Method for producing lithium metal composite oxide

The method of supplying low dew point gas and using countercurrent oxygen in a rotary kiln addresses the stability issues in producing lithium metal composite oxide by preventing dew condensation, ensuring stable production and material flow.

WO2024219262A1PCT designated stage expired Publication Date: 2024-10-24SUMITOMO CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014185
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-05
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Fluidized firing furnaces face challenges in stably producing lithium metal composite oxide due to issues with dew condensation causing blockages in the material supply system, leading to unstable production.

Method used

A method involving a firing device with a low dew point gas supply upstream of the heating means and countercurrent oxygen-containing gas contact during firing, using a rotary kiln or similar setup, to dehumidify and dry water vapor, preventing condensation and ensuring stable material flow and production.

Benefits of technology

This approach effectively prevents dew condensation, maintains stable raw material supply, and enables consistent production of lithium metal composite oxide, enhancing the reliability of the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014185_24102024_PF_FP_ABST
    Figure JP2024014185_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for producing a lithium metal composite oxide, the method including a step in which an object to be treated is burned using a burning device to obtain a burned object. The burning device comprises an introduction part through which the object to be treated is introduced, a conveyance part for conveying the object to be treated introduced through the introduction part, a cylindrical kiln main body, a discharge opening for discharging the burned object, and a gas supply means. In the step, a low-dew-point gas having a dew point of 10°C or lower is supplied from the upstream side of a heating means, an oxygen-containing gas is supplied from the downstream side of the heating means, and a value shown by expression (A) is 0.0001 Nm3 / kg to 0.30 Nm3 / kg. Expression (A): [supply amount of low-dew-point gas (Nm3 / hr)] / [supply amount of object to be treated (kg / hr)]
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing lithium metal composite oxide

[0001] The present invention relates to a method for producing a lithium metal composite oxide. This application claims priority to Japanese Patent Application No. 2023-067067, filed on April 17, 2023, the contents of which are incorporated herein by reference.

[0002] A method for producing a lithium metal composite oxide used as a positive electrode active material for a lithium secondary battery includes a step of mixing a metal composite compound precursor with a lithium compound and calcining the resulting mixture. The calcination step is carried out using a continuous calcination furnace such as a tunnel kiln or a roller hearth kiln, or a fluidized bed calcination furnace such as a rotary kiln.

[0003] For the purpose of accelerating the firing reaction, Patent Document 1 discloses a method for producing a positive electrode active material using a firing furnace equipped with two air supply systems.

[0004] JP-A-2019-75253

[0005] The fluidized bed calciner has the problem that it is difficult to stably produce lithium metal composite oxide.

[0006] An object of the present invention is to provide a method for producing a lithium metal composite oxide that allows stable production.

[0007] The present invention encompasses the following [1] to [7]: [1] A method for producing a lithium metal composite oxide, comprising a step of calcining a material to be treated using a calcination device to obtain a calcined material, the material to be treated comprising a mixture of a metal composite compound and a lithium compound, the calcination device comprising an input section into which the material to be treated is charged, a transport section for transporting the material to be treated charged from the input section, a cylindrical kiln body, an outlet for discharging the calcined material, and gas supply means, the kiln body comprising heating means, and in the step, a low dew point gas having a dew point of 10°C or less is supplied from the upstream side of the heating means, an oxygen-containing gas is supplied from the downstream side of the heating means, the material to be treated is calcined by countercurrent contact with the oxygen-containing gas, and a value represented by the following formula (A) is 0.0001 Nm 3 / kg or more 0.30Nm 3 / kg or less. 3 / hour) / supply amount of material to be treated (kg / hour) [2] The method for producing a lithium metal composite oxide according to [1], wherein the calcination apparatus is a rotary kiln. [3] The method for producing a lithium metal composite oxide according to [1] or [2], wherein the proportion of Li contained in the lithium compound is 5% by mass or more and 50% by mass or less. [4] The method for producing a lithium metal composite oxide according to [3], wherein the proportion of Li is 5% by mass or more and 30% by mass or less. [5] The method for producing a lithium metal composite oxide according to [3], wherein the value represented by the following formula (C) is 0.3 Nm 3 / kg or more 1Nm 3 The method for producing a lithium metal composite oxide according to any one of [1] to [4], wherein the oxygen-containing gas supply amount (Nm 3 / hour) / supply amount of material to be treated (kg / hour) [6] The method for producing a lithium metal composite oxide according to any one of [1] to [5], wherein the calcination device is provided with an exhaust port upstream of the heating means, and in the step, the calcination is performed while the oxygen-containing gas in the calcination device is exhausted from the exhaust port. [7] The method for producing a lithium metal composite oxide according to any one of [1] to [6], wherein the lithium metal composite oxide is represented by the following composition formula (I): Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a ]O 2 ...Composition formula (I) (In composition formula (I), M1 is at least one element selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, W, Nb, B, Si, S, and P, and composition formula (I) satisfies −0.1≦a≦0.2, 0≦x≦0.7, 0<y≦0.7, and x+y<1.)

