Treatment solution and method for treating object to be treated
The processing liquid, composed of specific alicyclic heterocyclic compounds and additional additives, addresses the issue of surface roughness in cobalt-containing metal films within semiconductor devices, achieving improved smoothness and manufacturing efficiency.
Patent Information
- Application Number
- PCT/JP2024/014399
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-24
AI Technical Summary
Current processing liquids for semiconductor devices fail to effectively suppress surface roughness of metal films containing cobalt during etching and cleaning processes, leading to irregularities and performance issues.
A processing liquid comprising water, an alicyclic heterocyclic compound with a nitrogen atom as a ring member, and a second alicyclic heterocyclic compound with a hydroxyl group, along with optional components like chelating agents, organic solvents, and corrosion inhibitors, is developed to treat cobalt-containing metal films, improving surface smoothness and performance.
The proposed processing liquid significantly reduces surface roughness of cobalt-containing metal films, enhancing the accuracy and efficiency of semiconductor device manufacturing by maintaining a smooth film surface, thereby improving device performance.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Treatment liquid and treatment method for object to be treated
[0001] The present invention relates to a processing liquid and a method for processing an object to be processed.
[0002] 2. Description of the Related Art As semiconductor devices become increasingly miniaturized, there is an increasing demand for highly efficient and accurate etching, cleaning, and other processes using processing liquids during the semiconductor device manufacturing process.
[0003] For example, Patent Document 1 discloses a technique relating to a cleaning composition containing an oxidation-reducing agent, two types of chelating agents, a metal corrosion inhibitor, an organic solvent, water, and a desired pH adjuster, and a method including contacting a semiconductor substrate with the cleaning composition.
[0004] Special table 2017-504190 publication
[0005] The present inventors have studied the treatment solution described in Patent Document 1 and have found that when the treatment solution is applied to a workpiece having a metal film containing cobalt, which is used as a wiring material, plug material, etc., the surface of the metal film may become rough, resulting in the formation of fine irregularities, and that there is room for further improvement in this regard.
[0006] In view of the above circumstances, an object of the present invention is to provide a treatment liquid for semiconductor devices that is excellent in suppressing surface roughness of a metal film containing cobalt, and a method for treating an object using the treatment liquid.
[0007] As a result of extensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by including two specific components in a treatment liquid, and have thus completed the present invention. That is, they have found that the above-mentioned problems can be solved by the following configuration.
[0008] [1] A treatment liquid for semiconductor devices, the treatment liquid comprising: water; a first component that is an alicyclic heterocyclic compound containing a nitrogen atom as a ring member; and a second component that is a compound different from the first component and is an alicyclic heterocyclic compound having a hydroxyl group. [2] The treatment liquid according to [1], wherein the first component has two or more nitrogen atoms as ring member atoms. [3] The treatment liquid according to [1] or [2], wherein the first component contains at least one selected from the group consisting of 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5-diazabicyclo[4.3.0]non-5-ene. [4] The treatment liquid according to any one of [1] to [3], wherein the second component contains a nitrogen atom or an oxygen atom as a ring member atom. [5] The treatment liquid according to any one of [1] to [4], wherein the second component is a compound represented by formula (1) described below or a compound represented by formula (2) described below. [6] The treatment liquid according to any one of [1] to [5], wherein the content of the water is 70% by mass or more relative to the total mass of the treatment liquid. [7] The treatment liquid according to any one of [1] to [6], further comprising a chelating agent having a carboxylic acid group or a chelating agent having a phosphonic acid group. [8] The treatment liquid according to any one of [1] to [7], further comprising an organic solvent. [9] The treatment liquid according to [8], wherein the organic solvent comprises at least one selected from the group consisting of glycol-based solvents, glycol ether-based solvents, amide-based solvents, alcohol-based solvents, and sulfoxide-based solvents.
[10] The treatment liquid according to any one of [1] to [9], further comprising a corrosion inhibitor.
[11] The treatment liquid according to
[10] , wherein the corrosion inhibitor comprises at least one compound selected from the group consisting of a compound represented by the formula (A) described below, a compound represented by the formula (B) described below, a compound represented by the formula (C) described below, and a substituted or unsubstituted tetrazole.
[12] The treatment liquid according to any one of [1] to
[11] , further comprising at least one hydroxylamine compound selected from the group consisting of hydroxylamine, hydroxylamine derivatives, and salts thereof.
[13] The treatment liquid according to any one of [1] to
[12] , further comprising an inorganic acid.
[14] A method for treating an object to be treated, comprising a step of contacting an object to be treated having a cobalt-containing layer with the treatment liquid according to any one of [1] to
[13] .
[0009] According to the present invention, there is provided a treatment liquid for semiconductor devices that is excellent in the ability to suppress surface roughness of a metal film containing cobalt. The present invention also provides a method for treating an object to be treated using the treatment liquid.
[0010] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. The term "preparation" in this specification includes the provision of specific materials by synthesis or blending, as well as the procurement of a specific item by purchase, etc. In this specification, when two or more types of a component are present, unless otherwise specified, the "content" of that component refers to the total content of those two or more components. Unless otherwise specified, the compounds described in this specification are used to include structural isomers, optical isomers, and isotopes of the compound. Furthermore, structural isomers, optical isomers, and isotopes may be present singly or in combination. In this specification, "ppm" means "parts per million (10 -6 ) and "ppb" stands for "parts-per-billion (10 -9 ) and "ppt" stands for "parts-per-trillion (10 -12 "Radiation" in this specification refers to, for example, the bright line spectrum of a mercury lamp, far ultraviolet light typified by an excimer laser, extreme ultraviolet light (EUV light), X-rays, or electron beams. Furthermore, light in this specification refers to actinic rays or radiation. Unless otherwise specified, "exposure" in this specification includes not only exposure with a mercury lamp, far ultraviolet light typified by an excimer laser, X-rays, or EUV light, but also exposure with particle beams such as electron beams or ion beams.
[0011] [Treatment Solution] (Reason for Claim 1) The treatment solution of the present invention (hereinafter also referred to as "the present treatment solution") is a treatment solution for semiconductor devices, and contains water, a first component which is an alicyclic heterocyclic compound containing a nitrogen atom as a ring member, and a second component which is an alicyclic heterocyclic compound different from the first component and has a hydroxyl group. The present treatment solution is characterized by containing the first and second components, each of which is an alicyclic heterocyclic compound having a predetermined structure. The treatment solution used to treat a metal film containing cobalt (hereinafter also referred to as "Co-containing film") contains the first and second components, thereby achieving the effect of suppressing the occurrence of surface roughness in the Co-containing film after treatment (hereinafter also referred to as "effect of the present invention"). Each component contained in the treatment solution will be described below.
[0012] [Water] The present treatment liquid contains water. The water is not particularly limited and examples thereof include distilled water, ion-exchanged water, and pure water, with ultrapure water used in the manufacture of semiconductor devices being preferred.
[0013] The water is preferably water in which inorganic anions and metal ions have been reduced, more preferably water in which the concentration of ions derived from metal atoms selected from Fe, Co, Na, K, Ca, Cu, Mg, Mn, Li, Al, Cr, Ni, and Zn has been reduced, and even more preferably water that has been adjusted to the order of ppt or less (in one embodiment, the metal content is less than 0.001 ppt by mass) when used to prepare the treatment solution. Preferred methods for adjustment include purification using a filtration membrane or an ion exchange membrane, or purification by distillation. Examples of adjustment methods include the methods described in paragraphs
[0074] to
[0084] of JP 2011-110515 A and the methods described in JP 2007-254168 A.
[0014] The water contained in the present treatment solution is preferably water obtained by the treatment described above. Furthermore, in order to obtain the effects of the present invention more significantly, it is more preferable that the water be used not only for the treatment solution but also for cleaning the container. Furthermore, it is also preferable that the water be used in the production process of the treatment solution, for measuring the components of the treatment solution, and for measuring the treatment solution evaluation.
[0015] The water content in the treatment liquid is not particularly limited, but is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 75% by mass or more, and even more preferably 85% by mass or more, relative to the total mass of the treatment liquid. The upper limit of the water content is, for example, 99.9% by mass or less, preferably 99.0% by mass or less, relative to the total mass of the treatment liquid. The water content in the treatment liquid is measured by a known measurement method such as the Karl Fischer method.
[0016] [First Component] The present treatment liquid contains a first component, which is an alicyclic heterocyclic compound containing a nitrogen atom as a ring member atom. In this specification, "alicyclic heterocyclic compound" refers to a compound having an alicyclic heterocycle (a non-aromatic heterocycle) and no aromatic ring. The first component is characterized by having an alicyclic heterocycle containing at least one nitrogen atom as a ring member atom. The first component may be ionized in the treatment liquid. In the treatment liquid, the first component may be, for example, in the form of an anion to which a proton has been added, or in the form of an anion to which a proton has been lost.
[0017] The alicyclic heterocycle contained in the first component may be a monocycle or a fused ring. When the alicyclic heterocycle is a fused ring, at least one of the monocycles constituting the fused ring contains at least one nitrogen atom as a ring member atom. In this case, at least one of the monocycles constituting the fused ring may be an alicyclic hydrocarbon. The alicyclic heterocycle may have an unsaturated bond or may be composed of only saturated bonds. The alicyclic heterocycle may have a substituent. The first component may have only one alicyclic heterocycle, or may have two or more alicyclic heterocycles. When the first component has two or more alicyclic heterocycles, at least one alicyclic heterocycle contains at least one nitrogen atom as a ring member atom. The first component preferably has only one alicyclic heterocycle that is a monocycle or a fused ring, and more preferably has only one alicyclic heterocycle that is a fused ring. The alicyclic heterocycle may contain a heteroatom other than a nitrogen atom as a ring member atom. Examples of heteroatoms other than nitrogen atoms include oxygen atoms and sulfur atoms. The ring atoms contained in the alicyclic heterocycle of the first component are preferably only carbon atoms and nitrogen atoms. The number of heteroatoms (more preferably nitrogen atoms) contained as ring atoms in the alicyclic heterocycle may be one or two or more, preferably two or more, more preferably two to four, and even more preferably two or three. The number of ring members in the monocycles constituting the alicyclic heterocycle (when the alicyclic heterocycle is a fused ring, each monocycle constituting the alicyclic heterocycle) is not particularly limited, but is, for example, 5 to 8, preferably 5 to 7.
[0018] Examples of the monocyclic ring containing a nitrogen atom as a ring member atom that constitutes the alicyclic heterocyclic ring contained in the first component include pyrrolidine, piperidine, piperazine, hexahydropyrimidine, hexahydropyridazine, 1,2,3,6-tetrahydropyrazine, 1,4,5,6-tetrahydropyrimidine, azepane, and azepine. When the alicyclic heterocyclic ring is a fused ring containing at least one alicyclic hydrocarbon, examples of the alicyclic hydrocarbon include cyclopentane, cyclohexane, and cycloheptane. The alicyclic heterocyclic ring contained in the first component is preferably a fused ring constituted by two or three monocyclic rings exemplified above, more preferably a fused ring constituted by two monocyclic rings exemplified above, and even more preferably a fused ring constituted by two monocyclic rings exemplified above that contain a nitrogen atom as a ring member atom.
[0019] The alicyclic heterocycle contained in the first component may have a substituent. Examples of the substituent include an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an amino group, an oxo group, and a keto group. On the other hand, the first component preferably does not have a hydroxyl group as a substituent on the alicyclic heterocycle. When the alicyclic heterocycle has a substituent, the number of substituents is not particularly limited, but one or two is preferable, and one is more preferable. The alicyclic heterocycle contained in the first component preferably has no substituent or has an alkyl group having 1 to 5 carbon atoms as a substituent, and more preferably has no substituent.
