Optical fiber and optical fiber ribbon
The optical fiber design with a specific resin composition enhances lateral pressure and hot water resistance by using a photopolymerizable compound and titanium oxide particles, addressing the issues of thinner coating layers in smaller diameter fibers and water exposure.
Patent Information
- Application Number
- PCT/JP2024/010302
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-24
AI Technical Summary
As optical fibers in cables become smaller in diameter, the coating resin layer becomes thinner, leading to deteriorated lateral pressure resistance and increased transmission loss when exposed to hot water, causing the resin layer to peel off from the glass fiber.
An optical fiber design featuring a glass fiber with a primary and secondary resin layer, topped by a colored resin layer containing a cured product of a resin composition including a photopolymerizable compound, polydimethylsiloxane compound, and titanium oxide particles, with controlled particle distribution and silicon content to enhance lateral pressure resistance and hot water resistance.
The solution provides optical fibers and ribbons with improved lateral pressure resistance and hot water resistance, maintaining transmission integrity even under increased mechanical stress and water exposure.
Smart Images

Figure JP2024010302_24102024_PF_FP_ABST
Abstract
Description
Optical Fiber and Optical Fiber Ribbons
[0001] This application claims priority to Japanese Patent Application No. 2023-069880, filed April 21, 2023, and incorporates by reference the entire contents of said Japanese application.
[0002] Generally, optical fibers have a resin coating layer to protect the glass fiber that serves as the optical transmission medium. The resin coating layer includes, for example, a primary resin layer and a secondary resin layer. The outermost layer of the resin coating layer is a colored resin layer for identifying the optical fiber (see, for example, Patent Documents 1 and 2).
[0003] International Publication No. 2016 / 017060 Special Publication No. 2002-516377
[0004] An optical fiber according to one embodiment of the present disclosure comprises a glass fiber including a core and a cladding, a primary resin layer that contacts and coats the glass fiber, a secondary resin layer that coats the primary resin layer, and a colored resin layer that coats the secondary resin layer, wherein the colored resin layer contains a cured product of a resin composition that contains a photopolymerizable compound, a photopolymerization initiator, a polydimethylsiloxane compound, and titanium oxide particles, and the number of titanium-containing particles with a diameter of 5 μm or more contained in the colored resin layer is less than 15 particles / mm in the length direction of the colored resin layer, and the amount of silicon on the surface of the colored resin layer is 0.9 at% or more and 11 at% or less.
[0005] Fig. 1 is a schematic cross-sectional view showing an example of an optical fiber, and Fig. 2 is a schematic cross-sectional view showing an example of an optical fiber ribbon.
[0006] [Problem to be Solved by the Present Disclosure] In recent years, as optical cables have become more numerous and thinner in diameter, the diameter of the optical fibers used in the optical cables has become thinner. As the diameter of the optical fiber becomes thinner, the coating resin layer that protects the glass fiber also becomes thinner, which can deteriorate the lateral pressure resistance of the optical fiber. Furthermore, when the optical fiber is immersed in warm water, the coating resin layer can peel off from the glass fiber, resulting in increased transmission loss.
[0007] An object of the present disclosure is to provide an optical fiber and an optical fiber ribbon that are excellent in lateral pressure resistance and hot water resistance.
[0008] Effect of the Present Disclosure According to the present disclosure, an optical fiber and an optical fiber ribbon having excellent lateral pressure resistance and hot water resistance can be provided.
[0009] [Description of Embodiments of the Present Disclosure] First, the contents of the embodiments of the present disclosure will be listed and described. (1) An optical fiber according to one aspect of the present disclosure includes a glass fiber including a core and a cladding, a primary resin layer that contacts the glass fiber and coats the glass fiber, a secondary resin layer that coats the primary resin layer, and a colored resin layer that coats the secondary resin layer, wherein the colored resin layer contains a cured product of a resin composition that contains a photopolymerizable compound, a photopolymerization initiator, a polydimethylsiloxane compound, and titanium oxide particles, the number of titanium-containing particles with a diameter of 5 μm or more contained in the colored resin layer is less than 15 particles / mm in the length direction of the colored resin layer, and the amount of silicon on the surface of the colored resin layer is 0.9 at % or more and 11 at % or less.
[0010] Such an optical fiber has excellent lateral pressure resistance and hot water resistance because the number of titanium-containing particles with a diameter of 5 μm or more is less than 15 per mm in the longitudinal direction and the amount of silicon on the surface is 0.9 at% or more and 11 at% or less.
