Cu-ag-sn alloy wire rod material and method for producing same, and probe pin obtained using cu-ag-sn alloy wire rod material for inspecting electrical / electronic component
The Cu-Ag-Sn alloy wire, with a specific composition and manufacturing process, addresses the balance of low resistance and high hardness, improving casting workability and reducing costs, making it suitable for probe pins in electronic component inspection.
Patent Information
- Application Number
- PCT/JP2024/000920
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-24
AI Technical Summary
Existing metal wires for probe pins in electronic component inspection lack a balance of low electrical resistance and high hardness, with insufficient casting processability and high manufacturing costs, particularly for achieving diameters of 110 μm or less.
A Cu-Ag-Sn alloy wire with 6 wt% to 10 wt% Ag, 0.1 wt% to 0.9 wt% Sn, and the remainder Cu, with a manufacturing method involving vacuum melting, solution treatment, cold working, and aging treatment to achieve a specific resistance of 5 μΩ·cm or less and Vickers hardness of 300 HV to 360 HV, while minimizing impurities and optimizing casting workability.
The Cu-Ag-Sn alloy wire achieves a well-balanced low electrical resistance and high hardness, excellent casting processability, and stable product quality, reducing manufacturing costs and enabling reliable probe pins for electronic components with narrow-pitch electrodes.
Smart Images

Figure JP2024000920_24102024_PF_FP_ABST
Abstract
Description
Cu-Ag-Sn alloy wire and its manufacturing method, and probe pin for inspecting electrical and electronic components obtained using Cu-Ag-Sn alloy wire
[0001] The present invention relates to a Cu-Ag-Sn alloy wire and its manufacturing method, and a probe pin for inspecting electric / electronic components obtained by using the Cu-Ag-Sn alloy wire.
[0002] Probe cards and contact probes have been known as probes for testing electrical and electronic components, such as semiconductor integrated circuits and semiconductor packages, that have narrow-pitch electrodes. These electrical and electronic component testing probes use multiple probe pins made of metal wires (also referred to as thin metal wires or thin alloy wires) with extremely small diameters. The metal wires for these probe pins are required to have a good balance of low electrical resistance and high hardness. Furthermore, extremely small-diameter metal wires that possess these characteristics are also in high demand as conductor materials for electrical wires and cables used in electronic devices, such as mobile devices and industrial robots, and medical devices.
[0003] Patent Document 1 discloses an invention relating to a Cu—Ag alloy thin wire that combines high electrical conductivity and high strength. The Cu—Ag alloy thin wire of Patent Document 1 is characterized in that "it is a Cu—Ag alloy thin wire having an Ag content of 1 to 10 wt % with the remainder being Cu and unavoidable impurities, and the entire structure of the Cu solid solution is composed of a recrystallized texture" (see claim 1 of Patent Document 1).
[0004] Furthermore, Patent Document 2 discloses "an alloy material containing 10 to 30 wt% of silver (Ag), 0.5 to 10 wt% of nickel (Ni), 0.01 to 0.1 wt% of iridium (Ir), 5 to 20 wt% of palladium (Pd), 0.5 to 5 wt% of tin (Sn), 0 to 0.09 wt% of ruthenium (Ru) in combination with Ir, with the upper limit being 0.1 wt%, and the balance being copper (Cu) and inevitable impurities" (see claim 1 of Patent Document 2).
[0005] Patent No. 5051647 Patent No. 6728057
[0006] However, the invention described in Patent Document 1 had insufficient castability when attempting to stably obtain metal wire rods with extremely small diameters, for example, 110 μm or less, and did not satisfy the "stable product quality" required industrially. Furthermore, the invention described in Patent Document 2 required the inclusion of five or more metals as components to obtain an alloy material with a hardness of 300 HV or more, which is necessary for use as a probe pin for inspecting electrical and electronic components, resulting in relatively high manufacturing costs (see Table 1 in Patent Document 2). Therefore, there is a market demand for a metal wire rod and a manufacturing method thereof that has a good balance of low electrical resistance and high hardness, excellent castability, stable product quality, and reduced manufacturing costs.
[0007] As a result of extensive research, the inventors of the present application have achieved the above-mentioned object by adopting the following means.
[0008] A. Cu—Ag—Sn Alloy Wire The Cu—Ag—Sn alloy wire according to the present application is characterized by containing 6 wt % to 10 wt % of Ag, 0.1 wt % to 0.9 wt % of Sn, and the balance consisting of Cu and inevitable impurities.
