Printed circuit board substrate reliability testing method

The nanoindenter-based method addresses the inefficiencies of traditional reliability testing for printed wiring board substrates by measuring crack loads and contact stiffness, offering a quicker and more effective evaluation of substrate reliability and predicting crack rates, thus enhancing the assessment of substrate integrity.

WO2024219249A1PCT designated stage expired Publication Date: 2024-10-24RESONAC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014015
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-05
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current reliability testing methods for printed wiring board substrates, such as temperature cycle tests, are time-consuming and inefficient, particularly due to increased stress from thermal expansion coefficient differences between resin and inorganic components, leading to cracks and reduced long-term reliability.

Method used

A nanoindenter-based method to measure the load at which cracks occur in printed wiring board substrates, specifically using a Berkovich indenter to analyze load-displacement and contact stiffness curves, providing a faster and more efficient evaluation of substrate reliability.

Benefits of technology

This method allows for rapid evaluation of substrate reliability, correlating crack generation load with temperature cycle test results, enabling prediction of crack rates and improving the assessment of substrate integrity without the need for lengthy testing periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014015_24102024_PF_FP_ABST
    Figure JP2024014015_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a printed circuit board substrate reliability testing method in which the load at which a crack is generated in a printed circuit board substrate is measured using a nanoindenter.
Need to check novelty before this filing date? Find Prior Art

Description

Reliability test method for printed wiring board substrates

[0001] The present embodiment relates to a reliability test method for a substrate for a printed wiring board.

[0002] In recent years, electronic devices such as computers have been using faster and larger signals, and the semiconductor packages used in these electronic devices have also been becoming more highly integrated and functional. Furthermore, semiconductor packages are required to be able to withstand a variety of temperature conditions depending on the equipment they are used in and the installation environment, making it increasingly important to ensure long-term reliability against temperature changes.

[0003] Substrates containing a resin component as an insulating material are used as substrates for printed wiring boards, but stress occurs during temperature changes due to the difference in thermal expansion coefficient between the resin component and inorganic components such as conductor layers, semiconductor chips, etc., and cracks may occur in the substrate for printed wiring boards. In particular, in recent years, the number of build-up layers has tended to increase, so stress caused by the difference in thermal expansion coefficients is becoming larger, and the problem of cracks occurring due to temperature changes has become apparent.

[0004] A temperature cycle test is generally carried out as a reliability test method for substrates for printed wiring boards (see, for example, Patent Document 1).

[0005] Japanese Patent Application Laid-Open No. 2006-093618

[0006] Temperature cycle testing is an effective method for verifying the long-term reliability of a test object against temperature changes by repeatedly heating and cooling it. However, since it takes several weeks to several months to obtain test results, a simpler reliability evaluation method is desired.

[0007] In view of the current situation, an object of this embodiment is to provide a method for testing the reliability of a substrate for a printed wiring board that can be easily carried out.

[0008] As a result of extensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by the present embodiment described below. Specifically, the present embodiment relates to the following [1] to [6]. [1] A reliability test method for a substrate for printed wiring boards, comprising measuring a load at which a crack occurs in the substrate for printed wiring boards using a nanoindenter. [2] The reliability test method for a substrate for printed wiring boards described in [1] above, wherein the substrate for printed wiring boards comprises a cured resin and a glass cloth. [3] The reliability test method for a substrate for printed wiring boards described in [1] or [2] above, wherein the substrate for printed wiring boards has two or more layers each comprising a cured resin and a glass cloth. [4] The reliability test method for a substrate for printed wiring boards described in [2] above, wherein an indenter of the nanoindenter is pressed into the cured resin. [5] The reliability test method for a substrate for a printed wiring board according to any one of [1] to [4] above, wherein an indenter of the nanoindenter is pressed into a cross section of the substrate for a printed wiring board. [6] The reliability test method for a substrate for a printed wiring board according to any one of [1] to [5] above, wherein the indenter of the nanoindenter is a Berkovich indenter.

