Multilayer coating film, coated article, and method for producing coated article

The multilayer coating film, comprising scaly glitter, colored pigment, and matting agent layers, addresses the lack of design diversity in automotive coatings by achieving high chroma and soft brilliance in highlight areas, providing a unique aesthetic beyond traditional tones.

WO2024219052A1PCT designated stage expired Publication Date: 2024-10-24NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/003689
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-02-05
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional multilayer coatings for automobiles lack diversity in design to cater to varying consumer tastes, particularly failing to provide high chroma in highlight areas with a soft brilliance effect.

Method used

A multilayer coating film comprising a first coating film with scaly glitter pigment, a second coating film containing colored pigment, and a clear coating film with a matting agent, optimized for spectral reflectance and light transmittance to achieve high chroma and soft brilliance in highlight areas, with a 60-degree specular gloss between 55 and 90.

Benefits of technology

The solution achieves high chroma in highlight areas with a soft brilliance effect, offering a new design aesthetic that is distinct from pastel, matte, and metallic tones, while maintaining adequate light transmittance and gloss levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A multilayer coating film comprising: a first coating film; a second coating film; and a clear coating film in the stated order, wherein the first coating film contains a scale-like glitter pigment, the second coating film contains a colored pigment, the clear coating film contains a matting agent, and the chroma C* 15 in the L*C*h color system, based on the spectral reflectance of reflected light produced when light that is incident on the surface of the multi-layer coating film at an angle of 45 degrees is received at an angle of 15 degrees with respect to normal reflected light, is at least 83, and the 60-degree mirror gloss level of the multi-layer coating film is 55-90.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer coating film and coated article, and method for manufacturing coated article

[0001] The present invention relates to a multi-layer coating and a coated article, as well as a method for producing the coated article.

[0002] Automobiles usually have a multi-layer paint film. Traditionally, a luxurious appearance has been required for the exterior of automobiles, and multi-layer paint films with a strong metallic tone and high flip-flop properties are often formed. For example, Patent Document 1 discloses a multi-layer paint film whose metallic texture changes depending on the viewing angle and whose flip-flop properties are pronounced. Patent Document 2 discloses a multi-layer paint film with a sparkling brilliance due to multi-directional reflection. Patent Document 3 discloses a multi-layer paint film with high gloss in highlights and high brightness overall from highlights to shades. Meanwhile, Patent Document 4 discloses a multi-layer paint film with a soft texture.

[0003] Japanese Patent Application Laid-Open No. 08-238451 Japanese Patent Application Laid-Open No. 2002-275421 International Publication No. 2017 / 135426 International Publication No. 2013 / 154168

[0004] In recent years, the diversification of consumer tastes and the pursuit of originality have led to a wide variety of designs being required for multilayer coating films. The present invention aims to provide a multilayer coating film with a design different from that of Patent Documents 1 to 4, which has high saturation in the highlight area and a soft, radiant feel.

[0005] In order to solve the above problems, the present invention provides the following aspects: [1] A multi-layer coating film comprising a first coating film, a second coating film, and a clear coating film in this order, wherein the first coating film contains a scaly luster pigment, the second coating film contains a color pigment, and the clear coating film contains a matting agent, and an L refractometer based on the spectral reflectance of light reflected at an angle of 15 degrees relative to incident light incident at an angle of 45 degrees to the surface of the multi-layer coating film is * C * Chroma C in the h color system * 15is 83 or more, and the 60-degree specular gloss of the multilayer coating film is 55 to 90. [2] The multilayer coating film of [1] above, wherein the average light transmittance of the second coating film at wavelengths of 400 to 700 nm is 25 to 45%. [3] The multilayer coating film of [1] or [2] above, wherein the content of the matting agent in the clear coating film is 0.5 to 6 parts by mass per 100 parts by mass of resin solids. [4] The multilayer coating film of any of [1] to [3] above, wherein the spectral reflectance of light incident on the surface of the first coating film at an angle of 45 degrees and reflected at an angle of 15 degrees relative to the specularly reflected light is 25 to 215% at wavelengths of 400 to 580 nm, and 95 to 220% at wavelengths of 650 to 700 nm. [5] A multilayer coating film according to any one of [1] to [4] above, wherein the first coating film further contains a coloring pigment. [6] A multilayer coating film according to any one of [1] to [5] above, wherein the light transmittance of the second coating film is 2% or more and 40% or less at a wavelength of 400 to 580 nm, and 85% or more and 100% or less at a wavelength of 650 to 700 nm. [7] A coated article comprising a substrate, and a multilayer coating film according to any one of [1] to [6] above, provided on the substrate. [8] A coated article comprising a first coating composition, a second coating composition, and a clear coating composition applied sequentially to the substrate to form a multilayer coating film, wherein the first coating composition contains a scaly luster pigment, the second coating composition contains a coloring pigment, and the clear coating composition contains a matting agent, and wherein the L * C * Chroma C in the h color system * 15 is 83 or more, and the 60-degree specular gloss of the multi-layer coating film is 55 or more and 90 or less.

[0006] According to the present invention, there are provided a multi-layer coating film that has high saturation in highlight areas and a soft, lustrous feel, a coated article that includes this multi-layer coating film, and a method for producing the same.

[0007] [Multilayer Coating Film] The multilayer coating film of the present disclosure comprises, in this order, a first coating film containing a scaly luster pigment, a second coating film containing a coloring pigment, and a clear coating film containing a matting agent.

[0008] The L is based on the spectral reflectance of the reflected light received at an angle of 15 degrees to the specular reflected light of the incident light incident at an angle of 45 degrees to the surface of the multi-layer coating film (the surface on the clear coating film side). * C * Chroma C in the h color system * 15 is greater than or equal to 83, which indicates that vivid colors are observed in the highlight area.

[0009] The 60-degree specular gloss of the multilayer coating film is 55 or more and 90 or less. This indicates that the reflection is not excessively strong (for example, it is a soft reflection, as if through a thin veil). The fact that the above-mentioned 60-degree specular gloss is obtained even though the first coating film containing the scaly luster pigment is covered with the second coating film indicates that the second coating film has a certain degree of light transmittance.

[0010] In this way, by combining a first coating film containing a scaly luster pigment with a second coating film containing a coloring pigment but having optical transparency, a high chroma color in the highlight region is achieved. In addition, by providing a clear coating film containing a matting agent so as to cover the second coating film, the multilayer coating film of the present disclosure can express a new design that is different from so-called pastel, matte, or metallic tones, and has a high chroma in the highlight region while giving a soft brilliance feeling.

[0011] The highlight region refers to a range of 25 degrees or less relative to the specular reflection of light incident at an angle of 45 degrees. In this disclosure, the highlight region is defined as the saturation at an angle of 15 degrees relative to the specular reflection, which can also be called the super highlight region.

[0012] (Saturation C * 15 ) Saturation C * 15 is 83 or more. * 15If the saturation C is less than 83, the color will be less vivid and the desired design will not be obtained. * 15 may be 84 or more, or may be 85 or more. * 15 may be 120 or less, or may be 115 or less.

[0013] Saturation C * 15 is the spectral reflectance of incident light incident on the surface of a multi-layer coating film at an angle of 45 degrees and reflected light received at an angle of 15 degrees relative to the specular reflection light. * C * It is the saturation in the h color system. * C * In the h color system, saturation C * As the value of increases, the vividness of the substance being measured increases, and as the value decreases, the dullness increases.

[0014] L * C * h color system is CIE * a * b Color system (CIE1976L * a * b * It is calculated based on the CIE 1976L color space. * a * b * The color space can be determined in accordance with JIS Z 8781-4. * a * The b color system has been established by the International Commission on Illumination and is described in Section 4.2 of CIE Publication 15.2 (1986).

[0015] Saturation C * 15 can be obtained using a spectrophotometer (for example, BYK-mac i manufactured by BYK Gardner).

