Semiconductor device and method for manufacturing semiconductor device

The semiconductor device addresses breakdown voltage issues by using plasma-nitrided AlN and SiON layers to enhance moisture resistance and prevent corrosion, improving reliability under harsh conditions without increasing film thickness or processing complexity.

WO2024219079A1PCT designated stage expired Publication Date: 2024-10-24MINEBEA POWER SEMICON DEVICE INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006265
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-02-21
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Power semiconductor chips face breakdown voltage deterioration due to electric field concentration at the chip termination, and existing solutions like silicon nitride passivation films are prone to cracking under thermal stress, reducing high temperature and high humidity bias test resistance.

Method used

A semiconductor device with a field plate electrode and interlayer insulating film featuring an AlN-based modified layer and a SiON-based modified layer, respectively, formed through plasma nitriding, which enhances moisture resistance and prevents corrosion without increasing film thickness or requiring additional processing steps.

Benefits of technology

The solution effectively suppresses film stress-induced cracking and improves high temperature and high humidity bias test resistance by maintaining moisture barrier functionality while simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006265_24102024_PF_FP_ABST
    Figure JP2024006265_24102024_PF_FP_ABST
Patent Text Reader

Abstract

An IGBT chip (1) comprises: a n-type semiconductor substrate (6); a p-type diffusion layer (8) that is partially formed on a surface portion of the n-type semiconductor substrate (6); an interlayer insulating film (9) that is in contact with the n-type semiconductor substrate (6) and the p-type diffusion layer (8); and a field plate electrode (12) that is in contact with the p-type diffusion layer (8) and the interlayer insulating film (9), wherein the field plate electrode (12) has on the surface thereof an AlN-based modified layer (21) comprising an inorganic film that contains a nitride, and the interlayer insulating film (9) has on the surface thereof a SiON-based modified layer (22) comprising an inorganic film that contains a nitride.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and method for manufacturing the same

[0001] The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device.

[0002] One of the causes of breakdown voltage degradation in power semiconductor chips is electric field concentration at the chip termination. When a junction is formed on the surface of a power semiconductor chip, a depletion layer spreads in a fan-shaped manner at the termination when a reverse bias is applied. The electric field lines of the charges in the fan-shaped region gather at the chip termination, resulting in so-called electric field concentration. As a result, avalanche breakdown (dielectric breakdown) occurs at a voltage significantly lower than the theoretical breakdown voltage. To mitigate electric field concentration at the chip termination, it is necessary to disperse the electric field lines from the charges in the depletion layer region that spread in a fan-shaped manner when a reverse bias is applied from the chip termination to the entire termination structure (hereinafter also referred to as the termination region).

[0003] Power semiconductors are used in a variety of harsh environments, so they must satisfy multiple reliability criteria. One of the required reliability criteria is resistance to high-temperature, high-humidity bias testing (H3TRB), in which a constant voltage is continuously applied in a high-temperature, high-humidity environment. It is known that in power semiconductors with a field plate structure formed with Al electrodes, moisture in a high-temperature, high-humidity environment corrodes the Al electrodes, causing an increase in leakage current and a deterioration in breakdown voltage.

[0004] Patent Document 1 describes a semiconductor device including a semiconductor portion, a termination insulating film, a first protective film, a second electrode, a termination electrode, a first insulating film, and a second protective film. The semiconductor device described in Patent Document 1 also describes that a passivation region made of an inorganic film that prevents moisture from penetrating is formed on the Al electrode.

[0005] Japanese Patent Application Laid-Open No. 2022-047410

[0006] Silicon nitride films, which have excellent moisture resistance, are often used for the passivation film that forms the passivation region. However, silicon nitride films have high stress, and depending on the film thickness, there is a risk of cracking due to thermal stress caused by heat treatment in the process after passivation film formation or stress during mounting. If cracks occur, the moisture-proof function is lost, leading to a decrease in H3TRB resistance. Furthermore, the passivation film must be removed from the active region located on the main surface of the semiconductor substrate. This requires a processing step for passivation film removal, which increases the number of processes.

[0007] The present invention has been made in view of the above circumstances, and has as its object to provide a semiconductor device that can prevent the occurrence of cracks due to film stress and improve resistance to high-temperature, high-humidity bias tests.

[0008] In order to solve the above problem, the semiconductor device of the present invention comprises a first semiconductor layer of a first conductivity type, a second semiconductor layer of a second conductivity type partially formed on a surface portion of the first semiconductor layer, an interlayer insulating film in contact with the first semiconductor layer and the second semiconductor layer, and a field plate electrode in contact with the second semiconductor layer and the interlayer insulating film, wherein the field plate electrode has a first modified layer on its surface made of an inorganic film containing a nitride, and the interlayer insulating film has a second modified layer on its surface made of an inorganic film containing the nitride.

