Method for coating a substrate with tetragonal vanadium nitride

The high-power pulsed magnetron sputtering process stabilizes tetragonal vanadium nitride at room temperature, providing a compatible and effective alternative to hard chrome coatings with equivalent resistance properties, addressing the need for a REACH-compliant, industrially viable solution.

WO2024218450A1PCT designated stage expired Publication Date: 2024-10-24SAFRAN SA +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/FR2024/050500
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing hard chrome coating, widely used for its physical, chemical, and wear resistance properties, is carcinogenic and incompatible with the REACH directive, necessitating a stable, economically viable, and industrially interesting alternative that matches its performance at room temperature.

Method used

A process using high-power pulsed magnetron cathode sputtering to deposit tetragonal vanadium nitride on substrates at controlled pressures and temperatures, with a specific polarization regime, stabilizing the metastable tetragonal phase of vanadium nitride at room temperature, which has never been achieved before.

Benefits of technology

The process produces dense, homogeneous, and defect-free tetragonal vanadium nitride coatings with equivalent or superior resistance properties to hard chrome, compatible with the REACH directive, and is industrially viable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FR2024050500_24102024_PF_FP_ABST
    Figure FR2024050500_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for coating a substrate with tetragonal vanadium nitride by means of high-power pulsed magnetron sputtering. It also relates to a substrate coated with at least one layer of tetragonal vanadium nitride. The method of the invention is particularly useful in the field of electronic components, of transducers for sensors, of optics, mechanics and micromechanics, of decorating and protecting surfaces, of motor vehicles, of aeronautics or of aerospace.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] DESCRIPTION

[0002] TITLE: METHOD FOR COATING A SUBSTRATE WITH TETRAGONAL VANADIUM NITRIDE

[0003] Technical field of the invention

[0004] The present invention relates to the general field of producing thin layers and more particularly to the metallization of various substrates. It relates more particularly to a method of coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique and to a substrate coated with at least one layer of tetragonal vanadium nitride. The method and the substrate of the invention are of particular interest in the field of electronic components, transducers for sensors, optics, photonics, mechanics and micromechanics, decoration and protection of surfaces, automobiles, aeronautics and aerospace.

[0005] Technical background

[0006] To improve the properties of metallic, composite, polymer or other materials, particularly in terms of corrosion and / or wear resistance, the substrates are covered with a protective layer. The coating commonly called hard chrome has numerous physical, chemical and wear resistance properties in various environments, which make it one of the most widely used versatile coatings and whose applications are found in different industrial sectors (machining, land, air or space transport). Hard chrome is obtained by electrolytic chromium deposition involving the presence of hexavalent chromium (Cr 6+). However, the latter has carcinogenic, mutagenic and reprotoxic (CMR) properties, which are incompatible with the REACH directive (a European Union regulation adopted to better protect human health and the environment against the risks associated with chemical substances, while promoting the competitiveness of the EU chemical industry). However, hard chromium has versatile properties that are difficult to match with a single universal solution. The family of transition metal nitrides has different structural and functional properties that can, for certain applications, position them as an alternative solution to the use of hard chromium. The ban by the REACH directive on the use of hexavalent chromium (Cr 6+) present during the production of electrolytic chromium or hard chromium deposits led the inventors of the present invention to study transition metal nitrides, including vanadium nitride, in order to approach the structural and functional properties of hard chromium. Vanadium nitride was therefore explored and its tribological properties studied. Hardness, electrical resistivity, thermal conduction, etc. are all interesting properties to develop, in line with the field concerned.

[0007] Vanadium nitrides have already been studied by researchers. Different crystallographic phases of vanadium nitride are predicted by ab initio calculations.

[0008] In 1988, F. Kubel et al., Physical Review B, 1988, vol. 38, no. 18, 12908- 12912, obtained the tetragonal phase of vanadium nitride at a transition temperature of 205 K (-68°C). This metastable phase was not stabilized at temperatures above 205 K (-68°C). In addition, the material was not in the form of a coating but in the form of a powder. The study of metastable phases of vanadium nitride not present on the binary VN phase diagram regardless of the temperature (> 0°C) and the nitrogen stoichiometry, was carried out from ab initio calculations with the aim of understanding the stabilization of these phases

[0009] Vanadium nitrides have also been studied as hardening reinforcements for steels.

[0010] AB Mei et al. (Physical Review B, vol. 91 , no. 5, 054101 ) have grown cubic-phase vanadium nitride thin films by direct current magnetron sputtering (dcMS). The authors also sought to study, by ab initio molecular dynamics calculations, the transition from cubic to tetragonal phase occurring at 205 K in order to correlate them with analyses carried out at temperatures below 205 K by X-ray diffraction and transmission electron microscopy.