[0020] Examples of the first component include 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.4.0]dec-5-ene, 1,5-diazabicyclo[4.3.0]non-5-ene (DBN), 1,4-diazabicyclo[2.2.2]octane, octahydro-2H-pyrimido[1,2-a]pyrimidine, 2,5,6,7-tetrahydro-3H-pyrrolo[1.2-a]imidazole, 1,8-diazabicyclo[5.4.0]undecane, 1,5-diazabicyclo[4.4.0]decane, 1,3-diazabicyclo[3.2.2]nonane, and hexahydro-1H-1,4-diazepine. Among these, DBU or DBN is preferred, and DBU is more preferred.
[0021] The first component may be used alone or in combination of two or more. The content of the first component is not particularly limited, but is preferably 0.01 to 10% by mass, and more preferably 0.1 to 5% by mass, based on the total mass of the treatment liquid.
[0022] [Second Component] The present treatment liquid contains a second component, which is a compound different from the first component and is an alicyclic heterocyclic compound having a hydroxyl group. The second component may be ionized in the treatment liquid. In the treatment liquid, the second component may be, for example, in the form of an anion to which a proton has been added, or in the form of an anion to which a proton has been lost.
[0023] The alicyclic heterocycle contained in the second component may be a monocycle or a fused ring. When the alicyclic heterocycle is a fused ring, at least one of the monocycles constituting the fused ring contains at least one heteroatom as a ring member atom. In this case, at least one of the monocycles constituting the fused ring may be an alicyclic hydrocarbon. Furthermore, the alicyclic heterocycle may have an unsaturated bond or may be composed of only saturated bonds. The second component may contain only one alicyclic heterocycle, or may contain two or more alicyclic heterocycles. The second component preferably contains only one alicyclic heterocycle that is a monocycle or a fused ring, and more preferably contains only one alicyclic heterocycle that is a fused ring. Examples of heteroatoms contained as ring members of the alicyclic heterocycle in the second component include a nitrogen atom, an oxygen atom, and a sulfur atom. The second component preferably contains a nitrogen atom or an oxygen atom as a ring member atom. The number of heteroatoms contained as ring member atoms in the alicyclic heterocycle is not particularly limited, but is preferably 1 to 4, more preferably 1 to 3, and even more preferably 1 or 2. The number of ring members in the monocycle constituting the alicyclic heterocycle (when the alicyclic heterocycle is a condensed ring, each monocycle constituting the alicyclic heterocycle) is not particularly limited, but is, for example, 5 to 8, preferably 5 to 7, more preferably 5 or 6, and even more preferably 6.
[0024] Examples of the monocyclic heterocyclic ring contained in the second component or the monocyclic ring constituting the fused alicyclic heterocyclic ring include rings containing a nitrogen atom as a ring member atom such as pyrrolidine, piperidine, piperazine, hexahydropyrimidine, hexahydropyridazine, 1,2,3,6-tetrahydropyrazine, 1,4,5,6-tetrahydropyrimidine, azepane, azepine, and hexahydro-1H-1,4-diazepine, and rings containing an oxygen atom as a ring member atom such as tetrahydrofuran, tetrahydropyran, and oxepane. When the alicyclic heterocyclic ring is a fused ring containing at least one alicyclic hydrocarbon, examples of the alicyclic hydrocarbon include cyclopentane, cyclohexane, and cycloheptane. The second component is preferably a fused ring constituted by two or three of the above-exemplified monocycles, more preferably a fused ring constituted by two of the above-exemplified monocycles, and even more preferably a fused ring constituted by two of the above-exemplified monocycles containing a nitrogen atom as a ring member atom, or a fused ring constituted by one of the above-exemplified monocycles containing an oxygen atom as a ring member atom and one of the above-exemplified alicyclic hydrocarbons.
[0025] The alicyclic heterocycle of the second component has a hydroxyl group as a substituent. The number of hydroxyl groups of the second component is, for example, 1 to 3, preferably 1 or 2, and more preferably 1. The hydroxyl group is substituted on a ring atom constituting the alicyclic heterocycle of the second component.
[0026] The alicyclic heterocycle of the second component may have a substituent other than a hydroxyl group. Examples of the substituent other than a hydroxyl group include an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an amino group, an oxo group, and a keto group, with an amino group or an oxo group being preferred. The number of substituents other than a hydroxyl group in the second component is, for example, 0 to 2, preferably 0 or 1, and more preferably 0. That is, it is preferable that the second component has no substituents other than a hydroxyl group.
[0027] Examples of the second component include a compound represented by the following formula (1) and a compound represented by the following formula (2).
[0028] In formula (1) and formula (2), X each independently represents an oxygen atom, an imino group, or an imino group having a substituent, and n represents an integer of 1 to 3. Here, the term "imino group" simply refers to an unsubstituted imino group (-NH-). Examples of the substituent in the substituted imino group represented by X include a hydroxyl group and the above-mentioned substituents other than a hydroxyl group. Preferred embodiments of the substituent other than a hydroxyl group possessed by the imino group are the same as the preferred embodiments of the substituent other than a hydroxyl group. X is preferably an oxygen atom or an imino group (-NH-). Among these, X in formula (1) is more preferably an imino group, and X in formula (2) is more preferably an oxygen atom. n is preferably 1 or 2, and more preferably 1. In the compound represented by formula (1) and the compound represented by formula (2), the hydroxyl group is preferably substituted (bonded) to a carbon atom contained in a ring containing X as a ring member atom.
[0029] The second component may be used alone or in combination of two or more. The content of the second component is not particularly limited, but is preferably 0.0001 to 5 mass %, and more preferably 0.001 to 0.5 mass %, relative to the total mass of the treatment liquid.
[0030] In the treatment liquid, the ratio (mass ratio) of the content of the second component to the content of the first component (content of the second component / content of the first component) is preferably 0.01 to 1000, and more preferably 0.1 to 50, in order to achieve a good balance between suppressing surface roughness of the Co-containing film and suppressing defects due to particulate foreign matter derived from the treatment liquid (hereinafter also referred to as "particle defects").
[0031] [Optional Components] The treatment liquid may contain other optional components in addition to the components described above. Examples of optional components include chelating agents, organic solvents, corrosion inhibitors, hydroxylamine compounds, inorganic acids, surfactants, and various additives. The treatment liquid preferably contains at least one selected from the group consisting of chelating agents, organic solvents, corrosion inhibitors, and hydroxylamine compounds. The optional components are described below.
[0032] <Chelating Agent> The treatment liquid may contain a chelating agent, and preferably contains a chelating agent in that it has better suppression of particle defects. The chelating agent is a compound that has the function of chelating with metal ions contained in the residue. Among them, a compound having two or more functional groups (coordinating groups) that form coordinate bonds with metal ions in one molecule is preferred.
[0033] Examples of the coordinating group possessed by the chelating agent include an acid group and a cationic group. Examples of the acid group include a carboxylic acid group, a phosphonic acid group, a phosphoric acid group, a sulfo group, and a hydroxy group, with a carboxylic acid group or a phosphonic acid group being preferred. Examples of the cationic group include an amino group. Among these, the chelating agent is preferably a carboxylic acid-based chelating agent having at least one carboxylic acid group, or a phosphonic acid-based chelating agent having at least one phosphonic acid group. The number of carbon atoms in the chelating agent is preferably 15 or less, more preferably 12 or less, and even more preferably 9 or less. There is no particular lower limit, but 2 or more is preferred.
[0034] (Carboxylic Acid-Based Chelating Agent) Examples of carboxylic acid-based chelating agents include polycarboxylic acid-based chelating agents, polyaminopolycarboxylic acid-based chelating agents, and amino acid-based chelating agents.
[0035] A polycarboxylic acid chelating agent is a compound having multiple carboxylic acid groups in one molecule. However, polyaminopolycarboxylic acid chelating agents and amino acid chelating agents, which will be described later, are not included in polycarboxylic acids. Examples of polycarboxylic acid chelating agents include citric acid, malonic acid, maleic acid, succinic acid, malic acid, tartaric acid, and citric acid.
[0036] The aminopolycarboxylic acid chelating agent is a compound having at least one amino group and multiple carboxylic acid groups in one molecule, and examples thereof include mono- or polyalkylenepolyaminepolycarboxylic acids, polyaminoalkanepolycarboxylic acids, polyaminoalkanolpolycarboxylic acids, and hydroxyalkyletherpolyaminepolycarboxylic acids.
[0037] Examples of aminopolycarboxylic acid chelating agents include butylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid (DTPA), ethylenediaminetetrapropionic acid, triethylenetetraminehexaacetic acid (TTHA), 1,3-diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid, propylenediaminetetraacetic acid, ethylenediaminetetraacetic acid (EDTA), trans-1,2-diaminocyclohexanetetraacetic acid (Cy-DTA), ethylenediaminediacetic acid (EDDA), ethylenediaminedipropionic acid, 1,6-hexamethylenediamine Examples of suitable amine-N,N,N',N'-tetraacetic acid include N,N-bis(2-hydroxybenzyl)ethylenediamine-N,N-diacetic acid, diaminopropanetetraacetic acid, 1,4,7,10-tetraazacyclododecane-tetraacetic acid, diaminopropanoltetraacetic acid, (hydroxyethyl)ethylenediaminetriacetic acid, hydroxyethyliminodiacetic acid (HIDA), iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), glycol ether diaminetetraacetic acid (GEDTA), and N,N-bis(2-hydroxyethyl)glycine (DHEG). Among these, DTPA, EDTA, HIDA, DHEG, Cy-DTA, IDA, or NTA is preferred, and DTPA, EDTA, HIDA, or DHEG is more preferred.
[0038] Examples of amino acid chelating agents include glycine, serine, α-alanine (2-aminopropionic acid), β-alanine (3-aminopropionic acid), L-lysine, leucine, isoleucine, cystine, ethionine, threonine, tryptophan, tyrosine, valine, histidine, histidine derivatives, asparagine, aspartic acid, glutamine, glutamic acid, L-arginine, proline, methionine, phenylalanine, and the compounds described in paragraphs
[0021] to
[0023] of JP 2016-086094 A, as well as salts thereof. Examples of histidine derivatives include compounds described in JP 2015-165561 A and JP 2015-165562 A, the contents of which are incorporated herein by reference. Examples of salts include alkali metal salts such as sodium salts and potassium salts, ammonium salts, carbonates, and acetates.
[0039] (Phosphonic Acid Chelating Agent) A phosphonic acid chelating agent is a chelating agent having at least one phosphonic acid group in the molecule. The number of phosphonic acid groups in the phosphonic acid chelating agent is preferably 2 to 5, more preferably 2, 4, or 5, and even more preferably 2 or 5. The phosphonic acid chelating agent may have a coordinating group other than the phosphonic acid group. When the phosphonic acid chelating agent has an amino group as the coordinating group, the number of amino groups is preferably 1 to 4, more preferably 2 or 3.