[0008] According to the present invention, it is possible to provide a method for producing a lithium metal composite oxide that allows stable production.

[0009] 1 is a schematic cross-sectional view of a calcination apparatus used in a method for producing a lithium metal composite oxide according to one aspect of the present embodiment.

[0010] In this specification, a metal composite compound (Metal Composite Compound) will be hereinafter referred to as "MCC", a lithium metal composite oxide (LiMO) will be hereinafter referred to as "LiMO", and a cathode active material for lithium secondary batteries will be hereinafter referred to as "CAM".

[0011] "Ni" refers to nickel atoms, not nickel metal. Similarly, "Co" and "Li" refer to cobalt atoms, lithium atoms, etc., respectively.

[0012] When a numerical range is described as, for example, "1-10 μm" or "1 to 10 μm," it means a range from 1 μm to 10 μm, including the lower limit of 1 μm and the upper limit of 10 μm.

[0013] In the present specification, the upper and lower limits of the ranges of values ​​can be arbitrarily combined. The ranges of values ​​of the respective physical properties, compositions, and manufacturing conditions can be arbitrarily combined.

[0014] <Method for Producing LiMO> This embodiment is a method for producing LiMO, including a step (hereinafter sometimes referred to as step A) of calcining a material to be treated using a calcination device to obtain a calcined product. The calcination device includes a feed section into which the material to be treated is introduced, a transport section for transporting the material introduced from the feed section, a cylindrical kiln body, an outlet for discharging the calcined material, and a gas supply means, and the kiln body includes a heating means. In step A, a low-dew-point gas having a dew point of 10°C or less is supplied from the upstream side of the heating means. This dehumidifies and dries water vapor remaining near the feed section of the material to be treated. As a result, condensation is less likely to occur, clogging near the feed section can be avoided, and stable LiMO production is possible. Here, "upstream of the heating means" means the feed section side of the heating means. For example, a low-dew-point gas can be supplied from a low-dew-point gas supply section 56 described below. The calcination device used in the LiMO production method will be described with reference to FIG. 1.

[0015] <<Overall Configuration>> Fig. 1 is a schematic cross-sectional view of a calcination apparatus used in the LiMO manufacturing method of this embodiment. The calcination apparatus 50 shown in Fig. 1 includes a charging section 51, a conveying section 58, a kiln body 52, an outlet 53, and a gas supply means 60. The conveying section 58 includes a conveying mechanism 581 and an electric motor 582.

[0016] The material to be treated is fed into the feeding section 51 and supplied to the conveying section 58, and then conveyed into the kiln main body 52 by the conveying mechanism 581 of the conveying section 58. The conveying section 58 is, for example, a screw feeder. The conveying mechanism 581 is, for example, a conveying screw.

[0017] The kiln body 52 is a facility for calcining the material to be treated. The material to be treated transported to the kiln body 52 is calcined, and the resulting calcined material is discharged from the discharge port 53.

[0018] As described above, the material to be treated passes through the feeding section 51, the conveying section 58, and the kiln main body 52, and is moved toward the discharge outlet 53, where it is heated inside the kiln main body 52, and is finally discharged from the discharge outlet 53.

[0019] The kiln body 52 is tubular, specifically cylindrical, and is rotatable about an axis O. The kiln body 52 is equipped with a heating means 54. The heating means 54 burns the material to be treated supplied into the kiln body 52.

[0020] The firing apparatus 50 includes a gas supply means 60. The gas supply means 60 includes an oxygen-containing gas supply section 601 that supplies an oxygen-containing gas into the kiln body 52 from downstream of the heating means 54. "Downstream of the heating means 54" means the side of the discharge port 53 of the heating means 54.

[0021] In order to allow the oxygen-containing gas to flow in the kiln body 52 in the opposite direction to the direction of movement of the material to be treated, the firing device 50 is provided with an exhaust port 55 upstream of the heating means 54, and in step A, it is preferable to perform firing while exhausting the oxygen-containing gas in the firing device 50 from the exhaust port 55 (EG1 in Figure 1).

