Transmission belt, production method therefor, and core wire
A multi-step adhesive treatment process using epoxy and silane coupling agents enhances the adhesion between the core wire and elastomer belt body, addressing bond strength issues in power transmission belts for high-load applications.
Patent Information
- Application Number
- PCT/JP2024/013782
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-24
AI Technical Summary
Existing power transmission belts face challenges in achieving high adhesion between the core wire and the elastomer belt body, particularly in high-load applications, where the bond strength is insufficient, leading to potential failure under stress.
The core wire is treated with a first agent containing an epoxy compound and a blocked isocyanate compound, followed by a second treatment with a silane coupling agent, enhancing the adhesion to the elastomer belt body through a multi-step adhesive process.
This method significantly improves the adhesion between the core wire and the elastomer belt body, enhancing the durability and performance of the power transmission belt in high-load applications by ensuring a strong and reliable bond.
Smart Images

Figure JP2024013782_24102024_PF_FP_ABST
Abstract
Description
Transmission belt, its manufacturing method and core wire
[0001] The present invention relates to a power transmission belt, a method for manufacturing the same, and a core wire.
[0002] The core wires embedded in the belt body of a transmission belt are subjected to an adhesive treatment for bonding to the belt body. For example, Patent Document 1 discloses that, for rubber-reinforcing carbon fibers used in transmission belts and the like, a carbon fiber bundle is treated with a first bath solution containing a urethane resin as a main component, and then treated with a second bath solution of an RFL-based adhesive containing a polynuclear chlorophenol compound.
[0003] JP 2011-241502 A
[0004] The present invention provides a power transmission belt having a core wire embedded in an elastomer belt body, wherein the core wire is subjected to an adhesive treatment in which the core wire is immersed in a first treating agent containing an epoxy compound and a blocked isocyanate compound and heated, and then immersed in a second treating agent containing a silane coupling agent and heated.
[0005] The present invention relates to a core wire embedded in an elastomer belt body of a transmission belt, which is subjected to an adhesive treatment in which the core wire is immersed in a first treating agent containing an epoxy compound and a blocked isocyanate compound and heated, and then immersed in a second treating agent containing a silane coupling agent and heated.
[0006] The present invention provides a method for manufacturing a power transmission belt having a core wire embedded in an elastomer belt body, the method comprising a core wire bonding process for subjecting the core wire to an adhesive treatment, the core wire bonding process including a first treatment step for immersing the core wire in a first treatment agent containing an epoxy compound and a blocked isocyanate compound and heating the same, and a second treatment step for immersing the core wire in a second treatment agent containing a silane coupling agent and heating the same after the first treatment step.
[0007] FIG. 1 is a perspective view of a piece of a toothed belt according to an embodiment; FIG. 2 is a longitudinal sectional view of a portion of a toothed belt according to an embodiment; FIG. 3 is a first explanatory view of a method for manufacturing a toothed belt according to an embodiment; FIG. 4 is a second explanatory view of a method for manufacturing a toothed belt according to an embodiment; FIG. 5 is a third explanatory view of a method for manufacturing a toothed belt according to an embodiment; FIG. 6 is a perspective view of an adhesion test piece.
[0008] Hereinafter, the embodiments will be described in detail with reference to the drawings.
[0009] 1A and 1B show a toothed belt B according to an embodiment. The toothed belt B according to the embodiment is a meshing power transmission belt and is suitable for use in high-load power transmission applications such as machine tools, printing machines, textile machines, and injection molding machines. The belt length of the toothed belt B is, for example, 500 mm or more and 3000 mm or less. The belt width is, for example, 10 mm or more and 200 mm or less. The belt thickness (maximum) is, for example, 3 mm or more and 20 mm or less.
[0010] The toothed belt B according to the embodiment includes an endless toothed belt main body 11 made of an elastomer formed from a polyurethane composition. The toothed belt main body 11 has a flat belt portion 111 having a horizontally elongated rectangular cross section and a plurality of toothed portions 112 integrally formed on the inner circumferential side of the flat belt portion 111. The plurality of toothed portions 112 are spaced apart at a constant pitch in the belt length direction.