[0016] (60-degree specular gloss) The 60-degree specular gloss of the multilayer coating film is 55 or more and 90 or less. If the 60-degree specular gloss is less than 55, the reflection is too small and the coating film becomes cloudy, resulting in a design with a so-called matte feel. If the 60-degree specular gloss is more than 90, the reflection is too strong and a soft, lustrous feel cannot be obtained. The 60-degree specular gloss may be 60 or more, or 65 or more. The 60-degree specular gloss may be 88 or less, or 85 or less.

[0017] The 60-degree specular gloss is measured in accordance with JIS Z 8741 Specular gloss - Measuring method using a gloss meter (for example, trade name: AG-4446, manufactured by BYK Gardner).

[0018] Saturation C * 15 The gloss and 60-degree specular gloss are measured for the multilayer coating film. The multilayer coating film to be measured is prepared as follows. First, a cationic electrodeposition paint and an undercoat paint are applied to a steel plate, and each is heat-cured to obtain a substrate. The substrate is spray-coated with the first coating composition described below to a dry coating thickness of 3 μm to 15 μm (typically 10 μm), then the second coating composition is spray-coated wet-on-wet to a dry film thickness of 3 μm to 15 μm (typically 10 μm), and then the clear coating composition is spray-coated wet-on-wet to a dry film thickness of 10 μm to 80 μm (typically 35 μm). Finally, these uncured three-layer coating films are heat-cured at 140°C for 20 minutes. The multilayer coating film refers to a laminate of a cured coating film of the first coating composition, a cured coating film of the second coating composition, and a cured coating film of the clear coating composition applied to the substrate.

[0019] (First coating film) The first coating film contains a scaly luster pigment. This provides light reflectivity to the multilayer coating film. The first coating film is typically a cured product of a first coating composition containing the scaly luster pigment and a coating film-forming resin.

[0020] The thickness of the first coating film may be, for example, 3 μm or more and 15 μm or less, 7 μm or more, 14 μm or less, or 13 μm or less.

[0021] Incident light I1 incident at an angle of 45 degrees to the surface of the first coating film 45 The reflected light R1 is received at an angle of 15 degrees with respect to the specular reflection light. 15 The spectral reflectance of the first coating film may be 25% or more and 220% or less at wavelengths of 400 to 700 nm, which allows the first coating film to exhibit good reflectivity in the visible light region and the highlight region, and allows the multi-layer coating film to exhibit a more vivid color regardless of the hue of the color pigment of the second coating film.

[0022] When the color pigment of the second coating film is red, the reflected light R1 15 The spectral reflectance of the multilayer coating film may be 25% or more and 215% or less in the wavelength range of 400 to 580 nm, and 95% or more and 220% or less in the wavelength range of 650 to 700 nm, thereby enabling the multilayer coating film to exhibit a more vivid red color in the highlight region.

[0023] When the color pigment of the second coating film is red, reflected light R1 at wavelengths of 400 to 580 nm 15 The spectral reflectance of the reflected light R1 at a wavelength of 650 to 700 nm may be 200% or less, 170% or less, or 150% or less. 15 The spectral reflectance of may be 110% or more, 120% or more, or 125% or more.

[0024] Reflected light R1 15 The spectral reflectance is measured for the first coating film alone, not for a multi-layer coating film. The first coating film alone to be measured is obtained by coating a steel plate with a cationic electrodeposition paint and an undercoat paint, each of which is heat-cured, and then spray-coating the first coating composition on the substrate so that the dry coating film has a thickness of 3 μm to 15 μm (typically 10 μm), and then heat-curing at 140° C. for 20 minutes. The first coating film alone to be measured refers to the cured coating film of the first coating composition applied to the substrate.

[0025] The spectral reflectance of the first coating film alone is measured using a spectrophotometer (for example, BYK-mac i manufactured by BYK Gardner) in the range of 400 to 700 nm in wavelength scan mode at a sampling interval of 10 nm.

[0026] Reflected light R1 15 The spectral reflectance of the reflected light R1 is not an average value. 15 The spectral reflectance of the reflected light R1 at a wavelength of 400 to 700 nm is 25% or more and 220% or less. 15 This means that the minimum and maximum values ​​of the spectral reflectance are in the range of 25% or more and 220% or less.

[0027] Reflected light R1 15 The spectral reflectance can be adjusted, for example, by the type and mass proportion of the scaly luster pigment contained in the first coating film, the presence or absence of a coloring pigment, the type and mass proportion of the coloring pigment, and the thickness of the first coating film.

[0028] (First Coating Composition) The first coating composition contains a scaly photoluminescent pigment and a film-forming resin. The first coating composition may be aqueous or solvent-based. The aqueous first coating composition may contain water as the main solvent, and optionally a water-soluble or water-miscible organic solvent. The solvent-based first coating composition may contain, as the main solvent, for example, an ester solvent, an ether solvent, an alcohol solvent, a ketone solvent, an aliphatic hydrocarbon solvent, or an aromatic solvent. The first coating composition may be diluted with a solvent suitable for application before use. The first coating composition may be aqueous. The main solvent accounts for 50% by mass or more of the total solvent.

[0029] The first coating composition is prepared by kneading and dispersing the scaly luster pigment, film-forming resin, curing agent, etc. using a disperser, homogenizer, kneader, etc. A pigment paste may be prepared in advance using a pigment such as the scaly luster pigment and a pigment dispersant, and this may then be mixed with the film-forming resin, etc.

[0030] <<Scaly Luster Pigment>> Examples of the scaly luster pigment include mica pigments such as interference mica, white mica, and colored mica; graphite pigments; glass flake pigments; and metal pigments such as aluminum, copper, zinc, iron, nickel, tin, aluminum oxide, chromium oxide, and alloys containing these. These may be used alone or in combination of two or more. The scaly luster pigment may be colored or uncolored. The scaly luster pigment may be an aluminum pigment.

[0031] The term "scaly pigment" refers to a shape in which the aspect ratio (average major axis of the pigment / average thickness of the pigment) exceeds 1.0. The aspect ratio of the scaly pigment is, for example, 20 or more and 300 or less. The aspect ratio of the scaly pigment may be 30 or more. The aspect ratio of the scaly pigment may be 200 or less.

[0032] The average particle size of the scaly luster pigment may be 4 μm or more, or 5 μm or more, and may be 12 μm or less, or 10 μm or less.

[0033] The average particle size of the scaly pigment is the average value of the long diameter, which can be obtained by observing the scaly pigment using a shape analysis laser microscope (for example, VK-X 250 manufactured by Keyence Corporation) and averaging the long diameters (maximum lengths) of 100 arbitrarily selected scaly pigment particles.

[0034] The average thickness of the scaly luster pigment is, for example, 0.01 μm or more and 0.1 μm or less. The average thickness of the scaly luster pigment may be 0.04 μm or more. The average thickness of the scaly luster pigment may be 0.08 μm or less.

[0035] The average thickness of the scaly pigments is obtained by observing the cross section of a coating film containing the scaly pigments using a transmission electron microscope (TEM) and averaging the thicknesses of 100 arbitrarily selected scaly pigments.

[0036] The scaly bright pigment may or may not be surface-treated. Examples of compounds used for surface treatment include metal oxide compounds, phosphorus compounds, amine compounds, and silane compounds.

[0037] The content of the scaly luster pigment in the first coating film, that is, the mass ratio of the scaly luster pigment to the total mass of the solid content of the resin and the scaly luster pigment contained in the first coating composition (PPWC 1g ) is, for example, 2% by mass or more and 20% by mass or less. This makes it easier to express a desired sense of brilliance.

[0038] PWC 1g may be 3 mass% or more, or 5 mass% or more. 1g The solid content of the resin is the solid content of all resin components such as the film-forming resin and the curing agent, which will be described later.

[0039] Other Pigments The first coating composition (first coating film) may further contain a pigment other than the scaly luster pigment. Examples of other pigments include color pigments, extender pigments, anti-rust pigments, and luster pigments other than scaly luster pigments. In particular, the first coating film may contain a color pigment. The color pigments contained in the first coating film and the second coating film may be the same or different. When the color pigments contained in the first coating film and the second coating film are the same, the multilayer coating film appears more vivid.