[0022] When the material to be treated is calcined inside the kiln body 52, moisture may be generated by reactions that occur during the calcination. Examples of reactions that generate moisture include the dehydration reaction of lithium hydroxide or MCC, and the desorption reaction of water molecules that occurs when a lithium compound reacts with MCC. The generated moisture becomes water vapor and travels with the countercurrent gas toward the conveying section 58. The water vapor that reaches the upstream side of the heating means 54 condenses due to a drop in temperature.

[0023] When the condensed water produced by condensation comes into contact with the raw materials supplied to the conveying section 58, a lump of raw materials forms, causing blockage of the conveying section 58. This hinders the supply of subsequent raw materials, making it difficult to stably produce LiMO. One method for solving this problem is to increase the rotation speed of the electric motor 582 of the conveying section 58 to keep the raw material supply speed constant, but this makes it difficult to eliminate blockage when long-term operation is assumed.

[0024] In this embodiment, by supplying a low dew point gas to a position where condensation is likely to occur, i.e., upstream of the heating means 54, it is possible to dehumidify and dry the water vapor remaining near the supply section of the material to be treated. As a result, clogging of the transport section 58 can be avoided, the raw material can be supplied stably, and LiMO can be produced stably.

[0025] Specifically, the gas supply means 60 includes a low dew point gas supply line 602 for supplying a low dew point gas, in addition to an oxygen-containing gas supply unit 601. The supply amounts of the oxygen-containing gas and the low dew point gas are controlled by a control unit 61.

[0026] Here, the "low dew point gas" refers to a gas with a dew point of 10° C. or less, specifically oxygen, nitrogen, air, and a mixed gas of two or more of the above three types, each having a dew point of 10° C. or less. The "oxygen-containing gas" refers to a gas containing oxygen, such as oxygen or a mixed gas of oxygen and nitrogen.

[0027] The dew point of the low dew point gas is preferably −10° C. or lower, more preferably −20° C. or lower. By using a low dew point gas having a dew point in the above range, LiMO can be produced more stably.

[0028] The low dew point gas is supplied to the low dew point gas supply unit 56. In FIG. 1 , the low dew point gas supply unit 56 is installed above the electric motor 582. However, this is not limitative as long as it is located upstream of the heating means 54. For example, the low dew point gas supply unit 56 may be installed in the circumferential direction upstream of the heating means 54 of the kiln body 52, or may be installed above the center of the conveying mechanism 581. Furthermore, the low dew point gas supply unit may be installed in two or more locations.

[0029] The calcination device is preferably a rotary kiln, which is a fluidized calcination furnace. In a rotary kiln, the kiln body rotates while sliding on the fixed part of the kiln body. Since gaps are likely to occur in the sliding part, a seal gas supply unit is typically provided mainly for the purpose of sealing the sliding part. The seal gas supply unit is installed near the sliding part, and is typically installed either upstream or downstream of the heating means of the kiln body, or both.

[0030] Since the rotary kiln is equipped with a seal gas supply unit as standard as described above, the manufacturing method of this embodiment can be carried out by simply changing the seal gas to a low dew point gas without modifying the firing apparatus.

[0031] As the calcining device, in addition to a rotary kiln, a rocking cylindrical furnace provided with a supply section and supply means for a low dew point gas can be used.

[0032] Generally, gases used as seal gases have a dew point exceeding 10° C., so the low dew point gas introduced in this embodiment is a gas that is different from the seal gas.

[0033] By using the seal gas supply unit installed upstream of the heating means of the kiln body as the low dew point gas supply unit, it is possible to supply low dew point gas from upstream of the heating means.

[0034] Next, the above-mentioned step A using the above-mentioned baking apparatus 50 will be described.

[0035] While rotating the kiln body 52, the material to be treated is supplied from the input section 51. In the calcination device 50, the material to be treated is continuously calcined while being moved from the input section 51 toward the kiln body 52 by the conveying section 58. In step A, a low dew point gas is supplied from the upstream side of the heating means 54, and an oxygen-containing gas is supplied from the downstream side of the heating means 54.

[0036] In step A, the value represented by the following formula (A) is 0.0001-0.30 Nm 3 / kg. Formula (A): The supply amount of low dew point gas (Nm 3 / hour) / amount of material to be treated (kg / hour)

[0037] The value represented by formula (A) is 0.06 Nm 3 / kg or more is preferable, and 0.065 Nm 3 / kg or more is more preferable, and 0.07 Nm 3 It is more preferable that the value represented by formula (A) is greater than 0.25 Nm 3 / kg or less is preferable, and 0.22 Nm 3 The value represented by formula (A) is, for example, 0.06 to 0.25 Nm 3 / kg, 0.065-0.22 Nm 3 / kg, or 0.07 Nm 3 / kg or more than 0.22 Nm 3 / kg or less.