[0040] Examples of phosphonic acid chelating agents include ethylidene diphosphonic acid, 1-hydroxyethylidene-1,1'-diphosphonic acid (HEDP), 1-hydroxypropylidene-1,1'-diphosphonic acid, 1-hydroxybutylidene-1,1'-diphosphonic acid, ethylaminobis(methylenephosphonic acid), dodecylaminobis(methylenephosphonic acid), nitrilotris(methylenephosphonic acid) (NTMP), ethylenediaminebis(methylenephosphonic acid) (EDDP), 1,3-propylenediaminebis(methylenephosphonic acid), and N,N,N',N'-ethylenediaminetetraacetic acid. Examples of suitable amines include tetra(methylene phosphonic acid) (EDTMP), ethylenediaminetetra(ethylene phosphonic acid), 1,3-propylenediaminetetra(methylene phosphonic acid) (PDTMP), 1,2-diaminopropanetetra(methylene phosphonic acid), 1,6-hexamethylenediaminetetra(methylene phosphonic acid), diethylenetriaminepenta(methylene phosphonic acid) (DEPP), diethylenetriaminepenta(ethylene phosphonic acid), triethylenetetraminehexa(methylene phosphonic acid), and triethylenetetraminehexa(ethylene phosphonic acid).
[0041] Furthermore, as the phosphonic acid chelating agent, the compounds described in paragraphs
[0026] to
[0036] of WO 2018 / 020878 and the compounds ((co)polymers) described in paragraphs
[0031] to
[0046] of WO 2018 / 030006 can be used, the contents of which are incorporated herein by reference.
[0042] The phosphonic acid chelating agent is preferably HEDP, NTMP, DTMP, PDTMP or EDDP, more preferably HEDP, NTMP or DTMP.
[0043] Examples of phosphate chelating agents having a phosphate group include condensed phosphoric acid and its salts, and organic compounds having two or more phosphate groups (phosphate ester groups) (excluding compounds that function as surfactants, as described below). Specific examples of phosphate chelating agents include pyrophosphoric acid, metaphosphoric acid, tripolyphosphoric acid, tetrapolyphosphoric acid, hexametaphosphoric acid, and phytic acid, as well as salts thereof.
[0044] Examples of amine-based chelating agents include at least one biguanide compound selected from the group consisting of compounds having a biguanide group and salts thereof. The number of biguanide groups contained in the biguanide compound is not particularly limited, and the biguanide compound may contain multiple biguanide groups. Examples of biguanide compounds include the compounds described in paragraphs
[0034] to
[0055] of JP-A No. 2017-504190, the contents of which are incorporated herein by reference.
[0045] The chelating agent may be used alone or in combination of two or more. When the treatment liquid contains a chelating agent, the content of the chelating agent is preferably 0.01 to 10.0 mass %, and more preferably 0.05 to 2.0 mass %, relative to the total mass of the treatment liquid, in terms of achieving a better balance between cleaning performance and corrosion prevention properties.
[0046] As the chelating agent, it is preferable to use a chelating agent that has been subjected to a purification treatment. The purification treatment method for the chelating agent is not particularly limited, and examples thereof include known methods such as filtration, ion exchange, distillation, adsorption purification, recrystallization, reprecipitation, sublimation, and purification using a column, as well as combinations of these methods. Among these, a method in which a raw material containing a chelating agent is subjected to the purification treatment described below to obtain a purified product containing a chelating agent is preferred.
[0047] <Organic Solvent> The treatment liquid may contain an organic solvent, and preferably contains an organic solvent. The organic solvent is not particularly limited, but a hydrophilic organic solvent is preferred. In this specification, a hydrophilic organic solvent refers to an organic solvent that dissolves at 0.1 g or more in 100 g of water at 25°C. The hydrophilic organic solvent is preferably an organic solvent that can be uniformly mixed with water at any ratio. The hydrophilic organic solvent is preferably at least one selected from the group consisting of glycol-based solvents, glycol ether-based solvents, amide-based solvents, alcohol-based solvents, and sulfoxide-based solvents.
[0048] The glycol solvent is not particularly limited, but examples thereof include ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, and tetraethylene glycol.
[0049] The glycol ether solvent is not particularly limited, and examples thereof include glycol monoethers. Examples of glycol monoethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, 1-methoxy-2-propanol, 2-methoxy-1-propanol, 1-ethoxy-2-propanol, 2-ethoxy-1-propanol, propylene glycol mono-n-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monobenzyl ether, and diethylene glycol monobenzyl ether.
[0050] The amide solvent is not particularly limited, but examples thereof include N,N-dimethylformamide, 1-methyl-2-pyrrolidone, 2-pyrrolidinone, 1,3-dimethyl-2-imidazolidinone, 2-pyrrolidinone, formamide, N-methylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropanamide, and hexamethylphosphoric triamide.
[0051] Alcohol-based solvents are not particularly limited, and examples thereof include alkanediols, alkoxy alcohols, saturated aliphatic monohydric alcohols, and unsaturated non-aromatic monohydric alcohols. Examples of alkanediols include glycol, 2-methyl-1,3-propanediol, 1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, and pinacol. Examples of alkoxy alcohols include 3-methoxy-3-methyl-1-butanol, 3-methoxy-1-butanol, 1-methoxy-2-butanol, and glycol monoethers. Examples of saturated aliphatic monohydric alcohols include methanol, ethanol, n-propyl alcohol, isopropanol (isopropyl alcohol), 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, 2-pentanol, t-pentyl alcohol, and 1-hexanol. Examples of unsaturated non-aromatic monohydric alcohols include allyl alcohol, propargyl alcohol, 2-butenyl alcohol, 3-butenyl alcohol, and 4-penten-2-ol. Examples of low molecular weight alcohols containing a ring structure include tetrahydrofurfuryl alcohol, furfuryl alcohol, and 1,3-cyclopentanediol.
[0052] An example of the sulfoxide solvent is dimethyl sulfoxide.
[0053] As the hydrophilic organic solvent, glycol ether solvents are preferred because they provide better effects for the present invention.
[0054] The organic solvent may be used alone or in combination of two or more. When the treatment liquid contains an organic solvent, the content of the organic solvent is preferably 50% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, relative to the total mass of the treatment liquid, in order to achieve the effects of the present invention more excellently. The lower limit is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, relative to the total mass of the treatment liquid.
[0055] <Corrosion inhibitor> The treatment solution may contain a corrosion inhibitor, and preferably contains a corrosion inhibitor. The corrosion inhibitor functions to prevent corrosion of the metal layer due to overetching or the like by coordinating with the surface of a metal layer (particularly a Co-containing layer) that will become wiring or the like of a semiconductor device to form a film. In this specification, the above-mentioned chelating agent (a compound having chelating ability) is not included in the corrosion inhibitor.
[0056] Examples of the corrosion inhibitor include a compound represented by formula (A) described below, a compound represented by formula (B) described below, a compound represented by formula (C) described below, and a substituted or unsubstituted tetrazole. More specific examples of the corrosion inhibitor include 1H-1,2,4-triazole (124TZ), 5-aminotetrazole (ATA), 5-amino-1,3,4-thiadiazole-2-thiol, 3-amino-1H-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, tolyltriazole, 3-amino-5-mercapto-1,2,4-triazole, 1-amino-1,2,4-triazole, 1-amino-1,2,3-triazole, 1 -amino-5-methyl-1,2,3-triazole, 3-mercapto-1,2,4-triazole, 3-isopropyl-1,2,4-triazole, naphthotriazole, 1H-tetrazole-5-acetic acid, 2-mercaptobenzothiazole (2-MBT), 1-phenyl-2-tetrazoline-5-thione, 2-mercaptobenzimidazole (2-MBI), 4-methyl-2-phenylimidazole, 2-mercaptothiazoline, 2,4-diamino-6- Methyl-1,3,5-triazine, thiazole, imidazole, benzimidazole, triazine, methyltetrazole, bismuthiol I, 1,3-dimethyl-2-imidazolidinone, 1,5-pentamethylenetetrazole, 1-phenyl-5-mercaptotetrazole, diaminomethyltriazine, imidazolinethione, 4-methyl-4H-1,2,4-triazole-3-thiol, 5-amino-1,3,4-thiadiazole-2-thiol, benzimidazole Zothiazole, tritolyl phosphate, indazole, adenine, cytosine, guanine, thymine, phosphate inhibitors, pyrazoles, propanethiol, silanes, benzohydroxamic acids, heterocyclic nitrogen inhibitors, thiourea, 1,1,3,3-tetramethylurea, urea, urea derivatives, uric acid, potassium ethylxanthate, dodecylphosphonic acid, iminodiacetic acid, boric acid, nitrilotriacetic acid, sulfolane, 2,3,5-trimethylpyrazine, 2-ethyl-3,5-dimethylpyrazine, quinoxaline, acetylpyrrole, pyridazine, histadine, pyrazine, glutathione (reduced form), cystine, thiophene, mercaptopyridine N-oxide, thiamine HCl, tetraethylthiuram disulfide, 2,5-dimercapto-1,3-thiadiazole ascorbic acid, ascorbic acid, catechol, t-butylcatechol, phenol, and pyrogallol.
[0057] The corrosion inhibitor may be a substituted or unsubstituted benzotriazole (hereinafter also referred to as a "benzotriazole compound"). The substituted benzotriazole is preferably a benzotriazole substituted with an alkyl group, an aryl group, a halogen group, an amino group, a nitro group, an alkoxy group, or a hydroxyl group. The substituted benzotriazole also includes one fused with one or more aryl groups (e.g., phenyl groups) or heteroaryl groups.
[0058] Benzotriazole compounds suitable as corrosion inhibitors include, for example, benzotriazole (BTA), 5-aminotetrazole, 1-hydroxybenzotriazole, 5-phenylthiol-benzotriazole, 5-chlorobenzotriazole, 4-chlorobenzotriazole, 5-bromobenzotriazole, 4-bromobenzotriazole, 5-fluorobenzotriazole, 4-fluorobenzotriazole, naphthotriazole, tolyltriazole, 5-phenyl-benzotriazole, 5-nitrobenzotriazole, 4-nitrobenzotriazole, 3-amino-5-mercapto-1,2,4-triazole, 2-(5-amino-pentyl)-benzotriazole, 1-amino-benzotriazole, 5-methyl-1H-benzotriazole (5MBTA), benzotriazole-5-carboxylic acid, 4-methylbenzotriazole, 4-ethylbenzotriazole, 5-ethylbenzotriazole, 4-propylbenzotriazole, triazole, 5-propylbenzotriazole, 4-isopropylbenzotriazole, 5-isopropylbenzotriazole, 4-n-butylbenzotriazole, 5-n-butylbenzotriazole, 4-isobutylbenzotriazole, 5-isobutylbenzotriazole, 4-pentylbenzotriazole, 5-pentylbenzotriazole, 4-hexylbenzotriazole, 5-hexylbenzotriazole, 5-methoxybenzotriazole, 5-hydroxybenzotriazole, dihydroxypropylbenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]-benzotriazole, 5-t-butylbenzotriazole, 5-(1',1'-dimethylpropyl)-benzotriazole, 5-(1',1',3'-trimethylbutyl)benzotriazole, 5-n-octylbenzotriazole, and 5-(1',1',3',3'-tetramethylbutyl)benzotriazole.Further, examples of the benzotriazole compound include 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, 2,2'-{[(5-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol, 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethane, or 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bispropane, and N,N-bis(2-ethylhexyl)-(4 or 5)-methyl-1H-benzotriazole-1-methylamine.