[0009] According to this embodiment, it is possible to provide a method for testing the reliability of a substrate for a printed wiring board, which can be easily carried out.

[0010] 1 is a graph for explaining a load-displacement curve. FIG. 2 is a graph for explaining a load-contact stiffness curve. FIG. 3 is a schematic diagram for explaining the observation position using an optical microscope in a liquid bath temperature cycle test. FIG. 4 is a schematic diagram for explaining the position where a test piece was taken and the test area for a destructive test using a nanoindenter. FIG. 5 is a diagram for explaining an analysis method for a load-contact stiffness curve. FIG. 6 is a graph created from the results of an example, showing the correlation between the crack initiation load W1 and the crack occurrence rate after a temperature cycle test (1,000 cycles).

[0011] The mechanism of action described in this specification is speculation and does not limit the mechanism by which the effects of this embodiment are achieved. Any combination of the items described in this specification is also included in this embodiment.

[0012] [Method for testing reliability of substrate for printed wiring board] The method for testing reliability of substrate for printed wiring board of this embodiment is a method for testing reliability of substrate for printed wiring board, in which a nanoindenter is used to measure the load at which cracks occur in the substrate for printed wiring board. The reliability test method of this embodiment does not require a long period of time as in the case of a temperature cycle test, and therefore the reliability of the substrate for printed wiring board can be easily evaluated.

[0013] <Nanoindenter> The nanoindenter used in the reliability testing method of this embodiment is a microhardness tester that can press a tiny indenter into the surface of a sample to a depth of several nanometers to several tens of micrometers and measure the relationship between the amount of displacement and the load at that time.

[0014] <Printed Wiring Board Substrate> The printed wiring board substrate to be tested in the reliability test method of this embodiment is not particularly limited, and known printed wiring board substrates can be used as the test subject. The insulating layer of the printed wiring board substrate may be a layer containing a resin but not glass cloth, or a layer containing a resin and glass cloth. The layer containing a resin and glass cloth is preferably a layer containing a cured resin and glass cloth. In this specification, the term "cured resin" refers to a cured product containing at least a resin but not glass cloth, and is preferably a cured product of a thermosetting resin composition containing a thermosetting resin. The thermosetting resin composition may contain, as necessary, a curing agent, a curing accelerator, an inorganic filler, etc., as components other than the thermosetting resin. The insulating layer of the printed wiring board substrate may be a single layer or multiple layers. A specific example of a test subject in the reliability test method of this embodiment is a printed wiring board substrate having two or more layers containing a cured resin and glass cloth. The printed wiring board substrate may have components other than the insulating layer that a printed wiring board substrate may generally have. Examples of members other than insulating layers include a conductor layer formed on the surface of the substrate, a conductor layer formed between insulating layers, and a semiconductor chip mounted on the surface of the substrate.

[0015] The content of the cured resin in the layer containing the cured resin and the glass cloth is not particularly limited and may be, for example, 25 to 75 mass %, 30 to 70 mass %, or 35 to 65 mass %. The thickness of each layer containing the cured resin and the glass cloth is not particularly limited and may be, for example, 200 to 1,900 μm, 500 to 1,800 μm, or 800 to 1,700 μm. When the substrate has two or more layers containing the cured resin and the glass cloth, the number of layers containing the cured resin and the glass cloth is not particularly limited and may be, for example, 2 to 19 layers, 5 to 18 layers, or 8 to 17 layers.

[0016] <Test Conditions> Next, the test conditions for the destructive test using a nanoindenter will be described. In the following description, a test using a nanoindenter to measure the load at which a crack occurs in a printed wiring board substrate will be referred to as a "destructive test." In the following description, the load at which a crack occurs in a printed wiring board substrate measured in the destructive test will be referred to as the "crack occurrence load."