[0038] When the value represented by formula (A) is equal to or greater than the lower limit, a sufficient amount of low dew-point gas is supplied to dehumidify and dry the water vapor that reaches the vicinity of the supply part of the material to be treated, so condensation is less likely to occur near the supply part of the material to be treated, and the raw material can be supplied stably.

[0039] When the value represented by formula (A) is equal to or less than the upper limit, the supply of oxygen-containing gas from the oxygen-containing gas supply unit 601 is unlikely to become excessive, and the heating energy of the heating means 54 is unlikely to increase.

[0040] In step A, the material to be treated is calcined by countercurrently contacting an oxygen-containing gas with the material. The supply amount of the oxygen-containing gas preferably satisfies the following formula (X): Formula (X): Supply amount of low dew-point gas (Nm 3 / hour) < supply amount of oxygen-containing gas (Nm 3 / time)

[0041] By performing firing while exhausting the oxygen-containing gas from the firing apparatus 50 through the exhaust port 55, firing can be performed under conditions in which the oxygen-containing gas flows in the opposite direction to the direction of movement of the material to be treated within the kiln body 52. ​​Under conditions that satisfy formula (X), gas containing water vapor can be exhausted from the interior of the firing apparatus 50, including the conveying section 58, to the exhaust port 55 in a short time (EG1 in FIG. 1). This shortens the time that the gas containing water vapor remains inside the firing apparatus 50, making it less likely that water vapor will remain near the supply section for the material to be treated. As a result, clogging of the conveying section 58 is avoided, allowing for a stable supply of raw materials and stable production of LiMO.

[0042] In step A, the value represented by the following formula (C) is 0.3-1 Nm 3 It is preferable to burn the material to be treated while supplying an oxygen-containing gas into the kiln body 52 so that the amount of oxygen-containing gas supplied (Nm 3 / hour) / amount of material to be treated (kg / hour)

[0043] The value represented by the above formula (C) is 0.4-1 Nm 3 / kg is preferred, and 0.5-1 Nm 3 / kg is more preferred.

[0044] When the value represented by formula (C) is equal to or greater than the lower limit, the dew point of the oxygen-containing gas in the kiln body 52 increases, making condensation less likely to occur, thereby enabling stable production of LiMO. When the value represented by formula (C) is equal to or less than the upper limit, an increase in the supply amount of oxygen-containing gas to be heated can be suppressed, thereby preventing an increase in heating energy, enabling stable production of LiMO.

[0045] In step A, the supply amount of oxygen-containing gas is 0.5 Nm 3 When the supply rate of the oxygen-containing gas is equal to or greater than the above lower limit, the reaction between the object to be treated and the oxygen-containing gas can be sufficiently enhanced. The upper limit of the supply rate of the oxygen-containing gas is, for example, 2 Nm 3 / hour. The supply rate of oxygen-containing gas is 0.5-2 Nm 3More preferably, it is / hour.

[0046] The firing temperature of the workpiece is, for example, 650-900°C, preferably 660-850°C, and more preferably 670-800°C. A firing temperature of 650°C or higher promotes the growth of LiMO particles, making it possible to obtain LiMO having a strong crystal structure. Furthermore, a heating temperature of 900°C or lower prevents cracks from forming in the particles of LiMO, maintains the strength of LiMO, and reduces the volatilization of lithium ions on the particle surfaces contained in LiMO.

[0047] In this specification, the firing temperature means the maximum temperature of the atmosphere inside the kiln body 52.

[0048] The holding time in the firing step is preferably 1 to 50 hours. When the holding time in the firing step is 1 hour or more, the crystals develop well. When the holding time in the firing step is 50 hours or less, the volatilization of lithium ions is unlikely to occur.

[0049] In this specification, the retention time during firing is defined as the time from when the workpiece reaches the area where the heating means 54 is provided until when it reaches the end of the area where the heating means 54 is provided.

[0050] The inner diameter of the kiln body 52 is preferably 0.05 to 10 m, more preferably 0.07 to 5 m, and even more preferably 0.09 to 2 m.

[0051] The filling rate of the material to be treated in the kiln body 52 is preferably 1 to 20%, more preferably 2 to 17%, and even more preferably 3 to 15%.

[0052] The rotation speed of the kiln body 52 in step A is preferably 0.003-0.5 rad / sec, more preferably 0.05-0.4 rad / sec, and even more preferably 0.08-0.3 rad / sec.