[0009] The Cu-Ag-Sn alloy wire according to the present application preferably has a total content of unavoidable impurities of 0.02 wt % or less.
[0010] The Cu-Ag-Sn alloy wire according to the present application preferably has a resistivity of 5 μΩ·cm or less and a Vickers hardness of 300 HV to 360 HV.
[0011] The Cu-Ag-Sn alloy wire according to the present application preferably has a diameter of 110 μm or less.
[0012] B. Probe Pin for Inspecting Electrical and Electronic Components The probe pin for inspecting electrical and electronic components according to the present application is characterized by being obtained using the Cu—Ag—Sn alloy wire according to the present application described above.
[0013] C. Manufacturing Method of Cu—Ag—Sn Alloy Wire The manufacturing method of Cu—Ag—Sn alloy wire according to the present application is the manufacturing method of Cu—Ag—Sn alloy wire according to the present application described above, and is characterized by comprising the following steps 1 to 4. Step 1: Metal raw materials are blended to have a composition of 6 wt % to 10 wt % Ag, 0.1 wt % to 0.9 wt % Sn, and the remainder Cu and unavoidable impurities, and the blended metal raw materials are melted in a vacuum or in an inert gas to obtain an ingot. Step 2: The ingot is solution-treated in an inert gas or a slightly reducing gas to obtain a solution-treated ingot. Step 3: The solution-treated ingot is cold-worked to a cross-sectional area reduction rate of 25% or more, and then aging-treated in an inert gas or a slightly reducing gas to obtain an aged ingot. Step 4: The aged ingot is further cold worked so that the cross-sectional area reduction rate is 99.95% or more, to obtain a Cu—Ag—Sn alloy wire.
[0014] In the method for producing a Cu—Ag—Sn alloy wire according to the present application, it is preferable that the total content of unavoidable impurities in the ingot in step 1 is 0.02 wt % or less.
[0015] According to the present invention, it is possible to provide a Cu-Ag-Sn alloy wire rod and a method for manufacturing the same, which have a good balance of low electrical resistance and high hardness, excellent castability, stable product quality, and reduced manufacturing costs. Also, according to the present invention, it is possible to provide a probe pin for inspecting electrical and electronic components, which has market value and high reliability and is capable of inspecting semiconductor integrated circuits, semiconductor packages, etc., which have narrow-pitch electrodes.
[0016] 1 is a graph showing the relationship between the working degree η of the aged ingot according to the present application and the Vickers hardness of the Cu—Ag—Sn alloy wire.
[0017] A. Cu-Ag-Sn alloy wire The Cu-Ag-Sn alloy wire according to the present application is characterized by containing 6 wt% to 10 wt% Ag, 0.1 wt% to 0.9 wt% Sn, and the remainder consisting of Cu and inevitable impurities. By having this composition, the Cu-Ag-Sn alloy wire according to the present application has a good balance of low electrical resistance and high hardness, excellent castability, stable product quality, and reduced manufacturing costs.
[0018] The main component of the Cu-Ag-Sn alloy wire according to the present application is copper (Cu). Although copper has low electrical resistance, its hardness is relatively low, and it alone cannot form a durable alloy wire. Therefore, a predetermined amount of silver (Ag) is added as an ingredient, and heat treatment (solution treatment and aging treatment) is performed together with the copper to produce a high-hardness alloy wire due to the precipitation hardening of the silver. The preferred silver content in the Cu-Ag-Sn alloy wire according to the present application is 6 wt% to 10 wt%. Here, if the silver content in this Cu-Ag-Sn alloy wire is less than 6 wt%, the effect of improving hardness due to the precipitation hardening of silver tends to be insufficient, which is undesirable. On the other hand, if the silver content in this Cu-Ag-Sn alloy wire exceeds 10 wt%, the hardness does not improve dramatically, and raw material costs tend to increase, worsening the cost balance of the product, which is undesirable.
[0019] Furthermore, the Cu—Ag—Sn alloy wire of the present application contains 0.1 wt% to 0.9 wt% tin (Sn). Adding a predetermined amount of tin as an ingredient during the production of the alloy wire lowers the melting point of the alloy used as the casting raw material and improves the flow of the molten metal. This significantly improves casting workability and stabilizes the quality of the cast ingot, resulting in extremely stable product quality for the resulting alloy wire. Here, a tin content of less than 0.1 wt% in the Cu—Ag—Sn alloy wire is undesirable because it tends to fail to achieve the effect of stabilizing the product quality of the alloy wire through improved casting workability. On the other hand, a tin content of more than 0.9 wt% in the Cu—Ag—Sn alloy wire is undesirable because it tends to reduce plastic workability and make it difficult to reproducibly obtain alloy wires with stable product quality.