[0011] There is therefore a real need for an alternative coating to hard chrome with at least equivalent physical, chemical and wear resistance properties.

[0012] In particular, there is a real need for an alternative coating to hard chrome with at least equivalent physical, chemical and wear resistance properties, and which is stable at room temperature (20 ± 5°C).

[0013] More specifically, there is a real need for an alternative coating to hard chrome as described above that is compatible with the REACH directive and whose implementation is simple, effective and economical and therefore industrially interesting.

[0014] Summary of the invention

[0015] The present invention relates to a method for coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated, the coating process taking place

[0016] - at a pressure between 0.1 and 20 Pa, and

[0017] - at a temperature between room temperature (20 ± 5°C) and 900°C, and

[0018] - under an atmosphere containing a mixture of nitrogen and argon with a nitrogen content of between 5 and 99%, the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) greater than 0 and less than or equal to -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100 V. The polarization of the target can be maintained for a duration of between 10 and 900 ps.

[0019] Target polarization can be performed at a frequency between 100 and 9000 Hz.

[0020] The device for carrying out deposition by high-power pulsed magnetron sputtering comprising a deposition chamber or enclosure illustrated in [Fig. 1] and described in detail in application FR 3 097 237, is entirely suitable for implementing the method of the invention.

[0021] As already indicated, the tetragonal crystallographic phase of vanadium nitride was predicted by calculations as a metastable phase, but could never be stabilized or observed at room temperature (20 ± 5°C). However, the inventors succeeded in obtaining and stabilizing the tetragonal crystallographic phase of vanadium nitride at room temperature (20 ± 5°C) and in characterizing it, thanks to the use and control of the parameters of a high-power pulsed magnetron sputtering (HiPIMS) process, which has never been done to date.

[0022] In the high-power pulsed magnetron sputtering (HiPIMS) technique, the target is polarized in a special way to form a tetragonal vanadium nitride coating, which is a material with satisfactory physical, chemical and wear resistance properties in various environments, for the replacement of hard chrome.

[0023] The invention also relates to a substrate coated with at least one thin layer of tetragonal vanadium nitride.

[0024] Indeed, the method of the invention can make it possible to coat the substrate with one or more thin layer(s) of tetragonal vanadium nitride depending on the operating conditions chosen.

[0025] When the substrate is coated with several layers, these layers can be optionally detected according to their microstructure. In HiPIMS, the layers will be dense and the distinction between two layers can be made, for example, by scanning electron microscopy (SEM). It is also possible to coat the substrate with one or more thin layers of tetragonal vanadium nitride and / or one or more layers of different materials and / or vanadium nitride of different phases.

[0026] The high-power pulsed magnetron sputtering (HiPIMS) technology implemented by the method of the invention makes it possible to develop dense, homogeneous and defect-free coatings, whose microstructure and chemical composition are perfectly controlled. The method of the invention adds new modifiable parameters such as pulse intensity and duration, frequency, etc. to those usually optimized for magnetron sputtering deposition, which has allowed the stabilization of new metastable crystalline phases.

[0027] Thus, the method of the invention is particularly interesting because it allows the stabilization at room temperature (20 ± 5°C) of the tetragonal vanadium nitride phase thanks to the use of high-power pulsed magnetron sputtering (HiPIMS). This phase, not predicted in the phase diagram and observed only once experimentally in powder during a low-temperature phase change (205 K) of the cubic phase, has never been able to be characterized at room temperature (20 ± 5°C).

[0028] Brief description of the figures

[0029] Other characteristics and advantages of the invention will appear during reading of the detailed description which follows and the appended figures.

[0030] [Fig.1] schematically represents a deposition chamber in which a process for coating a substrate with tetragonal vanadium nitride is carried out using the high-power pulsed magnetron sputtering technique according to one embodiment of the invention.

[0031] [Fig.2] represents a PANalytical X'Pert Pro X-ray diffractogram of 316L stainless steel substrates measuring 2.5 cm x 2.5 cm and 500 μm thick, coated with a layer of tetragonal vanadium nitride according to the method of the invention. Starting from the bottom, the first diffractogram is that of the bare substrate, i.e. the part on which the coating is deposited. The two diffractograms in the middle and at the top are the diffractograms of two tetragonal VN deposits carried out one month apart. By comparing the peaks and diffraction angles, we observe the reproducibility of the method of the invention.