[0011] (2) In the above (1), from the viewpoint of the visibility of the colored resin layer and the curability of the resin composition, the content of the titanium oxide particles may be 0.6 mass % or more and 20.0 mass % or less based on the total amount of the resin composition.
[0012] (3) In the above (1) or (2), from the viewpoint of further improving lateral pressure resistance and warm water resistance, the polydimethylsiloxane compound may have at least one organic group selected from the group consisting of a (meth)acryloyl group, an epoxy group, and a polyether group.
[0013] (4) In any of (1) to (3) above, from the viewpoint of lateral pressure resistance and stability of the resin composition, the amount of silicon atoms contained in the polydimethylsiloxane compound may be 6% by mass or more and 40% by mass or less.
[0014] (5) In any of the above (1) to (4), from the viewpoint of reducing the diameter of the optical fiber, the outer diameter of the optical fiber may be 140 μm or more and 255 μm or less.
[0015] (6) An optical fiber ribbon according to an aspect of the present disclosure includes a plurality of optical fibers according to any one of (1) to (5) arranged in parallel and coated with a ribbon resin. Such an optical fiber ribbon has excellent lateral pressure resistance and hot water resistance.
[0016] [Details of the Embodiments of the Present Disclosure] Specific examples of optical fibers and optical fiber ribbons according to the embodiments of the present disclosure will be described with reference to the drawings as necessary. The present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. In the following description, the same elements in the drawings will be designated by the same reference numerals, and redundant explanations will be omitted. In this specification, (meth)acrylate means acrylate or the corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl.
[0017] (Optical Fiber) The optical fiber according to this embodiment includes a glass fiber including a core and a cladding, a primary resin layer that contacts and coats the glass fiber, a secondary resin layer that coats the primary resin layer, and a colored resin layer that coats the secondary resin layer. The colored resin layer includes a cured product of a resin composition (hereinafter also referred to as "resin composition for the colored resin layer") that contains a photopolymerizable compound, a photopolymerization initiator, a polydimethylsiloxane compound, and titanium oxide particles.
[0018] Polydimethylsiloxane compounds have a dimethylsiloxane skeleton (-Si(CH 3 ) 2O-) as a repeating unit.
[0019] The amount of silicon atoms (Si) contained in the polydimethylsiloxane compound may be 6% by mass or more, 8% by mass or more, 10% by mass or more, or 12% by mass or more from the viewpoint of further improving lateral pressure resistance. The amount of Si may be 40% by mass or less, 30% by mass or less, 25% by mass or less, or 21% by mass or less from the viewpoint of improving the stability of the resin composition. The amount of Si may be 6% by mass or more and 40% by mass or less, 8% by mass or more and 30% by mass or less, 10% by mass or more and 25% by mass or less, or 12% by mass or more and 21% by mass or less from the viewpoint of lateral pressure resistance and the stability of the resin composition. The amount of Si contained in the polydimethylsiloxane compound can be measured by inductively coupled plasma optical emission spectroscopy (ICP-OES) of the polydimethylsiloxane compound.
[0020] The polydimethylsiloxane compound may have at least one organic group selected from the group consisting of a (meth)acryloyl group, an epoxy group, and a polyether group, from the viewpoint of further improving lateral pressure resistance and hot water resistance. That is, the polydimethylsiloxane compound may contain at least one selected from the group consisting of a polydimethylsiloxane compound having a (meth)acryloyl group, a polydimethylsiloxane compound having an epoxy group, and a polydimethylsiloxane compound having a polyether group, from the viewpoint of further improving lateral pressure resistance and hot water resistance. The polydimethylsiloxane compound may have these organic groups on a side chain or at a terminal. Among these organic groups, from the viewpoint of lateral pressure resistance and hot water resistance, a (meth)acryloyl group and an epoxy group are preferred, and a (meth)acryloyl group is more preferred.
[0021] The polydimethylsiloxane compound having a (meth)acryloyl group can be copolymerized with the photopolymerizable compound described below. The polydimethylsiloxane compound having a (meth)acryloyl group is not included in the photopolymerizable compound described below. The number of (meth)acryloyl groups in the polydimethylsiloxane compound may be 1 or more, 2 or more, or 10 or less, or 8 or less.
[0022] The number of epoxy groups contained in the polydimethylsiloxane compound may be 1 or more, or 2 or more, and may be 10 or less, or 8 or less.
[0023] The number of polyether groups contained in the polydimethylsiloxane compound may be 1 or more, or 2 or more, and may be 10 or less, or 8 or less.