[0020] Here, examples of unavoidable impurities that may be contained in this Cu—Ag—Sn alloy wire include various elements such as Si, Fe, Pt, Au, Bi, Ca, In, Ir, Mg, Mn, and Sb. However, the Cu—Ag—Sn alloy wire according to the present application preferably has a total content of unavoidable impurities of 0.02 wt% or less. This is because if the total content of unavoidable impurities in the Cu—Ag—Sn alloy wire exceeds 0.02 wt%, the unavoidable impurities tend to adversely affect the properties of the Cu—Ag—Sn alloy wire, such as increasing the specific resistance (also referred to as specific resistance or volume resistivity). The content of the constituent elements of the Cu—Ag—Sn alloy wire according to the present application can be measured using conventionally known methods, and there are no particular limitations. Therefore, for example, an ICP (inductively coupled plasma) optical emission spectrometer or an XRF (X-ray fluorescence) analyzer may be used for this measurement. Alternatively, a simple analysis method such as EDX (energy dispersive X-ray) spectroscopy or WDX (wavelength dispersive X-ray) spectroscopy may be used.
[0021] The Cu—Ag—Sn alloy wire according to the present application preferably has a resistivity of 5 μΩ·cm or less and a Vickers hardness of 300 HV to 360 HV. If the resistivity of the Cu—Ag—Sn alloy wire exceeds 5 μΩ·cm, the electrical resistance of the alloy wire becomes too high, which tends to severely limit its applications, which is undesirable. More specifically, if the resistivity of the Cu—Ag—Sn alloy wire exceeds 5 μΩ·cm, when used as a probe pin, for example, it tends to be difficult to accurately detect minute currents in an electrical circuit formed on a substrate material. On the other hand, while there is no particular limit on the lower limit of the resistivity of the Cu—Ag—Sn alloy wire, it is preferable that the resistivity of the Cu—Ag—Sn alloy wire be 2 μΩ·cm or more. Even if the resistivity of the Cu—Ag—Sn alloy wire is less than 2 μΩ·cm, this does not significantly improve the added value of the copper-based alloy wire, but simply tends to increase manufacturing costs.
[0022] Furthermore, if the Vickers hardness of the Cu—Ag—Sn alloy wire is less than 300 HV, the durability of the product tends to be insufficient, which is undesirable. More specifically, if the Vickers hardness of the Cu—Ag—Sn alloy wire is less than 300 HV, for example, when it is used as a probe pin to repeatedly perform continuity tests on electrical and electronic components, defects such as bending and bending occur, and the durability and reliability of the product tend to be insufficient. On the other hand, even if the Vickers hardness of the Cu—Ag—Sn alloy wire is more than 360 HV, when it is used as a probe pin for inspecting electrical and electronic components, for example, the surface may be damaged during continuity tests, depending on the type of material constituting the electrical circuit on the substrate material, which is undesirable.
[0023] The Cu—Ag—Sn alloy wire according to the present application preferably has a diameter of 110 μm or less. Here, if the diameter of the Cu—Ag—Sn alloy wire exceeds 110 μm, the diameter of the alloy wire exceeds the inter-electrode distance of narrow-pitch electrodes provided on semiconductor packages, etc., which severely limits its use as a probe pin for inspecting electrical and electronic components, such as a probe card or contact probe, and tends to reduce the added value of the copper-based alloy wire, which is undesirable. Furthermore, the Cu—Ag—Sn alloy wire according to the present application more preferably has a diameter of 30 μm or less. When the diameter of the Cu—Ag—Sn alloy wire is 30 μm or less, inspection accuracy tends to be significantly improved when used as a probe pin for inspecting electrical and electronic components for semiconductor integrated circuits equipped with fine-pitch electrodes having a miniaturized structure. On the other hand, although there is no particular limit on the lower limit of the diameter of the Cu—Ag—Sn alloy wire, the diameter of the Cu—Ag—Sn alloy wire is preferably 20 μm or more. If the diameter of the Cu—Ag—Sn alloy wire is less than 20 μm, the alloy wire becomes too thin, the strength decreases, and the durability as a product tends to be insufficient. More specifically, if the diameter of the Cu—Ag—Sn alloy wire is less than 20 μm, for example, when it is used as a probe pin to repeatedly perform continuity tests on electrical and electronic components, defects such as breaking and bending occur, and the durability and reliability of the product tend to be insufficient.