[0053] (Material to be treated) The material to be treated includes a mixture of MCC and a lithium compound. The mixture of MCC and a lithium compound is a mixture of MCC and a lithium compound without calcination. The material to be treated may also include other materials as long as it mainly contains the mixture. For example, in addition to the mixture, the material may also contain a reaction product of MCC and a lithium compound. The reaction product of MCC and a lithium compound is a substance obtained by calcining MCC and a lithium compound.

[0054] MCC is a compound that can be fired with a lithium compound to produce LiMO. MCC is, for example, a metal composite oxide or a metal composite hydroxide.

[0055] The proportion of Li contained in the lithium compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The proportion of Li contained in the lithium compound is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less. Examples of the proportion of Li contained in the lithium compound include 5-50% by mass, 5-30% by mass, 10-25% by mass, and 15-20% by mass.

[0056] Specifically, the lithium compound may be at least one of lithium carbonate (Li proportion: 19% by mass), lithium nitrate (Li proportion: 5-10% by mass), lithium acetate (Li proportion: 7-11% by mass), lithium hydroxide (Li proportion: 16-30% by mass), lithium oxide (Li proportion: 46% by mass), lithium chloride (Li proportion: 16% by mass), and lithium fluoride (Li proportion: 27% by mass). Of these, lithium hydroxide (Li proportion: 16-30% by mass) is preferred due to its high reactivity with MCC.

[0057] Lithium hydroxide is prone to generating water vapor during firing, but the LiMO production method described above allows stable production of LiMO even when lithium hydroxide is used as the lithium compound.

[0058] Although a mixture of MCC and a lithium compound contains a large amount of attached water and crystal water, which tends to generate water vapor, the LiMO production method described above can stably produce LiMO even when a mixture of MCC and a lithium compound is used.

[0059] The composition analysis of the lithium compound can be carried out, for example, by dissolving the lithium compound in hydrochloric acid and then using an ICP emission spectrometer (Optima 7300, manufactured by PerkinElmer Co., Ltd.).

[0060] The MCC preferably contains Ni and the element M1, and more preferably contains Ni, Co, and the element M1. The element M1 represents one or more elements selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, W, Nb, B, Si, S, and P.

[0061] MCC is, for example, a metal composite hydroxide or metal composite oxide containing Ni, Co, and Al.

[0062] When MCC is a metal composite hydroxide, the metal composite hydroxide can be produced, for example, by the continuous coprecipitation method described in JP-A-2002-201028. For example, it can be produced by the following procedure. First, at a temperature of 20-80°C in a reaction vessel, an alkaline aqueous solution is added to a mixed solution containing a metal salt solution and a complexing agent so that the pH is in the range of 9-13. Next, the resulting reaction precipitate is washed, dehydrated, and dried to obtain the metal composite hydroxide. Examples of the metal salt solution include an aqueous nickel sulfate solution, an aqueous cobalt sulfate solution, and an aqueous aluminum sulfate solution, and examples of the complexing agent include ammonium sulfate. Examples of the alkaline aqueous solution that can be used include an aqueous sodium hydroxide solution and an aqueous potassium hydroxide solution.

[0063] When MCC is a metal composite oxide, the metal composite oxide can be produced by heating the metal composite hydroxide at 300-700°C.

[0064] A lithium compound and MCC are mixed in consideration of the composition ratio of the final target product to produce a mixture. Specifically, the amount (molar ratio) of Li relative to the total amount of elements other than Li and oxygen atoms (e.g., Ni, Co, element M1) contained in MCC is preferably 0.98 or more, more preferably 1.04 or more, and even more preferably 1.05 or more. The amount of Li is preferably 1.20 or less. Examples of the amount of Li include 0.98-1.20, 1.04-1.20, and 1.05-1.20.

[0065] After step A, firing may be performed. In this case, firing in step A is called pre-firing, and the fired product obtained by step A is called the pre-firing product. The fired product is obtained by firing the pre-firing product. The firing apparatus used for firing is not particularly limited, and may be, for example, a continuous static firing furnace or a fluidized firing furnace. As the fluidized firing furnace, firing apparatus 50 may be used. The temperature and time during firing are, for example, 650-950°C and 3-50 hours.

[0066] The fired product may be washed, dehydrated, and dried as necessary. LiMO is obtained through the above steps.