[0024] From the viewpoint of lateral pressure resistance and hot water resistance, the content of the polydimethylsiloxane compound may be 0.3 mass% or more and 4.5 mass% or less, based on the total amount of the resin composition. When the content of the polydimethylsiloxane compound is 0.3 mass% or more, the dispersibility of the titanium oxide particles contained in the resin composition is easily improved, thereby reducing aggregates with a diameter of 5 μm or more caused by the titanium oxide particles. This reduces the surface irregularities of the formed colored resin layer and the frictional force of the colored resin layer, thereby further improving the lateral pressure resistance of the optical fiber. When the content of the polydimethylsiloxane compound is 4.5 mass% or less, the decrease in adhesion between the colored resin layer and the secondary resin layer is suppressed, and hot water resistance is further improved.
[0025] From the viewpoint of further improving lateral pressure resistance, the content of the polydimethylsiloxane compound may be 0.4% by mass or more or 0.5% by mass or more, based on the total amount of the resin composition, and from the viewpoint of further improving hot water resistance, the content of the polydimethylsiloxane compound may be 4.0% by mass or less, 3.5% by mass or less, 3.0% by mass or less, or 2.5% by mass or less, based on the total amount of the resin composition. From the viewpoint of further improving lateral pressure resistance and hot water resistance, the content of the polydimethylsiloxane compound may be 0.4% by mass or more and 4.0% by mass or less, 0.4% by mass or more and 3.5% by mass or less, 0.5% by mass or more and 3.0% by mass or less, or 0.5% by mass or more and 2.5% by mass or less, based on the total amount of the resin composition.
[0026] The photopolymerizable compound is distinguished from a polydimethylsiloxane compound having a (meth)acryloyl group in that it does not have a dimethylsiloxane skeleton. From the viewpoint of increasing the strength of the colored resin layer, the photopolymerizable compound may contain an epoxy di(meth)acrylate. As the epoxy di(meth)acrylate, for example, a reaction product of a diglycidyl ether compound having a bisphenol skeleton and a compound having a (meth)acryloyl group, such as (meth)acrylic acid, can be used.
[0027] Examples of epoxy di(meth)acrylates include (meth)acrylic acid adducts of bisphenol A diglycidyl ether, (meth)acrylic acid adducts of bisphenol AF diglycidyl ether, and (meth)acrylic acid adducts of bisphenol F diglycidyl ether.
[0028] From the viewpoint of further increasing the strength of the colored resin layer, the content of the epoxy di(meth)acrylate may be 30 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more, and 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, relative to 100 parts by mass of the total amount of the polydimethylsiloxane compound and the photopolymerizable compound. The content of the epoxy di(meth)acrylate may be 30 parts by mass or more and 70 parts by mass or less, 40 parts by mass or more and 65 parts by mass or less, or 45 parts by mass or more and 60 parts by mass or less, relative to 100 parts by mass of the total amount of the polydimethylsiloxane compound and the photopolymerizable compound. The content of the epoxy di(meth)acrylate may be 30% by mass or more and 70% by mass or less, 40% by mass or more and 65% by mass or less, 45% by mass or more and 60% by mass or less, relative to 100 parts by mass of the total amount of the photopolymerizable compound.
[0029] The photopolymerizable compound may further contain a photopolymerizable compound (hereinafter referred to as "monomer") other than epoxy di(meth)acrylate.
[0030] The monomer may be a monofunctional monomer having one polymerizable group or a polyfunctional monomer having two or more polymerizable groups. Two or more types of monomers may be used in combination.
[0031] Examples of monofunctional monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. (Meth)acrylate monomers such as acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3-phenoxybenzyl acrylate, phenoxydiethylene glycol acrylate, phenoxypolyethylene glycol acrylate, 4-tert-butylcyclohexanol acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, and isobornyl (meth)acrylate; (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, ω-carboxymethyl (meth)acrylate, Carboxy group-containing monomers such as carboxy-polycaprolactone (meth)acrylate; heterocycle-containing monomers such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, 3-(3-pyridine)propyl (meth)acrylate, and cyclic trimethylolpropane formal acrylate; maleimide-based monomers such as maleimide, N-cyclohexylmaleimide, and N-phenylmaleimide;Amide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; aminoalkyl (meth)acrylate-based monomers such as aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; and succinimide-based monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide.
[0032] Examples of polyfunctional monomers include polyethylene glycol di(meth)acrylate, isocyanuric acid ethylene oxide modified di(meth)acrylate, ethylene oxide modified bisphenol F di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, polypropylene glycol di(meth)acrylate, propylene oxide modified bisphenol A di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate, polytetraethylene glycol di(meth)acrylate, Acrylates, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, isopentyl glycol di(meth)acrylate, diethyl-1,8-octanediol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate; trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxypolypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate acrylate, pentaerythritol polyethoxytetra(meth)acrylate, pentaerythritol polypropoxytetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified tris[(meth)acryloyloxyethyl]isocyanurate.
