Metal sheet

A metal sheet with a network structure and controlled porosity and crystal grain distribution addresses the issues of handling and bondability in electronic device bonding, providing strong and flexible bonding solutions.

WO2024219381A1PCT designated stage expired Publication Date: 2024-10-24DAICEL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015090
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing metal sheets used for bonding electronic devices suffer from poor handling properties and insufficient bondability due to void generation and organic component evaporation, leading to weak bonding and brittleness.

Method used

A metal sheet with a network structure composed of metal, featuring a surface area of 50% or more with crystal grains of 40,000 nm², internal porosity of 50% or less, and a sinterable region with porosity of 20% or less near the surface, which suppresses void formation and enhances bonding strength.

Benefits of technology

The metal sheet exhibits excellent handling properties, prevents void generation during bonding, and achieves strong, reliable bonding with improved flexibility and reduced chipping or cracking, allowing for effective integration of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015090_24102024_PF_FP_ABST
    Figure JP2024015090_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a metal sheet having excellent handleability, suppressed void formation during bonding, and excellent bondability. A metal sheet 1 according to an embodiment of the present invention has, on at least one surface (surface 31a and / or 32a), a region in which grains having an area of 40,000 nm2 or less constitute at least 50% of the surface area. In addition, the metal sheet 1 according to another embodiment of the present invention has an internal porosity of 70% or less, and has, on at least one surface (surface 31a and / or 32a), a region having a porosity of 20% or less in the vicinity of the surface and having sinterability.
Need to check novelty before this filing date? Find Prior Art

Description

Metal sheet

[0001] This disclosure relates to a metal sheet. This application claims priority to Japanese Patent Application No. 2023-068159, filed on April 18, 2023, the contents of which are incorporated herein by reference.

[0002] When mounting electronic elements such as power semiconductor elements and LED elements, it is necessary to bond multiple materials with high strength, and for this purpose, conductor wiring, bonding structures, or wiring boards equipped with these are used.

[0003] An ink composition containing metal nanoparticles and a solvent is widely used to form the conductor wiring or as a bonding layer in a bonded structure. For example, the bonded structure (bonded body) can be produced by applying the ink composition to a bonded member, then volatilizing the solvent by heating to form a metal layer, further overlaying another bonded member on the metal layer, and then sintering (firing) the metal layer to form a bonding layer.

[0004] Also known is a method for producing a bonded body by bonding members to be bonded together using a plate- or sheet-shaped bonding material containing copper-based fine particles having an average particle diameter of 300 nm or less, with the fine particles being in close contact with each other (see Patent Documents 1 to 4).

[0005] JP 2021-116450 A JP 2019-203172 A JP 2018-12871 A JP 2018-3088 A

[0006] However, when an ink composition containing organic components such as a solvent or binder resin is used, there is a problem that the organic components volatilize during bonding, causing voids.

[0007] In order to suppress voids, it is conceivable to form a bonding sheet with a low content of organic components in the conductive paste. However, although such a bonding sheet can suppress the generation of voids and exhibit bonding properties, it has poor strength and is prone to chipping and cracking during handling, making it difficult to handle.

[0008] On the other hand, the bonding materials of Patent Documents 1 to 4 are capable of preventing the generation of voids, but have insufficient bonding properties.

[0009] Therefore, one object of the present disclosure is to provide a metal sheet that is easy to handle, suppresses the generation of voids during joining, and has excellent joinability. Another object of the present disclosure is to provide a metal sheet that is easy to handle and join, and can exhibit functionality.

[0010] The inventors of the present disclosure have conducted extensive research to solve the above problems and have found that a specific metal sheet is easy to handle, suppresses the generation of voids during bonding, and has excellent bondability. The present disclosure relates to a product completed based on these findings.

[0011] That is, the present disclosure provides a method for manufacturing a thin film having an area of ​​40,000 nm or more on at least one surface, the area of ​​which is 50% or more of the surface area being 40,000 nm or more. 2 A metal sheet is provided having regions made up of the following grains:

[0012] The internal porosity is preferably 50% or less.

[0013] The porosity near the surface of the above region is preferably 20% or less.