[0067] [Method for measuring the coefficient of variation of the agitator frequency] Whether or not a LiMO manufacturing method is capable of stable production is evaluated by measuring the coefficient of variation of the agitator frequency. In the calcination device 50, the agitator is rotated by the electric motor 582, and the material to be treated fed from the feed unit 51 is transported.

[0068] If the desired raw material supply rate (kg / h) can be maintained without changing or barely changing the frequency of the agitator blades, stable production is possible. When the frequency is adjusted during operation to maintain the desired raw material supply rate, the degree of frequency fluctuation is calculated as the "coefficient of variation of the agitator blade frequency."

[0069] Specifically, the coefficient of variation of the agitator blade frequency is calculated by the following formula: Coefficient of variation of agitator blade frequency=standard deviation of the agitator blade frequency of the transport mechanism 581 / average frequency of the agitator blade frequency of the transport mechanism 581

[0070] In calculating the coefficient of variation of the stirring blade frequency, the standard deviation of the frequency after the material to be treated has accumulated inside the kiln body 52 is used.

[0071] If the value of the coefficient of variation is large, it means that the frequency is adjusted each time during operation to maintain the desired raw material supply rate, which means that production is unstable. In this embodiment, if the value of the coefficient of variation is 0.035 or less, the risk of clogging during long-term operation is unlikely to occur, and it is evaluated as "stable production is possible."

[0072] <LiMO> The above-mentioned LiMO has the following properties.

[0073] LiMO preferably contains Li, Ni, and the element M1, and more preferably contains Li, Ni, Co, and the element M1. LiMO is represented, for example, by the composition formula (I): Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a ]O 2 ...Composition formula (I) (In composition formula (I), M1 is the element M1, and composition formula (I) satisfies −0.1≦a≦0.2, 0≦x≦0.7, 0<y≦0.7, and x+y<1.)

[0074] From the viewpoint of obtaining a lithium secondary battery with a high cycle retention rate, a in the composition formula (I) is preferably −0.05 or more, and more preferably −0.01 or more, and from the viewpoint of obtaining a lithium secondary battery with a high initial coulombic efficiency, a is preferably 0.08 or less, and more preferably 0.05 or less.

[0075] The upper and lower limits of a can be arbitrarily combined, and a is, for example, −0.01 to 0.2, −0.05 to 0.08, or −0.01 to 0.05.

[0076] From the viewpoint of improving cycle characteristics, x is preferably 0.01 or more, and more preferably 0.02 or more. From the viewpoint of obtaining a lithium secondary battery with a high charge capacity, x is preferably 0.5 or less, and more preferably 0.3 or less.

[0077] For example, x is 0.01-0.5, 0.02-0.3.

[0078] From the viewpoint of improving cycle characteristics, y is preferably 0.01 or more, and more preferably 0.02 or more. From the viewpoint of obtaining a lithium secondary battery with a high charge capacity, y is preferably 0.5 or less, and more preferably 0.3 or less.

[0079] y is, for example, 0.01-0.5, 0.02-0.3.

[0080] x+y is greater than 0 and less than 1, preferably greater than 0 and 0.7 or less, more preferably greater than 0 and 0.3 or less, and even more preferably greater than 0 and 0.25 or less.

[0081] From the viewpoint of obtaining a lithium secondary battery with a high cycle retention rate, M1 is preferably one or more elements selected from the group consisting of Mn, Ti, Mg, Al, W, Nb, B, and Zr, and more preferably one or more elements selected from the group consisting of Mn, Al, W, Nb, B, and Zr.

[0082] The composition analysis of LiMO can be carried out, for example, by dissolving LiMO in hydrochloric acid and then using an ICP emission spectrometer (Optima 7300, manufactured by PerkinElmer Co., Ltd.).

[0083] The crystal structure of LiMO is a layered structure, and is more preferably a hexagonal crystal structure or a monoclinic crystal structure.

[0084] [Method for Confirming Crystal Structure] The crystal structure of LiMO can be confirmed by observation using a powder X-ray diffraction measurement device (for example, Ultima IV manufactured by Rigaku Corporation).

[0085] The hexagonal crystal structure is P3, P3 1 , P3 2 , R3, P-3, R-3, P312, P321, P3 1 12. P3 1 21, P3 2 12. P3 2 21, R32, P3m1, P31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P61 , P6 5 , P6 2 , P6 4 , P6 3 , P-6, P6 / m, P6 3 / m, P622, P6 1 22, P6 5 22, P6 2 22, P6 4 22, P6 3 22, P6mm, P6cc, P6 3 cm, P6 3 mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P6 3 / mcm, and P6 3 / mmc.