[0033] The photopolymerizable compound may contain an alkylene oxide-modified polyfunctional monomer from the viewpoint of adjusting the Young's modulus of the colored resin layer. The alkylene oxide-modified polyfunctional monomer may have at least one selected from the group consisting of an ethylene oxide (EO) chain and a propylene oxide (PO) chain. The ethylene oxide chain can be represented as "(EO)n" and the propylene oxide chain can be represented as "(PO)n". n is an integer of 1 or more, and may be 2 or more or 3 or more, or may be 30 or less, 25 or less, or 20 or less.
[0034] Examples of alkylene oxide-modified polyfunctional monomers include alkylene oxide-modified di(meth)acrylates and alkylene oxide-modified tri(meth)acrylates.
[0035] Examples of alkylene oxide-modified di(meth)acrylates include polyethylene glycol di(meth)acrylate, isocyanuric acid ethylene oxide-modified di(meth)acrylate, ethylene oxide-modified bisphenol F di(meth)acrylate, ethylene oxide-modified bisphenol A di(meth)acrylate polypropylene glycol di(meth)acrylate, propylene oxide-modified bisphenol A di(meth)acrylate, and propylene oxide-modified neopentyl glycol di(meth)acrylate.
[0036] Examples of alkylene oxide-modified tri(meth)acrylates include trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxypolypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, and pentaerythritol tri(meth)acrylate.
[0037] The content of the alkylene oxide-modified polyfunctional monomer is not particularly limited, but may be 20% by mass or more and 70% by mass or less, 30% by mass or more and 60% by mass or less, or 40% by mass or more and 50% by mass or less, based on the total amount of the photopolymerizable compound.
[0038] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators. Examples of the photopolymerization initiator include 1-hydroxycyclohexylphenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one (Omnirad 907, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins).
[0039] The content of the photopolymerization initiator may be 1 part by mass or more and 10 parts by mass or less, 2 parts by mass or more and 8 parts by mass or less, or 3 parts by mass or more and 7 parts by mass or less, relative to 100 parts by mass of the total amount of the polydimethylsiloxane compound and the photopolymerizable compound.
[0040] From the viewpoint of coloring the resin layer, the resin composition according to the present embodiment contains titanium oxide particles. As the titanium oxide particles, surface-treated titanium oxide particles may be used. The surface-treated titanium oxide particles are particles of titanium oxide that have been surface-treated with an inorganic substance, and have excellent dispersibility in the resin composition. Examples of titanium oxide include anatase titanium oxide, rutile titanium oxide, and brookite titanium oxide. From the viewpoint of stability, the titanium oxide may be rutile titanium oxide.
[0041] Examples of inorganic substances used for surface treatment include aluminum oxide, silicon dioxide, and zirconium dioxide. When the surface-treated titanium oxide particles have a surface treatment layer containing at least one selected from the group consisting of aluminum oxide, silicon dioxide, and zirconium dioxide, dispersibility can be further improved. The surface treatment layer may be formed on at least a portion of the surface of the titanium oxide, or may be formed on the entire surface of the titanium oxide. The surface treatment layer is formed by surface treatment of the titanium oxide.
[0042] The amount of the surface treatment layer in the surface-treated titanium oxide particles may be 1.0% by mass or more, 1.5% by mass or more, or 2.0% by mass or more from the viewpoint of improving dispersibility, and may be 10.0% by mass or less, 9.0% by mass or less, or 8.0% by mass or less from the viewpoint of improving hiding power. The amount of the surface treatment layer in the surface-treated titanium oxide particles may be 1.0% by mass or more and 10.0% by mass or less, 1.5% by mass or more and 9.0% by mass or less, or 2.0% by mass or more and 8.0% by mass or less from the viewpoint of dispersibility and hiding power. The amount of the surface treatment layer can be calculated by measuring the amounts of titanium element and inorganic elements other than titanium contained in the surface-treated titanium oxide particles using inductively coupled plasma mass spectrometry (ICP-MS).