[0011] The tooth profile of the toothed portion 112 in a side view may be, for example, an STS tooth profile with both sides bulging outward in an arc shape, or a trapezoidal tooth profile. The number of teeth in the toothed portion 112 is, for example, 30 to 400. The tooth width (maximum dimension in the belt length direction) is, for example, 2 mm to 10 mm. The tooth height is, for example, 2 mm to 8 mm. The arrangement pitch is, for example, 8 mm to 14 mm.
[0012] The polyurethane composition forming the toothed belt body 11 is a liquid urethane composition obtained by mixing a urethane prepolymer with compounding agents such as a curing agent and a plasticizer, and then curing the liquid urethane composition by heating and pressurizing it.
[0013] Urethane prepolymers are relatively low-molecular-weight urethane compounds having multiple NCO groups at their terminals, obtained by reacting an isocyanate component with a polyol component. Examples of the isocyanate component include tolylene 2,4-diisocyanate (TDI) and 4,4'-diphenylmethane diisocyanate (MDI). Examples of the polyol component include polytetramethylene ether glycol (PTMG). Urethane prepolymers may be composed of either a single urethane compound or a mixture of multiple urethane compounds.
[0014] Examples of the curing agent include amine compounds such as 1,4-phenylenediamine, 2,6-diaminotoluene, 1,5-naphthalenediamine, 4,4'-diaminodiphenylmethane, and 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA). The curing agent preferably contains one or more of these. The amine compound curing agent is a compound containing NH 2 The α value (NH 2 It is preferred that the copolymer is blended so that the ratio (NCO groups / NCO groups) is 0.70 or more and 1.10 or less.
[0015] Examples of the plasticizer include dialkyl phthalates such as dibutyl phthalate (DBP) and dioctyl phthalate (DOP); dialkyl adipates such as dioctyl adipate (DOA); and dialkyl sebacates such as dioctyl sebacate (DOS). The plasticizer preferably contains one or more of these. The amount of the plasticizer to be added is, for example, 3 to 20 parts by mass per 100 parts by mass of the urethane prepolymer.
[0016] Examples of other additives include colorants, antifoaming agents, stabilizers, etc.
[0017] The hardness of the polyurethane composition forming the toothed belt body 11 is, for example, 70° or more and 100° or less. The hardness of this polyurethane composition is measured in accordance with JIS K7312:1996.
[0018] In the toothed belt B according to the embodiment, a core wire 12 is embedded in the flat belt portion 111 of the toothed belt main body 11. The outer diameter D of the core wire 12 is, for example, 0.4 mm or more and 2.7 mm or less.
[0019] From the viewpoint of obtaining high durability, the core wire 12 is preferably a twisted yarn. Examples of the twisted yarn constituting the core wire 12 include single twisted yarn, double twisted yarn, and Lang twisted yarn. The twisted yarn core wire 12 may be an S twisted yarn, a Z twisted yarn, or a combination of both.
[0020] Examples of the fiber material forming the core wire 12 include inorganic fibers such as carbon fibers, glass fibers, and metal fibers, and organic fibers such as aliphatic polyamide fibers, aromatic polyamide fibers, polyethylene terephthalate fibers, polyethylene naphthalate fibers, and polyvinyl alcohol fibers. Of these, the core wire 12 is preferably formed from carbon fibers in order to obtain high durability.
[0021] The core wires 12 are arranged to form a spiral having a pitch in the belt width direction. The core wires 12 may be composed of two threads, an S-twisted thread and a Z-twisted thread, which are arranged to form a double spiral. The core wires 12 are arranged to extend parallel to each other at intervals in the belt width direction, and in this case, the number of core wires 12 per 10 mm of belt width is, for example, 3 threads / 10 mm or more and 16 threads / 10 mm or less.
[0022] The core wire 12 is subjected to an adhesive treatment in which it is immersed in a first aqueous liquid treatment agent containing an epoxy compound and a blocked isocyanate compound, pulled out, and heated, and then immersed in a second aqueous liquid treatment agent containing a silane coupling agent, pulled out, and heated.