[0009] According to the present invention, it is possible to prevent the occurrence of cracks due to film stress and improve resistance to high-temperature, high-humidity bias testing.

[0010] 3B. A cross-sectional view of the manufacturing process after the formation of the surface electrode of the semiconductor device according to the first embodiment of the present invention. FIG. 4B is a cross-sectional view of the manufacturing process after the formation of the surface electrode of the semiconductor device according to the first embodiment of the present invention. FIG. 5C is a cross-sectional view of the manufacturing process after the formation of the surface electrode of the semiconductor device according to the first embodiment of the present invention. FIG. 6C is a cross-sectional view of the manufacturing process after the removal of the modified layer in the active region of the semiconductor device according to the second embodiment of the present invention. FIG. 6D is a cross-sectional view of the manufacturing process after the formation of the surface electrode of the semiconductor device according to the first embodiment of the present invention. FIG. 6A is a cross-sectional view of the manufacturing process after the formation of the surface electrode of the semiconductor device according to the first embodiment of the present invention. FIG. 6B is a cross-sectional view of the manufacturing process after the formation of the organic protective film of the semiconductor device according to the first embodiment of the present invention. FIG. 6C is a cross-sectional view of the manufacturing process after the removal of the modified layer in the active region of the semiconductor device according to the second embodiment of the present invention. FIG. 6D is a cross-sectional view of the manufacturing process after the formation of the organic protective film of the semiconductor device according to the first embodiment of the present invention.

[0011] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the same components in each drawing are designated by the same reference numerals, and detailed descriptions of overlapping parts will be omitted. (First Embodiment) FIGS. 1 and 2 are diagrams showing the configuration of a semiconductor device according to a first embodiment of the present invention. FIG. 1 is a plan view showing the appearance of the semiconductor device of this embodiment, and FIG. 2 is a cross-sectional view taken along the line A-A' in FIG. 1. In the following, an IGBT (Insulated Gate Bipolar Transistor) chip will be used as an example of a semiconductor device, but the present invention is not limited to this and can also be applied to diodes, thyristors, power MOSFETs, DMOSFETs (Double-Diffused MOSFETs), and the like. An example of application to a diode will be described later.

[0012] 1, an IGBT chip 1 (semiconductor device) includes an active region 5 disposed on the main surface of a semiconductor substrate, and a termination region 4 disposed so as to surround the periphery of the active region 5. An emitter electrode 2 and a gate electrode pad 3 are formed on the active region 5. The termination region 4 is a termination structure that relieves electric field concentration at the chip termination portion of the IGBT chip 1, i.e., an electric field relief region.

[0013] 2 , the termination region 4 includes, for example, a plurality of guard rings 7 (second semiconductor layers of a second conductivity type) formed on the main surface of an n− type semiconductor substrate 6 (first semiconductor layer of a first conductivity type), a p-type diffusion layer 8 (second semiconductor layer of a second conductivity type), an interlayer insulating film 9 formed on the main surface of the semiconductor substrate 6, a gate wiring 10 formed in the interlayer insulating film 9, a gate electrode 11 formed on the interlayer insulating film 9 and connected to the gate wiring 10 through an opening formed in the interlayer insulating film 9, a field plate electrode 12 formed on the interlayer insulating film 9 and connected to the guard ring 7 through an opening formed in the interlayer insulating film 9, an emitter electrode 2 formed on the interlayer insulating film 9 and connected to the p-type diffusion layer 8 through an opening formed in the interlayer insulating film 9, and an organic protective film 13 formed to cover the interlayer insulating film 9 and the Al electrodes (emitter electrode 2, gate electrode 11, and field plate electrode 12). The gate electrode 11 is electrically connected to the gate electrode pad 3 shown in FIG.

[0014] The IGBT chip 1 has an active section 31 which is an active region that conducts current, a gate finger section 32 which is a region having gate wiring 10 and gate electrode 11, and a termination section 33 which is a termination region that maintains a breakdown voltage. The gate finger section 32 has a well region (P-well) which is a diffusion layer and a gate electrode 11 electrically connected to the well region, and the termination region (termination section 33) has a well region (P-well) which is a diffusion layer and a field plate electrode 12 electrically connected to the well region.

[0015] The n-type semiconductor substrate 6 is a Si substrate. Alternatively, a SiC substrate or a GaN substrate may be used for the n-type semiconductor substrate 6. The guard ring 7 and the p-type diffusion layer 8 are p-type diffusion layers formed on the surface of the semiconductor substrate 6 by ion implantation. The interlayer insulating film 9 is made of a gate oxide film formed by pyrogenic oxidation or the like, which will be described later, and an interlayer film such as a TEOS (Tetra Ethoxy Silane) film or a BPSG (Boron-phospho silicate glass) film, both of which are silicon oxide films (SiO 2 )

[0016] The field plate electrode 12 is an electrode film made of a laminated film such as Ti / (in the following description, " / " indicates "or") TiN / Al or MoSi / Al, and is formed in the same layer as the emitter electrode 2 and gate electrode pad 3 (FIG. 1) in the active region (active portion 31).