[0014] The present disclosure also provides a metal sheet having an internal porosity of 50% or less and a sinterable region on at least one surface of which the porosity near the surface is 20% or less.

[0015] The present disclosure also provides a metal sheet having a non-metallic region therein, the non-metallic region being impregnated with an organic component, and having a sinterable region on at least one surface.

[0016] The metal sheet preferably has a network structure formed of metal.

[0017] According to the metal sheet of one embodiment of the present disclosure, the generation of voids during bonding is suppressed, and the metal sheet of another embodiment of the present disclosure has excellent handleability and bondability, and can exhibit functionality.

[0018] Fig. 1 shows a partial cross-sectional view of a metal sheet according to an embodiment of the present disclosure; Fig. 2 shows a partial cross-sectional view of a metal sheet (organic component-impregnated metal sheet) according to an embodiment of the present disclosure; Fig. 3 shows a micrograph (before water-resistant polishing) of a cross-section of a bonding sheet of Example 1; Fig. 4 shows a micrograph (after water-resistant polishing) of a cross-section of a bonding sheet of Comparative Example 1; Fig. 5 shows a micrograph (after water-resistant polishing) of a cross-section of a bonding sheet of Comparative Example 1;

[0019] [Metal Sheet] The metal sheet according to the first embodiment of the present disclosure has a metal layer having an area of ​​40,000 nm or more on at least one surface thereof. 2 It has a region composed of the following crystal grains. In this specification, the term "metal sheet" refers to a sheet that has a network structure formed of metal and can maintain its sheet state with only the metal component. For example, a sheet in which metal particles are dispersed in a resin and that maintains its sheet state with the resin component does not fall under the category of a "metal sheet."

[0020] In addition, a metal sheet according to a second embodiment of the present disclosure has an internal porosity of 50% or less, and has a region on at least one surface having a porosity of 20% or less near the surface and having sinterability.

[0021] In this specification, when the term "metal sheet" is used simply, it refers to both the metal sheet according to the first embodiment and the metal sheet according to the second embodiment.

[0022] The metal sheet has a network structure formed of metal, which makes it easy to handle and less likely to chip or crack during handling. Furthermore, the metal sheet has a network structure formed of metal, which allows it to maintain its sheet shape without incorporating an organic component, and even if the organic component volatilizes, the network structure blocks the pathways through which the organic component passes, thereby suppressing void formation during sintering.

[0023] The metal sheet according to the first embodiment has a surface area of ​​40,000 nm or more, which is 50% or more of the surface area of ​​at least one surface. 2Since the metal sheet has a region composed of the following crystal grains, when the metal sheet is laminated on the workpiece and the crystal grains in the region are sintered by heating or the like, the metal sheet forms a bonding layer and is bonded to the workpiece, thereby exhibiting excellent bonding properties.

[0024] The metal sheet according to the second embodiment has an internal porosity of 50% or less, which makes it highly flexible and less likely to chip or crack during handling. Furthermore, at least one surface of the metal sheet has a surface-near porosity of 20% or less and a sinterable region. When the metal sheet is laminated on a workpiece and the metal in the region is sintered by heating or the like, the metal sheet forms a bonding layer that bonds to the workpiece, providing excellent bonding properties.

[0025] The metal sheet has a surface area of ​​40,000 nm or more, which is 50% or more of the surface area of ​​at least one surface. 2 It is preferable that the metal sheet has a region (sometimes referred to as a "nanocrystalline grain region") composed of the following crystal grains. When the nanocrystalline grain region is present, the metal sheet is laminated on the workpiece and the crystal grains in the region are sintered by heating or the like, whereby the metal sheet forms a bonding layer and is bonded to the workpiece, thereby exhibiting excellent bonding properties. The size (area) of the crystal grains is 10,000 nm or less. 2 The crystal grain size can be measured by clarifying the crystal grain boundaries on the sheet surface by ion milling or the like, observing the surface of the metal sheet with a scanning electron microscope (SEM), drawing lattice lines corresponding to 50 nm on the SEM photograph on a PC or printed matter, and visually judging the size of each crystal grain at two levels: 200 nm or less and 100 nm or less.