[0023] Examples of the epoxy compound contained in the first treatment agent include glycerol polyglycidyl ether, sorbitol polyglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, etc. The epoxy compound preferably contains one or more of these, and more preferably contains glycerol polyglycidyl ether from the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11.
[0024] From the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11, the epoxy equivalent of the epoxy compound is preferably 140 to 160, more preferably 145 to 155. From the same viewpoint, the total chlorine content of the epoxy compound is preferably 5 to 15% by mass, more preferably 8 to 12% by mass.
[0025] The content of the epoxy compound in the first treatment agent is preferably 3% by mass or more and 9% by mass or less, more preferably 5% by mass or more and 7% by mass or less, from the viewpoint of obtaining high adhesion of the core wire 12 to the toothed belt main body 11.
[0026] The blocked isocyanate compound contained in the first treating agent is an isocyanate compound in which the NCO group is blocked with a blocking agent.
[0027] Examples of the isocyanate compound that constitutes the blocked isocyanate compound include 4,4'-diphenylmethane diisocyanate (MDI), tolylene 2,4-diisocyanate (TDI), polymethylene polyphenyl diisocyanate, hexamethylene diisocyanate, and polyaryl polyisocyanate.
[0028] Examples of blocking agents include oximes such as methyl ethyl ketone oxime (MEKO), acetoxime, and cyclohexanone oxime; lactams such as ε-caprolactam and valerolactam; and phenols such as phenol, cresol, and resorcinol.
[0029] The isocyanate compound constituting the blocked isocyanate compound is preferably 4,4'-diphenylmethane diisocyanate (MDI) from the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11. From the same viewpoint, the blocking agent is preferably an oxime, and more preferably methyl ethyl ketone oxime (MEKO). From the same viewpoint, the blocked isocyanate compound preferably contains MDI whose NCO group is blocked with MEKO.
[0030] The dissociation temperature of the blocked isocyanate compound is preferably 160° C. or lower, more preferably 140° C. or lower, from the viewpoint of obtaining high adhesiveness of the cord 12 to the toothed belt body 11 .
[0031] The content of the blocked isocyanate compound in the first treating agent is preferably 6% by mass or more and 12% by mass or less, more preferably 8% by mass or more and 10% by mass or less, from the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11. The content of the blocked isocyanate compound in the first treating agent is preferably greater than the content of the epoxy compound. From the same viewpoint, the mass ratio of the content of the blocked isocyanate compound to the content of the epoxy compound in the first treating agent (content of blocked isocyanate compound / content of epoxy compound) is preferably 1.1 or more and 2 or less, more preferably 1.4 or more and 1.6 or less.
[0032] The first treating agent may contain, in addition to the epoxy compound and the blocked isocyanate compound, a curing agent for the epoxy compound, a surfactant, and the like.
[0033] From the viewpoint of obtaining high adhesion of the core wire 12 to the toothed belt body 11, the solid content concentration of the first treatment agent is preferably 5% by mass or more and 25% by mass or less, and more preferably 10% by mass or more and 20% by mass or less.
[0034] The heating temperature (set temperature in the heating furnace) after immersing the core wires 12 in the first treatment agent is preferably 140° C. or higher and 200° C. or lower, more preferably 160° C. or higher and 180° C. or lower, from the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11. From the same viewpoint, the heating time is preferably 300 seconds or higher and 720 seconds or lower, more preferably 420 seconds or higher and 600 seconds or lower.
[0035] In order to obtain high adhesion of the core wire 12 to the toothed belt main body 11, the amount of solid content of the first treatment agent adhered to the core wire 12 is preferably 2 mass% or more and 10 mass% or less, more preferably 3 mass% or more and 6 mass% or less, relative to the mass of the core wire 12.
[0036] Examples of the silane coupling agent contained in the second treatment agent include amino-based silane coupling agents, epoxy-based silane coupling agents, vinyl-based silane coupling agents, methacrylic acid-based silane coupling agents, mercapto and sulfur-based silane coupling agents, ureido-based silane coupling agents, and isocyanate-based silane coupling agents.
[0037] Examples of amino-based silane coupling agents include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-(N-phenyl)aminopropyltrimethoxysilane.
