be explained later in this description). In this respect, the invention seeks to position the junction 10 in an optimized manner and as close as possible to the critical threshold. Another alternative would be to increase the radial height h of the junction 10, but this implies a high radial extent of the stub 6, this means a lower stiffness of the stubs on the disc side during welding.However, the rigidity of the stubs to be welded is crucial to ensure a robust weld. A stub that is too flexible will disperse part of the energy provided by the machine into its deformation instead of keeping it in pure friction energy. The eccentricity actually seen at the stubs will be reduced if the stubs are flexible.

[0054] The invention proposes a means for determining the optimal radial height of the junction 10 so as to guarantee the structural and dimensional quality of the weld 10 and the bladed disc 2.

[0055] In this regard, the radial junction height h is determined during the manufacturing method according to the invention. The latter comprises a step of determining the radial junction height h as a function of a maximum thickness of the weld e maxThe step of determining the position of the junction 10 is carried out from the design of the bladed disc 2, prior to its manufacture, and will be explained later in this description.

[0056] Schematically illustrates a side view of one of the blades 4 of the bladed disc 2 of the.

[0057] It can be observed that the junction 10 has a diabolo or butterfly shape, with a wider peripheral end (along the radial direction) than its inner central part, this is due to a concentration of the excess material displaced during orbital welding. For this purpose, the maximum thickness max is measured at the peripheral end of junction 10.

[0058] It can also be seen that the weld joint 10 comprises a weld plane 10.1 illustrated in a central position relative to the maximum thickness maxof said junction 10. Advantageously, the welding plane 10.1 corresponds to the optimal radial position of junction h. The latter being arranged radially above the determined critical threshold SC.

[0059] Indeed, the positioning of the weld junction 10 must guarantee the absence of breakage of the bladed disc 2 in the event of deviation of a material characteristic, i.e. propagation of a crack from the blade 4 for example, in said junction 10.

[0060] In this respect, the critical threshold SC corresponds to a limit of non-propagation towards the disc 2 of a crack initiated in the blade 4, said critical threshold SC comprising a radial height h SC from the external surface 8.

[0061] Advantageously, the radial height h SCof the critical threshold SC makes it possible to distinguish a first zone classified as "N1" in which a crack initiated, for example in the event of an impact with debris, can lead to a propagation of the crack in the rotor hub by the combination of static and vibratory stresses leading to a growth of the crack in the rotor body leading to bursting, this corresponds to a "Dangerous Engine Effect" defined according to the certification: "CS-E 510" of the EASA (European Aviation Safety Agency). The critical threshold SC also distinguishes a second zone "N2" in which the deviation of one of the uncontrollable material and / or process characteristics can produce a "Major Engine Effect". For this purpose, the critical threshold SC is commonly designated by: threshold N1 / N2.

[0062] Fleet experience has historically shown that the area of ​​blade 4 above a certain height in the blade (height relative to the blade / disc fillet) can be considered non-hazardous or non-critical. Blade breakage is then contained and does not cause the rotor to burst, thus meeting the “CS-E 515” certification specifications.

[0063] The radial heighth SC of the critical threshold can be determined by means of crack propagation calculations from appropriate damage tolerance methodologies (eg 3D crack propagation simulation), tests or from experience accumulated on similar Blisks.

[0064] Preferably, the radial height h SC of the critical threshold is calculated based on the value of the blade / disc radius. More preferably, the radial height h SCis greater than or equal to twice a fillet radius between the blade and the vein.

[0065] In the configuration of the blades 4 of the bladed disc 2, the radial height h SC is preferably equal to twice a radius R of the fillet 7 of the stubs 6.

[0066] Advantageously, the weld plane 10.1 being arranged radially above the critical threshold SC, the weld junction 10 makes it possible to avoid the risk of the appearance of the “Dangerous Engine Effect” in the turbomachine.

[0067] In order to optimally position the welding plane 10.1 from the design of the bladed disc 2, the manufacturing method according to the invention comprises a step of estimating a tolerance interval IT of the junction 10 comprising the e max . Preferably, the critical threshold SC determined corresponds to the lower limit of the tolerance interval IT.