[0026] The area of ​​the nanocrystalline grain region of the metal sheet composed of the crystal grains is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more. The nanocrystalline grain region corresponds to the joining area when the metal sheet is joined to the workpiece, and can be appropriately designed depending on the joining area. For example, it is preferable that the entire surface of at least one side of the metal sheet is the nanocrystalline grain region. Furthermore, when the metal sheet is used to join two workpieces via the metal sheet, both sides of the metal sheet may have the nanocrystalline grain region.

[0027] The metal sheet may have voids therein. In this case, the void ratio of the metal sheet is preferably 50% or less, more preferably 30% or less, even more preferably 20% or less, and particularly preferably 10% or less. When the void ratio is 50% or less, the mechanical strength is such that chipping or cracking is less likely to occur during handling.

[0028] The internal porosity can be calculated by exposing a cross section of the metal sheet, observing the cross section of the metal sheet near the center in the thickness direction using a scanning electron microscope, and analyzing the obtained cross-sectional image to calculate the metal occupancy rate, using the following formula: porosity [%] = 100 - occupancy rate [%]

[0029] The metal sheet preferably has a region on at least one surface where the porosity near the surface is 20% or less and where the metal is sinterable (sometimes referred to as a "low-porosity region"). The low-porosity region allows the metal sheet to be laminated on the workpieces and sintered by heating or other means, forming a bonding layer that bonds the metal sheet to the workpieces and exhibits excellent bonding properties. The low-porosity region corresponds to the bonding region when the metal sheet is bonded to the workpieces and can be appropriately designed depending on the area to be bonded. For example, it is preferable that the entire surface of at least one surface of the metal sheet is the low-porosity region. Furthermore, when the metal sheet is used to bond two workpieces via the metal sheet, both surfaces of the metal sheet may have the low-porosity region. The low-porosity region may also coincide with the nanocrystalline grain region.

[0030] In this specification, a region having sinterability, i.e., a region where the surface metal can be sintered and bonded to the workpiece, is sometimes referred to as a “sinterable region.” The nanocrystalline grain region and the low-porosity region both fall under the category of a “sinterable region.”

[0031] The metal sheet may have voids near the surface. In this case, the porosity near the surface of the metal sheet (particularly the porosity near the surface in the sinterable region) is preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less. When the porosity is 20% or less, better bonding properties can be achieved.

[0032] The porosity near the surface can be calculated by exposing a cross section of the metal sheet, observing the cross section of the metal sheet near the edge in the thickness direction (for example, 5% inside the metal sheet thickness (for example, 2 μm inside) from the surface of the metal sheet) using a scanning electron microscope, and analyzing the obtained cross-sectional image to calculate the metal occupancy rate, and then using the following formula. Note that if the boundary between the surface vicinity and the interior of the metal sheet can be recognized by the difference in porosity, the porosity near the surface can be measured in a region that can be distinguished from the interior, regardless of the distance from the surface. Porosity [%] = 100 - occupancy [%]

[0033] The thickness of the metal sheet is, for example, 20 to 500 μm, preferably 50 to 200 μm, and more preferably 80 to 150 μm. When the thickness is 20 μm or more, excellent bonding properties are achieved. When the thickness is 500 μm or less, excellent electrical conductivity and small diameter bonding components are achieved.

[0034] The thickness of the metal sheet near the surface (one of the thicknesses) is, for example, 0.5 to 15 μm, preferably 1 to 10 μm, and more preferably 2 to 5 μm. A thickness of 0.5 μm or more provides excellent bonding properties. A thickness of 15 μm or less suppresses rapid sintering of crystal grains near the surface, promoting sintering of the electrode and the sheet.

[0035] In the metal sheet, the ratio of the thickness of the surface vicinity (one thickness) to the thickness of the metal sheet is, for example, 0.5 to 20%, preferably 1 to 10%, and more preferably 3 to 5%. When the thickness is 0.5% or more, excellent bonding and conductivity are achieved. When the thickness is 20% or less, sintering of the crystal grains near the surface and the crystal grains in the inner layer can be suppressed, and sintering of the electrode and the sheet can be promoted.