[0038] Examples of epoxy-based silane coupling agents include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0039] Examples of vinyl-based silane coupling agents include vinyltriethoxysilane, vinyltrimethoxysilane, vinyltris(2-methoxyethoxy)silane, and vinylmethyldimethoxysilane.
[0040] Examples of the methacrylic acid-based silane coupling agent include 3-methacryloxypropyltriethoxysilane and 3-methacryloxypropyltrimethoxysilane.
[0041] Examples of mercapto and sulfur-based silane coupling agents include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-octanoylthio-1-propyltriethoxysilane.
[0042] Examples of ureido-based silane coupling agents include 3-ureidopropyltriethoxysilane.
[0043] Examples of the isocyanate-based silane coupling agent include 3-isocyanatepropyltriethoxysilane and 3-isocyanatepropyltrimethoxysilane.
[0044] The silane coupling agent preferably contains one or more of these, and from the viewpoint of obtaining high adhesion of the core wire 12 to the toothed belt main body 11, it is more preferable that it contains an amino-based silane coupling agent, and it is even more preferable that it contains 3-aminopropyltriethoxysilane and / or N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane.
[0045] The content of the silane coupling agent in the second treatment agent is preferably 3% by mass or more and 15% by mass or less, more preferably 8% by mass or more and 12% by mass or less, from the viewpoint of obtaining high adhesion of the core wire 12 to the toothed belt main body 11.
[0046] The second treatment agent may contain other components in addition to the silane coupling agent.
[0047] From the viewpoint of obtaining high adhesion of the core wire 12 to the toothed belt body 11, the solid content concentration of the second treatment agent is preferably 3% by mass or more and 15% by mass or less, and more preferably 8% by mass or more and 12% by mass or less.
[0048] The heating temperature (set temperature in the heating furnace) after immersing the core wires 12 in the second treatment agent is preferably 210° C. or higher and 270° C. or lower, more preferably 230° C. or higher and 250° C. or lower, from the viewpoint of obtaining high adhesion of the core wires 12 to the toothed belt body 11. From the same viewpoint, the heating time is preferably 300 seconds or higher and 720 seconds or lower, more preferably 420 seconds or higher and 600 seconds or lower.
[0049] In order to obtain high adhesion of the core wire 12 to the toothed belt main body 11, the amount of solid content of the second treatment agent adhered to the core wire 12 is preferably 1 mass% or more and 6 mass% or less, more preferably 2 mass% or more and 4 mass% or less, relative to the mass of the core wire 12.
[0050] In the toothed belt B according to the embodiment, a nonwoven fabric 13 is embedded along the belt length direction, on the inner side of the position in the belt thickness direction of the toothed belt main body 11 where the core wires 12 are embedded. The nonwoven fabric 13 may be composed of one layer or multiple layers.
[0051] The nonwoven fabric 13 contains the polyurethane composition that forms the toothed belt main body 11, and is provided so as to form a layer in side view. The portions of the nonwoven fabric 13 that correspond to the tooth portions 112 penetrate into the tooth portions 112 so as to bulge outward in side view, and expand thickly in the belt thickness direction. The portions of the nonwoven fabric 13 that correspond to the spaces between the tooth portions 112 contact the core wires 12 and are compressed thinly in the belt thickness direction.
[0052] Examples of fiber materials that can be used to form the nonwoven fabric 13 include nylon fibers, polyester fibers, aramid fibers, polyketone fibers, and carbon fibers. The nonwoven fabric 13 is preferably subjected to an adhesive treatment such as immersion in a liquid adhesive and then drying before molding.
[0053] According to the toothed belt B of the embodiment having the above configuration, the core wire 12 is subjected to an adhesion treatment in which it is immersed in a first treatment agent containing an epoxy compound and a blocked isocyanate compound and heated, and then immersed in a second treatment agent containing a silane coupling agent and heated, thereby achieving high adhesion of the core wire 12 to the toothed belt main body 11 made of an elastomer.
[0054] Next, a method for manufacturing the toothed belt B according to the embodiment will be described.