[0040] The color pigment may be inorganic or organic. The color pigment may be chromatic or achromatic. Examples of organic color pigments include azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, phthalocyanine pigments, indigo pigments, perinone pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments. Examples of inorganic color pigments include yellow lead, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide. These may be used alone or in combination of two or more.

[0041] Examples of extender pigments include calcium carbonate, barium sulfate, clay, and talc, which may be used alone or in combination of two or more.

[0042] The content of the color pigment in the first coating film, that is, the mass ratio of the color pigment to the total mass of the solid content of the resin and the color pigment contained in the first coating composition (PWC 1c ) is, for example, 0.05 mass % or more and 35 mass % or less. 1c may be 5% by mass or more, or 7% by mass or more. 1c may be 20% by mass or less, or may be 15% by mass or less.

[0043] <Film-forming resin> Examples of the film-forming resin include acrylic resin, acrylic silicone resin, polyester resin, polyurethane resin, epoxy resin, fluororesin, and silicone resin. These may be used alone or in combination of two or more. Among these, acrylic resin is preferred.

[0044] In the aqueous first coating composition, these resins may be contained as an emulsion, a dispersion, or in a state of being dissolved in a solvent.

[0045] For example, the acrylic resin emulsion can be prepared by emulsion polymerization of α,β-ethylenically unsaturated monomers. Examples of the α,β-ethylenically unsaturated monomers include (meth)acrylic acid esters, α,β-ethylenically unsaturated monomers having an acid group, and α,β-ethylenically unsaturated monomers having a hydroxyl group. The monomers can be used alone or in combination of two or more.

[0046] Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dihydrodicyclopentadienyl (meth)acrylate. (Meth)acrylic acid esters refer to acrylic acid esters and methacrylic acid esters.

[0047] Examples of α,β-ethylenically unsaturated monomers having an acid group include acrylic acid, methacrylic acid, crotonic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinylacetylsalicylic acid, 2-acrylamido-2-methylpropanesulfonic acid, p-hydroxystyrene, and 2,4-dihydroxy-4′-vinylbenzophenone.

[0048] Examples of the α,β-ethylenically unsaturated monomer having a hydroxyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, methallyl alcohol, and adducts of these with ε-caprolactone.

[0049] Other α,β-ethylenically unsaturated monomers may be used in combination. Examples of the other α,β-ethylenically unsaturated monomers include polymerizable amide compounds, polymerizable aromatic compounds, polymerizable nitriles, polymerizable alkylene oxide compounds, polyfunctional vinyl compounds, polymerizable amine compounds, α-olefins, dienes, polymerizable carbonyl compounds, polymerizable alkoxysilyl compounds, and other polymerizable compounds.

[0050] The emulsion polymerization method is not particularly limited. For example, an emulsifier is dissolved in an aqueous medium containing water or, if necessary, an organic solvent such as an alcohol or an ether (e.g., dipropylene glycol methyl ether, propylene glycol methyl ether, etc.), and an α,β-ethylenically unsaturated monomer and a polymerization initiator are added dropwise with heating and stirring. The α,β-ethylenically unsaturated monomer may be previously emulsified with an emulsifier.

[0051] Polymerization initiators and emulsifiers commonly used by those skilled in the art can be used. If necessary, a chain transfer agent such as a mercaptan (e.g., lauryl mercaptan) or α-methylstyrene dimer may be used to adjust the molecular weight. The reaction temperature, reaction time, and the like can be appropriately selected within ranges commonly used by those skilled in the art. The resulting acrylic resin emulsion is neutralized with a base, if necessary.

[0052] The acrylic resin (acrylic resin emulsion) obtained by emulsion polymerization may have a number average molecular weight of 3,000 or more. The acrylic resin may have a hydroxyl value (solid content hydroxyl value) of 20 mg KOH / g or more and 180 mg KOH / g or less. The acrylic resin may have an acid value (solid content acid value) of 1 mg KOH / g or more and 80 mg KOH / g or less.

[0053] The number average molecular weight is determined by GPC using polystyrene as a standard. The acid value and hydroxyl value of the film-forming resin are calculated from the monomer composition used in the preparation, in accordance with JIS regulations.

[0054] The acrylic resin dispersion can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomers and dispersing the resultant with a basic compound.

[0055] The water-soluble acrylic resin can be prepared, for example, by solution polymerizing the above-mentioned α,β-ethylenically unsaturated monomer and then solubilizing it in water using a basic compound.

[0056] The acrylic resin blended in the solvent-based first coating composition can be prepared, for example, by solution polymerization of an α,β-ethylenically unsaturated monomer. The acrylic resin has a number average molecular weight of, for example, 1,000 or more and 20,000 or less. The acrylic resin may have an acid value (solid content acid value) of 1 mgKOH / g or more and 80 mgKOH / g or less. The acrylic resin may have a hydroxyl value (solid content hydroxyl value) of 101 mgKOH / g or more and 200 mgKOH / g or less.

[0057] Curing Agent The first coating composition may contain a curing agent, which reacts with the film-forming resin to form the first coating film therewith.

[0058] Examples of curing agents include melamine resins, blocked isocyanate compounds, epoxy compounds, aziridine compounds, carbodiimide compounds, oxazoline compounds, and metal ions. These may be used alone or in combination of two or more. Among these, at least one of melamine resins and blocked isocyanate compounds may be used.

[0059] The melamine resin may be water-soluble or water-insoluble. The melamine resin has a structure in which hydrogen atoms or substituents (such as alkyl ether groups and methylol groups) are bonded to the periphery of a melamine nucleus (triazine nucleus) via three nitrogen atoms. The melamine resin is generally composed of a polynuclear compound in which multiple melamine nuclei are bonded to each other. The melamine resin may also be a mononuclear compound consisting of a single melamine nucleus.

[0060] Commercially available melamine resins may be used. Examples of commercially available melamine resins include the Cymel series (trade name) manufactured by Allnex, specifically Cymel 202, Cymel 204, Cymel 211, Cymel 232, Cymel 235, Cymel 236, Cymel 238, Cymel 250, Cymel 251, Cymel 254, Cymel 266, Cymel 267, Cymel 272, Cymel 285, Cymel 301, Cymel 303, Cymel 325, Cymel 327, Cymel 350, Cymel 370, Cymel 701, Cymel 703, and Cymel 1141; and the U-Ban (trade name) series manufactured by Mitsui Chemicals, Inc. These may be used alone or in combination of two or more.

[0061] The blocked isocyanate compound can be prepared by adding a blocking agent having an active hydrogen to a polyisocyanate such as trimethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, or isophorone diisocyanate.

[0062] The content of the curing agent may be 10% by mass or more and 80% by mass or less of the resin solid content contained in the first coating composition. The content of the curing agent may be 15% by mass or more. The content of the curing agent may be 60% by mass or less.

[0063] <<Phosphate Group-Containing Organic Compound>> The first coating composition may further contain a phosphate group-containing organic compound, which facilitates improving the dispersibility of the scaly luster pigment.

[0064] The content of the phosphate group-containing compound may be 0.1% by mass or more and 15% by mass or less of the total solid content of the first coating composition. The content of the phosphate group-containing compound may be 1% by mass or more. The content of the phosphate group-containing compound may be 12% by mass or less.

[0065] The phosphate group-containing compound is a compound having a phosphate group (-P(=O)(OR) 2(wherein each R is independently hydrogen or a hydrocarbon group) The phosphate group-containing compound is not particularly limited as long as it has such a structure. For example, the phosphate group-containing compound is at least one of an alkyl phosphate ester having an alkyl group having 4 to 30 carbon atoms and a phosphate group-containing polymer having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less.

[0066] <Alkyl Phosphate Ester> The alkyl phosphate ester has an alkyl group having 4 to 30 carbon atoms. Examples of the alkyl phosphate ester include monoalkyl phosphate esters, dialkyl phosphate esters, and mixtures thereof. In the dialkyl phosphate ester, the two alkyl groups may be the same or different. The dialkyl phosphate ester preferably has the same two alkyl groups.

[0067] Examples of alkyl groups having 4 to 30 carbon atoms include butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, docosyl, tetracosyl, hexacosyl, and octacosyl. The alkyl group may be linear or branched.