[0036] A metal sheet containing voids can be produced, for example, by sintering a composition containing metal particles and forming it into a sheet. In this case, the metal particles are fused together by melting the surfaces of the metal particles to form a metal network structure, and the metal sheet is formed. At the same time, the gaps between the metal particles are not completely filled, resulting in the presence of voids in the metal sheet. The porosity of the metal sheet can be adjusted by appropriately selecting the particle size of the metal particles, the type of metal, the sintering conditions, etc.

[0037] Examples of metals constituting the metal sheet include conductive metals such as gold, silver, copper, aluminum, and indium. Among these, silver and copper are preferred because they can be easily bonded to bonded members at low temperatures and can form a bonding layer even on general-purpose plastic substrates with low heat resistance. The metals may be one type or two or more types.

[0038] FIG. 1 shows a cross-sectional view of one embodiment of the metal sheet. The metal sheet 1 shown in FIG. 1 has an internal metal portion 2 and surface metal portions 31 and 32 located on both sides of the internal metal portion 2. The internal metal portion 2 has a metal network 2a formed by bonding between metals and voids 2b surrounded by the metal network 2a, and has a porosity of, for example, 50% or less. Each of the multiple voids 2b may be an independent void that is not connected to other voids 2b, or a connected void that is connected to other voids 2b, or a mixture of these. The surface metal portions 31 and 32 each correspond to the surface vicinity, including the surface of the metal sheet 1, and have a porosity of 20% or less. The surface 31a of the surface metal portion 31 and the surface 32a of the surface metal portion 32 are the sinterable regions.

[0039] The metal sheet can be manufactured, for example, by forming the sinterable region on at least a portion of the surface of a non-sinterable region-forming metal sheet that does not have the sinterable region by roughening treatment such as polishing, friction, chemical etching, localized heating, or fine particle support treatment such as ultrasonic support.

[0040] The sinterable region-free metal sheet is a metal sheet (e.g., metal foil) having no crystal grains on the surface, or a metal sheet having a surface area of ​​40,000 nm or more of which is 50% or more of its surface area. 2 By performing the above-mentioned surface roughening treatment on the surface of such a sinterable region-free metal sheet, it is possible to form a bulk layer of metal or a region having an area of ​​40,000 nm or more. 2 The crystal grains are scraped off and the surface has an area of ​​40,000 nm 2 The following crystal grains are formed, and the sinterable region is formed. Furthermore, the fine particle supporting treatment causes metal fine particles to adhere to the surface of the metal sheet on which the sinterable region is not formed, and the metal fine particles are grown as needed to form the sinterable region.

[0041] 50% or more of the surface area is 40,000 nm 2A metal sheet having a region composed of crystal grains exceeding 100 microns can be produced, for example, by heating and / or pressurizing a composition containing metal particles to melt the surfaces of the metal particles and fuse them together to form a metal network. The porosity within the metal sheet can be adjusted by adjusting the particle size of the metal particles, the heating temperature, the pressure during pressing, and the heating and pressing times. The heating and pressing may be performed either singly or both. When both heating and pressing are performed, they may be performed simultaneously or sequentially. The heating temperature is, for example, 180 to 400°C. The pressing pressure is, for example, 0.3 to 40 MPa.

[0042] The composition contains metal particles, which may be surface-modified metal particles whose surfaces are coated with an organic protective agent.

[0043] The average particle size of the metal particles is preferably 1000 μm or less, more preferably 100 μm, even more preferably 10 μm, even more preferably 1000 nm or less, even more preferably 200 nm or less, even more preferably 100 nm or less, even more preferably 80 nm or less, and particularly preferably 70 nm or less. The lower limit is, for example, 0.5 nm, and may be 1 nm or 5 nm. The metal particles are preferably metal nanoparticles. In this specification, "metal nanoparticles" refers to metal particles having a primary particle size (average primary particle size) of less than 1000 nm.