[0017] The position of the printed wiring board substrate where the destructive test is performed using the nanoindenter is not particularly limited. However, it is preferable to select a location where cracks are likely to occur during a temperature cycle test. The location where cracks are likely to occur during a temperature cycle test is a location where stress is likely to occur in the printed wiring board substrate, making it easier to obtain the crack initiation load within the range of the destructive test using the nanoindenter. In a plan view of the printed wiring board substrate, an example of a location where the destructive test is performed is preferably the edge of the printed wiring board substrate, from the viewpoint of ease of obtaining the crack initiation load. Furthermore, from the viewpoint of ease of obtaining the crack initiation load, it is preferable that the indenter of the nanoindenter be pressed into the cross section of the printed wiring board substrate. Since the printed wiring board substrate is obtained by cutting the outer shape in a plan view into a desired shape, the end face of the printed wiring board substrate corresponds to the cross section. In a cross-sectional view of the printed wiring board substrate, an example of a location where the destructive test is performed is approximately the center in the thickness direction of the printed wiring board substrate. That is, the location where the destructive test is carried out is preferably a cross section of an end portion of the substrate for printed wiring boards in a plan view, and also approximately the center of the substrate for printed wiring boards in a cross section.

[0018] In addition, when performing a destructive test, it is preferable to process the printed wiring board substrate by cutting or the like to form a test piece including an area where the destructive test will be performed so that it can be attached to a nanoindenter. The surface of the test piece into which the indenter of the nanoindenter is pressed is preferably polished smooth before or after being collected as a test piece, from the viewpoint of suppressing the occurrence of variations in test results due to surface irregularities. The polishing method is not particularly limited, but mechanical polishing or chemical mechanical polishing is preferred.

[0019] If necessary, the test specimens taken from the substrate for printed wiring boards may be pretreated before the destructive test. Examples of pretreatment include heating and cooling. By performing the heating and cooling pretreatments, internal stress accumulates in the test specimens, making it easier to obtain the crack initiation load within the range of the destructive test using a nanoindenter.

[0020] (Conditions for Destructive Testing) The type of indenter of the nanoindenter is not particularly limited, but from the viewpoint of versatility, a Berkovich indenter is preferred. A Berkovich indenter is an indenter in which the shape of the surface that presses into the test piece is a triangular pyramid (edge ​​spacing 115°). The type and edge spacing of the indenter are not particularly limited, and a Berkovich indenter (edge ​​spacing 100°), a Rockwell indenter, a Vickers indenter, a Knoop indenter, or a Shore indenter may be used.

[0021] Because the indenter of the nanoindenter is very small, when the test subject is a substrate containing multiple materials, such as a layer containing a cured resin and glass cloth, the load-displacement curve obtained may vary depending on the position at which the indenter is pressed. When the test subject is a substrate having a layer containing a cured resin and glass cloth, if the position at which the indenter is pressed is the glass cloth or the cured resin located close to the glass cloth, cracks in the glass cloth are likely to occur. If the cured resin is located a moderate distance from the glass cloth, cracks at the interface between the glass cloth and the cured resin and cracks in the cured resin are likely to occur. If the cured resin is located even further away from the glass cloth, cracks are likely to occur only in the cured resin. In temperature cycle tests of substrates having a layer containing a cured resin and glass cloth, cracks at the interface between the cured resin and the glass cloth and cracks in the cured resin are likely to become a problem, so it is preferable to adjust the position at which the indenter is pressed so that cracks at the interface between the cured resin and the glass cloth and cracks in the cured resin are likely to occur. From the above viewpoints, it is preferable to press the indenter into the cured resin product, and it is preferable to press the indenter into the cured resin product at a position that is appropriately distanced from the glass cloth. On the surface where the indenter is pressed, the shortest distance between the glass cloth and the center position where the indenter is pressed on the cured resin product may be, for example, 1 to 10 μm, 2 to 8 μm, or 3 to 7 μm. The position where the indenter is pressed can be adjusted using an optical microscope and micrometer attached to the nanoindenter.