[0017] The emitter electrode 2, the gate wiring 10, the gate electrode 11, and the field plate electrode 12 are made of Al electrodes (Al-based electrodes).

[0018] The surfaces of the emitter electrode 2, gate electrode 11, and field plate electrode 12 in the inactive region are such that the Al electrodes themselves are plasma-nitrided (for example, N 2 Plasma and NH 3 The emitter electrode 2, the gate electrode 11, and the field plate electrode 12 in the inactive region are subjected to a plasma nitriding treatment to form an AlN-based modified layer 21 (first modified layer). That is, the emitter electrode 2, the gate electrode 11, and the field plate electrode 12 in the inactive region have an AlN-based modified layer 21 formed on their surface by the plasma nitriding treatment. In this embodiment, plasma nitriding is used, but nitriding treatments other than plasma, such as thermal nitriding, ion nitriding, and radical nitriding, may also be used.

[0019] The AlN-based modified layer 21 only modifies the surface of each electrode, so the film thickness of each electrode remains the same as before the plasma nitriding treatment.

[0020] When the AlN-based modified layer 21 is formed on the surfaces of the emitter electrode 2, gate electrode 11, and field plate electrode 12 by the above-mentioned plasma nitriding process, a SiON-based modified layer 22 (second modified layer) is also simultaneously formed on the surface of the interlayer insulating film between each electrode.

[0021] That is, in a single plasma nitriding process, an AlN-based modified layer 21 is formed on the surfaces of the emitter electrode 2, gate electrode 11, and field plate electrode 12, and a SiON-based modified layer 22 is formed on the surface of the interlayer insulating film 9 between each electrode.

[0022] For example, a polyimide film is used as the organic protective film 13. On the back surface of the semiconductor substrate 6, an n-type buffer layer 14, a p-type collector layer 15, and a collector electrode 16 are formed in this order from the substrate side.

[0023] The operation of the IGBT chip 1 configured as described above will now be described. [Operation of IGBT Chip 1] When a voltage is applied between the gate electrode 11 and the emitter electrode 2 in the active region (active portion 31), an n-channel inversion layer is formed directly below the gate oxide film of the gate wiring 10, and the MOSFET portion turns ON. When a voltage is applied between the collector electrode 16 and the emitter electrode 2, an avalanche of holes occurs from the collector electrode 16 toward the emitter electrode 2, current flows between the collector electrode 16 and the emitter electrode 2, and the IGBT turns ON. When the voltage between the gate electrode 11 and the emitter electrode 2 is returned to 0 (zero), the inversion layer disappears, the n-channel of the MOSFET portion is cut off, and the IGBT turns OFF.

[0024] [Method of Manufacturing IGBT Chip 1] Figures 3A to 3E are cross-sectional views showing the manufacturing process of the IGBT chip 1. Figure 3A is a cross-sectional view of the manufacturing process before forming a surface electrode, Figure 3B is a cross-sectional view of the manufacturing process after forming a surface electrode, Figure 3C is a cross-sectional view of the manufacturing process after plasma nitriding treatment, Figure 3D is a cross-sectional view of the manufacturing process after forming an organic protective film, and Figure 3E is a cross-sectional view of the manufacturing process after removing a modified layer in the active region. Note that each figure mainly shows a cross section of the manufacturing process of the termination region (termination portion 33).

[0025] First, dry oxygen (O 2Dry oxidation using oxygen (O 2 ) and hydrogen gas (H 2 ) by selective oxidation using wet oxidation (pyrogenic oxidation) using water vapor due to a combustion reaction of 2 ) (not shown) is formed on the gate oxide film using a low-pressure CVD apparatus or the like. A polysilicon film (Poly-Si) (not shown) is then formed on the gate oxide film using photolithography patterning and etching to form a gate electrode (reference numeral 11 in FIG. 2). Next, p-type impurities such as boron (B) are implanted into the main surface of the semiconductor substrate 6 by ion implantation to form p-type diffusion layers 7 and 8. This p-type diffusion layer 7 functions as a guard ring (reference numeral 7 in FIG. 2).