[0059] In terms of achieving the effects of the present invention more effectively, the treatment liquid preferably contains at least one compound selected from the group consisting of a compound represented by the following formula (A), a compound represented by the following formula (B), a compound represented by the following formula (C), and a substituted or unsubstituted tetrazole:
[0060]
[0061] In the above formula (A), R 1A ~R 5A each independently represents a hydrogen atom, a substituted or unsubstituted hydrocarbon group, a hydroxyl group, a carboxyl group, or a substituted or unsubstituted amino group, provided that the structure contains at least one group selected from a hydroxyl group, a carboxyl group, and a substituted or unsubstituted amino group. 1B ~R 4B each independently represents a hydrogen atom or a substituted or unsubstituted hydrocarbon group. 1C , R 2C and R N each independently represents a hydrogen atom or a substituted or unsubstituted hydrocarbon group. 1C and R 2C may be bonded to form a ring.
[0062] In the above formula (A), R 1A ~R 5AExamples of the hydrocarbon represented by include an alkyl group (preferably having 1 to 12 carbon atoms, more preferably having 1 to 6 carbon atoms, and even more preferably having 1 to 3 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, and more preferably having 2 to 6 carbon atoms), an alkynyl group (preferably having 2 to 12 carbon atoms, and more preferably having 2 to 6 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 14 carbon atoms, and even more preferably having 6 to 10 carbon atoms), and an aralkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 15 carbon atoms, and even more preferably having 7 to 11 carbon atoms). In addition, examples of the substituent in the case where the hydrocarbon group is substituted include a hydroxyl group, a carboxy group, and a substituted or unsubstituted amino group (in the case where the amino group is substituted, the substituent is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms). In addition, in formula (A), the structure contains at least one group selected from a hydroxyl group, a carboxy group, and a substituted or unsubstituted amino group (when the amino group is substituted, the substituent is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms).
[0063] In formula (A), R 1A ~R 5A Examples of the substituted or unsubstituted hydrocarbon group represented by formula (A) include hydrocarbon groups having 1 to 6 carbon atoms substituted with a hydroxyl group, a carboxyl group, or an amino group. Examples of the compound represented by formula (A) include 1-thioglycerol, L-cysteine, and thiomalic acid.
[0064] In formula (B), R 1B ~R 4B is a substituted or unsubstituted hydrocarbon group represented by R 1A ~R 5A R has the same meaning as the substituted or unsubstituted hydrocarbon group represented by 1B ~R 4B Examples of the substituted or unsubstituted hydrocarbon group represented by formula (B) include hydrocarbon groups having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, a propyl group, and a t-butyl group. Examples of the compound represented by formula (B) include catechol and t-butylcatechol.
[0065] In formula (C), R 1C , R 2C and R N The substituted or unsubstituted hydrocarbon group represented by the formula (A) is 1A ~R 5A R has the same meaning as the substituted or unsubstituted hydrocarbon group represented by 1C , R 2C and R N Examples of the substituted or unsubstituted hydrocarbon group represented by R include hydrocarbon groups having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, a propyl group, and a butyl group. 1C and R 2C may be bonded to form a ring. 1C and R 2C Examples of the ring formed by bonding R include a benzene ring. 1C and R 2C and , when bonded to form a ring, the ring may further have a substituent (for example, a hydrocarbon group having 1 to 5 carbon atoms). Examples of the compound represented by formula (C) include 1H-1,2,3-triazole (123TZ), benzotriazole (BTA), 5-methyl-1H-benzotriazole (5M-BTA), tolyltriazole, 2,2'-{[(4-methyl-1H-benzotriazol-1-yl)methyl]imino}bisethanol (trade name "IRGAMET 42", manufactured by BASF), and N,N-bis(2-ethylhexyl)-(4 or 5)-methyl-1H-benzotriazole-1-methylamine (trade name "IRGAMET 39", manufactured by BASF), and the like. In view of the superior effects of the present invention, 1H-1,2,3-triazole, benzotriazole, 5-methyl-1H-benzotriazole, and tolyltriazole are preferred.
[0066] Examples of the substituted or unsubstituted tetrazole include unsubstituted tetrazole and tetrazole having a hydroxyl group, a carboxyl group, or a substituted or unsubstituted amino group as a substituent. When the amino group is substituted, the substituent is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms.
[0067] The corrosion inhibitor may be used alone or in combination of two or more. When the treatment liquid contains a corrosion inhibitor, the content of the corrosion inhibitor in the treatment liquid is preferably 0.01 to 5 mass %, more preferably 0.05 to 3 mass %, and even more preferably 0.1 to 1 mass %, relative to the total mass of the treatment liquid.
[0068] The corrosion inhibitor is preferably of a high purity grade, and more preferably further purified before use. The method for purifying the corrosion inhibitor is not particularly limited, but known methods such as filtration, ion exchange, distillation, adsorption purification, recrystallization, reprecipitation, sublimation, and purification using a column can be used, and these methods can also be used in combination.
[0069] <Hydroxylamine Compound> The treatment liquid contains hydroxylamine (NH 2 The composition may contain at least one hydroxylamine compound selected from the group consisting of hydroxylamine derivatives, hydroxylamine derivatives, and salts thereof, and preferably contains the above-mentioned hydroxylamine compound. The hydroxylamine compound promotes the decomposition and solubilization of residues, such as etching residues and ashing residues.
[0070] The hydroxylamine derivative is not particularly limited, and examples thereof include O-methylhydroxylamine, O-ethylhydroxylamine, N-methylhydroxylamine, N,N-dimethylhydroxylamine, N,O-dimethylhydroxylamine, N-ethylhydroxylamine, N,N-diethylhydroxylamine, N,O-diethylhydroxylamine, O,N,N-trimethylhydroxylamine, N,N-dicarboxyethylhydroxylamine, and N,N-disulfoethylhydroxylamine.
[0071] Hydroxylamine (NH 2 The salts of hydroxylamine derivatives are the same as those of the above hydroxylamine (NH 2Hydroxylamine (NH OH) and inorganic or organic acid salts of hydroxylamine derivatives are preferred, and salts of inorganic acids formed by the bonding of a nonmetallic atom such as Cl, S, N, or P with a hydrogen atom are more preferred, and salts of any of hydrochloric acid, sulfuric acid, and nitric acid are even more preferred. 2 Hydroxylamine (NH OH) and inorganic acid salts of hydroxylamine derivatives are preferably hydroxylamine nitrate, hydroxylamine sulfate, hydroxylamine hydrochloride, hydroxylamine phosphate, N,N-diethylhydroxylamine sulfate, N,N-diethylhydroxylamine nitrate, or mixtures thereof. 2 Examples of organic acid salts of hydroxylamine derivatives and hydroxylammonium citrate, hydroxylammonium oxalate, and hydroxylammonium fluoride are listed. As the hydroxylamine compound, hydroxylamine (NH 2 OH) is preferred.
[0072] The hydroxylamine compound may be used alone or in combination of two or more. When the treatment liquid contains a hydroxylamine compound, the content of the hydroxylamine compound is preferably 0.1 to 20 mass %, and more preferably 0.5 to 10 mass %, relative to the total mass of the treatment liquid, in terms of more excellent performance in suppressing particle defects.
[0073] <pH Adjuster> The treatment liquid may contain a pH adjuster to adjust the pH of the treatment liquid. Examples of the pH adjuster include acidic compounds and basic compounds.
[0074] (Acidic Compound) The treatment liquid may contain an acidic compound as a pH adjuster. The acidic compound may be an inorganic acid or an organic acid (excluding the above-mentioned chelating agents). The treatment liquid preferably contains an inorganic acid. Examples of inorganic acids include sulfuric acid, hydrochloric acid, nitric acid, boric acid, phosphonic acid, and phosphoric acid, with hydrochloric acid, phosphoric acid, or sulfuric acid being preferred. Examples of organic acids include lower (C1 to C4) aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, and butyric acid. Furthermore, the above-mentioned chelating agents may also serve as the acidic compound.
[0075] (Basic Compound) The treatment liquid may contain a basic compound as a pH adjuster. A basic compound is intended to be a compound that, when 1 g of the compound is dissolved in 100 g of water, results in a solution with a pH of 9 or higher. In this specification, the compounds contained in the first component, second component, and amine-based chelating agent are not included in the basic compound.
[0076] Examples of basic compounds include ammonium hydroxide, water-soluble amines, and quaternary ammonium salts.
[0077] In this specification, the term "water-soluble amine" refers to an amine that can dissolve 50 g or more in 1 L of water. None of the above are included in the water-soluble amine. Examples of water-soluble amines include those that have a primary amino group (-NH 2 Examples of water-soluble amines include primary amines having a hydroxyl group (>NH) in the molecule, secondary amines having a secondary amino group (>NH) in the molecule, tertiary amines having a tertiary amino group (>N-) in the molecule, and salts thereof. The water-soluble amine may also be a compound having at least one hydroxyl alkyl group in the molecule (amino alcohol).
[0078] Examples of quaternary ammonium salts include quaternary ammonium hydroxides, such as tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), tetrapropylammonium hydroxide, tetrabutylammonium hydroxide (TBAH), methyltripropylammonium hydroxide, methyltributylammonium hydroxide, ethyltrimethylammonium hydroxide, dimethyldiethylammonium hydroxide, benzyltrimethylammonium hydroxide (BzTMAH), hexadecyltrimethylammonium hydroxide, (2-hydroxyethyl)trimethylammonium hydroxide, and spiro-(1,1')-bipyrrolidinium hydroxide, with TMAH, TEAH, TBAH, or BzTMAH being preferred.
[0079] The pH adjuster may be used alone or in combination of two or more. The type and content of the pH adjuster may be appropriately selected (acidic compound and basic compound) and the content adjusted so that the pH of the treatment liquid falls within the preferred range described below. When the treatment liquid contains a pH adjuster, the content is preferably 0.01 to 20% by mass, more preferably 0.01 to 10% by mass, based on the total mass of the treatment liquid.
[0080] The treatment liquid may contain additives other than the above components, such as surfactants, antifoaming agents, and rust inhibitors.
[0081] The content of each of the above components contained in the treatment liquid can be measured by known methods such as gas chromatography-mass spectrometry (GC-MS), liquid chromatography-mass spectrometry (LC-MS), and ion-exchange chromatography (IC).
[0082] [Physical Properties of Treatment Solution] <pH> The pH of the treatment solution is preferably 5 to 14, more preferably 6 to 11, at 25°C. By having the pH of the treatment solution within the above range, the effects of the present invention and residue removability can be achieved at an even better level. The pH of the treatment solution is a pH value obtained by measuring at 25°C using a known pH meter according to a method in accordance with JIS Z8802-1984. The pH of the treatment solution can be adjusted by using any of the above-mentioned pH adjusters, and components that function as pH adjusters, such as the first component and surfactants.
[0083] <Metal Content> In the treatment solution, the content (measured as ion concentration) of each metal (metal element Fe, Co, Na, Cu, Mg, Mn, Li, Al, Cr, Ni, Zn, Sn, and Ag) contained as an impurity in the solution is preferably 5 mass ppm or less, more preferably 1 mass ppm or less. Since it is expected that treatment solutions of even higher purity will be required in the manufacture of cutting-edge semiconductor devices, the metal content is more preferably lower than 1 mass ppm, that is, more preferably on the order of ppb by mass or less, particularly preferably 100 mass ppb or less, and most preferably less than 10 mass ppb. The lower limit is preferably 0.
[0084] The type and content of metals in the treatment solution can be measured by ICP-MS (Inductively Coupled Plasma Mass Spectrometry). Examples of instruments that can be used to perform ICP-MS include Agilent 8900 Triple Quadrupole ICP-MS (for semiconductor analysis, option #200) manufactured by Agilent Technologies, NexION350S manufactured by PerkinElmer, and Agilent 8800 manufactured by Agilent Technologies.