[0068] Examples of alkyl phosphate esters include butyl acid phosphate (a mixture of monobutyl phosphate ester and dibutyl phosphate ester), 2-ethylhexyl acid phosphate (a mixture of mono-2-ethylhexyl phosphate ester and di-2-ethylhexyl phosphate ester), isodecyl acid phosphate (a mixture of monoisodecyl phosphate ester and diisodecyl phosphate ester), dilauryl acid phosphate, lauryl acid phosphate (a mixture of monolauryl phosphate ester and dilauryl phosphate ester), tridecyl acid phosphate (monotridecyl phosphate), Examples of suitable phosphates include monostearyl acid phosphate, distearyl acid phosphate, stearyl acid phosphate (a mixture of monostearyl phosphate and distearyl phosphate), isostearyl acid phosphate (a mixture of monoisostearyl phosphate and diisostearyl phosphate), oleyl acid phosphate (a mixture of monooleyl phosphate and dioleyl phosphate), and behenyl acid phosphate (a mixture of monobehenyl phosphate and dibehenyl phosphate).

[0069] <Phosphate Group-Containing Polymer> The phosphate group-containing polymer has a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less. The phosphate group value of the phosphate group-containing polymer may be 10 mgKOH / g or more, or 50 mgKOH / g or more. The phosphate group value of the phosphate group-containing polymer may be 250 mgKOH / g or less, or 150 mgKOH / g or less.

[0070] The phosphate value is the number of mg of potassium hydroxide (KOH) required for neutralization, calculated based on the blend amount of the phosphate group-containing component, such as a phosphate ester, used in preparing the phosphate group-containing polymer.

[0071] The number average molecular weight of the phosphate group-containing polymer is, for example, 1,000 or more and 50,000 or less. The number average molecular weight of the phosphate group-containing polymer may be 3,000 or more, or 5,000 or more. The number average molecular weight of the phosphate group-containing polymer may be 30,000 or less, or 20,000 or less.

[0072] Examples of the phosphate group-containing polymer include acrylic resins, polyester resins, polyether resins, and epoxy resins, each having a phosphate group value of 5 mgKOH / g or more and 300 mgKOH / g or less. These may be used alone or in combination of two or more. Among these, a phosphate group-containing acrylic resin may be used. The phosphate group-containing acrylic resin may be obtained, for example, by polymerizing a phosphate group-containing α,β-ethylenically unsaturated monomer, or by copolymerizing this monomer with another α,β-ethylenically unsaturated monomer that does not contain a phosphate group.

[0073] The first coating composition may contain additives commonly used by those skilled in the art, such as a surface conditioner, a viscosity control agent, a thickener, an antioxidant, an ultraviolet inhibitor, and an antifoaming agent.

[0074] (Second Coating Film) The second coating film contains a coloring pigment. This imparts a desired hue to the multilayer coating film. The second coating film is typically a cured product of a second coating composition containing a coloring pigment and a film-forming resin.

[0075] The thickness of the second coating film may be, for example, 3 μm or more and 15 μm or less, 7 μm or more, 14 μm or less, or 13 μm or less.

[0076] The light transmittance of the second coating film can affect the saturation of the multilayer coating film. The average light transmittance of the second coating film in the wavelength range of 400 to 700 nm may be 25% or more and 45% or less. When the average light transmittance of the second coating film in the visible light range is 25% or more, the color expressed by the multilayer coating film becomes more vivid. When the average light transmittance of the second coating film in the visible light range is 45% or less, the color expressed by the multilayer coating film becomes deeper. The above average light transmittance may be 30% or more, or may be 35% or more. The above average light transmittance may be 44% or less, or may be 43% or less.

[0077] The average light transmittance is measured not for the multi-layer coating film but for the single second coating film. The single second coating film to be measured is obtained by spray-coating the second coating composition onto a polypropylene plate so that the dry film thickness is 3 μm or more and 15 μm or less (typically 10 μm), heating and curing at 140° C. for 20 minutes, and then peeling the coating film from the polypropylene plate. The single second coating film to be measured refers to a cured film of the second coating composition.

[0078] The light transmittance of the second coating film alone is measured using a spectrophotometer (for example, Hitachi, product name: U-4100) in the range of 400 to 700 nm under the conditions of wavelength scan mode, scan speed of 300 nm / min, and sampling interval of 0.5 nm. The arithmetic mean value of the obtained light transmittances every 10 nm is defined as the average light transmittance.

[0079] When the color pigment of the second coating film is red, the light transmittance of the second coating film may be 2% or more and 40% or less at wavelengths of 400 to 580 nm, and 85% or more and 100% or less at wavelengths of 650 to 700 nm. This allows the multilayer coating film to exhibit a more vivid red color. This light transmittance is not an average value. For example, a light transmittance of 2% or more and 40% or less at wavelengths of 400 to 580 nm means that the minimum and maximum light transmittance values ​​in that wavelength range are within the range of 2% or more and 40% or less.

[0080] The light transmittance of the second coating film can be adjusted, for example, by the type and mass proportion of the color pigment contained in the second coating film, the presence or absence of a luster pigment, and the thickness of the second coating film.

[0081] (Second Coating Composition) The second coating composition contains a color pigment and a coating film-forming resin. The second coating composition may be water-based or solvent-based. The second coating composition may be water-based. The solvent contained in the second coating composition and the method for preparing it are the same as those for the first coating composition.

[0082] <<Coloring Pigment>> The second coating composition (second coating film) contains a coloring pigment. Examples of the coloring pigment include the same pigments that can be contained in the first coating composition. The coloring pigments may be used alone or in combination of two or more.

[0083] The content of the color pigment in the second coating film, that is, the mass ratio of the color pigment to the total mass of the resin solid content and the color pigment contained in the second coating composition (PWC 2c ) is, for example, 0.05 mass % or more and 35 mass % or less. 2c may be 1 mass% or more, or may be 2 mass% or more. 2c may be 20% by mass or less, or may be 10% by mass or less.

[0084] Other Pigments The second coating film may further contain a pigment other than the color pigment. Examples of other pigments include a luster pigment, an extender pigment, and an anti-rust pigment. In particular, the second coating film may contain a luster pigment. The luster pigments contained in the first coating film and the second coating film may be the same or different.

[0085] The content of the bright pigment in the second coating film, that is, the mass ratio of the bright pigment to the total mass of the resin solid content and the bright pigment contained in the second coating composition (PWC 2g ) is, for example, 0.05 mass % or more and 30 mass % or less. 2g may be 0.1 mass% or more, or 0.2 mass% or more. 2g may be 10% by mass or less, or may be 5% by mass or less.

[0086] <Film-forming resin> Examples of the film-forming resin include those contained in the first coating composition. The film-forming resins contained in the first and second coating compositions may be the same or different. In addition, the second coating composition may contain the same components as the first coating composition.

[0087] (Clear Coating Film) The clear coating film contains a matting agent. This softens the glossiness of the multi-layer coating film. The clear coating film is typically a cured product of a clear coating composition containing a matting agent and a clear coating material.

[0088] The thickness of the clear coating film may be, for example, 10 μm or more and 80 μm or less, 20 μm or more, or 50 μm or less.

[0089] (Clear Coating Composition) The clear coating composition includes a matting agent and a clear coating. The clear coating composition may be a solvent-based, water-based, or powder-type. The clear coating composition may be a solvent-based.

[0090] Matting agents create minute irregularities on the surface of the clear coating, causing light diffusion. This reduces the particle size of the scaly luster pigment contained in the first coating, particularly, and softens the luster.

[0091] The matting agent is, for example, fine particles of an inorganic or organic substance, and any of those conventionally known in paints can be used as the matting agent.

[0092] Examples of inorganic fine particles include silica particles, aluminum oxide particles, titanium dioxide particles, zirconium dioxide particles, zircon particles, tin oxide particles, and magnesium oxide particles. These may be used alone or in combination of two or more. Among them, silica particles are preferred from the viewpoints of matting ability and storage stability. The shape of the silica particles is not particularly limited and may be spherical, hollow, porous, rod-like, plate-like, fibrous, or irregular.