[0026] Next, as shown in FIG. 3A, an interlayer insulating film (SiO 2 ) such as a TEOS film or a BPSG film is formed on the main surface of the semiconductor substrate 6 by using a plasma CVD apparatus, an atmospheric pressure CVD apparatus, or the like so as to cover the gate oxide film (not shown) and the gate wiring 10. 2 ) 9 is formed. Thereafter, by patterning and etching using photolithography, an opening (contact hole) 17 is formed in the interlayer insulating film 9, penetrating through to the p-type diffusion layer 8 and the guard ring 7. At this time, the opening (contact hole) 17 is also formed on the gate wiring 10.

[0027] 3B, an electrode film (not shown) made of, for example, Ti / TiN / Al or MoSi / Al is formed on the main surface of semiconductor substrate 6 using a plasma CVD apparatus, a sputtering apparatus, or the like so as to cover interlayer insulating film 9 and fill openings (contact holes) 17 formed in interlayer insulating film 9. Thereafter, emitter electrode 2, gate electrode 11, and field plate electrode 12 (FIG. 2) are formed by patterning and etching using photolithography.

[0028] 3C, a plasma nitriding process using N2 plasma or NH3 plasma is performed to form modified layers (AlN-based modified layer 21 and SiON-based modified layer 22) on the surfaces of the Al electrodes (emitter electrode 2, gate electrode 11, and field plate electrode 12) and interlayer insulating film 9. That is, by a single plasma nitriding process, AlN-based modified layer 21 is formed on the surfaces of emitter electrode 2, gate electrode 11, and field plate electrode 12, and SiON-based modified layer 22 is formed on the surface of interlayer insulating film 9 between the electrodes.

[0029] The AlN-based modified layer 21 only modifies the surface of each electrode, so the film thickness of each electrode remains the same as before the plasma nitriding treatment.

[0030] Next, as shown in FIG. 3D , an organic protective film (polyimide film) 13 is applied to the main surface of the semiconductor substrate 6 using a coating device so as to cover the emitter electrode 2 having the AlN-based modified layer 21, the gate electrode 11, and the field plate electrode 12.

[0031] Next, as shown in FIG. 3E, the AlN-based modified layer 21 on the surface of the emitter electrode 2 in the active region is removed by patterning and etching using photolithography.

[0032] Finally, in a back surface process, an n-type buffer layer 14, a p-type collector layer 15, and a collector electrode 16 are formed in this order from the substrate side on the back surface of the semiconductor substrate 6. Through the manufacturing processes described above, the termination structure shown in FIG.

[0033] As described above, the IGBT chip 1 (semiconductor device) (FIGS. 1 and 2) of this embodiment includes an n-type semiconductor substrate 6 (first semiconductor layer of a first conductivity type), a p-type diffusion layer 8 (second semiconductor layer of a second conductivity type) partially formed on a surface portion of the n-type semiconductor substrate 6, an interlayer insulating film 9 in contact with the n-type semiconductor substrate 6 and the p-type diffusion layer 8, and a field plate electrode 12 in contact with the p-type diffusion layer 8 and the interlayer insulating film 9, and the field plate electrode 12 has, on its surface, an AlN-based modified layer 21 (first modified layer) made of an inorganic film formed by plasma nitriding, and the interlayer insulating film 9 has, on its surface, a SiON-based modified layer 22 (second modified layer) made of an inorganic film formed by nitriding (for example, plasma nitriding).

[0034] Furthermore, the manufacturing method of the IGBT chip 1 (FIGS. 3A to 3E) includes the steps of partially forming a p-type diffusion layer 8 (a second semiconductor layer of a second conductivity type) on the surface portion of an n-type semiconductor substrate 6 (a first semiconductor layer of a first conductivity type), forming an interlayer insulating film 9 in contact with the n-type semiconductor substrate 6 and the p-type diffusion layer 8, forming a field plate electrode 12 in contact with the p-type diffusion layer 8 and the interlayer insulating film 9, and nitriding (e.g., plasma nitriding) the field plate electrode 12 and the interlayer insulating film 9 to form modified layers containing nitride on the surface (AlN-based modified layer 21, SiON-based modified layer 22).

[0035] After the field plate electrode 12 is formed in this way, the Al electrodes (the emitter electrode 2, the gate electrode 11, and the field plate electrode 12) themselves are subjected to plasma nitriding (for example, N 2 Plasma and NH 3 By the plasma nitriding process, an AlN-based modified layer 21 is formed on the surfaces of the emitter electrode 2, the gate electrode 11, and the field plate electrode 12, and at the same time, a SiON-based modified layer 22 is also formed on the surface of the interlayer insulating film 9 between the electrodes.

[0036] The AlN-based modified layer 21 of the IGBT chip 1 (FIGS. 1 and 2) of this embodiment improves the moisture resistance of the Al electrode surface, thereby preventing corrosion of the Al electrode and improving H3TRB resistance. Because the AlN-based modified layer 21 only modifies the surface of each Al electrode, the film thickness of each electrode remains the same as before the plasma nitriding treatment. This prevents cracks from occurring due to film stress.