[0085] Examples of methods for reducing the metal content include distillation and purification treatments such as filtration using an ion exchange resin or a filter at the stage of raw materials used in producing the treatment liquid or at the stage after the production of the treatment liquid. Another method for reducing the metal content is to use a container that is less likely to leach out impurities, as described below, as a container for containing the raw materials or the produced treatment liquid. Another method is to apply a fluororesin lining to the inner wall of a pipe or the like to prevent metal components from leaching out from the pipe during the production of the treatment liquid.
[0086] <Coarse Particles> The treatment liquid may contain coarse particles, but preferably is substantially free of them. Coarse particles refer to particles with a diameter of 0.2 μm or more, assuming a spherical shape. Furthermore, being substantially free of coarse particles means that, when the treatment liquid is measured using a commercially available measuring device for light-scattering liquid-borne particle measurement, there are 10 or fewer particles of 0.2 μm or more per mL of treatment liquid. Note that coarse particles contained in the treatment liquid include particles such as dust, dirt, organic solids, and inorganic solids contained as impurities in raw materials, as well as particles such as dust, dirt, organic solids, and inorganic solids introduced as contaminants during the preparation of the treatment liquid, which ultimately remain undissolved in the treatment liquid. Furthermore, it is preferable that the treatment liquid is substantially free of abrasive grains. The amount of coarse particles present in the treatment liquid can be measured in the liquid phase using a commercially available measuring device for light-scattering liquid-borne particle measurement using a laser as a light source. Methods for removing coarse particles include, for example, filtering.
[0087] [Preparation of Treatment Solution] <Treatment Solution Preparation Step> The method for preparing the treatment solution is not particularly limited and can be prepared by a known method. The treatment solution can be prepared, for example, by mixing the above-mentioned components. The order and / or timing for mixing the above-mentioned components can be, for example, by sequentially adding the first component, the second component, and optional components such as a chelating agent, an organic solvent, and a corrosion inhibitor, as needed, to a container containing purified pure water, followed by stirring to mix, and adding a pH adjuster as needed to adjust the pH of the mixed solution. When adding water and the components to a container, they may be added all at once or in multiple installments.
[0088] The stirring device and stirring method used to prepare the treatment solution may be a known device such as a stirrer or disperser. Examples of the stirrer include an industrial mixer, a portable stirrer, a mechanical stirrer, and a magnetic stirrer. Examples of the disperser include an industrial disperser, a homogenizer, an ultrasonic disperser, and a bead mill.
[0089] The mixing of the components in the preparation step of the treatment solution, the purification treatment described below, and storage of the produced treatment solution are preferably carried out at 40° C. or less, and more preferably at 30° C. or less. The lower limit is preferably 5° C. or more, and more preferably 10° C. or more. By preparing, treating, and / or storing the treatment solution within the above temperature range, the performance can be maintained stably for a long period of time.
[0090] <Purification Treatment> It is preferable to perform a purification treatment in advance on one or more of the raw materials for preparing the treatment solution. Examples of the purification treatment include known methods such as distillation, ion exchange, and filtration. The degree of purification is preferably such that the raw material has a purity of 99% by mass or more, and more preferably such that the raw solution has a purity of 99.9% by mass or more. The upper limit is preferably 99.9999% by mass or less.
[0091] Examples of purification methods include passing the raw material through an ion exchange resin or a reverse osmosis membrane (RO membrane), distilling the raw material, and filtering, which will be described later. The purification method may be a combination of two or more of the above purification methods. For example, the raw material may be subjected to primary purification by passing it through an RO membrane, and then subjected to secondary purification by passing it through a purification device made of a cation exchange resin, an anion exchange resin, or a mixed-bed ion exchange resin. Furthermore, the purification process may be performed multiple times.
[0092] (Filtering) Filters used for filtering include known filtration filters. Examples include filters made of fluororesins such as polytetrafluoroethylene (PTFE) and tetrafluoroethylene perfluoroalkyl vinyl ether copolymer (PFA), polyamide resins such as nylon, and polyolefin resins (including high-density or ultra-high molecular weight) such as polyethylene and polypropylene (PP). Among these materials, materials selected from the group consisting of polyethylene, polypropylene (including high-density polypropylene), fluororesins (including PTFE and PFA), and polyamide resins (including nylon) are preferred, and fluororesin filters are more preferred. Filtering raw materials using filters made of these materials can effectively remove highly polar foreign matter that is likely to cause defects.
[0093] The critical surface tension of the filter is preferably 70 to 95 mN / m, more preferably 75 to 85 mN / m. The critical surface tension value of the filter is the manufacturer's nominal value. Using a filter with a critical surface tension within the above range can effectively remove highly polar foreign matter that is likely to cause defects. The filter pore size is preferably 2 to 20 nm, more preferably 2 to 15 nm. By setting the pore size within this range, it is possible to reliably remove impurities and fine foreign matter such as aggregates contained in the raw material while suppressing filtration clogging. The pore size here can refer to the filter manufacturer's nominal value.
[0094] Filtering may be performed only once or two or more times. When filtering is performed two or more times, the filters used may be the same or different. The filtering temperature is preferably room temperature (25°C) or lower, more preferably 23°C or lower, and even more preferably 20°C or lower. The filtering temperature is preferably 0°C or higher, more preferably 5°C or higher, and even more preferably 10°C or higher. By filtering within the above temperature range, the amount of particulate foreign matter and impurities dissolved in the raw material can be reduced, and foreign matter and impurities can be efficiently removed.
[0095] [Processing Liquid Container] The processing liquid may be stored in a container until use. Such a container and the processing liquid stored in the container are collectively referred to as a processing liquid container. The processing liquid is taken out of the stored processing liquid container and used. The processing liquid may also be transported as a processing liquid container.
[0096] For semiconductor applications, the container preferably has a high level of cleanliness within the container and inhibits the elution of impurities from the inner wall of the container's storage compartment into each liquid. Examples of such containers include various commercially available containers for semiconductor processing liquids, such as the "Clean Bottle" series manufactured by Aicello Chemical Co., Ltd. and the "Pure Bottle" manufactured by Kodama Resin Industry Co., Ltd., but are not limited to these. The inner wall of the container is preferably formed from one or more resins selected from the group consisting of polyethylene resin, polypropylene resin, and polyethylene-polypropylene resin, or a different resin. It is also preferable that the inner wall of the container be formed from a metal that has been treated to prevent rust and metal elution, such as stainless steel, Hastelloy, Inconel, or Monel.
[0097] As the different resin, a fluororesin (perfluororesin) is preferred. By using a container whose inner wall is a fluororesin, the occurrence of the problem of elution of ethylene or propylene oligomers can be suppressed compared to containers whose inner wall is made of polyethylene resin, polypropylene resin, or polyethylene-polypropylene resin. An example of a container whose inner wall is made of a fluororesin is the FluoroPure PFA composite drum manufactured by Entegris. Also usable are containers described on page 4 of JP-A-3-502677, page 3 of WO 2004 / 016526, and pages 9 and 16 of WO 99 / 046309.
[0098] In addition to the above-mentioned fluororesin, quartz and electropolished metal materials (i.e., electropolished metal materials) are also preferably used for the inner wall of the container. The metal material used to manufacture the electropolished metal material preferably contains at least one selected from the group consisting of chromium and nickel, and the total content of chromium and nickel is preferably more than 25% by mass relative to the total mass of the metal material, such as stainless steel and nickel-chromium alloys. The total content of chromium and nickel in the metal material is more preferably 30% by mass or more relative to the total mass of the metal material. The upper limit is preferably 90% by mass or less.
[0099] Known methods can be used to electropolish metal materials, such as those described in paragraphs
[0011] to
[0014] of JP 2015-227501 A and paragraphs
[0036] to
[0042] of JP 2008-264929 A.
[0100] The interior of these containers is preferably washed before filling with the treatment liquid. The liquid used for washing is preferably one that has a reduced amount of metal impurities. After production, the treatment liquid may be bottled in containers such as gallon bottles or coated bottles, and then transported and stored.
[0101] To prevent changes in the components of the treatment solution during storage, the container may be filled with an inert gas (such as nitrogen or argon) with a purity of 99.99995% by volume or higher. Gases with low water content are particularly preferred. The treatment solution may be transported and stored at room temperature, or the temperature may be controlled to a range of -20°C to 20°C to prevent deterioration.
[0102] (Clean Room) It is preferable that all handling, processing, analysis, and measurement, including production of the processing solution, opening and cleaning of containers, and filling of the processing solution, be carried out in a clean room. The clean room preferably meets the 14644-1 clean room standard. Among these, it is more preferable that the clean room meets any of ISO (International Organization for Standardization) Class 1, ISO Class 2, ISO Class 3, ISO Class 4, ISO Class 5, and ISO Class 6, even more preferable that the clean room meets any of ISO Class 1, ISO Class 2, ISO Class 3, and ISO Class 4, particularly preferable that the clean room meets ISO Class 1 or ISO Class 2, and most preferable that the clean room meets ISO Class 1.
[0103] [Uses] Next, uses of the present treatment liquid will be described. The present treatment liquid is a treatment liquid for semiconductor devices. In this specification, "for semiconductor devices" means that it is used in the manufacturing process of semiconductor devices. The present treatment liquid can be used in any step for manufacturing semiconductor devices.
[0104] The present treatment liquid can be used, for example, as a cleaning liquid for cleaning semiconductor substrates (semiconductor substrate cleaning liquid), and as a treatment liquid for removing target substances such as metal-containing substances on semiconductor substrates (semiconductor substrate treatment liquid).
[0105] The semiconductor substrate cleaning liquid is not particularly limited as long as it is a cleaning liquid that is applied to a semiconductor substrate and used for the purpose of removing residues such as metal impurities or fine particles adhering to the semiconductor substrate, and examples thereof include a cleaning liquid for a semiconductor substrate that has been subjected to an etching treatment (post-etching residue cleaning liquid), a cleaning liquid for a semiconductor substrate that has been subjected to a chemical mechanical polishing (CMP) treatment (pCMP cleaning liquid), a cleaning liquid for buffing a semiconductor substrate that has been subjected to a CMP treatment (buff cleaning cleaning liquid), a cleaning liquid for cleaning a semiconductor substrate that has been subjected to backgrinding, and a cleaning liquid for a semiconductor substrate to which electronic components have been soldered using flux or a semiconductor substrate on which solder bumps have been formed.
[0106] Examples of the semiconductor substrate treatment liquid include treatment liquids to be applied to semiconductor substrates, such as an etching liquid that dissolves and removes metal-containing substances on a semiconductor substrate, a pre-wet liquid that is applied to a substrate to improve the applicability of an actinic ray-sensitive or radiation-sensitive treatment liquid before the step of forming a resist film using the actinic ray-sensitive or radiation-sensitive treatment liquid, and a rinse liquid that rinses away substances adhering to the semiconductor substrate.
[0107] The present treatment liquid may be used for only one of the above uses, or for two or more uses.