[0024] B. Probe Pin for Inspecting Electrical and Electronic Components The probe pin for inspecting electrical and electronic components according to the present application is characterized in that it is obtained using the Cu-Ag-Sn alloy wire according to the present application. By satisfying the requirements, the probe pin for inspecting electrical and electronic components according to the present application can be suitably used as a probe pin for inspecting electrical and electronic components such as semiconductor integrated circuits and semiconductor packages that have narrow-pitch electrodes, and therefore has high market value and excellent reliability.
[0025] C. Manufacturing Method of Cu—Ag—Sn Alloy Wire The manufacturing method of Cu—Ag—Sn alloy wire according to the present application is the manufacturing method of Cu—Ag—Sn alloy wire according to the present application described above, and is characterized by comprising the following steps 1 to 4. By satisfying these requirements, the manufacturing method of Cu—Ag—Sn alloy wire according to the present application can manufacture an alloy wire that has a good balance of low electrical resistance and high hardness, excellent castability, stable product quality, and reduced manufacturing costs. The details of each step are explained below.
[0026] Step 1: Metal raw materials are blended to have a composition of 6 wt % to 10 wt % Ag, 0.1 wt % to 0.9 wt % Sn, and the remainder Cu and unavoidable impurities, and melted in a vacuum or in an inert gas to obtain an ingot.
[0027] This step 1 is for forming an ingot (cast metal) that serves as a raw material for obtaining a Cu-Ag-Sn alloy wire having a predetermined composition by casting. The preferred silver (Ag) content in this ingot is 6 wt% to 10 wt%. If the silver content in the ingot is less than 6 wt%, the effect of improving hardness due to precipitation hardening of silver tends to be insufficient, which is undesirable. On the other hand, if the silver content in the ingot exceeds 10 wt%, the hardness of the alloy wire does not improve dramatically, and raw material costs tend to increase, worsening the cost balance of the product, which is undesirable.
[0028] The preferred tin (Sn) content in this ingot is 0.1 wt% to 0.9 wt%. Here, if the tin content in the ingot is less than 0.1 wt%, the effect of improving castability tends not to be obtained, which is undesirable. On the other hand, if the tin content in the ingot exceeds 0.9 wt%, the plastic workability decreases, and the alloy wire tends to be easily broken when cold working to a predetermined cross-sectional area reduction rate in step 4 described below, which is also undesirable. The alloy composition of the ingot used in this casting is essentially the composition of the Cu-Ag-Sn alloy wire.
[0029] Here, examples of unavoidable impurities that may be contained in this ingot include various elements such as Si, Fe, Pt, Au, Bi, Ca, In, Ir, Mg, Mn, and Sb. However, the total content of unavoidable impurities in this ingot is preferably 0.02 wt% or less. If the total content of unavoidable impurities in the ingot exceeds 0.02 wt%, the total content of unavoidable impurities in the Cu-Ag-Sn alloy wire obtained in step 4 will also exceed 0.02 wt%. As a result, the unavoidable impurities tend to adversely affect the properties of the Cu-Ag-Sn alloy wire, such as increasing the resistivity of the Cu-Ag-Sn alloy wire obtained in step 4. Note that the content of the constituent elements of the ingot in step 1 can be measured using conventionally known methods without any particular limitations. Therefore, for example, an ICP (inductively coupled plasma) optical emission spectrometer or an XRF (X-ray fluorescence) analyzer may be used for this measurement. Alternatively, a simple analysis method such as EDX (energy dispersive X-ray) spectroscopy or WDX (wavelength dispersive X-ray) spectroscopy may be used.
[0030] The ingot manufacturing conditions in this step 1 may be conventionally known and are not particularly limited. For example, the melting temperature is 1200 to 1300°C, the vacuum degree is 1×10 3 Pa ~ 1 x 10 -2 The metal raw material may be placed in a heat-resistant container and melted under vacuum at 100 Pa. Alternatively, the metal raw material may be melted by continuous casting in an inert gas such as argon.
[0031] Step 2: The ingot obtained in step 1 is subjected to solution treatment in an inert gas or a slightly reducing gas to obtain a solution-treated ingot.