[0068] For this purpose, the radial junction height h is greater than or equal to twice the radius R of the fillet 7, increased by half the maximum thickness max and / or increased by half of the tolerance intervalIT.

[0069] In this configuration, the radial junction height h is between twice the radius R and 4 R, and is more precisely between 2.2 and 3 R.

[0070] The tolerance interval IT is preferably based on the maximum thickness maxof the junction 10. The tolerance interval IT may also, or alternatively, be determined as a function of at least one of the following factors: the parametric variability during welding, which implies a total thickness of the junction that is more or less thick compared to a nominal junction (the parametric variability depends on the frequencies of the oscillations, the welding pressures, etc.); the precision of the radial position of the junction 10 (depending on the tolerances of the heights on the blade and / or stub side, and on the variability of the movements of the tools carrying out the welding; the obliquity of the junction 10 relative to the external surface 8, which corresponds to an inclination variability (the obliquity depends on the alignment of the blade to the stub before welding).

[0071] The illustration is an example showing the oblicity ob presented between two peaks belonging respectively to a misaligned junction 10' and to the junction 10 (corresponding here to a nominal weld junction free from geometric defects), the appearance of the oblicity at the welded junction corresponds to a variability of inclination which can depend on at least one of the following causes: the effect of the plane and out-of-plane misalignment of the two faces to be welded; the misalignment between the two stubs (the concentricity); the section to be welded and the torque of the welded materials.

[0072] With reference to figures 2 and 3, the tolerance interval IT is greater than or equal to the maximum thickness of the weld max. . The tolerance interval IT can extend radially from about 5% to 70% more than the maximum thickness max and preferably ranges from about 10 to 50%.

[0073] Preferably, the junction 10 is radially distant from the critical threshold SC by a distance corresponding to a radial extent of a heat-affected zone (HAZ) of the stump 6.

[0074] The radial junction height h can be defined using the following equation:

[0075] h=h SC + IT / 2

[0076] More preferably, the tolerance interval IT can be estimated, before the manufacture of the bladed disc 2, by means of an estimation of the maximum thickness max . Advantageously, the e max is determined as a function of a geometric parameter of the section of the blades 4 and the stubs 6 at the junction 10. Said section preferably corresponds to a flat section. The stub 6 of the disc and the corresponding blade 4, which are intended to be welded by orbital friction, have an identical junction section.

[0077] Determining the e maxdepending on the geometric parameterz will be explained following figures 3 to 5.

[0078] Advantageously, the estimation of the tolerance interval IT prior to manufacturing makes it possible to overcome the methods of verifying the IT of the prior art, for example, by avoiding the carrying out of a series of samplings during manufacturing and the carrying out of cuts in order to verify by measurement the position of the welded junction. The invention then makes it possible to ensure considerable efficiency and savings during the manufacture of the bladed disc 2.

[0079] Illustrates schematically the section 11 of the blade 4 and / or the stub 6 at the weld junction 10 visible in the. Preferably, the section 11 is identical for the blade 4 and for the stub 6 of the disc 2.

[0080] Section 11 is modeled from an aerodynamic profile 4.1 of the blade 4, the latter comprising a section widening by means of an excess thickness corresponding, preferably, at least to the eccentric of the orbital oscillation movement during welding. The eccentric corresponds to the offset value of the tool (for holding the blade) and the disc relative to a reference center, making it possible to create the orbital oscillation movement. In other words, the eccentric corresponds to the distance between the axis of rotation of the tool and the central point around which it performs its orbital movement.

[0081] The excess thickness is not necessarily constant around profile 4.1; it may present variations around said profile 4.1.

[0082] It should be noted that prior to orbital friction welding, a sacrificial volume of material (extending essentially radially) is provided on each of the blades 4 and stubs 6 to be assembled. This sacrificial volume is caused to be expelled outside the contact interface between the sections 11, thus forming a burr, commonly referred to as: "flash", which will then be removed, for example by machining, in order to form the bladed disc 2 illustrated in the. However, the flash risks causing the recirculation of material within the narrowest regions of the contact section and risks creating recesses in the welded joint, which is detrimental to the quality of the weld.