[0093] Commercially available silica particles include, for example, the Sylysia series (Sylysia 350, Sylysia 430, Sylysia 435, Sylysia 436, Sylysia 450, etc.), the Sylohobic series (Sylohobic 100, Sylohobic 200, Sylohobic 702, Sylohobic 100, 4004, etc.), and the Sylosphere series (Sylosphere 1504, Sylosphere 1510, etc.) manufactured by Fuji Silysia Ltd., the Syloid series (Syloid W300, Syloid W500, etc.) manufactured by Grace Japan, and the Acematt series (ACEMATT HK460, Acematt K400, Acematt OK412, Acematt OK520, Acematt TS100, Acematt 3200, Acematt 3300, Acematt TS100, Acematt TS200, Acematt TS300, Acematt TS400, Acematt TS500, Acematt TS600, Acematt TS700, Acematt TS800, Acematt TS900, Acematt TS100, Acematt TS110, Acematt TS1200, Acematt TS1300, Acematt TS1400, Acematt TS15 ... 3600, etc.), the NIPGEL series (NIPGEL AZ-200, etc.) and the NIPSIL series (NIPSIL E-200A, NIPSIL SS-50B, NIPSIL SS-178B, etc.) manufactured by Nippon Silica Industry Co., Ltd., the Mizukasil series (MIZUKASIL P-73, P-526, etc.) manufactured by Mizusawa Chemicals, Ltd., the Carplex series (CARPLEX CS-8, etc.) manufactured by Shionogi & Co., Ltd., the AEROSIL series (AEROSIL 200, AEROSIL R805, AEROSIL R972, etc.) manufactured by Nippon Aerosil Co., Ltd., and the Radiolite series (Radiolite 100, Radiolite 200, Radiolite 500, Radiolite 500R, Radiolite 500RS, etc.) manufactured by Showa Chemical Industry Co., Ltd.

[0094] The inorganic fine particles may be surface-treated with an organic compound and / or an inorganic compound. In particular, from the viewpoint of storage stability, the inorganic fine particles may be surface-treated with an organic compound. Examples of treatments with organic compounds include polyethylene wax treatment and silane compound treatment. In particular, polyethylene wax treatment is preferred.

[0095] Examples of organic fine particles (hereinafter sometimes referred to as resin beads) include PMMA (polymethyl methacrylate) resin beads, MMA-EGDM (ethylene glycol dimethacrylate) copolymer resin beads, nylon resin beads, and polytetrafluoroethylene resin beads.

[0096] Commercially available resin beads include, for example, "Techpolymer Series (trade name)" manufactured by Sekisui Plastics Co., Ltd. and "Dyneon Series (trade name)" manufactured by Sumitomo 3M Limited.

[0097] The average particle size of the matting agent may be 1 μm or more, 2 μm or more, or 3 μm or more from the viewpoints of matting ability, storage stability, etc. From the same viewpoints, the average particle size of the matting agent may be 10 μm or less, 9 μm or less, or 8 μm or less.

[0098] The average particle size of the matting agent is the 50% average particle size (D50) in the volumetric particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer. D50 is measured after adding the matting agent to a mixed solvent of acetone and isopropyl alcohol, dispersing it with ultrasonic waves for 1 minute, and adjusting the concentration to a predetermined transmittance range.

[0099] The oil absorption of the matting agent may be 100 mL / 100 g or more from the viewpoint of matting ability, etc. From the same viewpoint, the oil absorption of the matting agent may be 400 mL / 100 g or less, 380 mL / 100 g or less, or 360 mL / 100 g or less. The oil absorption is measured in accordance with JIS K 5101-13-2:2004.

[0100] Matting agent content (PWC m ) may be 0.5 parts by mass or more and 6 parts by mass or less per 100 parts by mass of the resin solid content of the clear coating composition. m When the amount of PWC is 0.5 parts by mass or more, the glittering feeling tends to be soft. m When the amount of PWC is 6 parts by mass or less, the cloudiness is suppressed, and sufficient saturation and a sense of depth of color are easily expressed. mmay be 0.8 parts by mass or more, 1.0 parts by mass or more, or 1.2 parts by mass or more. m may be 5.5 parts by mass or less, or may be 5.0 parts by mass or less.

[0101] The clear coating may be, for example, an acid epoxy curing type containing a polyepoxide and a polycarboxylic acid, or a urethane curing type containing a hydroxyl group-containing resin and a polyisocyanate curing agent. The urethane curing type clear coating may be a two-component type.

[0102] The acid-epoxy curing clear coating composition contains, for example, an acid anhydride group-containing acrylic resin (a), a carboxyl group-containing polyester resin (b), and an acrylic resin (c) having a hydroxyl group and an epoxy group. From the viewpoint of storage stability, the acid anhydride group of the acid anhydride group-containing acrylic resin (a) may be half-esterified with a low-molecular-weight alcohol or the like. The carboxyl group-containing polyester resin (b) may further contain a hydroxyl group.

[0103] The resins (a) to (c) are blended so that, for example, the molar ratio of the carboxyl groups contained in the acrylic resin (a) and the polyester resin (b) to the epoxy groups contained in the acrylic resin (c) is 1 / 1.4 to 1 / 0.6 (preferably 1 / 1.2 to 1 / 0.8), and the molar ratio of the carboxyl groups derived from the acid anhydride groups contained in the acrylic resin (a) to the hydroxyl groups contained in the polyester resin (b) and the acrylic resin (c) is 1 / 2.0 to 1 / 0.5 (preferably 1 / 1.5 to 1 / 0.7).

[0104] The urethane curing clear coating composition contains, for example, a hydroxyl group-containing resin and a polyisocyanate curing agent. Examples of the polyisocyanate curing agent include aliphatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), and trimethylhexamethylene diisocyanate; aliphatic cyclic isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, and 1,2-cyclohexane diisocyanate; aromatic isocyanates such as xylylene diisocyanate (XDI), 2,4-tolylene diisocyanate (TDI), and 2,6-tolylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate (IPDI) and norbornane diisocyanate methyl; and polymers and mixtures thereof, such as biuret and nurate forms.

[0105] The hydroxyl value of the hydroxyl group-containing resin is, for example, 20 mgKOH / g or more and 200 mgKOH / g or less. The hydroxyl value may be 30 mgKOH / g or more. The hydroxyl value may be 180 mgKOH / g or less. The weight average molecular weight of the hydroxyl group-containing resin is, for example, 1,000 or more and 20,000 or less. The weight average molecular weight may be 2,000 or more. The weight average molecular weight may be 15,000 or less. The acid value of the hydroxyl group-containing resin is, for example, 2 mgKOH / g or more and 30 mgKOH / g or less. The acid value may be 3 mgKOH / g or more. The acid value may be 25 mgKOH / g or less.

[0106] The hydroxyl group-containing resin and the polyisocyanate curing agent are blended, for example, so that the equivalent ratio (NCO / OH) of the isocyanate group (NCO) to the hydroxyl group (OH) is 0.5 or more and 1.7 or less. The equivalent ratio may be 0.7 or more. The equivalent ratio may be 1.5 or less.

[0107] Alternatively, an acrylic melamine curing type clear paint may be used.

[0108] [Coated Article] The coated article according to the present disclosure comprises a substrate and the above-described multilayer coating film provided on the substrate. In the coated article, the clear coating film is disposed on the outside. The coated article comprising the above-described multilayer coating film has a unique design, with high saturation in highlight areas and a soft, radiant glow.

[0109] (Substrate) Examples of the material of the substrate include metal, plastic, and foam. Among them, metal (particularly, casting) may be used, and metal that can be electrocoated may be used. Examples of such metals include iron, copper, aluminum, tin, zinc, etc., and alloys containing these metals.

[0110] The shape of the substrate is not particularly limited, and may be flat or three-dimensional. Specific examples of the substrate include automobile bodies and parts thereof, such as passenger cars, trucks, motorcycles, and buses.