[0055] The manufacturing method of the toothed belt B according to the embodiment includes a urethane composition preparation process for preparing a liquid urethane composition for forming the toothed belt main body 11, a core wire bonding process for applying an adhesive treatment to the core wire 12, and a nonwoven fabric bonding process for applying an adhesive treatment to the nonwoven fabric 13.
[0056] In the urethane composition preparation step, compounding ingredients such as a curing agent and a plasticizer are blended with the urethane prepolymer to prepare a liquid urethane composition.
[0057] In the cord bonding process, a dipping device is used to bond the cord 12. The dipping device has a supply bobbin attachment section on the upstream side and a take-up bobbin attachment section on the downstream side, and a treatment agent tank on the upstream side and a heating furnace on the downstream side of the cord running path between them.
[0058] In the first treatment step, a bobbin wound with a pre-bonded core wire 12 is attached to the payout bobbin attachment section, and an empty bobbin is attached to the take-up bobbin attachment section. A first treatment agent is filled into a treatment agent tank, and the temperature inside a heating furnace is raised to a predetermined set temperature. The core wire 12 is paid out from the bobbin attached to the payout bobbin attachment section, passed through a core wire travel path, and wound onto a bobbin attached to the take-up bobbin attachment section. The core wire 12 is run from the payout bobbin attachment section to the take-up bobbin attachment section. As a result, the core wire 12 is immersed in the first treatment agent containing an epoxy compound and a blocked isocyanate compound in the treatment agent tank, pulled out, introduced into a heating furnace, and heated. After the first treatment step, the bobbin wound with the core wire 12 is removed from the take-up bobbin attachment section. This first treatment step may be performed once or repeatedly multiple times.
[0059] In the second treatment step, a bobbin wound with the core wire 12 after the first treatment step is attached to the payout bobbin attachment section, and an empty bobbin is attached to the take-up bobbin attachment section, respectively. The first treatment agent in the treatment agent tank is replaced with a second treatment agent, and the temperature inside the heating furnace is changed to a predetermined set temperature. The core wire 12 is paid out from the bobbin attached to the payout bobbin attachment section, passed through the core wire travel path, and wound onto a bobbin attached to the take-up bobbin attachment section. The core wire 12 is run from the payout bobbin attachment section to the take-up bobbin attachment section. As a result, the core wire 12 is immersed in the second treatment agent containing a silane coupling agent in the treatment agent tank, pulled out, introduced into the heating furnace, and heated, and then continuously wound onto a bobbin at the take-up bobbin attachment section. The bobbin wound with the core wire 12 after the second treatment step is then removed from the take-up bobbin attachment section. This second treatment step may also be performed once or repeatedly.
[0060] In the nonwoven fabric bonding process, the nonwoven fabric 13 is immersed in a liquid adhesive and then dried.
[0061] After preparing the above components, as shown in Fig. 2A, adhesively treated nonwoven fabric 13 is placed on a cylindrical inner mold 21, and adhesively treated core wire 12 is spirally wound on top of it. At this time, grooves 22 extending in the axial direction and having cross sections corresponding to the tooth portions 112 are provided at regular intervals in the circumferential direction on the outer periphery of inner mold 21, and ridges 23 extending in the axial direction are formed between each groove 22, so that nonwoven fabric 13 and core wire 12 are supported by ridges 23.
[0062] 2B, the inner mold 21 is placed inside a cylindrical outer mold 24. At this time, a cavity C for molding the toothed belt main body is formed between the inner mold 21 and the outer mold 24.
[0063] Next, as shown in Figure 2C, a liquid urethane composition is injected into the sealed cavity C, filling it, and heated. At this time, the urethane composition flows and hardens, forming the toothed belt main body 11 of the polyurethane composition. Also, teeth 112 are formed in the recessed grooves 22. The core wires 12 are adhered to and embedded in the toothed belt main body 11. Furthermore, the nonwoven fabric 13 is impregnated with the urethane composition and hardens, and is also adhered to and embedded in the toothed belt main body 11. In this way, the toothed belt main body 11, the core wires 12, and the nonwoven fabric 13 are integrated into one composite, and a cylindrical belt slab S is molded.