[0032] X-rays penetrate the sample (i.e. substrate + coating) with a depth greater than that of the coating. Therefore, on the sample diffractogram (the middle and top diffractograms), we observe peaks corresponding to the coating and peaks corresponding to the substrate. The diffractogram of the uncoated metal substrate allows us to recognize the substrate peaks and the coating peaks on the sample diffractogram.

[0033] Detailed description of the invention

[0034] The present invention relates to a method for coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated, the coating process taking place

[0035] - at a pressure between 0.1 and 20 Pa, and

[0036] - at a temperature between room temperature (20 ± 5°C) and 900°C, and

[0037] - under an atmosphere containing a mixture of nitrogen and argon with a nitrogen content of between 5 and 99%, the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) greater than 0 and less than or equal to -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100V. In the context of the present invention, the expression "massive vanadium target" designates a vanadium target whose purity is at least 99.5% by mass of vanadium. The polarization of the target can be carried out at a frequency of between 100 and 9000 Hz.

[0038] According to one embodiment, the coating process takes place at a pressure of 1 Pa.

[0039] Although an atmosphere containing a mixture of nitrogen and argon as described above is preferred, it may be envisaged to carry out the coating method of the invention under a nitrogen atmosphere mixed with other plasma-forming gases known to those skilled in the art. In the context of the invention, the expression "between ... and ..." should be understood as including the limits.

[0040] In the context of the invention, the expression "greater than... or less than..." should be understood as not including the limits.

[0041] The coating is in the form of a thin layer.

[0042] The thin layer is produced in a low-pressure deposition chamber, with a basic vacuum of less than 10' 4 mbar, preferably less than 10' 6mbar. Vanadium is present in the deposition chamber in the form of a massive vanadium target, facing which is the substrate to be coated. The target constitutes the cathode. The substrate to be coated constitutes an anode.

[0043] The substrate is maintained at a temperature between room temperature (20 ± 5°C) and 900°C throughout the deposition period.

[0044] During deposition, a mixture of plasma gases as described above is introduced into the deposition chamber. The target is in contact with a cooled cathode coupled to permanent magnets while the substrate is connected to ground or possibly positively polarized or left at floating potential. A potential difference is imposed between the two electrodes, making it possible to reach the breakdown voltage of the gas or gas mixture to initiate a low-pressure plasma, i.e. a pressure between 1.10 -4 at 1 mbar, especially between 10' 3and 5.10-1 mbar during deposition.

[0045] In addition to the continuous electric field (from 0 to -900V, greater than 0 and less than or equal to -900V according to one embodiment, or from -100 to -600V according to another embodiment), the generator transmits a high voltage pulsed current. The voltages used are between -1200 and -100V or -1000 and -500V according to another embodiment. The voltage peaks are maintained for durations between 10 and 900 ps or between 50 and 400 ps according to another embodiment, and frequencies of 100 and 9000 Hz or from 100 to 5000 Hz according to another embodiment. As indicated previously, the coating process takes place under an atmosphere containing nitrogen mixed with argon, with a nitrogen content between 5 and 99%.

[0046] The thickness of each layer of coating / tetragonal vanadium nitride deposited on the substrate can be between 5 nm and 15 pm. When the coating is in the form of a multi-layer, the thickness of the multi-layer can be between 10 nm and 100 pm, for example. The diffractograms of 316L stainless steel substrates with dimensions of 2.5 cm x 2.5 cm and thickness of 500 μm, coated with a layer of stabilized tetragonal vanadium nitride and obtained by the process of the invention, carried out using a PANalytical X'Pert Pro X-ray diffractometer, clearly show the characteristic peaks of tetragonal vanadium nitride as shown in [Fig.2], thus confirming that the parameters of the process of the invention described above allow the obtaining of a coating of 1 μm thickness by the process of the invention based on the use of HiPIMS technology to stabilize the tetragonal phase of vanadium nitride.

[0047] The invention also relates to a substrate coated with at least one thin layer of tetragonal vanadium nitride.

[0048] The method of the invention applies to the coating of a wide variety of substrates depending on the intended application, provided that they can withstand a temperature of 40°C.

[0049] The substrate can be metallic, ceramic, composite, elastomer, glass, metallic glass, plastic, fabric.

[0050] In one embodiment, the substrate is a stainless steel, such as 316L stainless steel.

[0051] In one embodiment, the substrate is an aircraft part such as an aircraft landing gear part or an aircraft engine turbine part. In one embodiment, the substrate is a gas turbine part or a marine turbine part.