[0043] The average primary particle size of the surface-treated titanium oxide particles may be 300 nm or less, 295 nm or less, or 290 nm or less from the viewpoint of further improving lateral pressure resistance. The average primary particle size of the surface-treated titanium oxide particles may be 100 nm or more, 150 nm or more, or 200 nm or more, and preferably 200 nm or more and 300 nm or less, from the viewpoint of improving hiding power. The average primary particle size can be measured, for example, by image analysis of electron microscope photographs, light scattering method, BET method, etc.
[0044] The content of the titanium oxide particles may be 0.6% by mass or more, 1.0% by mass or more, 2.0% by mass or more, or 3.0% by mass or more, based on the total amount of the resin composition, from the viewpoint of improving the visibility of the colored resin layer, and may be 20.0% by mass or less, 15.0% by mass or less, 10.0% by mass or less, or 8.0% by mass or less, from the viewpoint of improving the curability of the resin composition. The content of the titanium oxide particles may be 0.6% by mass or more and 20.0% by mass or less, 1.0% by mass or more and 15.0% by mass or less, 2.0% by mass or more and 10.0% by mass or less, or 3.0% by mass or more and 8.0% by mass or less, based on the total amount of the resin composition, from the viewpoint of the visibility of the colored resin layer and the curability of the resin composition.
[0045] The resin composition may further contain a silane coupling agent, a leveling agent, an antifoaming agent, an antioxidant, a sensitizer, and the like.
[0046] The silane coupling agent is not particularly limited as long as it does not interfere with the curing of the resin composition. Examples of the silane coupling agent include tetramethyl silicate, tetraethyl silicate, mercaptopropyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ β-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamyltetrasulfide, and γ-trimethoxysilylpropylbenzothiazyltetrasulfide.
[0047] The resin composition according to this embodiment is applied at 900 mJ / cm 2 More than 1100mJ / cm 2 A resin layer having excellent toughness can be formed when the elongation at break of a resin film cured with the following integrated light amount is 6% or more and 50% or less at 23° C. The elongation at break of the resin film may be 6.5% or more, 7% or more, or 10% or more, or may be 45% or less, 40% or less, or 30% or less.
[0048] From the viewpoint of the wet heat resistance of the optical fiber, the Young's modulus of the resin film may be 400 MPa or more, 450 MPa or more, or 500 MPa or more at 23° C. From the viewpoint of forming a resin layer with excellent toughness, the Young's modulus of the resin film may be 1500 MPa or less, 1200 MPa or less, or 1000 MPa or less at 23° C.
[0049] Fig. 1 is a schematic cross-sectional view showing the configuration of an optical fiber according to one embodiment. As shown in Fig. 1, the optical fiber 1 includes a glass fiber 10 and a coating resin layer 20 that contacts the glass fiber 10 and covers the outer periphery of the glass fiber 10. The glass fiber 10 includes a core 12 and a cladding 14. The coating resin layer 20 includes a primary resin layer 22, a secondary resin layer 24, and a colored resin layer 26.
[0050] The glass fiber 10 is a light-guiding optical transmission body that transmits light introduced into the optical fiber 1. The glass fiber 10 is a glass member, and is made of, for example, silica (SiO 2 The glass fiber 10 is constructed using pure silica (SiO ) glass as a base material (main component). The glass fiber 10 includes a core 12 and a cladding 14 that covers the core 12. The glass fiber 10 transmits light introduced into the optical fiber 1. The core 12 is provided, for example, in a region that includes the central axis of the glass fiber 10. The core 12 is made of, for example, pure silica (SiO 2 ) Glass or SiO 2 Glass with germanium dioxide (GeO 2The cladding 14 is provided in the region surrounding the core 12. The cladding 14 has a refractive index lower than that of the core 12. The cladding 14 is made of, for example, pure SiO 2 Glass or SiO2 doped with fluorine 2 The glass fiber 10 is made of glass and has an outer diameter of, for example, about 100 μm to 125 μm, and a core 12 constituting the glass fiber 10 has a diameter of, for example, about 7 μm to 15 μm.
[0051] The coating resin layer 20 is an ultraviolet-curable resin layer that covers the clad 14. The coating resin layer 20 includes a primary resin layer 22 that coats the outer periphery of the glass fiber 10, a secondary resin layer 24 that coats the outer periphery of the primary resin layer 22, and a colored resin layer 26 that coats the outer periphery of the secondary resin layer 24. The primary resin layer 22 is in contact with the outer periphery of the clad 14 and coats the entire clad 14. The secondary resin layer 24 is in contact with the outer periphery of the primary resin layer 22 and coats the entire primary resin layer 22. The colored resin layer 26 is in contact with the outer periphery of the secondary resin layer 24 and coats the entire secondary resin layer 24. The thickness of the primary resin layer 22 is, for example, 10 μm or more and 50 μm or less. The thickness of the secondary resin layer 24 is, for example, 10 μm or more and 40 μm or less. The thickness of the colored resin layer 26 is, for example, 3 μm or more and 10 μm or less.