[0037] In addition, the interlayer insulating film 9 is made of SiO 2 At the same time, the surface is nitrided to form a SiON layer, which makes it possible to prevent moisture from penetrating through the interlayer insulating film 9, and is expected to improve H3TRB resistance.

[0038] As described above, it is possible to prevent the occurrence of cracks due to film stress, reliably prevent moisture from penetrating from the surface side of the IGBT chip 1, and improve resistance to high-temperature, high-humidity bias tests.

[0039] Furthermore, the step of removing the passivation film is no longer necessary in the active region disposed on the main surface of the semiconductor substrate, thereby reducing the number of steps.

[0040] The IGBT chip 1 (FIGS. 1 and 2) of this embodiment includes an emitter electrode 2 in contact with a p-type diffusion layer 8 (second semiconductor layer) and an interlayer insulating film 9, and the emitter electrode 2 has an AlN-based modified layer 21 formed on its surface by plasma nitriding treatment.

[0041] By doing so, the AlN-based modified layer 21 (first modified layer) improves the moisture resistance of the surface of the emitter electrode 2, thereby preventing corrosion of the emitter electrode 2 and improving H3TRB resistance in the IGBT chip 1. In addition, the occurrence of cracks due to film stress in the emitter electrode 2 can be suppressed.

[0042] In the IGBT chip 1 (FIGS. 1 and 2) of this embodiment, the field plate electrode 12 is an aluminum-based electrode, and the AlN-based modified layer 21 is aluminum nitride obtained by modifying the aluminum-based electrode by plasma nitriding.

[0043] By doing so, the AlN-based modified layer 21 of the IGBT chip 1 improves the moisture resistance of the surface of the emitter electrode 2, thereby preventing corrosion of the emitter electrode 2 and improving H3TRB resistance.

[0044] In the IGBT chip 1 (FIGS. 1 and 2) of this embodiment, the SiON-based modified layer 22 (second modified layer) is silicon oxynitride.

[0045] By doing so, the SiON-based modified layer 22 of the IGBT chip 1 can also prevent moisture from penetrating through the interlayer insulating film 9, and the H3TRB resistance can be improved.

[0046] The IGBT chip 1 (FIGS. 1 and 2) of this embodiment comprises an active region (active portion 31) arranged on the main surface of the semiconductor substrate, and a termination region (termination portion 33) arranged on the main surface so as to surround the active region, and the termination region comprises a field plate electrode 12 and an interlayer insulating film 9.

[0047] By doing this, the IGBT chip 1 can realize a highly reliable semiconductor device that can improve the high-temperature, high-humidity bias resistance of the chip's termination structure (termination region) in a relatively simple manner while suppressing the impact on device characteristics.

[0048] In the IGBT chip 1 (FIGS. 1 and 2) of this embodiment, the AlN-based modified layer 21 (first modified layer) of the emitter electrode 2 in the active region arranged on the main surface of the semiconductor substrate is removed.

[0049] By doing so, the IGBT chip 1 can be electrically connected to the emitter electrode 2 by removing the AlN-based modified layer 21 of the emitter electrode 2 in the active region.

[0050] 4 and 5 are diagrams showing the configuration of a semiconductor device according to a second embodiment of the present invention. Fig. 4 is a plan view showing the appearance of the semiconductor device of this embodiment, and Fig. 5 is a cross-sectional view taken along line BB' in Fig. 4. This is an example in which the semiconductor device is applied to a diode.

[0051] 4, diode 50 (semiconductor device) includes an active region 55 disposed on the main surface of a semiconductor substrate, and a termination region 54 disposed so as to surround the periphery of active region 55. Termination region 54 is a termination structure that relieves electric field concentration at the chip termination portion of diode 50, i.e., an electric field relief region.

[0052] As shown in FIG. 4 , termination region 54 includes, for example, a plurality of guard rings 57 formed on the main surface of n-type semiconductor substrate 56, a P layer 58, an interlayer insulating film 59 formed on the main surface of semiconductor substrate 56, a field plate electrode 61 formed on interlayer insulating film 59 and connected to guard ring 57 through an opening formed in interlayer insulating film 59, an anode electrode 60 formed on interlayer insulating film 59 and connected to P layer 58 through an opening formed in interlayer insulating film 59, and an organic protective film 63 formed so as to cover interlayer insulating film 59 and Al electrodes (anode electrode 60, field plate electrode 61).

[0053] Diode 50 has an active portion 81, which is an active region that conducts current, and a termination portion 82, which is a termination region that maintains a breakdown voltage. The active region (active portion 81) has a P layer 58 and an anode electrode 60. The termination region (termination portion 82) has a well region (P-well), which is a diffusion layer, and a field plate electrode 61 electrically connected to the well region.