[0022] The pressing speed of the indenter is not particularly limited, but may be, for example, 15 to 55 mN / s, 25 to 50 mN / s, or 35 to 45 mN / s. The temperature at which the destructive test is performed is not particularly limited, but from the viewpoint of workability, it may be 5 to 50°C, 10 to 40°C, or 20 to 30°C. The atmosphere in which the destructive test is performed is not particularly limited, but from the viewpoint of workability, it is preferably in air.

[0023] (Analysis Conditions) A load-displacement curve is obtained by the above-described fracture test. An example of a load-displacement curve is shown in FIG. 1. As shown in the load-displacement curve in FIG. 1, the load tends to increase overall as the depth to which the indenter is pressed into the test piece, i.e., the displacement, increases. However, due to cracks in the test piece, a region where the load increases more slowly occurs, as shown in region A in FIG. 1. FIG. 2 shows a curve (hereinafter also referred to as the "load-contact stiffness curve") obtained by plotting the contact stiffness calculated as the slope of the load-displacement curve shown in FIG. 1 on the vertical axis and the load on the horizontal axis. As shown in FIG. 2, region A in FIG. 1 appears as a downward peak where the contact stiffness decreases. Hereinafter, this peak will be referred to as the "crack initiation peak."

[0024] As described in the examples below, the load at which the crack initiation peak appears correlates with the crack initiation rate in a temperature cycle test. Therefore, the reliability of a printed wiring board substrate can be evaluated by measuring the load at which the crack initiation peak appears (hereinafter also referred to as the "crack initiation load"). For example, by previously understanding the correlation between the crack initiation load and the crack initiation rate in a temperature cycle test, the crack initiation rate in a temperature cycle test can be predicted from the crack initiation load.

[0025] When multiple crack initiation peaks appear, a threshold value may be set for the magnitude of the crack initiation peak, and crack initiation peaks having a predetermined magnitude or greater may be used as an index for reliability evaluation. The threshold value for the magnitude of the crack initiation peak may be, for example, the contact rigidity reduction rate (%) calculated by the following formula (1): Contact rigidity reduction rate (%) = (S1 - S2) × 100 / S1 (1) (In the formula, S1 refers to the contact rigidity at the crack initiation peak when the contact rigidity begins to decrease, and S2 refers to the contact rigidity at the peak top of the crack initiation peak.) The "contact rigidity at which the contact rigidity begins to decrease" can be determined, for example, by the method described in the Examples. The "peak top" refers to the apex of the crack initiation peak (the point showing the minimum value of contact rigidity at the peak). After the crack initiation peak to be used as an index for reliability evaluation is determined, for example, the load that gives the peak top of the crack initiation peak may be used for reliability evaluation. When multiple crack initiation peaks that satisfy the threshold value appear, it is preferable to use the crack initiation peak that appears at the lowest load for reliability evaluation.

[0026] The crack initiation peak, which is an appropriate indicator of reliability, may vary depending on the position where the indenter is pressed in. Therefore, it is preferable to determine the position where the indenter is pressed in, and then perform a temperature cycle test and a destructive test using a nanoindenter in advance on multiple types of test objects under the condition where the indenter is pressed in that position, and identify, among the crack initiation peaks that appear, those that have a high correlation with the temperature cycle test.

[0027] The present embodiment will be specifically described below with reference to examples, although the present embodiment is not limited to the following examples.