[0052] From the viewpoint of reducing the diameter, the outer diameter of the optical fiber 1 may be 255 μm or less, 220 μm or less, 180 μm or less, or 160 μm or less, or may be 140 μm or more. The outer diameter of the optical fiber 1 may be 140 μm or more and 255 μm or less, 140 μm or more and 220 μm or less, 140 μm or more and 180 μm or less, or 140 μm or more and 160 μm or less.
[0053] When the outer diameter of the glass fiber 10 is about 125 μm and the thickness of the coating resin layer 20 is 20 μm or more and 48 μm or less, the thickness of each of the primary resin layer 22 and the secondary resin layer 24 may be about 8 μm to 38 μm, for example, the thickness of the primary resin layer 22 may be 25 μm and the thickness of the secondary resin layer 24 may be 10 μm. The outer diameter of the optical fiber 1 may be about 165 μm to 221 μm.
[0054] When the outer diameter of the glass fiber 10 is about 100 μm and the thickness of the coating resin layer 20 is 22 μm or more and 37 μm or less, the thickness of each of the primary resin layer 22 and the secondary resin layer 24 may be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 22 may be 25 μm and the thickness of the secondary resin layer 24 may be 10 μm. The outer diameter of the optical fiber 1 may be about 144 μm to 174 μm.
[0055] The primary resin layer 22 can be formed by curing a resin composition containing, for example, urethane (meth)acrylate, a monomer, and a photopolymerization initiator. The resin composition for the primary resin layer can be formed using a conventionally known technique.
[0056] The secondary resin layer 24 can be formed by curing a resin composition containing, for example, urethane (meth)acrylate, a monomer, and a photopolymerization initiator. The resin composition for the secondary resin layer can be formed using a conventionally known technique.
[0057] The colored resin layer 26 can be formed by curing the resin composition for the colored resin layer. The number of titanium-containing particles having a diameter of 5 μm or more (hereinafter also referred to as "particles having a diameter of 5 μm or more") contained in the colored resin layer 26 is less than 15 particles / mm in the length direction of the colored resin layer from the viewpoint of lateral pressure resistance. From the viewpoint of further improving lateral pressure resistance, the number of particles having a diameter of 5 μm or more contained in the colored resin layer 26 may be 14 particles / mm or less, 13 particles / mm or less, 12 particles / mm or less, 11 particles / mm or less, 10 particles / mm or less, or 5 particles / mm or less in the length direction of the colored resin layer. The number of particles having a diameter of 5 μm or more contained in the colored resin layer 26 may be 0 particles / mm in the length direction of the colored resin layer. Particles having a diameter of 5 μm or more refer to particles having a diameter of 5 μm or more (maximum diameter in the case of shapes other than spherical) when observed using an optical microscope. The particles having a diameter of 5 μm or more contained in the colored resin layer 26 include aggregates resulting from titanium oxide particles. The number of particles having a diameter of 5 μm or more can be measured using an optical microscope, and whether or not titanium element is contained can be determined by X-ray analysis.
[0058] The amount of silicon (Si) in the surface of the colored resin layer 26 is 0.9 at% or more and 11 at% or less from the viewpoints of lateral pressure resistance and hot water resistance. At% is atomic percent. That is, the ratio of silicon element to the elements in the surface of the colored resin layer 26 is 0.9 at% or more and 11 at% or less. From the viewpoint of lateral pressure resistance, the amount of Si in the surface of the colored resin layer 26 may be 1 at% or more, 1.5 at% or more, or 2 at% or more. From the viewpoint of hot water resistance, the amount of Si in the surface of the colored resin layer 26 may be 1 at% or more and 10.5 at% or less, 1 at% or more and 10 at% or less, 1.5 at% or more and 10 at% or less, or 2 at% or more and 10 at% or less. The amount of Si in the surface of the colored resin layer 26 may be 1 at% or more and 10.5 at% or less, 1 at% or more and 10 at% or less, 1.5 at% or more and 10 at% or less, or 2 at% or more and 10 at% or less.
[0059] (Optical Fiber Ribbon) The optical fibers according to this embodiment can be used to fabricate an optical fiber ribbon, which is formed by arranging a plurality of the optical fibers in parallel and coating them with a ribbon resin.