[0111] The metal substrate may have been subjected to a chemical conversion treatment using a phosphate-based chemical conversion treatment agent, a zirconium-based chemical conversion treatment agent, or the like, and may have been subjected to electrodeposition coating. The electrodeposition coating composition may be either a cationic type or an anionic type. A cationic electrodeposition coating composition can form a coating film with excellent corrosion resistance.

[0112] The metal substrate may have an electrodeposition coating and an intermediate coating applied thereon. The intermediate coating is usually applied to improve the adhesion and durability of the multi-layer coating. The intermediate coating composition may contain, for example, a film-forming resin, a curing agent, a color pigment, and an extender pigment. Examples of the film-forming resin and curing agent include those contained in the first coating composition.

[0113] [Method for producing a coated article] The method for producing a coated article according to the present disclosure comprises sequentially applying a first coating composition, a second coating composition, and a clear coating composition to an article to be coated to form a multi-layer coating film.

[0114] In one embodiment, the coated article is produced by sequentially applying a first coating composition and a second coating composition to a substrate, curing the applied compositions, and then applying and curing a clear coating composition. After applying the first coating composition, preheating may be performed before applying the second coating composition.

[0115] In another embodiment, the coated article is produced by successively applying a first coating composition, a second coating composition, and a clear coating composition wet-on-wet to a substrate, and then curing these coating compositions all at once. Preheating may be performed after applying the first coating composition and before applying the second coating composition, and after applying the second coating composition and before applying the clear coating composition.

[0116] Examples of the coating method include air spray coating, airless spray coating, electrostatic spray coating, multi-stage coating (preferably two-stage coating) using air electrostatic spray coating, and coating that combines air electrostatic spray coating with a rotary atomization type electrostatic coater.

[0117] The curing of each coating composition is carried out, for example, at a heating temperature of 80° C. to 180° C. (preferably 100° C. to 160° C.) for a heating time of 5 to 60 minutes (preferably 10 to 30 minutes).

[0118] The present invention will be described in more detail with reference to the following examples, but is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0119] The number average molecular weight was measured using a GPC apparatus with a trade name of "HLC8220GPC" (manufactured by Tosoh Corporation) and four columns with trade names of "Shodex F-606M" and "Shodex KF-603" (both manufactured by Showa Denko K.K.), under the conditions of a mobile phase of tetrahydrofuran, a measurement temperature of 40°C, a flow rate of 0.6 cc / min, and a detector of RI.

[0120] The phosphate value is the number of milligrams of potassium hydroxide (KOH) required for neutralization, calculated based on the amount of phosphate group-containing components such as phosphate esters used in the preparation of the phosphate group-containing polymer. The acid value and hydroxyl value were calculated from the monomer composition used in the preparation, based on the JIS regulations.

[0121] [Production Example 1] Production of acrylic resin emulsion 633 parts of deionized water was added to a reaction vessel, and the temperature was raised to 80°C while mixing and stirring in a nitrogen stream. Separately, 75.65 parts of styrene (ST), 178.96 parts of methyl methacrylate (MMA), 75.94 parts of n-butyl acrylate (BA), 64.45 parts of 2-ethylhexyl acrylate (2-EHA), and 105.0 parts of hydroxyethyl methacrylate (HEMA) were mixed to prepare a first-stage monomer mixture. Next, this monomer mixture was mixed with 25.0 parts of Aqualon HS-10 (polyoxyethylene alkylpropenyl phenyl ether sulfate, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), 25.0 parts of Adeka Reasoap NE-20 (α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxyoxyethylene, manufactured by Asahi Denka Co., Ltd.), and 400 parts of deionized water to prepare a monomer emulsion. Separately, an initiator solution consisting of 1.2 parts of ammonium persulfate and 500 parts of deionized water was prepared. The monomer emulsion and the initiator solution were added dropwise in parallel to the reaction vessel over 1.5 hours. After completion of the dropwise addition, the mixture was aged at the same temperature for 1 hour.

[0122] Separately, a second-stage monomer mixture was prepared by mixing 53.65 parts of styrene (ST), 178.96 parts of methyl methacrylate (MMA), 75.94 parts of n-butyl acrylate (BA), 64.45 parts of 2-ethylhexyl acrylate (2-EHA), 105.0 parts of hydroxyethyl methacrylate (HEMA), and 22 parts of acrylic acid. This monomer mixture was then mixed with 10 parts of Aqualon HS-10 and 250 parts of deionized water to prepare a monomer emulsion. Separately, an initiator solution consisting of 3.0 parts of ammonium persulfate and 500 parts of deionized water was prepared. The monomer emulsion and initiator solution were added dropwise to the reaction vessel over 1.5 hours. After the completion of the dropwise addition, the mixture was aged at the same temperature for 2 hours.

[0123] The reaction mixture was then cooled to 40°C and filtered through a 400-mesh filter. Finally, 100 parts of deionized water and 1.6 parts of dimethylaminoethanol were added to the reaction mixture to adjust the pH to 6.5. In this way, an acrylic resin emulsion having an average particle size of 150 nm, a solid content concentration of 35%, a solid content acid value of 20 mgKOH / g, and a hydroxyl value of 100 mgKOH / g was obtained.

[0124] [Production Example 2] Production of Phosphate Group-Containing Polymer 40 parts of ethoxypropanol were charged into a 1-liter reaction vessel equipped with a stirrer, temperature controller, and condenser. Separately, 20 parts of Phosmer PP (acid phosphooxyhexa(oxypropylene) monomethacrylate, manufactured by Unichemical Co., Ltd.) were dissolved in 20 parts of ethoxypropanol to prepare a solution. 40 parts of this solution, 4 parts of styrene, 35.96 parts of n-butyl acrylate, 18.45 parts of ethylhexyl methacrylate, 13.92 parts of 2-hydroxyethyl methacrylate, 7.67 parts of methacrylic acid, and 1.7 parts of azobisisobutyronitrile were mixed to prepare a monomer solution. 121.7 parts of the monomer solution were added dropwise to the reaction vessel at 120°C over 3 hours. The mixture was stirred for an additional hour to obtain a phosphate group-containing polymer. The phosphate group-containing polymer thus obtained had an acid value of 105 mgKOH / g, a phosphate group value of 55 mgKOH / g, a hydroxyl group value of 60 mgKOH / g, a number average molecular weight of 6,000, and a solids concentration of 63%.

[0125] [Production Example 3] Production of Water-Soluble Acrylic Resin 23.89 parts of tripropylene glycol methyl ether and 16.11 parts of propylene glycol methyl ether were added to a reaction vessel, and the temperature was raised to 105°C while mixing and stirring in a nitrogen stream. Next, a monomer mixture containing 13.1 parts of methyl methacrylate, 68.4 parts of ethyl acrylate, 11.6 parts of 2-hydroxyethyl methacrylate, and 6.9 parts of methacrylic acid was prepared, and an initiator solution consisting of 100 parts of this monomer mixture, 10.0 parts of tripropylene glycol methyl ether, and 1 part of tert-butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel in parallel over 3 hours. After completion of the dropwise addition, the mixture was aged at the same temperature for 0.5 hours.

[0126] Further, an initiator solution consisting of 5.0 parts of tripropylene glycol methyl ether and 0.3 parts of tertiary butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel over 0.5 hours. After the completion of the addition, the mixture was aged at the same temperature for 2 hours.

[0127] Using a solvent remover, 16.1 parts of the solvent was distilled off under reduced pressure (70 torr) at 110°C, and then 204 parts of deionized water and 7.1 parts of dimethylaminoethanol were added to obtain a water-soluble acrylic resin solution. The resulting water-soluble acrylic resin solution had a solids concentration of 30%, a solids acid value of 40 mgKOH / g, a hydroxyl value of 50 mgKOH / g, and a viscosity of 140 poise (E-type viscometer, 1 rpm, 25°C).

[0128] [Example 1] (1) Preparation of first coating composition (1-1) Preparation of color pigment dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 11.7 parts of a color pigment (perylene red, trade name: PALIOGEN RED L-3875, manufactured by BASF Corporation), 14.0 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 34.9 parts of ion-exchanged water, and 0.5 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Subsequently, using a disperser filled with 0.05 mm zirconia beads at a volume filling rate of 70%, this mixture was dispersed to obtain a color pigment dispersion.