[0086] In addition, the monoclinic crystal structure is P2, P2 1 , C2, Pm, Pc, Cm, Cc, P2 / m, P2 1 / m, C2 / m, P2 / c, P2 1 It is assigned to any one space group selected from the group consisting of C1 / c, C2 / c, and C3 / c.

[0087] Among these, in order to obtain a lithium secondary battery with a high discharge capacity, the crystal structure is more preferably a hexagonal crystal structure belonging to the space group R-3m or a monoclinic crystal structure belonging to the space group C2 / m.

[0088] <CAM> The LiMO can be suitably used as a CAM.

[0089] <Lithium Secondary Battery> An example of a suitable lithium secondary battery when using LiMO as a CAM includes a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.

[0090] Furthermore, an example of a lithium secondary battery includes a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and a solid electrolyte disposed between the positive electrode and the negative electrode. The configuration, materials, and manufacturing method of the lithium secondary battery can be described in paragraphs

[0104] to

[0181] of WO2022 / 113904A1.

[0091] Next, the present invention will be described in more detail with reference to examples.

[0092] <Composition Analysis> Composition analysis of LiMO and lithium compounds was carried out by dissolving LiMO or lithium compounds in hydrochloric acid and then using an ICP emission spectrometer (Optima 7300, manufactured by PerkinElmer Co., Ltd.).

[0093] <Coefficient of Variation of Agitating Impeller Frequency> The coefficient of variation was measured as described in [Method for measuring coefficient of variation of agitating impeller frequency] above.

[0094] Example 1 Water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added thereto, and the liquid temperature (temperature of the reaction vessel) was maintained at 50°C.

[0095] A mixed raw material solution was prepared by mixing an aqueous solution of nickel sulfate, an aqueous solution of cobalt sulfate, and an aqueous solution of aluminum sulfate in such a ratio that the atomic ratio of Ni, Co, and Al was 0.88:0.09:0.03.

[0096] Next, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material solution in a reaction vessel under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times so that the pH of the mixed solution in the reaction vessel became 11.6 (measurement temperature: 40°C), and a reaction precipitate 1 was obtained.

[0097] After washing the reaction precipitate 1, it was dehydrated using a centrifuge, isolated, and dried at 105° C. to obtain a metal composite hydroxide 1 containing Ni, Co, and Al.

[0098] Metal composite hydroxide 1 was heated and held at 650° C. for 5 hours in an air atmosphere, and then cooled to room temperature to obtain metal composite oxide MCC1.

[0099] Lithium hydroxide was weighed out so that the amount of Li (molar ratio) relative to the total amount of Ni, Co, and Al contained in MCC1 was 1 was 1.10. MCC1 and lithium hydroxide were mixed in a mortar to obtain mixture 1.

[0100] The proportion of Li contained in the lithium hydroxide used was 16.5 mass %.

[0101] This mixture 1 was placed in a fluidized bed calcination furnace (trade name: Desktop Rotary Kiln, manufactured by Noritake Company Limited) corresponding to calcination device 50. An oxygen-containing gas was supplied from the outlet side under conditions satisfying the relationship of formula (X), and while exhausting from an exhaust port corresponding to exhaust port 55, the oxygen-containing gas was brought into countercurrent contact with mixture 1, and calcined at 680°C for 2 hours, to obtain calcined product 1.

[0102] At this time, the value of formula (A) is 0.20 (Nm 3 / kg), and the value represented by formula (C) is 0.67 (Nm 3 / kg), and oxygen having a dew point of −23.6° C. was supplied as the low dew point gas from the low dew point gas supply part.

[0103] The coefficient of variation during pre-baking was 0, confirming that LiMO could be stably produced.

[0104] Next, the obtained pre-fired product 1 was placed in a stationary batch-type firing furnace (manufactured by Motoyama Corporation, product name: Oxidizing Atmosphere Furnace SKA-3050F-SP) and fired in an oxygen atmosphere at 720°C for 5 hours, thereby obtaining a fired product 1.

[0105] The obtained fired product 1 was washed, dehydrated using a centrifuge, isolated, and dried at 250° C. in a nitrogen atmosphere to obtain LiMO-1.

[0106] Composition analysis of LiMO-1 revealed that in the composition formula (I), a=0.02, x=0.09, y=0.03, and the element M1 was Al.

[0107] Example 2: The value of formula (A) was set to 0.07 (Nm 3 Preliminary calcined product 2 was obtained in the same manner as in Example 1 except that the calcined product was changed to a calcined product (1 / kg).

[0108] The coefficient of variation during pre-baking was 0.034, confirming that LiMO could be stably produced.