[0054] The n-type semiconductor substrate 56 is a Si substrate. Alternatively, a SiC substrate or a GaN substrate may be used for the n-type semiconductor substrate 56. The guard ring 57 is a p-type diffusion layer formed on the surface of the semiconductor substrate 56 by ion implantation. The P layer 58 is connected to an anode electrode 60 and serves as the anode of the diode 50. The interlayer insulating film 59 is made of a gate oxide film formed by pyrogenic oxidation or the like, and an interlayer film such as a TEOS film or a BPSG film, both of which are silicon oxide films (SiO 2 )

[0055] The field plate electrode 61 is an electrode film made of a laminated film such as Ti / TiN / Al or MoSi / Al, and is formed in the same layer as the anode electrode 60 in the active region (active section 81).

[0056] The anode electrode 60 and the field plate electrode 61 are made of Al electrodes (Al-based electrodes).

[0057] The surfaces of the anode electrode 60 and the field plate electrode 61 in the inactive region are formed by plasma nitriding (e.g., N 2 Plasma and NH 3 The anode electrode 60 and the field plate electrode 61 in the inactive region have the AlN-based modified layer 71 formed on their surface by plasma nitriding.

[0058] The AlN-based modified layer 71 only modifies the surface of each electrode, so the film thickness of each electrode remains the same as before the plasma nitriding treatment.

[0059] When the AlN-based modified layer 71 is formed on the surfaces of the anode electrode 60 and the field plate electrode 61 by the plasma nitriding treatment, a SiON-based modified layer 72 is also formed on the surface of the interlayer insulating film between the electrodes.

[0060] That is, in one plasma nitriding process, an AlN-based modified layer 71 is formed on the surfaces of the anode electrode 60 and the field plate electrode 61, and a SiON-based modified layer 72 is formed on the surface of the interlayer insulating film 59 between the electrodes.

[0061] The organic protective film 63 is made of, for example, a polyimide film. The back surface of the semiconductor substrate 6 is provided with an n-type buffer layer 64, an N-type buffer layer 65, and an N-type buffer layer 66 in this order from the substrate side. + A layer 65 and a cathode electrode 66 are formed.

[0062] A method for manufacturing the diode 50 configured as described above will be described below. Figures 6A to 6E are cross-sectional views showing the manufacturing process of the diode 50. Figure 6A is a cross-sectional view of the manufacturing process before the formation of the surface electrode, Figure 6B is a cross-sectional view of the manufacturing process after the formation of the surface electrode, Figure 6C is a cross-sectional view of the manufacturing process after the plasma nitriding treatment, Figure 6D is a cross-sectional view of the manufacturing process after the formation of the organic protective film, and Figure 6E is a cross-sectional view of the manufacturing process after the modified layer in the active region is removed. Note that each figure mainly shows a cross section of the manufacturing process of the termination region (termination portion 82).

[0063] First, dry oxygen (O 2 Dry oxidation using oxygen (O 2 ) and hydrogen gas (H2) by selective oxidation using wet oxidation (pyrogenic oxidation) using water vapor generated by the combustion reaction of hydrogen gas (H2) and a gate oxide film (SiO 2 ) (not shown) is formed on the gate oxide film using a low-pressure CVD apparatus or the like. A polysilicon film (Poly-Si) (not shown) is then formed on the gate oxide film using photolithography patterning and etching to form a gate electrode (reference numeral 11 in FIG. 2). Next, p-type impurities such as boron (B) are implanted into the main surface of the semiconductor substrate 56 by ion implantation to form a p-type diffusion layer 57 and a P layer 58. This p-type diffusion layer 57 functions as a guard ring (reference numeral 57 in FIG. 5). The P layer 58 becomes the anode of the diode 50.

[0064] Next, as shown in FIG. 6A, an interlayer insulating film (SiO 2 ) such as a TEOS film or a BPSG film is formed on the main surface of the semiconductor substrate 56 by using a plasma CVD apparatus or an atmospheric pressure CVD apparatus. 2 ) 59 is formed. Thereafter, an opening (contact hole) 67 is formed in the interlayer insulating film 9 so as to penetrate to the guard ring 57 by patterning and etching using photolithography.

[0065] 6B , an electrode film (not shown) made of, for example, Ti / TiN / Al or MoSi / Al is formed on the main surface of semiconductor substrate 56 using a plasma CVD apparatus, a sputtering apparatus, or the like so as to cover interlayer insulating film 59 and fill openings (contact holes) 67 formed in interlayer insulating film 59. Thereafter, anode electrode 60 and field plate electrode 61 ( FIG. 5 ) are formed by patterning and etching using photolithography.