[0052] The method of the invention is of particular interest in the field of electronic components, transducers for sensors, optics, photonics (i.e. lasers, light-emitting diodes, optical fibers, optical modulators, optical amplifiers or even photonic crystals, lenses, prisms, and networks), mechanics and micromechanics, decoration and protection of surfaces, automobiles, aeronautics or even aerospace.

[0053] Another object of the invention is therefore the use of the method of the invention for the manufacture of electronic components, transducers for sensors, optical and photonic components, mechanical and micromechanical components, components for the decoration and protection of surfaces, components for the automobile, aeronautics or even aerospace industries.

[0054] EXAMPLES

[0055] The coating is deposited on 316L stainless steel substrates. The substrate is pre-cleaned by immersion in a beaker of boiling isopropanol. The base vacuum of the chamber reached before deposition is 3.0E-6 T. The plasma is initiated at 5 Pa in an Argon / Dinitrogen mixture. The imposed voltage and current are -1000 V and 200 mA respectively, with a continuous background of -50 V and 10 mA. The frequency and width of the high-power pulse (HiPIMS) are 100 Hz and 200 ps respectively. The pressure is then decreased to 1 Pa. The chamber is preheated to 400 °C under an Ar / N2 mixture at 1 Pa, 40 sccm of Argon, 5 sccm of Dinitrogen. The Ar / N2 mixture can be described by the percentage of N2 in the total gas volume [Ar+lxh]. It is 5 / (40+5) = 11%. The ratio can, however, be a good way to describe the process (N2 ratio = N2 flow rate / Ar flow rate). The Nitrogen ratio is 12.5.The plasma is stabilized at this point of the process for 15 minutes and then the substrate is brought in front of the Vanadium target (purity greater than or equal to 99.9%). The deposition time is 3 hours. The coating thickness was determined by Scanning Electron Microscopy (SEM JEOL 6360 A) and the crystal structure was determined by X-ray Diffraction (DRX PANalytical X'Pert Pro).

Claims

CLAIMS 1. Method for coating a substrate with tetragonal vanadium nitride using the high-power pulsed magnetron sputtering technique, characterized in that the coating of the substrate is carried out in a deposition chamber in which the vanadium is in the form of a massive vanadium target, facing which is the substrate to be coated, the coating process taking place - at a pressure between 0.1 and 20 Pa, and - at a temperature between room temperature (20 ± 5°C) and 900°C, and - under an atmosphere containing a mixture of nitrogen and argon with a nitrogen content of between 5 and 99%, the polarization of the target being controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) greater than 0 and less than or equal to -900V and a pulsed polarization whose pulses have a potential (Vp) between -1200 and -100 V.

2. Method according to claim 1, characterized in that it takes place at a pressure of 1 Pa.

3. Method according to one of claims 1 or 2, characterized in that the polarization of the target is carried out at a frequency between 100 and 9000 Hz.

4. Method according to any one of claims 1 to 3, characterized in that the polarization of the target is controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) between -100 and -600V.

5. Method according to any one of claims 1 to 4, characterized in that the polarization of the target is controlled during the deposition of the coating by imposing on it a superposition of a continuous polarization at a potential (Vc) as described in claims 1 and 4, and of a pulsed polarization whose pulses have a potential (Vp) between -1000 and -500 V.

6. Method according to any one of claims 1 to 5, characterized in that the substrate is coated with one or more thin layer(s) of tetragonal vanadium nitride, the thickness of each layer being between 5 nm and 15 pm.

7. Method according to claim 6, characterized in that when the coating is in the form of a multi-layer, the thickness of the multi-layer is between 10 and 100 μm.

8. Method according to any one of claims 1 to 7, characterized in that the vanadium is in the form of a massive vanadium target whose purity is at least 99.5% by mass of vanadium.

9. Use of the method according to any one of claims 1 to 8, for the manufacture of electronic components, transducers for sensors, optical components, mechanical and micromechanical components, components for decoration and for the protection of surfaces, components for the automobile, aeronautics or even aerospace industries.

10. Substrate coated with at least one thin layer of tetragonal vanadium nitride by a method according to any one of claims 1 to 8.

11. Substrate according to claim 10, characterized in that it is - a part of an aircraft landing gear, or - an aircraft engine turbine part, or - a part of gas turbines or marine industry turbines.

Citation Information

Patent Citations

  • Sputter device

    EP2325349A1

  • METHOD FOR COATING A SUBSTRATE WITH TANTALUM NITRIDE

    FR3097237A1