[0044] The average particle size is the size excluding the protective agent coating the surface (i.e., the size of the metal particles themselves). The average particle size is calculated as the average particle size (median size) converted into a volume distribution based on particle sizes determined by transmission electron microscope (TEM) observation, assuming that the particles have an aspect ratio of 1. The particle size of micro-sized (1 μm or more) metal particles can be obtained, for example, by observing the metal particles using a scanning electron microscope (SEM), binarizing the solid body and the rest, analyzing the outer diameters of multiple particles as equivalent circle diameters, and calculating the average value. When two or more types of metal particles are included, the average particle size refers to the average particle size of all metal particles.

[0045] The metal constituting the metal particles is appropriately selected depending on the metal constituting the metal sheet. Among them, silver particles or copper particles are preferred because they can form connecting members for electronic components and the like that have electrical conductivity even on substrates with low heat resistance.

[0046] The composition can take various forms without any particular limitation. For example, an ink composition called a metal ink can be prepared by dispersing metal particles in a suspension state in an appropriate solvent (dispersion medium, particularly an organic solvent). Alternatively, an ink composition called a metal paste can be prepared by dispersing metal particles in a kneaded state in a solvent. However, from the viewpoint of forming a metal network to prepare a metal sheet, it is preferable that the composition contains as few impurities other than metal (particularly organic components such as organic solvents) as possible.

[0047] The composition may contain other components in addition to the metal nanoparticles and the organic solvent. The composition may contain water or a binder resin, for example, to adjust the viscosity of the composition. Only one type of binder resin may be used, or two or more types may be used. Examples of the binder resin include known or commonly used binder resins that are incorporated into conductive ink compositions, such as vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, polyester-based resins, acrylic-based resins, and cellulose-based resins (e.g., ethyl cellulose). The content of the binder resin in the composition is, for example, 10% by mass or less. From the viewpoint of achieving excellent conductivity of the metal sheet, the content is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0.01% by mass or less.

[0048] The metal content in the composition is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, based on 100% by mass of the total composition. The organic component content in the composition is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the total composition.

[0049] When the metal sheet has voids, the metal sheet can be impregnated with an organic component to fill at least a portion of the voids with the organic component, thereby forming a non-metallic region, thereby producing an organic component-impregnated metal sheet. The organic component-impregnated metal sheet has a non-metallic region therein, the non-metallic region is impregnated with an organic component, and has a sinterable region (sinterable region) on at least one surface.

[0050] By impregnating the metal sheet with an organic component, the functionality of the organic component can be imparted to the metal sheet, and the organic component-impregnated metal sheet has excellent handleability and bondability and can exhibit functionality. Because the organic component-impregnated metal sheet has a network structure formed by metal, even if the organic component volatilizes during sintering, the network structure is not destroyed and voids are unlikely to occur.

[0051] FIG. 2 shows a cross-sectional view of one embodiment of the organic component-impregnated metal sheet. The organic component-impregnated metal sheet 10 shown in FIG. 2 has an internal metal portion 2 and surface metal portions 31 and 32 located on both sides of the internal metal portion 2. The internal metal portion 2 has a metal network 2a and a non-metallic region 2c surrounded by the metal network 2a, and has a porosity of, for example, 70% or less. The non-metallic region 2c is filled with an organic component. However, all of the non-metallic region 2c may be filled with the organic component, or some may be voids 2b not filled with the organic component. If the voids 2b in the metal sheet 1 are isolated voids, they are difficult to fill with the organic component through impregnation, and may also exist as voids 2b in the organic component-impregnated metal sheet 10. On the other hand, if the voids 2b in the metal sheet 1 are directly or indirectly connected to the outside of the metal sheet, the organic component is easily filled into the voids 2b through impregnation with the organic component.

[0052] Examples of the organic component include a reducing agent and an adhesive. When the metal sheet is made of an oxidizable metal such as copper, the use of a reducing agent can prevent the oxidation of copper during and after sintering. Furthermore, the use of an adhesive can improve the adhesion between the workpiece and the metal sheet during and after joining.

[0053] The organic component preferably has a boiling point higher than the sintering temperature, from the viewpoint of being less likely to volatilize and form voids during sintering. Specifically, the organic component preferably has a boiling point of, for example, more than 100° C. The boiling point is more preferably 120° C. or higher, and even more preferably 150° C. or higher.