[0083] Advantageously, the widening by the eccentric of section 11 makes it possible to enlarge the contact surface during orbital friction welding so as to ensure thermal homogeneity during welding, precisely in the final section 4.1 of the blade 4. Indeed, if we add an excess thickness at least equal to the value of the eccentric, this means that the points of the final aerodynamic surface 4.1 are always in contact during welding (between the two stubs). Unlike the points in this excess thickness which, by the orbital movement, are in contact with the opposite surface only during part of the orbital oscillation movement.

[0084] Thus, during welding, a material consumption rate remains constant at the right of section 11, which makes it possible to avoid recirculation of the material (potentially harmful because it prevents the evacuation of impurities) at the level of the section of the final aerodynamic profile 4.1 of the blade and thus allow homogeneity and continuity of the mixing of the material of the stub with that of the blade making it possible to further preserve the aerodynamic profile of the blade and to obtain a resistant junction.

[0085] The modeled section 11 allows to establish the geometric parameter z. Indeed, z is an average of the average radii z i sweeping section 11 at any point of the periphery 11.1 of said section 11.

[0086] Each of the average rays i corresponds to an average length i of rays i,αextending entirely in section 11 from a point i at the periphery 11.1 of said section 11 and sweeping said section 11. Preferably, the rays z i,α correspond to projections of the point on an entire portion of the periphery 11.1 which is opposite said point.

[0087] Advantageously, the evolution of the average rays i on the periphery of the section 11 to be welded physically represents the homogeneity of the length to be sheared during rotation (orbital movement during welding) and therefore the homogeneity of the material flow expelled in the flash along the contour of the blade. It is representative of the homogeneity of contaminant ejection from the weld.

[0088] In this regard, the determination of the geometric parameter z includes the determination of the mean radius z i for the plurality of points on the entire periphery 11.1.

[0089] Preferably, the determination of the geometric parameter is an automated process using a computer algorithm. In this respect, an algorithm applying a “ray tracing” type method can be adapted, the latter also being known under the English name “ray tracing”.

[0090] Advantageously, the inventors have wisely adopted an innovative approach by introducing the ray tracing technique, which is hitherto unknown in the field of mechanics. They realized that this is the optimal way to characterize the joint section intended for orbital friction, in order to arrive at a more accurate estimate of the radial position (height) of the weld, and this prior to the orbital welding operation.

[0091] The ray tracing method on section 11 can be performed using the following steps:

[0092] - model a first section 11 (visible in) based on the final aerodynamic profile 4.1 of the blade with the addition of the overthickness (which shares the same value as that of the eccentric which is planned to be applied to the tool during orbital welding); and

[0093] - divide the periphery 11.1 evenly into several pointsi from which the raysz i,α will be projected, preferably at around 2000 points distributed evenly (this number may vary depending on the desired calculation precision); and

[0094] - project rays i,α which sweep the entire section 11 from a first point on the periphery 11.1, the number of rays z i,α projected preferentially depends on an angle α between 0.001° and 10°; and

[0095] - measure the average length i of all rays i,α projected from the first point; and

[0096] - repeat the ray projection step i,α as well as that of the measurement of the average length i , successively for all points on the periphery 11.1; and

[0097] - calculate the average length of all average lengthsz i measured from each of the total points to arrive at the geometric parameter of the junction section.

[0098] Figures 5 and 6 illustrate an example of ray projectionz A,α etz B,α , respectively, from points A and B of the periphery 11.1. These are two schematic examples of determining the average length i of all rays i,α using the ray tracing method described above.

[0099] The two points A and B correspond to the two points which respectively allowed the measurement of an average length A and an average length B. For this purpose, the determination of the geometric parameter z for section 11 corresponds to the calculation of the average of all the average lengthsz i , for example, 2000 average lengths including the average lengthsz A etz B .

[0100] Illustrates section 11 when determining an average radius A scanning said section 11 from a point A of the periphery 11.1.

[0101] It can be seen that from point A, a plurality of raysz A,α are projected onto a portion of the periphery 11.1 visible from said point A. In this configuration, the rays z A,α can be included between two extreme radii A,α tangents to the periphery 11.1.

[0102] The number of rays A,α projected can depend on the angle α chosen, the latter allows to establish the precision of determination of the average radius AFor this purpose, the angle α can be between 0.001° and 10°.