[0066] 6C, plasma nitriding using N plasma or NH plasma is performed to form modified layers (AlN-based modified layer 71 and SiON-based modified layer 72) on the surfaces of the Al electrodes (anode electrode 60 and field plate electrode 61) and interlayer insulating film 9. That is, by a single plasma nitriding process, AlN-based modified layer 71 is formed on the surfaces of anode electrode 60 and field plate electrode 61, and SiON-based modified layer 72 is formed on the surface of interlayer insulating film 59 between the electrodes.

[0067] The AlN-based modified layer 71 only modifies the surface of each electrode, so the film thickness of each electrode remains the same as before the plasma nitriding treatment.

[0068] Next, as shown in FIG. 6D, an organic protective film (polyimide film) 63 is applied to the main surface of the semiconductor substrate 56 using a coating device so as to cover the anode electrode 60 having the AlN-based modified layer 71 and the field plate electrode 61.

[0069] Next, as shown in FIG. 6E, the AlN-based modified layer 71 on the surface of the anode electrode 60 in the active region is removed by patterning and etching using photolithography.

[0070] Finally, in a back surface process, an n-type buffer layer 64, an N + Then, a layer 65 and a cathode electrode 66 are formed. Through the manufacturing steps described above, the termination structure shown in FIG.

[0071] As described above, the diode 50 (semiconductor device) (FIGS. 4 and 5) of this embodiment includes an n-type semiconductor substrate 56 (a first semiconductor layer of a first conductivity type), a p-type diffusion layer 57 (a second semiconductor layer of a second conductivity type) partially formed on a surface portion of the n-type semiconductor substrate 56, an interlayer insulating film 59 in contact with the n-type semiconductor substrate 56 and the p-type diffusion layer 57, and a field plate electrode 61 in contact with the p-type diffusion layer 57 and the interlayer insulating film 59. The field plate electrode 61 has, on its surface, an AlN-based modified layer 71 (a first modified layer) made of an inorganic film (containing nitride) formed by nitriding (e.g., plasma nitriding), and the interlayer insulating film 59 has, on its surface, a SiON-based modified layer 72 (a second modified layer) made of an inorganic film (containing nitride) formed by nitriding (e.g., plasma nitriding).

[0072] The method for manufacturing the diode 50 ( FIGS. 6A to 6E ) includes the steps of partially forming a p-type diffusion layer 57 (a second semiconductor layer of a second conductivity type) on a surface portion of an n-type semiconductor substrate 56 (a first semiconductor layer of a first conductivity type), forming an interlayer insulating film 59 in contact with the n-type semiconductor substrate 56 and the p-type diffusion layer 57, forming a field plate electrode 61 in contact with the p-type diffusion layer 57 and the interlayer insulating film 59, and nitriding the field plate electrode 61 and the interlayer insulating film 59 (for example, plasma nitriding) to form modified layers (AlN-based modified layer 71, SiON-based modified layer 72) made of an inorganic film containing nitride on the surface.

[0073] By doing this, the diode 50 (Figures 4 and 5) of this embodiment, like the IGBT chip 1 (Figures 1 and 2) of the first embodiment, can prevent corrosion of the Al electrode by the AlN-based modified layer 71 improving the moisture resistance of the surface of the Al electrode, thereby improving H3TRB resistance.

[0074] The AlN-based modified layer 71 only modifies the surface of each Al electrode, so the film thickness of each electrode remains the same as before the plasma nitriding treatment, preventing cracks from occurring due to film stress.

[0075] The interlayer insulating film 59 is made of SiO 2At the same time, the surface is nitrided to form a SiON layer, which makes it possible to prevent moisture from penetrating through the interlayer insulating film 59, and is expected to improve H3TRB resistance.

[0076] As described above, it is possible to prevent the occurrence of cracks due to film stress, reliably prevent moisture from penetrating from the surface side of the diode 50, and improve resistance to high-temperature, high-humidity bias tests.

[0077] Furthermore, the step of removing the passivation film is no longer necessary in the active region disposed on the main surface of the semiconductor substrate, thereby reducing the number of steps.

[0078] The diode 50 (FIGS. 4 and 5) of this embodiment includes an anode electrode 60 in contact with a p-type diffusion layer 57 (second semiconductor layer) and an interlayer insulating film 59, and the anode electrode 60 has an AlN-based modified layer 71 formed on its surface by plasma nitriding.

[0079] In this way, the AlN-based modified layer 71 (first modified layer) of the diode 50 improves the moisture resistance of the surface of the emitter electrode 2, thereby preventing corrosion of the anode electrode 60 and improving H3TRB resistance. Also, the occurrence of cracks due to film stress in the anode electrode 60 can be suppressed.