[0064] Finally, the belt slab S is removed from the inner mold 21 and the outer mold 24 and cut into rings to obtain the toothed belt B according to the embodiment.
[0065] In the above embodiment, the toothed belt B is composed of the toothed belt main body 11, the core wire 12, and the nonwoven fabric 13, but this is not particularly limited to this, and a reinforcing fabric may be provided on the toothed portion side surface on the inner periphery of the toothed belt main body and / or on the back surface on the outer periphery of the toothed belt main body.
[0066] In the above embodiment, the toothed belt B has the toothed belt main body 11 formed of a polyurethane composition, but this is not particularly limited, and the toothed belt main body may be formed of a cross-linked rubber composition. In this case, after the second treatment step, the core wires 12 may be subjected to an RFL treatment step in which they are immersed in an RFL aqueous solution and then heated, and / or a rubber cement treatment step in which they are immersed in rubber cement and then heated.
[0067] In the above embodiment, the toothed belt B is used as the transmission belt, but the present invention is not limited to this, and a flat belt, a V-belt, a V-ribbed belt, or the like may also be used.
[0068] (Core Wire) The following core wires were fabricated by applying adhesive treatment to Examples 1 to 4 and a comparative example. The configurations of each are also shown in Table 1.
[0069] Example 1 As a core wire, a single twist yarn was prepared by twisting a bundle of 12,000 carbon fiber filaments with a filament diameter of 7 μm in one direction.
[0070] An aqueous first treating agent with a solids concentration of 15% by mass was prepared, containing 5.91% by mass of glycerol polyglycidyl ether (epoxy equivalent: 141, total chlorine content: 9% by mass) of an epoxy compound, 8.88% by mass of MDI (dissociation temperature: 120°C or higher) in which the NCO group of a blocked isocyanate compound has been blocked with MEKO, 0.07% by mass of an imidazole-based epoxy resin curing agent, 0.15% by mass of a surfactant, and 85% by mass of water.
[0071] An aqueous second treatment agent with a solids concentration of 5% by mass was prepared, containing 5% by mass of 3-aminopropyltriethoxysilane, an amino-silane coupling agent, and 95% by mass of water.
[0072] The core wire was subjected to an adhesion treatment consisting of a first treatment step in which the core wire was immersed in a first treatment agent and heated, and a second treatment step in which the core wire was subsequently immersed in a second treatment agent and heated. The heating temperature in the first treatment step was 170°C and the heating time was 470 seconds. The heating temperature in the second treatment step was 240°C and the heating time was 470 seconds. The resulting adhesively treated core wire was designated Example 1.
[0073] Example 2 A core wire subjected to an adhesive treatment was obtained in the same manner as in Example 1, except that the second treatment agent used had a solid content concentration of 10% by mass.
[0074] Example 3 was a core wire that had been subjected to an adhesive treatment and obtained in the same manner as in Example 1, except that N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane was used as the amino-based silane coupling agent in the second treatment agent.
[0075] Example 4 A core wire subjected to an adhesive treatment was obtained in the same manner as in Example 3, except that the second treatment agent used had a solid content concentration of 10% by mass.
[0076] Comparative Example A comparative example was a cord that had been subjected to adhesive treatment in the same manner as in Examples 1 to 4, except that the second treatment step was not carried out.
[0077] An attempt was made to prepare a one-component treatment agent containing all of the epoxy compound, blocked isocyanate compound, and amino-silane coupling agent, but it gelled, and it was not possible to obtain a product that could be used for adhesive treatment.
[0078]
[0079] (Urethane Composition) A liquid urethane composition A was prepared by blending 16.58 parts by mass of a curing agent, MOCA, and 1.6 parts by mass of a colorant with 100 parts by mass of a urethane prepolymer having TDI as the isocyanate component and PTMG as the polyol component.
[0080] (Test Method and Results) For the core wires subjected to the adhesive treatment of each of Examples 1 to 4 and the Comparative Example, adhesion test specimens T as shown in Figure 3 were prepared. These adhesion test specimens T were prepared by curing urethane composition A to form urethane block pieces U of the polyurethane composition, 5 mm thick and 10 mm square, and then embedding a core wire V cut into a short length in the center so that one tip of the core wire V penetrated through the thickness direction.