[0103] The average ray A thus corresponds to the average of all projectionsz A,α .

[0104] Illustrates section 11 when determining an average radius B scanning said section 11 from a point B of the periphery 11.1.

[0105] Preferably, the angle α is identical for all projections of the rays z i,α for the plurality of points on the periphery 11.1. Preferably, the number of points on the periphery 11.1 from which the rays will be projected is approximately 2000 points, this number being able to vary according to the desired calculation precision.

[0106] Similar to point A, the rays z B,α are projected from point B onto a portion of the periphery 11.1 visible at said point B. The average radius B corresponds to the average of all projectionsz B,α .

[0107] The geometric parameter z is therefore the average of all the mean radii z i (including medium rays) A etz B ,) points around the entire periphery 11.1.

[0108] The geometric parameter z corresponds to a geometric dimension that can be expressed in mm. Advantageously, this parameter z is the optimal dimension that best distinguishes the geometric shape of the section 11. Indeed, the surfaces of the section 11 including the projected rays z i,α from each point can be assimilated to the mixing surface of the material during orbital friction welding.

[0109] The geometric parameter zallows to take into account the specificities of orbital friction welding in the manufacturing process. Indeed, the friction force provided during welding rotates cyclically, which implies that a welding point at the end of section 11 of the stump (eg point A or B) sees a fraction of section 11 of the blade between the two extreme projected radii (z A,α ouz B,α ), these can therefore be assimilated to equivalent lengths of material to be sheared.

[0110] Moreover, the parameter z is relevant because it allows to take into account more the camber of the specific shape of the periphery 11.1, in a better way than the area of ​​said section 11 or the chord of its profile.

[0111] Determination of the maximum thickness max is a function of the geometric parameter z, the e maxis also a function of additional parameters, following two embodiments:

[0112] The first embodiment comprising the determination of the e max as a function of the geometric parameterzet by at least one of the following orbital friction welding parameters: eccentricity (corresponding to the eccentricity of the orbital oscillation movement during welding); frequency (oscillation speed); and forging pressure (the force applied to the section during a final forging phase following the cessation of the oscillation movement). Advantageously, the welding parameters may be predefined as input setpoints on a welding machine prior to the execution of said weld and / or may be measured during welding.

[0113] The second embodiment comprising the determination of the e maxas a function of the geometric parameterzet by the material consumption rate during orbital friction welding. Said material consumption rate (which can be expressed in mm / s) is determined either empirically, for example, following an actual measurement during a parameter orbital friction welding carried out with the same parameters as the orbital friction welding of the blades of the bladed disc, ie use of the same junction sections 11 modeled similarly to section 11 of thefor example on test specimens, or analytically by an estimation of said consumption rate as a function of the following orbital friction welding parameters: eccentricity, frequency, and forging pressure.

[0114] The estimate of the e maxaccording to the first and / or second embodiment using the welding parameters (eccentricity, frequency, and forging pressure), can be carried out by means of artificial intelligence.

[0115] Determination of the maximum thickness max . depending on the geometric parameter z allows us to establish that: the larger the parameter z, the greater the e max determined is great.

[0116] Schematically represents a perspective view, during orbital friction welding, of the blade 4 to the stub 6 of the disc 2, by means of the joining section 11 illustrated in figures 4 to 6.

[0117] The determination, from the design of the disc 2, of the welding plane 10.1 makes it possible to dimension the blade 4 and the stub 6 so as to ensure an optimal radial position of the junction 10.

[0118] The manufacturing method of the present invention comprises the application of the oscillation 12 by a welding machine (not shown) comprising a tool for holding the blade 4. In this configuration, a lower end 4.2 of the blade 4 preferably comprises a reinforcement 4.3 which will be machined after the welding together with a volume 6.1 of reinforcement of the stub 6 on the disc 2.

[0119] Advantageously, the orbital oscillation 12 comprises an amplitude which can be controlled by an electric motor allowing very rapid oscillation while minimizing energy losses, and also ensuring self-centering of the oscillation 12 at the end of welding.