[0129] (1-2) Preparation of first coating composition 122.1 parts of the acrylic resin emulsion of Production Example 1, 2.0 parts of dimethylaminoethanol, 28.4 parts of melamine resin (trade name: Cymel 370N, mixed alkylated melamine resin, manufactured by Allnex, solids content 90%), 109.3 parts of the above colored pigment dispersion, 18.9 parts of aluminum paste (trade name: WL-Z440, pulverized scaly aluminum pigment, average particle size 14 μm, manufactured by Toyo Aluminum Co., Ltd., active ingredient 66%) per 100 parts of resin solids, 5 parts of the phosphate group-containing polymer of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of a surfactant (trade name: Noigen EA-207D, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., number average molecular weight 4200, solids content 55%) (3 parts in terms of solids), 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion to adjust the pH to 8.1, and the dispersion was diluted with deionized water to obtain a water-based first coating composition with a resin solids concentration of 33%.

[0130] (2) Preparation of second coating composition (2-1) Preparation of color pigment dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 11.7 parts of a color pigment (perylene red, trade name: PALIOGEN RED L-3875, manufactured by BASF Corporation), 14.0 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 34.9 parts of ion-exchanged water, and 0.5 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Subsequently, this mixture was dispersed using a disperser filled with 0.05 mm zirconia beads at a volume filling rate of 70%, to obtain a color pigment dispersion.

[0131] (2-2) Preparation of the second coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 28.4 parts of melamine resin (trade name: Cymel 370N), 34.8 parts of the above color pigment dispersion, 50 parts of butyl cellosolve, 5.5 parts of surfactant (trade name: Noigen EA-207D) (3 parts in terms of solids), 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion to make the pH 8.1, and the mixture was diluted with deionized water to prepare an aqueous second coating composition with a resin solids concentration of 15%.

[0132] (3) Preparation of clear coating composition A clear coating composition was prepared by adding 1.6 parts of a matting agent (silica, polyethylene wax-treated silica, trade name: ACEMATT OK520, manufactured by Evonik Degussa Japan, D50: 6.5 μm, oil absorption 300 mL / 100 g) to 100 parts of resin solids of an acid epoxy curing clear coating (trade name: MACFLOW-O-1810 CLEAR, manufactured by Nippon Paint Automotive Coatings Co., Ltd.) and mixing with a stirrer.

[0133] (4) Formation of Multilayer Coating Films A zinc phosphate-treated dull steel plate, 0.8 mm thick, 30 cm long, and 40 cm wide, was electrodeposited with the cationic electrodeposition coating composition "Power Top U-50" (manufactured by Nippon Paint Automotive Coatings) to a dry film thickness of 20 μm, and baked at 160°C for 30 minutes. The resulting coated plate was air-sprayed with the intermediate coating composition "OP-30P Middle Gray" (manufactured by Nippon Paint Automotive Coatings, polyester-melamine paint, pre-diluted to 25 seconds (measured at 20°C using a No. 4 Ford cup)) using an Anest Iwata air spray gun W-101-132G to a dry film thickness of 35 μm, and then heated at 140°C for 30 minutes. In this way, a coated object having an electrodeposition coating film and an intermediate coating film was obtained.

[0134] The first coating composition was air spray coated on the substrate to a dry film thickness of 10 μm at room temperature of 23 ° C. and humidity of 68%. After setting for 4 minutes, the substrate was preheated at 80 ° C. for 5 minutes. Subsequently, the second coating composition was air spray coated wet-on-wet to a dry film thickness of 10 μm at room temperature of 23 ° C. and humidity of 68%. After setting for 4 minutes, the substrate was preheated at 80 ° C. for 5 minutes. The coated plate was allowed to cool to room temperature, and the clear coating composition was air spray coated to a dry film thickness of 35 μm and set for 7 minutes. Finally, the coated plate was heated in a dryer at 140 ° C. for 30 minutes to obtain a coated article having a multi-layer coating film.

[0135] [Example 2] A clear coating composition was prepared in the same manner as in Example 1, except that the amount of silica as a matting agent was changed to 3.2 parts. A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0136] [Example 3] A clear coating composition was prepared in the same manner as in Example 1, except that the amount of silica used as a matting agent was changed to 4.8 parts. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0137] Example 4 A second coating composition was prepared in the same manner as in Example 1, except that 0.4 parts of a colored pearl pigment (Xirallic NXT M260-30 SW Leonis Gold: manufactured by MERCK) was further mixed in the second coating composition. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0138] [Example 5] A first coating composition was prepared in the same manner as in Example 1, except that no color pigment dispersion was mixed in the preparation of the first coating composition. A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that this first coating composition was used.

[0139] Example 6 A clear coating composition was prepared by mixing 3.2 parts of a matting agent (product name: ACEMATT OK520) with 100 parts of the resin solids of a urethane-curing clear coating (trade name: PU Excel O-2100, manufactured by Nippon Paint Automotive Coatings Co., Ltd., two-component type). A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0140] Comparative Example 1 A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that no matting agent was added and Macflow-O-1810 Clear was used as the clear coating composition.

[0141] [Comparative Example 2] A clear coating composition was prepared in the same manner as in Example 1, except that the amount of silica as a matting agent was changed to 6.4 parts. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this clear coating composition was used.

[0142] Comparative Example 3 A second coating composition was prepared in the same manner as in Example 1, using a mixture of 7.0 parts of a color pigment (trade name: PALIOGEN RED L-3875), 8.4 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 20.9 parts of ion-exchanged water, and 0.3 parts of an antifoaming agent (trade name: BYK-011) as a color pigment dispersion. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0143] Comparative Example 4 A second coating composition was prepared in the same manner as in Example 1, using a mixture of 37.4 parts of a color pigment (trade name: PALIOGEN RED L-3875), 44.8 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 111.7 parts of ion-exchanged water, and 1.6 parts of an antifoaming agent (trade name: BYK-011) as a color pigment dispersion. A multilayer coating film and a coated article were obtained in the same manner as in Example 1, except that this second coating composition was used.

[0144] Comparative Example 5 A multi-layer coating film and a coated article were obtained in the same manner as in Example 1, except that the first coating composition was not applied.

[0145] [Comparative Example 6] (1) Preparation of Coating Composition (1-1) Preparation of Colored Pigment Dispersion 38.9 parts of the water-soluble acrylic resin solution of Production Example 3, 21.1 parts of a colored pigment (trade name: PALIOGEN RED L-3875), 25.2 parts of a pigment dispersant (trade name: DISPEX ULTRA PA 4550AN), 62.8 parts of ion-exchanged water, and 0.9 parts of an antifoaming agent (trade name: BYK-011) were mixed with a stirrer. Subsequently, this mixture was dispersed using a disperser filled with 0.05 mm zirconia beads at a volume filling rate of 70%, to obtain a colored pigment dispersion.

[0146] (1-2) Preparation of coating composition 143.3 parts of the acrylic resin emulsion of Production Example 1, 1.4 parts of dimethylaminoethanol, 28.4 parts of melamine resin (trade name: Cymel 370N), 1.6 parts of pearl pigment (trade name: XIRALLIC F60-51WNT RADIANT RED, manufactured by MERCK Corporation), 34.8 parts of the above colored pigment dispersion, 3.9 parts of colored aluminum pigment (trade name: F120-58CWT Wahiva Orange, manufactured by MERCK Corporation) per 100 parts of resin solids, 5 parts of the phosphate group-containing polymer of Production Example 2, 0.4 parts of lauryl acid phosphate, 50 parts of butyl cellosolve, 5.5 parts of a surfactant (trade name: Noigen EA-207D) (3 parts in terms of solids), and 3 parts of linoleic acid (manufactured by Kishida Chemical Co., Ltd.) were uniformly dispersed. Dimethylaminoethanol was added to this dispersion to adjust the pH to 8.1, and the dispersion was diluted with deionized water to obtain a coating composition with a resin solids concentration of 33%.