[0081] Using a tensile tester, the urethane block piece U of the adhesive test piece T was attached to one chuck and the core wire V to the other chuck, and the pull-out force required to pull the core wire V from the urethane block piece U was measured at an ambient temperature of 25°C and a pulling rate of 500 mm / min, and this was divided by the embedded length of the core wire V, 5 mm, to calculate the pull-out adhesive strength per mm. The test results are shown in Table 1.
[0082] The present invention is useful in the technical fields of power transmission belts, their manufacturing methods, and core wires.
[0083] B: Toothed belt (power transmission belt) C: Cavity S: Belt slab T: Adhesion test piece U: Urethane block piece V: Core wire 11: Toothed belt body 111: Flat belt portion 112: Tooth portion 12: Core wire 13: Nonwoven fabric 21: Inner mold 22: Groove 23: Protrusion 24: Outer mold
Claims
1. A power transmission belt having a core wire embedded in an elastomer belt body, the core wire being subjected to an adhesion treatment in which it is immersed in a first treating agent containing an epoxy compound and a blocked isocyanate compound and heated, and then immersed in a second treating agent containing a silane coupling agent and heated.
2. The power transmission belt according to claim 1, wherein the belt body is formed of a polyurethane composition.
3. A power transmission belt according to claim 1 or 2, wherein the core wire is made of carbon fiber.
4. A power transmission belt according to any one of claims 1 to 3, wherein the epoxy compound contains polyglycerol polyglycidyl ether.
5. A power transmission belt according to any one of claims 1 to 4, wherein the content of the epoxy compound in the first treatment agent is 3% by mass or more and 9% by mass or less.
6. A power transmission belt according to any one of claims 1 to 5, wherein the blocked isocyanate compound contains 4,4'-diphenylmethane diisocyanate in which the NCO group is blocked with methyl ethyl ketone oxime.
7. The power transmission belt according to any one of claims 1 to 6, wherein the content of the blocked isocyanate compound in the first treatment agent is 6% by mass or more and 12% by mass or less.
8. The power transmission belt according to any one of claims 1 to 7, wherein the content of the blocked isocyanate compound in the first treatment agent is greater than the content of the epoxy compound.
9. The power transmission belt according to claim 8, wherein the mass ratio of the content of the blocked isocyanate compound to the content of the epoxy compound in the first treatment agent is 1.1 or more and 2 or less.
10. A power transmission belt according to any one of claims 1 to 9, wherein the amount of solid matter of the first treatment agent adhering to the core wire is 2 mass % or more and 10 mass % or less with respect to the mass of the core wire.
11. A power transmission belt according to any one of claims 1 to 10, wherein the silane coupling agent contains an amino-silane coupling agent.
12. The power transmission belt according to claim 11, wherein the silane coupling agent contains 3-aminopropyltriethoxysilane and / or N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, which are amino-based silane coupling agents.
13. A power transmission belt according to any one of claims 1 to 12, wherein the amount of solid matter of the second treatment agent adhering to the core wire is 1 mass % or more and 6 mass % or less with respect to the mass of the core wire.
14. A core wire embedded in an elastomer belt body of a transmission belt, the core wire being subjected to an adhesive treatment in which the core wire is immersed in a first treating agent containing an epoxy compound and a blocked isocyanate compound and heated, and then immersed in a second treating agent containing a silane coupling agent and heated.
15. A method for manufacturing a power transmission belt having a core wire embedded in an elastomer belt body, comprising a core wire bonding process step of bonding the core wire, the core wire bonding process step including: a first treatment step of immersing the core wire in a first treatment agent containing an epoxy compound and a blocked isocyanate compound, and heating the core wire; and a second treatment step of immersing the core wire in a second treatment agent containing a silane coupling agent, after the first treatment step, and heating the core wire.
Citation Information
Patent Citations
Power transmission belt and its manufacturing method
JP2008082538A
Rubber-reinforcing fiber and method for producing the same
JP2009275303A
Treatment agent for transmission belt core wire, and core wire and method for producing the same
JP2020158947A