[0120] In addition, the orbital welding of the blade 4 makes it possible to ensure, at the right of the junction sections, a permanent relative movement of the blade 4 with the stub 6 which makes it possible to obtain greater homogeneity of temperatures and better expulsion of the material. In this configuration, the orbital friction welding process of the invention will generate lower stress gradients thanks to better thermal heterogeneity, and ultimately a lower deformation throughout the manufacturing range.

[0121] Preferably, the junction section S of each of the blades 4 and stub 6 comprises a total surface area greater than or equal to 200 mm 2 and less than or equal to 7000 mm 2 , and more preferably between 2000 mm 2 and 3000 mm 2 .

[0122] Illustrates a mapping of the amplitude of the average rays isweeping the junction section 11 at any point i of its periphery 11.1.

[0123] The scale visible to the right of the corresponds to the mapping of the evolution of the value of z i , this being normalized to 1, i.e. the maximum value of z i of section 11 is equal to 1.

[0124] It can be seen that the points i of the periphery 11.1 at the ends 11.2 and 11.3 of the section 11 have the averagesz i rays i,α launched from the said points which are the weakest compared to the averages i of rays i,α launched from points which are positioned between ends 11.2, 11.3.

[0125] Advantageously, the geometric parameter z (the total mean z of all the means z i rays i,αlaunched from the pointsi) is able to take into account specific details of the shape of the section, such as its camber, unlike a simple measurement of the area or other methods of the prior art which are not able to take them into account. These details of the shape of the junction section 11 that the geometric parameterzis able to intrinsically take into account, make it possible to arrive with greater precision at a determination of the maximum thickness max , then to the determination of the radial height of the welded joint.

[0126] It should be noted that the prior art does not propose any solution for estimating the e max of the welded joint, and no document discloses a correlation between the e max and the shape of the section.

[0127] In general, it is important to note that a configuration where two sections to be welded have a perfect circle shape allows for optimal orbital welding. This configuration ensures perfectly homogeneous and constant mixing, which guarantees a stable temperature rise of the materials. In addition, the circular shape of the sections allows for uniformity of friction over 360°, without any change in shape.

[0128] The inventors took the inventive step of introducing the ray tracing method described above, an unconventional technique in the field of mechanics, to characterize the junction section in order to take into account all directions of friction. Indeed, scanning the section with rays i,αlaunched from each of all points on its periphery, is similar to the movements of mixing material between the surfaces in contact during orbital welding, said movements being in all directions and over 360°.

[0129] This correlation between the mixing physics during orbital friction and the theoretical calculation of the z parameter offers the possibility of predicting the material mixing behavior even before orbital welding is carried out. Thus, the z parameter allows for considerably more accurate estimation of the parameters after welding (e max and radial height) at an early stage of the process (when modeling the shape of the joint section and before welding is carried out).

[0130] Indeed, Figures 9 and 10A-C clearly illustrate the precision of determining the final radial height of the welded joint, in that the e max(from which the height depends) estimated for the junction section 11 is very close to the e max actual measured after orbital welding.

[0131] Illustrates the joint section 11 of the showing three marks for measuring the thickness of the welded joint 11, with two of these joint sections 11 identical. Each mark defines the total local width of the section, following the corresponding direction illustrated in dotted lines.

[0132] Figures 10A to 10C represent graphs showing the normalized evolution of the thickness of the joint of section 11 of the, measured on the welds made and estimated numerically using the parameter z.

[0133] This is a first graph representing the evolution of the estimated thickness of the welded joint (see plot S) compared to points P of actual measurements of said thickness, at the right of the first mark positioned at 1 / 4 of a total extent (along the profile chord) of section 11 visible at.

[0134] This is a second graph representing the evolution of the estimated thickness of the welded joint (see plot S) compared to points P of actual measurements of said thickness, at the right of the second mark positioned at 1 / 2 of the total extent of section 11 visible at.

[0135] This is a third graph representing the evolution of the estimated thickness of the welded joint (see plot S) compared to points P of actual measurements of said thickness, at the right of the third mark positioned at 3 / 4 of the total extent of section 11 visible at.

[0136] With reference to Figures 10A to 10C, the S plots are preferentially obtained by simulation provided by an artificial intelligence basing the determination of the e max as a function of the parameter z according to the present invention.