[0032] This step 2 is intended to dissolve (solid-solve) the silver and tin, which are additives for modification, in their atomic state into the copper (Cu) base material. Conventional known conditions may be used as the solution treatment (heat treatment) conditions. For example, the ingot obtained in step 1 described above may be placed in a heat-resistant container and heat-treated at 700°C to 900°C for approximately 1 to 3 hours in an inert gas atmosphere such as nitrogen or argon, or in a slightly reducing gas atmosphere such as a mixed gas of 95% nitrogen and 5% hydrogen, and then allowed to cool.
[0033] Here, if necessary, it is also preferable to use a shaper to cut and remove (also referred to as shaving) the metal near the surface of the solution-treated ingot obtained in the above-mentioned step 2. By cutting and removing the metal from the solution-treated ingot to a thickness of about 1 mm from the surface, it is possible to remove oxide films formed on the surface and impurities that have entered and become embedded in the vicinity of the surface of the ingot from a heat-resistant container such as a crucible during production due to contact with the crucible, thereby increasing the purity.
[0034] Step 3: The solution-treated ingot obtained in step 2 is cold-worked to a cross-sectional area reduction rate of 25% or more, and then aged in an inert gas or a slightly reducing gas to obtain an aged ingot.
[0035] In step 3, the solution-treated ingot obtained in step 2 is first cold-worked at about room temperature using a grooved rolling mill or the like to a predetermined area reduction (area reduction = (cross-sectional area of Cu-Ag-Sn alloy before cold working - cross-sectional area of Cu-Ag-Sn alloy after cold working) ÷ cross-sectional area of Cu-Ag-Sn alloy before cold working × 100), thereby improving its hardness by work hardening. Here, the area reduction of the cold working in step 3 is preferably 25% or more. If the area reduction of the cold working in step 3 is less than 25%, the effect of improving the hardness of the solution-treated ingot by work hardening tends not to be obtained, which is undesirable. On the other hand, although there is no particular upper limit to the area reduction, the area reduction of the cold working in step 3 is preferably 60% or less. Even if the area reduction rate of the cold working in step 3 exceeds 60%, the hardness of the Cu-Ag-Sn alloy wire rod does not become extremely high, but the working becomes time-consuming and tends to increase the manufacturing cost.
[0036] Next, the ingot cold-worked under the above conditions is subjected to aging (heat treatment), which precipitates the silver and tin dissolved in the copper base material in an atomic state (solid solution), thereby improving hardness. The aging conditions may be conventionally known. For example, the ingot cold-worked to a predetermined cross-sectional area reduction rate is placed in a heat-resistant container and heat-treated at 350°C to 550°C for approximately 8 to 20 hours in an inert gas atmosphere such as nitrogen or argon, or in a slightly reducing gas atmosphere such as a mixed gas of 95% nitrogen and 5% hydrogen, and then allowed to cool.
[0037] Step 4: The aged ingot obtained in step 3 is further cold worked so that the cross-sectional area reduction rate is 99.95% or more, to obtain a Cu—Ag—Sn alloy wire.
[0038] In this step 4, the aged ingot obtained in the above step 3 is subjected to cold wire drawing at around room temperature using a grooved rolling mill or a wire drawing machine so as to have a predetermined reduction in area, thereby improving the hardness of the ingot by work hardening and processing it into an ultrafine wire (a metal wire having an extremely small diameter) with high added value as a copper-based alloy wire.
[0039] FIG. 1 shows the working ratio η (working ratio η=ln(A 0 / A 1 ), A 0 : Cross-sectional area of Cu—Ag—Sn alloy before cold working, A 1 1 shows the relationship between the cross-sectional area of the Cu—Ag—Sn alloy after cold working (where η is the cross-sectional area of the Cu—Ag—Sn alloy after cold working) and the Vickers hardness of the Cu—Ag—Sn alloy wire. In Fig. 1, the horizontal axis represents the degree of working rather than the area reduction in order to clearly show the transition of Vickers hardness in the heavily worked region where the area reduction is 99.95% or more (i.e., the working degree η is 8 or more). The Vickers hardness of the Cu—Ag—Sn alloy wire was measured using a Vickers hardness tester with a test load of HV 0.005 on test specimens prepared by cutting a portion of the alloy wire to 10 mm and polishing the cross section to make it smooth.