[0060] 2 is a schematic cross-sectional view showing an optical fiber ribbon according to one embodiment. The optical fiber ribbon 100 includes a plurality of optical fibers 1 and a connecting resin layer 40 in which the optical fibers 1 are coated with a ribbon resin and connected. In FIG. 2, four optical fibers 1 are shown as an example, but the number is not particularly limited.
[0061] The ribbon resin may be a resin material generally known as a ribbon material. From the viewpoint of preventing damage to the optical fiber and facilitating separation, the ribbon resin may contain a thermosetting resin such as a silicone resin, an epoxy resin, or a urethane resin, or an ultraviolet-curing resin such as an epoxy acrylate, a urethane acrylate, or a polyester acrylate.
[0062] The optical fiber ribbon according to this embodiment uses the above optical fibers, and therefore has excellent lateral pressure resistance and hot water resistance.
[0063] The present disclosure will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0064] [Resin Composition for Colored Resin Layer] (Polydimethylsiloxane Compound) The polydimethylsiloxane compounds (PDMS) shown in Table 1 were prepared. The amount of Si contained in the polydimethylsiloxane compounds was measured using ICP-OES according to the following procedure. First, 2 mL of hydrofluoric acid and 6 mL of nitric acid were added to 0.1 g of the polydimethylsiloxane compound, and the mixture was heated to 200°C in 30 minutes using a microwave decomposition device, maintained for 20 minutes, and then cooled to room temperature (25°C), thereby obtaining a decomposition solution of the polydimethylsiloxane compound. Next, the decomposition solution was diluted 50 times with ultrapure water to prepare a sample. The amount of Si contained in the polydimethylsiloxane compound was calculated by quantifying the amount of Si in the sample using an ICP optical emission spectrometer ("iCAP6300" manufactured by Thermo Fisher Scientific Co., Ltd.).
[0065]
[0066] (Photopolymerizable Compound) Examples of the photopolymerizable compound include bisphenol A epoxy diacrylate (EA), tripropylene glycol diacrylate (TPGDA), and EO-modified trimethylolpropane triacrylate (TMP(EO)). 3 TA) and EO-modified bisphenol A diacrylate (BPA(EO) 30 DA) was prepared.
[0067] (Photopolymerization Initiator) As photopolymerization initiators, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO) and 1-hydroxycyclohexylphenyl ketone (Omnirad 184) were prepared.
[0068] (Titanium oxide particles) As titanium oxide particles, aluminum oxide (Al 2 O 3 The surface-treated titanium oxide particles had an average primary particle size of 200 to 300 nm, and the Al content calculated by ICP-MS was 2 O 3 The amount was 2.5% by mass.
[0069] The photopolymerizable compound and photopolymerization initiator were mixed in the amounts (parts by mass) shown in Table 2, and then the resin compositions were mixed so that the contents of the surface-treated titanium oxide particles and PDMS in the resin compositions were the mass % shown in Table 2, thereby preparing the resin compositions of Test Examples 1 to 10. Test Examples 1 to 8 correspond to Examples, and Test Examples 9 and 10 correspond to Comparative Examples.
[0070] [Resin composition for primary resin layer] A urethane acrylate oligomer obtained by reacting polypropylene glycol having a molecular weight of 4000, isophorone diisocyanate, and hydroxyethyl acrylate was prepared. 65 parts by mass of this urethane acrylate oligomer, 25 parts by mass of nonylphenol polyethylene glycol (meth)acrylate, 10 parts by mass of N-vinyl caprolactam, and 1 part by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide (manufactured by BASF under the trade name "Lucirin TPO") were mixed to prepare resin composition P.
[0071] [Resin Composition for Secondary Resin Layer] Resin composition S was prepared by mixing 40 parts by mass of urethane acrylate oligomer (UA), which is a reaction product of polypropylene glycol having a molecular weight of 600, 2,4-tolylene diisocyanate, and 2-hydroxyethyl acrylate, 35 parts by mass of isobornyl acrylate (IBOA), 24 parts by mass of epoxy acrylate (EA), which is an acrylic acid adduct of bisphenol A diglycidyl ether, 1 part by mass of Omnirad TPO, and 1 part by mass of Omnirad 184.
[0072] [Fabrication of Optical Fiber] A 35 μm thick primary resin layer was formed around a 125 μm diameter glass fiber composed of a core and a cladding using resin composition P, and a 25 μm thick secondary resin layer was further formed around the primary resin layer using resin composition S, to fabricate an optical fiber with a diameter of 245 μm. Next, the optical fiber was temporarily wound up, and then a 5 μm thick colored resin layer was formed around the secondary resin layer using the resin compositions of Test Examples 1 to 10 while the optical fiber was re-unwound using a coloring machine, thereby fabricating an optical fiber with a diameter of 255 μm and a colored resin layer (hereinafter referred to as "colored optical fiber"). The linear speed during the formation of each resin layer was 1500 m / min.