[0080] In the diode 50 (FIGS. 4 and 5) of this embodiment, the AlN-based modified layer 71 (first modified layer) of the anode electrode 60 in the active region arranged on the main surface of the semiconductor substrate is removed.

[0081] In this way, the diode 50 can be electrically connected to the anode electrode 60 by removing the AlN-based modified layer 71 of the anode electrode 60 in the active region.

[0082] The present invention is particularly effective for high-voltage products that often have a structure in which guard rings 7, 57 and field plate electrodes 12, 61 are provided in the termination region as described above, but is not necessarily limited to this. It can also be applied to semiconductor chips that employ other termination structures that do not use guard rings 7, 57 or field plate electrodes 12, 61, and to relatively low-voltage products.

[0083] Furthermore, the present invention is not limited to the above-described embodiments and includes various modifications. For example, the above-described embodiments have been described in detail to facilitate understanding of the present invention, and the present invention is not necessarily limited to those including all of the described configurations. Furthermore, it is possible to replace part of the configuration of one embodiment with the configuration of another embodiment, or to add the configuration of another embodiment to the configuration of one embodiment. Furthermore, it is possible to add, delete, or replace part of the configuration of each embodiment with other configurations. For example, although IGBTs are used, this is not limiting and other types of elements can also be applied. Depending on the device, the names of the main terminals and sense terminals may be referred to as "drain" and "source" instead of the above-described "collector" and "emitter."

[0084] 1 IGBT chip (semiconductor device) 2 Emitter electrode 3 Gate electrode pad 6, 56 Semiconductor substrate (first semiconductor layer of first conductivity type) 7, 57 Guard ring 8 P-type diffusion layer (second semiconductor layer of second conductivity type) 9, 59 Interlayer insulating film 10 Gate wiring 11 Gate electrode 12, 61 Field plate electrode 13, 63 Organic protective film 14 N-type buffer layer 15 P-type collector layer 16 Collector electrode 21, 71 AlN-based modified layer (first modified layer) 22, 72 SiON-based modified layer (second modified layer) 31, 81 Active portion (active region) 32 Gate finger portion 33, 82 Termination portion (termination region) 50 Diode (semiconductor device) 58 P layer 64 N-type buffer layer 65 N + Layer 66: Cathode electrode

Claims

1. A semiconductor device comprising: a first semiconductor layer of a first conductivity type; a second semiconductor layer of a second conductivity type partially formed on a surface portion of the first semiconductor layer; an interlayer insulating film in contact with the first semiconductor layer and the second semiconductor layer; and a field plate electrode in contact with the second semiconductor layer and the interlayer insulating film, wherein the field plate electrode has a first modified layer on its surface made of an inorganic film containing nitride, and the interlayer insulating film has a second modified layer on its surface made of an inorganic film containing nitride.

2. The semiconductor device according to claim 1, further comprising an emitter electrode in contact with the second semiconductor layer and the interlayer insulating film, the emitter electrode having on its surface the first modified layer containing the nitride.

3. The semiconductor device according to claim 1, further comprising an anode electrode in contact with the second semiconductor layer and the interlayer insulating film, the anode electrode having the first modified layer containing the nitride on a surface thereof.

4. The semiconductor device according to claim 1, characterized in that the field plate electrode is an aluminum-based electrode, and the first modified layer is aluminum nitride obtained by modifying the aluminum-based electrode through the nitriding treatment.

5. The semiconductor device according to claim 1, characterized in that the second modified layer is silicon oxynitride.

6. The semiconductor device according to claim 1, comprising: an active region arranged on a main surface of a semiconductor substrate; and a termination region arranged on the main surface so as to surround the active region, the termination region comprising the field plate electrode and the interlayer insulating film.

7. The semiconductor device according to claim 2, wherein the first modified layer of the emitter electrode in the active region disposed on the main surface of the semiconductor substrate is removed.

8. The semiconductor device according to claim 3, wherein the first modified layer of the anode electrode in the active region disposed on the main surface of the semiconductor substrate is removed.

9. A method for manufacturing a semiconductor device, comprising the steps of: partially forming a second semiconductor layer of a second conductivity type on a surface portion of a first semiconductor layer; forming an interlayer insulating film in contact with the first semiconductor layer and the second semiconductor layer; forming a field plate electrode in contact with the second semiconductor layer and the interlayer insulating film; and nitriding the field plate electrode and the interlayer insulating film to form a modified layer made of an inorganic film containing nitride on a surface.

Citation Information

Patent Citations

  • Nitride semiconductor heterostructure field effect transistor

    JP2009147264A

  • Manufacturing method of semiconductor device

    JP2020107917A

  • Semiconductor device and power conversion device

    JP2021185593A

  • Semiconductor device and manufacturing method for the same

    JP2021190647A

  • Semiconductor device

    JP2023004072A