[0040] As can be seen from Fig. 1, as the working ratio η of the aged ingot increases, the Vickers hardness of the Cu-Ag-Sn alloy wire tends to improve. When the working ratio η of the aged ingot is 8 or more (i.e., the area reduction ratio is 99.95% or more), the Vickers hardness of the Cu-Ag-Sn alloy wire becomes 300 HV or more. Therefore, from an experimental point of view, it can be said that the preferable area reduction ratio of the cold working in step 4 is 99.95% or more (i.e., the working ratio η is 8 or more). Here, when the area reduction ratio of the cold working in step 4 is less than 99.95%, the Vickers hardness of the Cu-Ag-Sn alloy wire becomes less than 300 HV, which is undesirable because it tends to result in insufficient durability as a product. More specifically, if the area reduction rate of the cold working in step 4 is less than 99.95%, the Vickers hardness of the Cu—Ag—Sn alloy wire will be less than 300 HV, and defects such as breakage and bending will occur when the wire is used as a probe pin for repeated continuity tests of electrical and electronic components, for example, resulting in a tendency for the durability and reliability of the product to be insufficient. On the other hand, although there is no particular upper limit on the area reduction rate of the cold working in step 4, it is preferable that the area reduction rate of the cold working in step 4 be 99.9999% or less (a working ratio of 13.5 or less). If the area reduction rate of the cold working in step 4 exceeds 99.9999%, the wire will be subjected to extremely heavy working, resulting in large residual stresses inside the Cu—Ag—Sn alloy wire, which will reduce its strength. This will tend to result in insufficient durability when processed into products such as probe pins for inspecting electrical and electronic components, or conductor materials for electric wires and cables used in electronic devices such as mobile devices and industrial robots, medical devices, etc., and used continuously.
[0041] The invention of the present application will be explained in more detail below by way of examples, but the invention of the present application is not limited to these examples.
[0042] In this example, first, metal raw materials of silver (Ag), tin (Sn), and copper, which were blended to have an alloy composition of 6.19 wt % of silver (Ag), 0.20 wt % of tin (Sn), and the remainder of copper (Cu) and unavoidable impurities, were placed in an aluminum oxide (alumina) crucible and melted to a concentration of 1 × 10 2The ingot was obtained by melting the alloy at 1250°C in a vacuum of 100 Pa. Commercially available oxygen-free copper (C1020) was used as the copper raw material. The alloy composition of the ingot was measured using an ICP (inductively coupled plasma) optical emission spectrometer. The ingot was then subjected to solution treatment at 800°C for 2 hours in a nitrogen atmosphere, and then allowed to cool to obtain a solution-treated ingot. The metal near the surface of the solution-treated ingot was then cut to a thickness of 1 mm using a shaper to remove the surface oxide film and impurities that had been introduced into the ingot surface from the crucible during production and embedded therein. The surface-treated solution-treated ingot was then cold-worked using a grooved rolling mill to a cross-sectional area reduction rate of 30% at room temperature (25°C), followed by aging treatment at 450°C for 16 hours in a nitrogen gas atmosphere. Furthermore, this aging-treated ingot was subjected to a grooved rolling mill and a wire drawing machine at room temperature of 25°C to obtain a cross-sectional area reduction rate of 99.9999% and a working ratio η of 13.5 (working ratio η = ln(A 0 / A 1 ), A 0 : Cross-sectional area of Cu—Ag—Sn alloy before cold working, A 1 = cross-sectional area of the Cu—Ag—Sn alloy after cold working) to obtain a Cu—Ag—Sn alloy wire having a diameter of 20 μm.
[0043] Here, in this example, the casting workability was extremely good. Therefore, it can be determined that under the conditions of this example, Cu—Ag—Sn alloy wire rods with stable product quality can be reproducibly obtained. Table 1 shows the alloy composition of this Cu—Ag—Sn alloy wire rod (i.e., the alloy composition of the ingot used in this example) and the evaluation results of its casting workability and plastic workability. The total content of inevitable impurities in the Cu—Ag—Sn alloy wire rod (i.e., the total content of inevitable impurities in the ingot used in this example) was 0.02 wt% or less. In Table 1, the "casting workability" is indicated as "Good" when the molten metal had good flowability (fluidity) and no molten metal remained in the funnel, and a sound Cu—Ag—Sn alloy ingot with a smooth surface and no defects such as chips was obtained. In contrast, when the molten metal had poor flowability and the molten metal remained in the funnel, a sound Cu—Ag—Sn alloy ingot was not obtained, and an "X" was indicated. The "plastic workability" was marked as "good" when a Cu-Ag-Sn alloy wire having a diameter of 110 μm or less was obtained without cracks or breakage, and marked as "poor" when a Cu-Ag-Sn alloy wire having a diameter of 110 μm or less was not obtained due to cracks or breakage.