[0109] LiMO-2 was obtained in the same manner as in Example 1, except that the pre-calcined product 2 was used.

[0110] Composition analysis of LiMO2 revealed that in the composition formula (I), a = 0.02, x = 0.09, y = 0.03, and the element M1 was Al.

[0111] Comparative Example 1: No low dew point gas was supplied, and the value represented by formula (C) was 1.72 (Nm 3 Preliminary calcined product 11 was obtained in the same manner as in Example 1, except that the calcined product was changed to a calcined product (1 / kg).

[0112] The coefficient of variation during the calcination was 0.058. Since the value of the coefficient of variation was large and continued operation would have increased the risk of clogging, the calcination was stopped midway.

[0113] Comparative Example 2: No low dew point gas was supplied, and the value represented by formula (C) was 0.10 (Nm 3 Preliminary calcined product 12 was obtained in the same manner as in Example 1, except that the calcined product was changed to (1 / kg).

[0114] The coefficient of variation during the calcination was 0.040. The value of the coefficient of variation was large, and the risk of clogging was high if the operation was continued, so the calcination was stopped midway.

[0115] As shown by the above results, in a countercurrent contact calcination method, when a low dew-point gas with a dew point of 10°C or less is supplied from the upstream side of the heating means and calcination is performed under conditions that satisfy formula (A), it has been confirmed that blockage due to condensation near the raw material supply section is unlikely to occur and LiMO can be stably produced.

[0116] 50: Burning device, 51: Feeding section, 52: Kiln body, 53: Discharge port, 54: Heating means, 55: Exhaust port, 56: Low dew point gas supply section, 58: Conveying section, 581: Conveying mechanism, 582: Electric motor, 60: Gas supplying means, 601: Oxygen-containing gas supply section, 602: Low dew point gas supply line, 61: Control section

Claims

1. A method for producing a lithium metal composite oxide, comprising a step of calcining a material to be treated using a calcination device to obtain a calcined material, wherein the material to be treated includes a mixture of a metal composite compound and a lithium compound, the calcination device comprises an input section into which the material to be treated is fed, a transport section for transporting the material to be treated fed from the input section, a cylindrical kiln body, an outlet for discharging the calcined material, and a gas supply means, the kiln body comprises a heating means, and in the step, a low dew point gas having a dew point of 10°C or less is supplied from the upstream side of the heating means, an oxygen-containing gas is supplied from the downstream side of the heating means, the material to be treated is calcined by countercurrent contact with the oxygen-containing gas, and the value represented by the following formula (A) is 0.0001 Nm 3 / kg or more 0.30Nm 3 / kg or less. Formula (A): The supply amount of low dew point gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour) 2. The method for producing lithium metal composite oxide according to claim 1, wherein the calcination apparatus is a rotary kiln.

3. The method for producing a lithium metal composite oxide according to claim 1 or 2, wherein the proportion of Li contained in the lithium compound is 5 mass % or more and 50 mass % or less.

4. The method for producing a lithium metal composite oxide according to claim 3, wherein the proportion of Li is 5 mass % or more and 30 mass % or less.

5. The value represented by the following formula (C) is 0.3 Nm 3 / kg or more 1Nm 3 The method for producing a lithium metal composite oxide according to claim 1 or 2, wherein the amount of oxygen-containing gas supplied (Nm 3 / hour) / supply amount of material to be treated (kg / hour) 6. A method for producing a lithium metal composite oxide as described in claim 1 or 2, wherein the calcination apparatus is provided with an exhaust port upstream of the heating means, and in the process, calcination is performed while exhausting the oxygen-containing gas in the calcination apparatus from the exhaust port.

7. The method for producing a lithium metal composite oxide according to claim 1 or 2, wherein the lithium metal composite oxide is represented by the following composition formula (I): Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a ]O 2 ... Composition formula (I) (In composition formula (I), M1 is at least one element selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, W, Nb, Sn, Zr, B, Si, S, and P, and composition formula (I) satisfies -0.1≦a≦0.2, 0≦x≦0.7, 0<y≦0.7, and x+y<1.)

Citation Information

Patent Citations

  • High density nickel hydroxide coprecipitated with cobalt and manganese, and method for producing the same

    JP2002201028A

  • Toner cartridge with barrier member to reduce cross-sectional area

    JP2023067067A

  • Method for producing lithium metal composite oxide

    WO2022113904A1

  • Lithium titanium complex oxide, production method thereof and electrode for battery

    JP2014001110A

  • Method for manufacturing positive electrode active material for lithium secondary battery

    JP2019075253A