[0028] [Preparation of Substrates for Printed Wiring Boards] Production Examples 1 to 6 Using a laminate obtained by laminating and molding 12 sheets of a predetermined insulating layer-forming material (prepreg containing a thermosetting resin composition and glass cloth) as a core layer, and a build-up material (manufactured by Ajinomoto Co., Inc., product name "GX92", thickness 30 μm) (hereinafter also referred to as "Bu") and copper foil (thickness 18 μm or 12 μm), printed wiring board substrates 1 to 6 (substrates with a thickness of 1.7 to 2.0 mm, cut into a rectangular shape with an outer shape of 60 mm x 60 mm in plan view) having the following multilayer structure were prepared. Note that the core layers of the obtained printed wiring board substrates 1 to 6 were each different. <Substrate Structure> Copper foil (18 μm) / Bu (30 μm) / Bu (30 μm) / Copper foil (18 μm) / Bu (30 μm) / Bu (30 μm) / Copper foil (18 μm) / Bu (30μm) / Bu (30μm) / Copper foil (18μm) / Bu (30μm) / Bu (30μm) / Copper foil (12μm) / Core layer (1150 〜1350μm) / copper foil (12μm) / Bu (30μm) / Bu (30μm) / copper foil (18μm) / Bu (30μm) / Bu (30μm) / copper foil (18μm) / Bu (30μm) / Bu (30μm) / copper foil (18μm) / Bu (30μm) / Bu (30μm) / copper foil (18μm) Note that the thickness in parentheses above means the thickness of each layer before lamination.

[0029] Next, a silicon semiconductor chip (a rectangle with an outer shape of 20 mm x 20 mm in plan view and a thickness of 0.775 mm) was placed in the center of one surface of the substrate for printed wiring board obtained above, with the circuit side facing downward, and the gap between the semiconductor chip and the substrate was sealed with a liquid sealant (Resonac Inc., product name "CEL-C-3730 series"), thereby obtaining semiconductor chip-mounted substrates 1 to 6 for liquid bath temperature cycle tests.

[0030] [Liquid Bath Temperature Cycle Test] For the liquid bath temperature cycle test, five semiconductor chip-mounted substrates of the same type were prepared. Each of the five substrates was subjected to a temperature cycle test in which heating and cooling were repeated under conditions of -65°C for 5 minutes, 150°C for 5 minutes, and a transfer time of 18 seconds between the low-temperature and high-temperature baths. After 1,000 cycles, the substrates were removed and predetermined positions on the substrates were observed with an optical microscope to check for the presence or absence of cracks. A perspective view illustrating the observation positions using the optical microscope is shown in Figure 3. The observation positions were eight positions on substrate 1 shown in Figure 3, each of the four corners of the substrate indicated by area 10 (shaded area) being observed from two directions. Each observation area was an area of ​​1,500 μm x 1,500 μm. The above eight locations were observed for each of the five substrates, and the ratio of locations where cracks were observed out of a total of 40 locations [number of locations where cracks were observed x 100 / 40 locations] (unit: %) was taken as the crack occurrence rate in the liquid bath temperature cycle test.

[0031] [Destructive Testing Using a Nanoindenter] Examples 1 to 6 1. Preparation of Test Pieces FIG. 4 shows a perspective view illustrating the positions where the test pieces were taken and the positions where the destructive testing was performed on the test pieces. The printed wiring board substrates 1 to 6 obtained in Production Examples 1 to 6 were cut, and test pieces measuring 1.5 mm (cutting width W) × 60 mm (substrate length L) × 1.7 to 2.0 mm (substrate thickness T), as shown by area 20 in FIG. 4, were taken. The test area of ​​the taken test piece where the destructive testing was performed was the area shown by area 30 in FIG. 4. Area 30 is a cross section of the edge of the printed wiring board substrate 1 and is approximately the center of the printed wiring board substrate 1 in a cross-sectional view. Furthermore, area 30 is approximately 10 mm away from the corner of the printed wiring board substrate 1 (distance B in FIG. 4). The cross section of the printed wiring board substrate including area 30 was mechanically polished in advance using 4000-grit abrasive paper. The obtained test piece was heat-treated in an air atmosphere at 260° C. for 6 hours, and cooled to room temperature, and used as the object of measurement with the nanoindenter.