[0044] Next, a portion of the Cu—Ag—Sn alloy wire obtained by the above method was cut to a length of 1000 mm to prepare a test piece for resistivity measurement, and the resistivity was measured using a resistance meter. Subsequently, a portion of the Cu—Ag—Sn alloy wire obtained by the above method was separately cut to a length of 10 mm, and the cross section was polished to make a smooth test piece for hardness measurement, and the Vickers hardness was measured using a Vickers hardness tester at a test load of HV 0.005. These measurement results are shown in Table 1. Comparative Example
[0045] This comparative example differs from the examples only in that the silver, tin, and copper metal raw materials were blended to produce an alloy composition of 6.00 wt% silver (Ag), 1.00 wt% tin (Sn), and the remainder copper (Cu) and unavoidable impurities. Therefore, the manufacturing and evaluation methods for Cu-Ag-Sn alloy wire are omitted. Here, the plastic workability of the cast ingot (especially the aged ingot) in this comparative example was poor, and attempting cold wire drawing to a diameter of 500 μm or less resulted in wire breakage, making it impossible to obtain a Cu-Ag-Sn alloy wire with a diameter of 110 μm or less. Therefore, the resistivity and Vickers hardness of the Cu-Ag-Sn alloy wire were not measured. Therefore, Table 1 lists the alloy composition of the ingot used in the comparative example and the evaluation results for the castability and plastic workability of the Cu-Ag-Sn alloy.
[0046]
[0047] The Cu—Ag—Sn alloy wire and its manufacturing method according to the present application can be applied to probe pins for inspecting electrical and electronic components and to the manufacture thereof. In particular, the Cu—Ag—Sn alloy wire according to the present application can be suitably used for probes for inspecting electrical and electronic components such as semiconductor integrated circuits and semiconductor packages that have narrow-pitch electrodes. The Cu—Ag—Sn alloy wire according to the present application can also be suitably used as a conductor material for electric wires and cables used in electronic devices such as mobile devices and industrial robots, and medical devices.
Claims
1. A Cu-Ag-Sn alloy wire containing 6 wt% to 10 wt% Ag, 0.1 wt% to 0.9 wt% Sn, and the remainder being Cu and unavoidable impurities.
2. A Cu-Ag-Sn alloy wire as claimed in claim 1, wherein the total content of unavoidable impurities is 0.02 wt% or less.
3. A Cu-Ag-Sn alloy wire according to claim 1 or 2, having a resistivity of 5 μΩ·cm or less and a Vickers hardness of 300 HV to 360 HV.
4. The Cu-Ag-Sn alloy wire according to claim 1, having a diameter of 110 μm or less.
5. A probe pin for inspecting electrical / electronic components, obtained by using the Cu-Ag-Sn alloy wire according to claim 1.
6. The method for producing a Cu-Ag-Sn alloy wire according to claim 1, characterized in that it comprises the following steps 1 to 4. Step 1: A metal raw material is blended so as to have a composition of 6 wt% to 10 wt% Ag, 0.1 wt% to 0.9 wt% Sn, and the balance being Cu and unavoidable impurities, and melted in a vacuum or in an inert gas to obtain an ingot. Step 2: The ingot is solution-treated in an inert gas or a slightly reducing gas to obtain a solution-treated ingot. Step 3: The solution-treated ingot is cold-worked so that the area reduction rate is 25% or more, and then aging-treated in an inert gas or a slightly reducing gas to obtain an aged ingot. Step 4: The aged ingot is further cold-worked so that the area reduction rate is 99.95% or more to obtain a Cu-Ag-Sn alloy wire.
7. The method for producing a Cu-Ag-Sn alloy wire according to claim 6, wherein the total content of inevitable impurities in the ingot in step 1 is 0.02 wt % or less.
Citation Information
Patent Citations
High-strength high-conductivity Cu-Ag-Sn alloy and preparation method thereof
CN116162820A
Sliding contact material
JP1990228439A
High flexural fatigue resistant copper-based alloy wire
JP2017002337A
Cu-ag alloy wire
WO2023085305A1