[0108] [Method for Treating a Workpiece] The present treatment solution is used, for example, in a method for treating a workpiece (hereinafter also referred to as the "present treatment method") that includes a step of contacting the workpiece with the present treatment solution. Examples of the workpiece include the above-mentioned target objects for the present treatment solution. By using the present treatment solution in the present treatment method, the workpiece can be cleaned (e.g., removing residues on the workpiece) or one or more metal-containing substances contained in the workpiece can be removed. More specifically, a cleaning method using the present treatment solution to remove residues attached to the workpiece (e.g., a method for cleaning etching residues on a semiconductor substrate) can be mentioned. Other examples include an etching treatment method using the present treatment solution to dissolve and remove metal-containing substances on a semiconductor substrate, a pre-wet treatment method in which the present treatment solution is applied to a semiconductor substrate before a step of forming a resist film using an actinic ray-sensitive or radiation-sensitive treatment solution, and a rinse treatment method in which the semiconductor substrate is rinsed with the present treatment solution.
[0109] The object to be treated by the present treatment method is not particularly limited as long as it is a member used in the manufacturing process of a semiconductor device, and examples thereof include the above-mentioned semiconductor substrates. Among these, semiconductor substrates having a metal layer are preferred.
[0110] Examples of the metal layer of the workpiece include simple metals and alloys. Examples of metal atoms contained in the metal layer include cobalt (Co), ruthenium (Ru), tungsten (W), molybdenum (Mo), aluminum (Al), copper (Cu), titanium (Ti), and tantalum (Ta). The content of the metal atoms in the metal layer is preferably 30 to 100 mass%, more preferably 40 to 100 mass%, and even more preferably 50 to 100 mass%, relative to the total mass of the metal layer.
[0111] The metal layer preferably contains cobalt, ruthenium, tungsten, molybdenum, aluminum, copper, titanium, or tantalum as a primary component, more preferably cobalt or copper as a primary component, and even more preferably cobalt as a primary component. In this specification, for example, "containing cobalt as a primary component" means that the cobalt content is the highest among the metal atoms contained in the metal layer. Examples of metal layers containing cobalt as a primary component (hereinafter also referred to as "cobalt-containing layers") include simple cobalt (metallic cobalt) and cobalt alloys (alloys in which the metal atom present in the highest concentration is cobalt). The content of the metal atoms (preferably cobalt atoms) contained as a primary component in the metal layer is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 95 to 100 mass%, based on the total mass of the metal layer.
[0112] The form of the metal layer on the workpiece is not particularly limited, and examples thereof include a form in which the metal layer is arranged in the form of a film (metal-containing film) and a form in which the metal layer is arranged in the form of a wiring (metal-containing wiring film). When the metal layer is in the form of a film or wiring, its thickness is not particularly limited and may be appropriately selected depending on the application. The thickness of the metal layer in the form of a film or wiring is preferably 500 nm or less, more preferably 20 nm or less. There is no particular lower limit, but a thickness of 1 nm or more is preferred.
[0113] [Semiconductor Substrate Processing Method] Hereinafter, a semiconductor substrate, which is an example of an object to be processed in this processing method, and this processing method in which this processing solution is applied to a semiconductor substrate will be described in more detail.
[0114] The present treatment liquid can be used in a method for treating a semiconductor substrate, which includes a step of contacting the semiconductor substrate with the present treatment liquid. In particular, it is preferably used in the method for treating a semiconductor substrate having a metal layer. The semiconductor substrate may have a metal layer on only one side of the main surface of the semiconductor substrate, or on both sides of the main surface of the semiconductor substrate. The metal layer may be disposed over the entire main surface of the semiconductor substrate, or may be disposed over a portion of the main surface of the semiconductor substrate. The metal layer of the semiconductor substrate is as described above. The semiconductor substrate may also have two or more metal layers with different structures and / or compositions. In this specification, the term "semiconductor substrate" includes, for example, a single-layer semiconductor substrate and a multi-layer semiconductor substrate.
[0115] The semiconductor substrate may be, for example, a semiconductor substrate having the above-mentioned metal layer (preferably a cobalt-containing layer), a barrier layer, and an insulating layer on the surface of a wafer constituting the substrate.
[0116] The type of semiconductor substrate is not particularly limited, and examples thereof include semiconductor wafers, glass substrates for photomasks, glass substrates for liquid crystal displays, glass substrates for plasma displays, substrates for FEDs (Field Emission Displays), substrates for optical disks, substrates for magnetic disks, and substrates for magneto-optical disks. Examples of wafers constituting semiconductor substrates include wafers made of silicon-based materials such as silicon (Si) wafers, silicon carbide (SiC) wafers, and silicon-containing resin wafers (glass epoxy wafers), as well as gallium phosphide (GaP) wafers, gallium arsenide (GaAs) wafers, and indium phosphide (InP) wafers. Among these, wafers made of silicon-based materials such as silicon wafers, silicon carbide wafers, and silicon-containing resin wafers (glass epoxy wafers) are preferred. Examples of silicon wafers include n-type silicon wafers doped with pentavalent atoms (e.g., phosphorus (P), arsenic (As), and antimony (Sb)), and p-type silicon wafers doped with trivalent atoms (e.g., boron (B), gallium (Ga)). Examples of silicon in silicon wafers include amorphous silicon, single crystal silicon, polycrystalline silicon, and polysilicon. There are no particular limitations on the size, thickness, shape, and layer structure of the semiconductor substrate, and these can be selected as desired.
[0117] The barrier layer is not particularly limited, and examples thereof include a barrier layer containing one or more materials selected from the group consisting of Ta, tantalum nitride (TaN), Ti, titanium nitride (TiN), titanium tungsten (TiW), W, and tungsten nitride (WN). Among these, Ta, TaN, Ti, or TiN is preferred. The insulating layer is not particularly limited, and examples thereof include an insulating layer containing one or more materials selected from the group consisting of silicon nitride (SiN), silicon oxide, silicon carbide (SiC), silicon carbonitride, silicon oxycarbide (SiOC), silicon oxynitride, and tetraethoxysilane (TEOS). Among these, silicon nitride (SiN), TEOS, silicon carbide (SiC), or silicon oxycarbide (SiOC) is preferred. The insulating layer may also be composed of multiple layers.
[0118] The semiconductor substrate may have a removal target on the semiconductor substrate to be removed by the treatment liquid. In this specification, "on the semiconductor substrate" includes, for example, the front and back surfaces, side surfaces, and inside grooves of the semiconductor substrate. Furthermore, the removal target on the semiconductor substrate includes not only a case where the removal target is directly on the surface of the semiconductor substrate, but also a case where the removal target is present on the semiconductor substrate via another layer.
[0119] The semiconductor substrate may have various other layers and / or structures as desired. For example, the semiconductor substrate may have metal wiring, gate electrodes, source electrodes, drain electrodes, insulating layers, ferromagnetic layers, and / or nonmagnetic layers. The semiconductor substrate may have exposed integrated circuit structures, such as interconnect mechanisms, including metal wiring and dielectric materials. Metals and alloys used for interconnect mechanisms include, for example, aluminum, copper-aluminum alloys, copper, titanium, tantalum, cobalt, silicon, titanium nitride, tantalum nitride, and tungsten. The substrate may also have layers of silicon oxide, silicon nitride, silicon carbide, and / or carbon-doped silicon oxide.
[0120] The method for manufacturing a semiconductor substrate is not particularly limited. For example, a semiconductor substrate having an insulating layer, a barrier layer, and a metal layer on a substrate can be manufactured by forming an insulating layer on a substrate, forming holes (or grooves) in the insulating layer, forming a barrier layer and a metal layer on the insulating layer in this order, and then performing a planarization process such as chemical mechanical polishing (CMP). The method for forming the barrier layer and the metal layer on the insulating layer is not particularly limited, and examples thereof include sputtering, physical vapor deposition (PVD), atomic layer deposition (ALD), chemical vapor deposition (CVD), and molecular beam epitaxy (MBE). Alternatively, the above method may be performed through a predetermined mask to form a patterned metal layer on a substrate.
[0121] <Semiconductor Substrate Cleaning Method> A preferred example of the present treatment method is a semiconductor substrate cleaning method including a cleaning step of cleaning a semiconductor substrate by contacting the semiconductor substrate with the present treatment solution. In the semiconductor device manufacturing process, when a metal layer and / or an insulating layer of a semiconductor substrate is etched by plasma etching using a resist pattern as a mask, residues derived from the photoresist, metal layer, and insulating layer are generated on the semiconductor substrate. Furthermore, when an unnecessary resist pattern is removed by plasma ashing, residues derived from the ashed photoresist are also generated on the semiconductor substrate. The semiconductor substrate cleaning method is a process for removing these residues, such as etching residues and ashing residues, from a semiconductor substrate. The present treatment solution can be used as a cleaning solution in the semiconductor substrate cleaning method. Use of the present treatment solution can remove the etching residues and / or ashing residues generated on an etched semiconductor substrate and suppress surface roughness of a metal layer (particularly a cobalt-containing layer) of the semiconductor substrate.
[0122] The method of contacting the semiconductor substrate with the treatment solution is not particularly limited, and known methods used in the field of semiconductor device manufacturing may be appropriately adopted, such as an immersion method in which the semiconductor substrate is immersed in the treatment solution, a spin (drop) method in which the treatment solution is dripped onto the rotating semiconductor substrate, a spray (spray) method in which the treatment solution is sprayed onto the semiconductor substrate, and a scrub cleaning method in which a cleaning member such as a brush is physically brought into contact with the surface of the semiconductor substrate while the treatment solution is supplied to the semiconductor substrate to remove residues. In cleaning the semiconductor substrate, a mechanical agitation method may be used to further reduce impurities remaining on the surface of the semiconductor substrate and further enhance the cleaning ability of the treatment solution. Examples of mechanical agitation methods include a method in which the treatment solution is circulated over the semiconductor substrate, a method in which the treatment solution is passed over or sprayed onto the semiconductor substrate, and a method in which the treatment solution is agitated using ultrasonic waves or megasonics. The above-mentioned cleaning may be performed only once or two or more times. When cleaning two or more times, the same method may be repeated, or different methods may be combined.
[0123] The semiconductor substrate cleaning method may be either a single wafer method or a batch method. The single wafer method generally processes semiconductor substrates one by one, while the batch method generally processes multiple semiconductor substrates simultaneously.
[0124] The temperature of the treatment liquid used to clean semiconductor substrates is not particularly limited as long as it is a temperature typically used in this field. While cleaning is often performed at room temperature (approximately 25°C), the temperature can be selected arbitrarily to improve cleaning performance and minimize damage to components. The temperature of the treatment liquid is preferably 10 to 60°C, more preferably 15 to 50°C. The cleaning time for cleaning semiconductor substrates can be appropriately adjusted depending on the type and content of components contained in the treatment liquid. In practice, 10 to 120 seconds is preferred, 20 to 90 seconds is more preferred, and 30 to 60 seconds is even more preferred. When the treatment liquid is dripped or sprayed onto the semiconductor substrate, the supply amount (supply rate) of the treatment liquid is preferably 50 to 5,000 mL / min, more preferably 500 to 2,000 mL / min.
[0125] (Rinsing Step) After the above cleaning step, a step of rinsing the semiconductor substrate with a solvent to clean it (hereinafter referred to as the "rinsing step") may be carried out. The rinsing step is preferably carried out continuously following the above cleaning step, and is a step of rinsing the semiconductor substrate with a rinse liquid for 5 to 300 seconds. The rinsing step may be carried out using the above mechanical stirring method.
[0126] Examples of the rinse liquid include water (preferably deionized (DI) water), methanol, ethanol, isopropanol, N-methylpyrrolidinone, γ-butyrolactone, dimethyl sulfoxide, ethyl lactate, and propylene glycol monomethyl ether acetate. An aqueous rinse liquid having a pH greater than 8.0 (such as diluted aqueous ammonium hydroxide) may also be used. The method of contacting the rinse liquid with the semiconductor substrate can be the same as the method of contacting the treatment liquid with the semiconductor substrate.