[0032] 2. Destruction Test Using a Nanoindenter The test piece obtained above was attached to a nanoindenter so that the indenter of the nanoindenter was pressed into the test area of ​​the test piece. Next, the position of the indenter was adjusted using the optical microscope and micrometer attached to the nanoindenter so that the shortest distance between the glass cloth and the center position of the indenter on the cured resin surface where the indenter was pressed was 5 μm, and a destructive test was carried out under the following conditions: (Conditions) - Apparatus: Shimadzu Corporation, product name "DUH-211S" - Indenter type: Berkovich indenter (edge ​​spacing 115°) - Indentation speed: 39 mN / s - Maximum load: 490 mN - Measurement temperature: 25°C - Measurement atmosphere: Air

[0033] 3. Analysis of measurement results Among the crack initiation peaks that appeared in the load-contact stiffness curve obtained by the above-mentioned destructive test, crack initiation peaks for which the contact stiffness reduction rate calculated by the above-mentioned formula (1) was 37% or more were identified. S1 in the above-mentioned formula (1) was identified by the following procedure. A schematic diagram for explaining the method for identifying S1 is shown in Figure 5. The contact stiffness at the peak top of the peak to be analyzed is S2, and the load that applies S2 is W. S2、 W S2 -25mN to W 1A , W S2 -15mN to W 1B Next, W 1A ~W 1B In the range of , the approximate line of the load-contact stiffness curve is found by the least squares method, and this is called "approximate line 1". Next, the contact stiffness S2 and W S2 Calculate the absolute value D of the difference between the contact stiffness of the approximate line 1 at and the load that gives the contact stiffness of S2 + 0.7D as W 2A、 The load that gives the contact stiffness of S2 + 0.5D is W 2B、 And W 2A ~W 2B In the range of , an approximate line of the load-contact stiffness curve was found by the least squares method, and this was designated as "approximate line 2." The contact stiffness at the intersection of approximate line 1 and approximate line 2 obtained above was designated as S1.

[0034] Among the crack initiation peaks identified by the above method at which the contact rigidity reduction rate was 37% or more, the crack initiation peak that appeared at the lowest load was identified, and the load at which the peak top of that crack initiation peak was determined as the crack initiation load W1. Figure 6 shows a graph plotting the crack initiation load W1 obtained above on the horizontal axis and the crack initiation rate after the liquid bath temperature cycle test (1,000 cycles) on the vertical axis, along with a linear approximation line obtained by the least squares method for the plot. As is clear from Figure 6, there is a high correlation between the crack initiation load W1 and the crack initiation rate after the liquid bath temperature cycle test (1,000 cycles), demonstrating that the reliability test method of this embodiment is useful as a reliability test method for substrates for printed wiring boards.

[0035] REFERENCE SIGNS LIST 1 printed wiring board substrate 10 observation area 20 sample area for test piece 30 test area W width L length T thickness B distance S1, S2 contact stiffness W 1A , W 1B , W 2A , W 2B , W S2 Weighted A area

Claims

1. A reliability test method for a substrate for printed wiring boards, comprising using a nanoindenter to measure the load at which a crack occurs in the substrate for printed wiring boards.

2. The reliability test method for a substrate for a printed wiring board according to claim 1, wherein the substrate for a printed wiring board comprises a cured resin and a glass cloth.

3. The reliability test method for a substrate for printed wiring board according to claim 1 or 2, wherein the substrate for printed wiring board has two or more layers containing a cured resin and a glass cloth.

4. The reliability test method for a substrate for printed wiring boards according to claim 2, wherein the indenter of the nanoindenter is pressed into the cured resin.

5. A reliability test method for a substrate for printed wiring boards according to claim 1 or 2, wherein an indenter of the nanoindenter is pressed into a cross section of the substrate for printed wiring boards.

6. The reliability test method for a substrate for printed wiring boards according to claim 1 or 2, wherein the type of indenter of the nanoindenter is a Berkovich indenter.

Citation Information

Patent Citations

  • Multilayer printed circuit board

    JP2006093618A

  • Method for measuring film peel load

    JP1995260658A

  • Physical property of thin film evaluating apparatus

    JP1995325029A

  • Material tester

    JP2001108586A

  • Core substrate for build-up multilayer printed wiring board

    JP2002151848A