[0073] (Number of particles with a diameter of 5 μm or more) The colored optical fiber was immersed in silicone oil and observed from the side with an optical microscope (magnification 300x) to measure the number of particles with a diameter of 5 μm or more (maximum diameter for shapes other than spherical) per mm in the length direction of the colored optical fiber. The number of measurement areas was set to 10, and the average value was calculated. Whether the particles contained titanium element was determined by performing X-ray analysis of the colored optical fiber and determining whether titanium element was detected.
[0074] (Si Amount on the Surface of the Colored Resin Layer) The Si amount on the surface of the colored resin layer of the colored optical fiber was measured by X-ray photoelectric spectroscopy using a Quantera SXM manufactured by ULVAC PHI. The measurement was carried out under the following conditions. The measurement results are shown in Table 2. X-ray conditions: 20 μm, 4.5 W, 15 kV Transmission energy: narrow 55 eV, depth 112 eV Photoelectron take-off angle: 45° Ion gun conditions at depth: 0.5 kV, 1 kV, 2 kV 1×1 Average sputtering rate: 1.04 nm / min
[0075] (Lateral pressure resistance characteristics) A colored optical fiber was wound in a single layer around a 280 mm diameter bobbin covered with sandpaper (number 240), and the colored optical fiber was wound around a 40 mm diameter mandrel, and the transmission loss of light with a wavelength of 1550 nm was measured by an OTDR (Optical Time Domain Reflectometer) method. The difference in the measured transmission losses was calculated, and the lateral pressure resistance characteristics were evaluated by assigning an "A" rating when the transmission loss difference was 0.5 dB / km or less and an "B" rating when the transmission loss difference was more than 0.5 dB / km.
[0076] (Warm Water Resistance) A 1000 m bundle of colored optical fiber was immersed in warm water at 60° C. for 30 days, and then the transmission loss of light with a wavelength of 1550 nm was measured using an OTDR (Optical Time Domain Reflectometer) method. Warm water resistance was evaluated by assigning an "A" rating to a case where the difference between the transmission loss before immersion and the transmission loss after immersion in warm water for 30 days was 0.05 dB / km or less, and a "B" rating to a case where the difference was more than 0.05 dB / km.
[0077]
[0078] REFERENCE SIGNS LIST 1... Optical fiber 10... Glass fiber 12... Core 14... Cladding 20... Coating resin layer 22... Primary resin layer 24... Secondary resin layer 26... Colored resin layer 40... Connecting resin layer 100... Optical fiber ribbon
Claims
1. An optical fiber comprising: a glass fiber including a core and a cladding; a primary resin layer in contact with and coating the glass fiber; a secondary resin layer coating the primary resin layer; and a colored resin layer coating the secondary resin layer, wherein the colored resin layer comprises a cured product of a resin composition containing a photopolymerizable compound, a photopolymerization initiator, a polydimethylsiloxane compound, and titanium oxide particles, the number of titanium-containing particles having a diameter of 5 μm or more contained in the colored resin layer is less than 15 particles / mm in the longitudinal direction of the colored resin layer, and the amount of silicon on the surface of the colored resin layer is 0.9 at% or more and 11 at% or less.
2. The optical fiber according to claim 1, wherein the content of the titanium oxide particles is 0.6% by mass or more and 20.0% by mass or less, based on the total amount of the resin composition.
3. The optical fiber according to claim 1, wherein said polydimethylsiloxane compound has at least one organic group selected from the group consisting of a (meth)acryloyl group, an epoxy group, and a polyether group.
4. The optical fiber according to claim 1, wherein the amount of silicon atoms contained in said polydimethylsiloxane compound is 6% by mass or more and 40% by mass or less.
5. The optical fiber according to claim 1, having an outer diameter of 140 μm or more and 255 μm or less.
6. An optical fiber ribbon comprising a plurality of optical fibers according to any one of claims 1 to 5 arranged in parallel and coated with a ribbon resin.
Citation Information
Patent Citations
Colored coated optical fiber core wire and optical fiber ribbon
JP2005165227A
Colored coated optical fiber and its manufacturing method
JP2006084770A
Optical fiber core wire and optical fiber ribbon
JP2016070966A
Light-diffusing optical fiber coating
JP2019504339A
Fiber marking with optical brighteners
US20170371122A1