[0127] (Drying Step) After the above-mentioned cleaning step or cleaning step, a drying step may be performed to dry the semiconductor substrate. Drying methods include, for example, spin drying, flowing a dry gas over the semiconductor substrate, heating the semiconductor substrate with a heating means such as a hot plate or an infrared lamp, Marangoni drying, Rotagoni drying, IPA (isopropanol) drying, and any combination thereof. The drying time in the drying step depends on the specific method used, but is preferably 20 seconds to 5 minutes.
[0128] <Etching Treatment of Semiconductor Substrate> Another specific example of the present treatment method is an etching treatment method in which a semiconductor substrate having a metal-containing layer (particularly a cobalt-containing layer) is contacted with the present treatment solution to dissolve and remove the metal-containing layer (particularly the cobalt-containing layer). That is, the present treatment solution can be used as an etching solution in an etching treatment to remove a metal-containing layer on a semiconductor substrate. Examples of etching treatments include a method in which a treatment solution is contacted with a semiconductor substrate to dissolve and remove metal-containing materials on the semiconductor substrate. There are no particular limitations on the method for contacting the treatment solution with the semiconductor substrate, and the methods described in the semiconductor substrate cleaning method can be applied.
[0129] A further specific example of the above-mentioned processing method is a processing method for a semiconductor substrate, comprising: a step P of performing an oxidation process on a semiconductor substrate containing a metal layer to oxidize the surface of the metal layer to form a metal oxide layer, and a step Q of bringing a processing liquid into contact with the surface of the metal oxide layer formed in the step P to dissolve the metal oxide layer. The metal layer, including preferred embodiments thereof, is the same as the metal layer contained in the above-mentioned object to be processed.
[0130] The metal oxide layer is a layer formed by oxidizing the surface of the metal layer and can be considered a form of metal-based material. A portion of the surface of the metal layer may be a metal oxide layer, or the entire surface of the metal layer may be a metal oxide layer. The metal oxide layer is an oxide of a metal element or an alloy, and is preferably a layer made of cobalt oxide, cobalt alloy oxide, ruthenium oxide, ruthenium alloy oxide, molybdenum oxide, molybdenum alloy oxide, aluminum oxide, aluminum alloy oxide, copper oxide, or copper alloy oxide. A layer made of cobalt oxide or cobalt alloy oxide is more preferred, and a layer made of cobalt oxide is even more preferred. The thickness of the metal oxide layer is, for example, 1 to 10 atomic layers. The thickness of one atomic layer of metal or metal oxide is 1 nm or less (e.g., 0.3 nm to 0.4 nm). Metal oxide layers are often more soluble in processing solutions (easier to be etched) than metal layers. That is, in step P, the surface of the metal layer is turned into a thin metal oxide layer, and in step Q, the treatment liquid is used to remove only the metal oxide layer (and the portion of the metal layer below the metal oxide layer that may inevitably be dissolved), thereby removing (dissolving) only a very thin surface of the metal layer contained in the semiconductor substrate. Furthermore, by alternately repeating step P and step Q, the etching amount can be controlled with high precision. When step P and step Q are alternately performed, the number of times each step is performed may be, for example, 1 to 20 cycles, with step P and step Q considered as one cycle. From the viewpoint of excellent control of the recess depth, when step P and step Q are alternately performed, the number of times each step is performed is preferably 3 cycles or more, and more preferably 5 cycles or more.
[0131] The semiconductor substrate may contain one or more metal layers. The semiconductor substrate may also contain metal-based materials other than the metal layer or metal oxide layer, and some or all of such metal-based materials may be intentionally or unavoidably removed through steps P and Q.
[0132] Process P is a process of subjecting a semiconductor substrate containing the metal layer to an oxidation treatment to oxidize the surface of the metal layer to form a metal oxide layer. The method of oxidation treatment for oxidizing the surface of the metal layer to form a metal oxide layer is not limited, and examples include a liquid treatment in which an oxidizing liquid is brought into contact with the semiconductor substrate, a gas treatment in which an oxidizing gas is brought into contact with the semiconductor substrate (such as an ozone treatment in which ozone gas is brought into contact with the substrate and an oxygen heating treatment in which heating is performed in an oxygen atmosphere, as described below), and a plasma treatment using oxygen gas. One type of oxidation treatment may be performed, or two or more types may be performed.
[0133] The oxidizing liquid may be any chemical liquid capable of oxidizing the surface of the metal layer. Preferably, the oxidizing liquid is a chemical liquid other than the main treatment liquid. The oxidizing liquid is preferably a chemical liquid selected from the group consisting of water, hydrogen peroxide solution, ammonia and hydrogen peroxide mixed solution (APM), hydrofluoric acid and hydrogen peroxide mixed solution (FPM), sulfuric acid and hydrogen peroxide mixed solution (SPM), hydrochloric acid and hydrogen peroxide mixed solution (HPM), oxygen-dissolved water, ozone-dissolved water, perchloric acid, and nitric acid (hereinafter also referred to as "specific chemical liquid"). The composition of hydrogen peroxide solution is, for example, H 2 O 2The content of the hydrogen peroxide solution is preferably 0.5 to 31% by mass, more preferably 3 to 15% by mass, based on the total mass of the hydrogen peroxide solution. The composition of the APM is preferably within a range (mass ratio) of, for example, "ammonia water: hydrogen peroxide solution: water = 1:1:1" to "ammonia water: hydrogen peroxide solution: water = 1:3:45." The composition of the FPM is preferably within a range (mass ratio) of, for example, "hydrofluoric acid: hydrogen peroxide solution: water = 1:1:1" to "hydrofluoric acid: hydrogen peroxide solution: water = 1:1:200." The composition of the SPM is preferably within a range (mass ratio) of, for example, "sulfuric acid: hydrogen peroxide solution: water = 3:1:0" to "sulfuric acid: hydrogen peroxide solution: water = 1:1:10." The composition of the HPM is preferably within a range (mass ratio) of, for example, "hydrochloric acid: hydrogen peroxide solution: water = 1:1:1" to "hydrochloric acid: hydrogen peroxide solution: water = 1:1:30." These preferred composition ratios refer to the case where the ammonia water is 28% by mass ammonia water, the hydrofluoric acid is 49% by mass hydrofluoric acid, the sulfuric acid is 98% by mass sulfuric acid, the hydrochloric acid is 37% by mass hydrochloric acid, and the hydrogen peroxide solution is 30% by mass hydrogen peroxide solution. The volume ratios are based on the volume at room temperature. The preferred range of ["A:B:C=x:y:z" to "A:B:C=X:Y:Z"] indicates that it is preferable to satisfy at least one (preferably two, more preferably all) of the ranges ["A:B=x:y" to "A:B=X:Y"], ["B:C=y:z" to "B:C=Y:Z"], and ["A:C=x:z" to "A:C=X:Z"]. The composition of oxygen-dissolved water can be, for example, O 2 The content of ozone in the water is 20 to 500 mass ppm relative to the total mass of the water containing dissolved oxygen. 3 The content of perchloric acid is, for example, HClO 4 The content of nitric acid is, for example, HNO 3 The content of the compound is 0.001 to 60% by mass based on the total mass of the solution.
[0134] The method for contacting the semiconductor substrate with the oxidizing liquid (preferably the specific chemical liquid) is not particularly limited, and examples thereof include a method of immersing the semiconductor substrate in the oxidizing liquid contained in a tank, a method of spraying the oxidizing liquid onto the semiconductor substrate, a method of pouring the oxidizing liquid onto the semiconductor substrate, and any combination thereof. The contact time between the semiconductor substrate and the oxidizing liquid is, for example, preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. The temperature of the oxidizing liquid is preferably 20 to 75°C, more preferably 20 to 60°C.
[0135] In the gas treatment, examples of the oxidizing gas that is brought into contact with the semiconductor substrate include dry air, oxygen gas, ozone gas, and a mixed gas thereof. The oxidizing gas may contain gases other than the above-mentioned gases. In the gas treatment, the oxidizing gas that is brought into contact with the semiconductor substrate is preferably oxygen gas or ozone gas. When oxygen gas or ozone gas is brought into contact with the semiconductor substrate, it is also preferable to bring the semiconductor substrate into contact with the oxygen gas, the ozone gas, or the mixed gas atmosphere of oxygen and ozone.
[0136] In the gas treatment, a preferred embodiment is heating the semiconductor substrate (for example, heating at 40 to 200°C) while contacting it with an oxidizing gas. Among these, the gas treatment is preferably an ozone treatment in which ozone gas is brought into contact with the semiconductor substrate, or a heat treatment in oxygen in which heating is carried out in an oxygen atmosphere. In the ozone treatment, the ozone gas may be brought into contact with the semiconductor substrate in an ozone atmosphere, or the ozone gas may be brought into contact with the semiconductor substrate in an atmosphere of a mixed gas of ozone gas and another gas (for example, oxygen gas). The ozone treatment may also be a treatment in which the semiconductor substrate is heated while being contacted with ozone gas.
[0137] Step Q is a step of contacting the semiconductor substrate obtained in step P with the present treatment solution to dissolve the metal oxide layer. The method for contacting the semiconductor substrate with the present treatment solution in step Q is not particularly limited, and examples include the same methods as those for contacting the semiconductor substrate with an oxidizing solution. The contact time between the semiconductor substrate and the treatment solution is, for example, preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. The temperature of the treatment solution is preferably 20 to 75°C, more preferably 20 to 60°C.
[0138] In step Q, the metal oxide layer may be removed partially or entirely. In step Q, a part or all of the metal layer (for example, the metal layer exposed on the surface after the metal oxide layer covering the surface has been removed) may be intentionally or unavoidably removed.
[0139] The treatment liquid to be subjected to step Q may be subjected to a degassing treatment or the like in advance to reduce the amount of dissolved oxygen. The metal layer exposed when the metal oxide layer is removed by the treatment liquid is oxidized by the dissolved oxygen in the treatment liquid to form a new metal oxide layer, and this metal oxide layer is then further removed by the treatment liquid, resulting in the removal of an excessive amount of metal layer. This can be prevented by reducing the amount of dissolved oxygen in the treatment liquid.
[0140] For specific aspects of the treatment method for removing target substances such as metal inclusions on a semiconductor substrate using this treatment solution, reference can be made to the descriptions in paragraphs
[0049] to
[0069] of the specification of International Publication No. 2019 / 138814, the contents of which are incorporated herein by reference.
[0141] Any of the present processing methods may be performed before or after other processes in the fabrication of semiconductor devices. The present processing methods may be incorporated into or between other processes. Examples of other processes include the formation of structures such as metal wiring, gate structures, source structures, drain structures, insulating layers, ferromagnetic and / or non-magnetic layers (layer formation, etching, CMP processing, modification, etc.), resist formation, exposure and removal, heat treatment, cleaning, and inspection. The above processes may be performed at any stage of the back end of the line (BEOL), middle end of the line (MOL), or front end of the line (FEOL).
[0142] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.
[0143] [Raw Materials] The following components were used as raw materials to prepare the treatment solutions of the Examples and Comparative Examples. In preparing the treatment solutions, raw materials classified as semiconductor grade or equivalent high-purity grade were used. The various components used as raw materials to prepare the treatment solutions are listed below.