[0137] The welds were made on the same machine and with constant welding parameters, i.e. eccentricity, oscillation frequency, forging speed and pressure which remain unchanged, only the shape of the sections which is modified.

[0138] As an indication, the maximum measured thickness of the welded joint from two sections 11 is equal to 0.97 mm, for a parameter z equal to 25 mm.

[0139] It was determined that an increase in the value of the parameter z (by modifying the profile of the junction section during modeling) is correlated with an increase in the e max , and similarly, the evolution of the e maxis also correlated to that of the radial height h.

[0140] It can be observed from the graphs that for each of the three measurement benchmarks, the difference (the margin of error) between the simulation (carried out upstream of the orbital welding) and the measurement of the e max carried out after the welding operation, is very minimal, which proves that the present invention makes it possible to ensure a precise determination of the height of the weld, so as to simulate orbital welding which is the most accurate and closest to reality.

[0141] A general bathtub shape of the S-traces can also be observed, this is due to the fact that at the peripheral ends of the welded joint, the thickness is wider than in the center, this is due to a concentration of the excess material displaced during orbital welding, giving a generally diabolo or straw shape to the welded joint (as visible in the).

Claims

Method for manufacturing a bladed disc (2) comprising blades (4) joined by orbital friction welding to stubs (6) on the disc (2) and extending radially outwardly, said method comprising a step of determining the radial junction height between the blades (4) and the stubs (6), characterized in that the radial junction height is determined as a function of a maximum thickness of the weld max , said radial junction height being all the greater as the maximum thickness of the weld max is large, said maximum thickness of the weld max being determined by a geometric parameter z of the section (11) of the blades (4) and the stubs (6) at the junction (10), where z is an average of the mean radii z i scanning said section (11) at any point on the periphery (11.1) of said section (11), the maximum thickness of the weld maxdetermined being all the smaller as the geometric parameter is small. A manufacturing method according to claim 1, wherein the maximum thickness of the weld max is also determined by at least one of the following orbital friction welding parameters: eccentricity; frequency; and forging pressure. A manufacturing method according to claim 1, wherein the maximum thickness of the weld max is also determined by a material consumption rate during orbital friction welding. Manufacturing method according to claim 3, wherein the material consumption rate is measured during a parameterization orbital friction welding carried out with the same parameters as the orbital friction welding of the blades (4). The manufacturing method of claim 3, wherein the material consumption rate is determined based on the following orbital friction welding parameters: eccentricity; frequency; and forging pressure. Manufacturing method according to one of claims 1 to 5, in which the radial junction height h, measured from an inter-blade surface (8) of the disc (2), is greater than or equal to a radial height h SC of a critical threshold (SC), increased by half of a tolerance interval IT determined according to the maximum thickness of the weld max . Manufacturing method according to claim 6, in which the tolerance interval IT is greater than or equal to the maximum thickness of the weld. max. Manufacturing method according to one of claims 6 and 7, in which the tolerance interval IT is determined as a function of an obliqueness tolerance of the junction (10) relative to the inter-blade surface (8) of the disc (2). A bladed disc (2) for a turbomachine, comprising a plurality of blades (4) joined by orbital friction welding to stubs (6) on the disc (2), at a radial junction heighth between the blades (4) and the stubs (6), characterized in that the radial junction heighth, measured from an inter-blade surface (8) of the disc (2), is greater than or equal to a radial heighth SC of a critical threshold (SC), increased by half of a maximum thickness of the weld max . Bladed disc (2) according to claim 9, wherein said bladed disc (2) corresponds to a moving wheel intended to be arranged upstream of a flow separation nozzle in an axial turbomachine.

Citation Information

Patent Citations

  • Method of linear friction welding of blades to aerofoil blisks and blade having a root with a taper ratio less than 2

    EP1495829A1

  • Method for friction soldering blades to an axial compressor drum, and corresponding device

    EP2535516A1

  • Linear friction welded blisk and method of fabrication

    US20090185908A1

  • Weld stub arrangement and a method of using the arrangement to make an article

    US20180243857A1

  • Tool for simultaneous local stress relief of each of a multiple of linear friction welds of a rotor forging

    US20210180605A1