[0147] (2) Formation of multilayer coating film The above coating composition was air spray coated onto a substrate obtained in the same manner as in Example 1 at a room temperature of 23°C and a humidity of 68% to a dry film thickness of 4 μm. After setting for 4 minutes, the coating was preheated at 80°C for 5 minutes. Next, the coated plate was allowed to cool to room temperature, and MACFLOW-O-1810 Clear was applied as a clear coating composition by air spray coating to a dry film thickness of 35 μm, and the coating was allowed to set for 7 minutes. Finally, the coated plate was heated in a dryer at 140°C for 30 minutes to obtain a multilayer coating film and a coated article.

[0148] [Evaluation] The multi-layer coating film, the single first coating film, or the single second coating film obtained in the Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in the table below.

[0149] (Preparation of a Single First Coating Film) The first coating composition was spray-coated onto a substrate obtained in the same manner as in Example 1 so that the dry coating film would be 10 μm thick, and the coating was then heat-cured for 20 minutes at 140° C. This resulted in a cured coating film (single first coating film) of the first coating composition applied to the substrate.

[0150] (Preparation of independent second coating film) The above second coating composition was spray-coated onto a polypropylene plate to a dry film thickness of 10 μm, and then heat-cured for 20 minutes at 140° C. The coating film was then peeled off from the polypropylene plate to obtain a film-like second coating film (independent second coating film).

[0151] (1) Spectral Reflectance The spectral reflectance was measured using a spectrophotometer (BYK-mac i, manufactured by BYK Gardner) in the range of 400 to 700 nm in wavelength scan mode at a sampling interval of 10 nm.

[0152] (2) Saturation: Measured using a spectrophotometer (BYK-mac i, manufactured by BYK Gardner).

[0153] (3) Light transmittance The light transmittance was measured using a spectrophotometer (Hitachi, product name: U-4100) in the range of 400 to 700 nm under the conditions of wavelength scan mode, scan speed of 300 nm / min, and sampling interval of 0.5 nm. The average light transmittance was obtained by averaging the light transmittance every 10 nm.

[0154] (4) 60 Degree Specular Glossiness Using a glossmeter (manufactured by BYK Gardner, AG-4446), the 60 degree specular glossiness was measured in accordance with JIS Z 8741 Specular Glossiness-Measuring Method.

[0155] (5) Color Vividness The multilayer coating film was viewed from an incident angle of 45° and an acceptance angle of about 15°, and evaluated based on the following criteria.

[0156] Evaluation criteria A: A vivid and deep red color is perceived. B: A slightly less vivid but deep red color is perceived. C: A dull red color is perceived.

[0157] (6) Brilliance The multilayer coating film was viewed from an incident angle of 45° and a receiving angle of about 15°, and evaluated based on the following criteria.

[0158] Evaluation criteria A: A soft, veiled sparkle is felt. B: A soft sparkle is felt, though it is slightly inferior to A. C: A cloudy feeling is felt, or a strong sparkle is felt.

[0159]

[0160] The present disclosure includes the following aspects: [1] A multi-layer coating film comprising a first coating film, a second coating film, and a clear coating film in this order, wherein the first coating film contains a scale-like luster pigment, the second coating film contains a color pigment, and the clear coating film contains a matting agent, and an L refractometer based on the spectral reflectance of light reflected at an angle of 15 degrees relative to incident light incident at an angle of 45 degrees to the surface of the multi-layer coating film. * C * Chroma C in the h color system * 15is 83 or more, and the 60-degree specular gloss of the multilayer coating film is 55 to 90. [2] The multilayer coating film of [1] above, wherein the average light transmittance of the second coating film at wavelengths of 400 to 700 nm is 25 to 45%. [3] The multilayer coating film of [1] or [2] above, wherein the content of the matting agent in the clear coating film is 0.5 to 6 parts by mass per 100 parts by mass of resin solids. [4] The multilayer coating film of any of [1] to [3] above, wherein the spectral reflectance of light incident on the surface of the first coating film at an angle of 45 degrees and reflected at an angle of 15 degrees relative to the specularly reflected light is 25 to 215% at wavelengths of 400 to 580 nm, and 95 to 220% at wavelengths of 650 to 700 nm. [5] A multilayer coating film according to any one of [1] to [4] above, wherein the first coating film further contains a coloring pigment. [6] A multilayer coating film according to any one of [1] to [5] above, wherein the light transmittance of the second coating film is 2% or more and 40% or less at a wavelength of 400 to 580 nm, and 85% or more and 100% or less at a wavelength of 650 to 700 nm. [7] A coated article comprising a substrate, and a multilayer coating film according to any one of [1] to [6] above, provided on the substrate. [8] A coated article comprising a first coating composition, a second coating composition, and a clear coating composition applied sequentially to the substrate to form a multilayer coating film, wherein the first coating composition contains a scaly luster pigment, the second coating composition contains a coloring pigment, and the clear coating film contains a matting agent, and wherein the L * C * Chroma C in the h color system * 15 is 83 or more, and the 60-degree specular gloss of the multi-layer coating film is 55 or more and 90 or less.

[0161] The multilayer coating film of the present disclosure has high saturation in the highlight region and a soft, radiant feel, making it possible to impart new designs to a variety of substrates.

[0162] This application claims priority based on Japanese Patent Application No. 2023-067692, filed on April 18, 2023, the entire contents of which are incorporated herein by reference.

Claims

1. A multi-layer coating film comprising a first coating film, a second coating film and a clear coating film in this order, wherein the first coating film contains a scale-like photoluminescent pigment, the second coating film contains a coloring pigment, and the clear coating film contains a matting agent, and the L is determined based on the spectral reflectance of reflected light received at an angle of 15 degrees to the regular reflected light when incident light is incident on the surface of the multi-layer coating film at an angle of 45 degrees. * C * Saturation C in the h color system * 15 is 83 or more, and the 60 degree specular gloss of the multilayer coating film is 55 or more and 90 or less.

2. The multi-layer coating film according to claim 1, wherein the average light transmittance of the second coating film in the wavelength range of 400 to 700 nm is 25% or more and 45% or less.

3. A multi-layer coating film according to claim 1 or 2, wherein the content of the matting agent in the clear coating film is 0.5 parts by mass or more and 6 parts by mass or less per 100 parts by mass of resin solids.

4. A multi-layer coating film according to any one of claims 1 to 3, wherein the spectral reflectance of light reflected at an angle of 15 degrees from the specular reflected light of incident light incident at an angle of 45 degrees on the surface of the first coating film is 25% or more and 215% or less in the wavelength range of 400 to 580 nm, and 95% or more and 220% or less in the wavelength range of 650 to 700 nm.

5. A multi-layer coating film according to any one of claims 1 to 4, wherein the first coating film further contains a coloring pigment.

6. A multi-layer coating film according to any one of claims 1 to 5, wherein the light transmittance of the second coating film is 2% or more and 40% or less at a wavelength of 400 to 580 nm, and 85% or more and 100% or less at a wavelength of 650 to 700 nm.

7. A coated article comprising: a substrate; and the multilayer coating film according to any one of claims 1 to 6 provided on the substrate.

8. A method for producing a multi-layer coating film by successively coating a first coating composition, a second coating composition and a clear coating composition on a substrate, the first coating composition containing a scale-like luster pigment, the second coating composition containing a coloring pigment, and the clear coating composition containing a matting agent, the L based on the spectral reflectance of reflected light received at an angle of 15 degrees to the regular reflected light of incident light incident at an angle of 45 degrees to the surface of the multi-layer coating film. * C * Saturation C in the h color system * 15 is 83 or more, and the 60 degree specular gloss of the multilayer coating film is 55 or more and 90 or less.

Citation Information

Patent Citations

  • Colored and clear coated metal board

    JP2005087954A

  • Method for forming luster multi-layer coating and coated article

    JP2006289247A

  • Coating composition and method for forming coating film

    JP2012041508A

  • Coating composition and coated film forming method

    JP2016089003A

  • Method for forming multilayer coating film