[0144] <First component> DBU: 1,8-diazabicyclo[5.4.0]undec-7-ene DBN: 1,5-diazabicyclo[4.3.0]non-5-ene
[0145] <Second component> Compound A
[0146] ・Compound B
[0147] <Hydroxylamine compounds (HA compounds)> HA: Hydroxylamine
[0148] <Organic solvents> EGME: Ethylene glycol monomethyl ether EGBE: Ethylene glycol mono-n-butyl ether MMB: 3-methoxy-3-methyl-1-butanol Sulfolane DEGEE: Diethylene glycol monoethyl ether PG: Propylene glycol DEGBE: Diethylene glycol monobutyl ether
[0149] <Corrosion inhibitors> Tetrazole: tetrazole 5M-BTA: 5-methyl-1H-benzotriazole (corresponding to the compound represented by formula (C)) BTA: benzotriazole (corresponding to the compound represented by formula (C)) 123TZ: 1H-1,2,3-triazole (corresponding to the compound represented by formula (C)) 124TZ: 1H-1,2,4-triazole
[0150] <Chelating agent> DHEG: N,N-bis(2-hydroxyethyl)glycine DTPA: diethylenetriaminepentaacetic acid EDTA: ethylenediaminetetraacetic acid HIDA: hydroxyethyliminodiacetic acid EDTMP: N,N,N',N'-ethylenediaminetetrakis(methylenephosphonic acid) NTMP: nitrilotrismethylenephosphonic acid (NTMP) HEDP: 1-hydroxyethylidene-1,1-diphosphonic acid
[0151] <Inorganic acid> ・H 3 P.O. 4 :phosphoric acid
[0152] <Water> ・Ultra pure water
[0153] Comparative Example 1: A commercially available DBU product was dehydrated by a column method using molecular sieves 3A (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The dehydrated product was then purified by distillation, starting from the first tray distillation column, using a distillation column consisting of a first tray distillation column (theoretical number of plates: 150) without a pressure reduction mechanism and a second tray distillation column (theoretical number of plates: 150) equipped with a pressure reduction mechanism, connected in series. The distilled product was then purified by circulating filtration using a filtration device equipped with a flow path in which the following ion exchange resins and filters were connected in series from upstream to downstream, and a return path for returning the product from the most downstream to the most upstream of the flow path. The circulation cycle was 50 times. Details of each component of the filtration device are shown below, starting from the upstream side. Anion exchange resin (anion exchange resin described in Production Example 1 in paragraph 0028 of JP-A-2009-155208) Ion exchange filter (IonKleen SL, manufactured by Pall Corporation) Nylon filter (Asymmetric, manufactured by Pall Corporation, pore size 5 nm) UPE filter (Purasol SP / SN solvent purifier, manufactured by Entegris) PTFE filter (XpressKLEEN, manufactured by Pall Corporation, pore size 3 nm) UPE filter (Microgard, manufactured by Entegris, pore size 3 nm) In this type of circulation filtration purification, the operation of passing the product to be purified from the most upstream purification element to the most downstream purification element is counted as one circulation cycle.
[0154] The composition of the purified product obtained by the above purification process was measured using GC-MS ("GCMS-QP2020 NX" manufactured by Shimadzu Corporation). For GC-MS measurement, a diluted solution prepared by diluting the first component with methanol as needed was used as the measurement target. Next, the purified product containing purified DBU, ultrapure water, and a chelating agent (NTMP) were mixed to obtain the composition shown in Table 1, and tetraethylammonium hydroxide (TEAH) was added to the mixture to adjust the pH to the value shown in the "Treatment Solution pH" column of Table 1, thereby preparing a treatment solution for Comparative Example 1.
[0155] [Examples 1 to 29] A commercially available product consisting of a first component (DBN or DBU) was purified in the same manner as in Comparative Example 1, and the composition of the purified product after the purification process was measured using GC-MS ("GCMS-QP2020 NX" manufactured by Shimadzu Corporation). Next, in accordance with the composition of each treatment solution listed in Tables 1 and 2, the purified product containing the purified first component was mixed with ultrapure water and components other than the first component and water, which were added as needed, and then hydrochloric acid or tetraethylammonium hydroxide (TEAH) was added to the mixture to adjust the pH to the value listed in the "Treatment solution pH" column in Tables 1 and 2, thereby preparing the treatment solution for each Example.
[0156] [Evaluation] <Co Film Roughness> A silicon wafer (300 mm diameter) with a metal film (wiring model, hereinafter also referred to as "Co film") made of cobalt on its surface was prepared. The Co film had a thickness of 30 nm. The Co film-coated wafer was set in a spin-rotation wafer processing apparatus (manufactured by EKC Technologies). Each of the treatment solutions from the Examples and Comparative Examples was sprayed onto the wafer surface at a flow rate of 1.5 L / min for 1 minute. Next, a rinse treatment was performed by spraying ultrapure water onto the wafer surface at a flow rate of 1 L / min for 30 seconds, and then the wafer was spin-dried. After drying, a 5 μm square area was arbitrarily selected from the surface of the Co film, and the surface roughness Ra of the selected area was measured using an atomic force microscope. Measurements were performed three times, each time changing the selected area, and the surface roughness Ra of the Co film after treatment with each treatment solution was calculated by arithmetically averaging the measured values. The degree of surface roughness (Co film roughness) of the Co film treated with each treatment solution was evaluated from the surface roughness Ra of the obtained Co film according to the following evaluation criteria. The results are shown in Tables 1 and 2.
[0157] (Co film roughness evaluation criteria) "A": The surface roughness Ra of the Co film is 1.0 nm or less. "B": The surface roughness Ra of the Co film is more than 1.0 nm and less than 2.0 nm. "C": The surface roughness Ra of the Co film is more than 2.0 nm and less than 3.0 nm. "D": The surface roughness Ra of the Co film is more than 3.0 nm.
[0158] <Particle Defect Suppression> A silicon wafer with a diameter of 300 mm was prepared, and the number and addresses of particulate foreign matter with a diameter of 28 nm or more present on the wafer surface were measured using a defect evaluation device "UVision 8" (manufactured by Applied Materials, Inc.). The wafer on which the above-mentioned foreign matter had been measured was set in a spin-rotation wafer processing device (manufactured by EKC Technologies, Inc.). Each processing solution of the examples and comparative examples was sprayed onto the surface of the set wafer at a flow rate of 1.5 L / min for 1 minute. Next, a rinse process was performed by spraying ultrapure water onto the surface of the wafer at a flow rate of 1 L / min for 30 seconds, and then the wafer was spin-dried. For the dried wafer obtained, the number and addresses of particulate foreign matter with a diameter of 28 nm or more present on the wafer surface were measured using the defect evaluation device. The number of particulate foreign matter with a diameter of 28 nm or more originating from the processing solution (hereinafter also referred to as the "number of particle defects") was calculated by subtracting the number of particulate foreign matter measured before processing from the number of particulate foreign matter measured after processing. Based on the number of particle defects resulting from the resulting treatment liquid, the particle defect suppression ability of each treatment liquid was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2.
[0159] (Evaluation criteria for particle defect suppression) "S": The number of particle defects originating from the treatment liquid is 0 or more and less than 100. "A": The number of particle defects originating from the treatment liquid is 100 or more and less than 500. "B": The number of particle defects originating from the treatment liquid is 500 or more and less than 1000. "C": The number of particle defects originating from the treatment liquid is 1000 or more.
[0160] Tables 1 and 2 below show the compositions of the treatment solutions prepared in each Example and Comparative Example and the evaluation results. In the tables, the "Content [mass %]" column indicates the content (unit: mass %) of the corresponding component. In the "Second component" column, "A" and "B" refer to the above-mentioned Compound A and Compound B, respectively. "HA compound" refers to a hydroxylamine compound.
[0161]
[0162]
[0163] From the results in Tables 1 and 2, it was confirmed that the treatment liquid of the present invention is excellent in suppressing the surface roughness of the Co film.
[0164] From a comparison of Examples 1 to 5, it was confirmed that when the treatment liquid contains a chelating agent, particle defects are more effectively suppressed.
[0165] From a comparison of Examples 1 to 8, it was confirmed that when the treatment liquid contains a corrosion inhibitor, the surface roughness of the Co film is more effectively suppressed.
[0166] Comparison of Examples 6, 7 and 19 etc. confirmed that when the content of the organic solvent was 20 mass % or less relative to the total mass of the treatment liquid, the surface roughness of the Co film was more effectively suppressed.
Claims
1. A treatment liquid for semiconductor devices, comprising: water; a first component which is an alicyclic heterocyclic compound containing a nitrogen atom as a ring member atom; and a second component which is a compound different from the first component and is an alicyclic heterocyclic compound having a hydroxyl group.
2. The treatment liquid according to claim 1, wherein the first component has two or more nitrogen atoms as ring member atoms.
3. The treatment solution according to claim 1, wherein the first component comprises at least one selected from the group consisting of 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5-diazabicyclo[4.3.0]non-5-ene.
4. The treatment liquid according to claim 1, wherein the second component contains a nitrogen atom or an oxygen atom as a ring member atom.
5. The treatment liquid according to claim 1, wherein the second component is a compound represented by the following formula (1) or a compound represented by the following formula (2). In formula (1) and formula (2), each X independently represents an oxygen atom, an imino group, or an imino group having a substituent; and n represents an integer of 1 to 3.
6. The treatment liquid according to claim 1, wherein the water content is 70 mass % or more based on the total mass of the treatment liquid.
7. The treatment liquid according to claim 1, further comprising a chelating agent having a carboxylic acid group or a chelating agent having a phosphonic acid group.
8. The processing solution according to claim 1, further comprising an organic solvent.
9. The treatment liquid according to claim 8, wherein the organic solvent includes at least one selected from the group consisting of glycol-based solvents, glycol ether-based solvents, amide-based solvents, alcohol-based solvents, and sulfoxide-based solvents.
10. The treatment solution of claim 1, further comprising a corrosion inhibitor.
11. The treatment solution according to claim 10, wherein the corrosion inhibitor comprises at least one compound selected from the group consisting of a compound represented by the following formula (A), a compound represented by the following formula (B), a compound represented by the following formula (C), and a substituted or unsubstituted tetrazole: In formula (A), R 1A ~R5A each independently represents a hydrogen atom, a substituted or unsubstituted hydrocarbon group, a hydroxyl group, a carboxyl group, or a substituted or unsubstituted amino group, provided that the structure contains at least one group selected from a hydroxyl group, a carboxyl group, and a substituted or unsubstituted amino group. 1B ~R 4B each independently represents a hydrogen atom or a substituted or unsubstituted hydrocarbon group. 1C , R 2C and R N each independently represents a hydrogen atom or a substituted or unsubstituted hydrocarbon group. 1C and R 2C may be bonded to form a ring.
12. The treatment solution according to claim 1, further comprising at least one hydroxylamine compound selected from the group consisting of hydroxylamine, hydroxylamine derivatives and salts thereof.
13. The processing solution according to claim 1, further comprising an inorganic acid.
14. A method for treating an object to be treated, comprising a step of contacting the object to be treated, having a cobalt-containing layer, with the treatment liquid according to any one of claims 1 to 13.
Citation Information
Patent Citations
The liquid chemical handling device
JP1991502677A
Purification method of hydrogen peroxide solution
JP2007254168A
Electrolytic polishing device
JP2008264929A
Method for purifying ester
JP2009155208A
Method and apparatus for purifying ion exchange resin
JP2011110515A