[0054] The organic component-impregnated metal sheet can be produced, for example, by impregnating the metal sheet with a composition containing an organic component, followed by drying as necessary. The composition may contain other components, such as a solvent, in addition to the organic component. The solvent can be removed by drying.

[0055] The metal sheet has excellent handleability, suppresses the generation of voids during bonding, and exhibits excellent bondability. Furthermore, the organic component-impregnated metal sheet has excellent handleability and bondability, and can demonstrate functionality. Therefore, the metal sheet has excellent flexibility and is less likely to chip or crack during handling. Furthermore, since there is no need to incorporate an organic component into the production of the metal sheet, a bonded body with excellent bondability can be produced without inhibiting the bonding of the metal sheets, increasing the pressure during sintering, or lengthening the sintering time.

[0056] The metal sheet (including an organic component-impregnated metal sheet) can be used to form a metal layer, such as metal wiring, on a workpiece or to bond two workpieces together. For example, the metal sheet can be placed on the workpieces so that the sinterable region of the metal sheet contacts the surface of the workpieces, and the metal in the sinterable region is sintered (fired) by heating, pressing, or active energy ray irradiation, thereby bonding the metal sheet and the workpieces together to obtain a bonded body having a metal layer (bonding layer) on the workpieces. Alternatively, a metal sheet can be placed between a first workpiece and a second workpiece, and the sinterable region can be sintered (fired) to obtain a bonded body in which the first and second workpieces are bonded together via a bonding layer. In this case, the metal sheet has the sinterable region on both sides. It is also preferable that a metallized layer be formed on the surface of the workpiece to be bonded to the metal sheet. The metal constituting the metal metallization layer may be any of the metals exemplified and explained as the metal constituting the metal sheet, and it is preferable that the metal has excellent bonding properties with the metal constituting the metal sheet, and it is preferable that the metal contains the same metal as the metal constituting the metal sheet.

[0057] [Bonded Members] Examples of the bonded members include substrates, semiconductor chips, etc. For example, a substrate can be used as the first bonded member, and a semiconductor chip can be used as the second bonded member.

[0058] (Substrate) As the substrate (substrate), a known or commonly used material used for providing the bonding layer can be used. The substrate may be a conductive substrate, a non-conductive substrate, or a dielectric. The substrate may be a single layer or a multi-layer structure in which multiple layers are laminated.

[0059] Examples of materials for forming the non-conductive substrate include resin, glass, ceramics, wood, paper, etc. Examples of the resin include heat-resistant plastics such as polyimide resin, polycarbonate resin, isocyanate resin, melamine resin, and glass epoxy resin, as well as resins with low heat resistance such as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, acrylic resin, epoxy resin, phenol resin, and polyamide resin, polychlorinated biphenyl (PCB), liquid crystal polymer (LCP), vinyl chloride, mold resin, and epoxy resin.

[0060] Examples of the conductive substrate include metal substrates such as metal foils and metal plates formed from metals (copper, iron, alloys thereof, etc.); carbon substrates such as carbon cloth, carbon paper, graphite, etc.; composite substrates such as conductive particle-containing films, metal mesh films, metal-plated films, and optical laminates having a transparent conductive layer; resin substrates such as conductive polymer films; metal wire-containing films; and metal film laminates (printed circuit boards, etc.) having a metal (silver, copper, etc.) film on a part or all of a non-conductive substrate.

[0061] Examples of the substrate include semiconductor elements such as IGBTs, diodes, Schottky barrier diodes, MOS-FETs, thyristors, logic circuits, sensors, analog integrated circuits, LEDs, semiconductor lasers, and oscillators; substrates for mounting semiconductor elements such as lead frames, metal plate-attached ceramic substrates (for example, DBC), piezoelectric ceramics, semiconductor packages, and LED packages; power supply members such as copper ribbons, metal blocks, and terminals; heat sinks; water-cooled plates; lenses for eyeglasses and sunglasses; glass (automotive glass such as windshields, side glass, and rear glass of automobiles); sensor covers; thermal transfer rollers; printed circuit boards; vias in printed circuit boards; displays of personal computers, televisions, and the like; convex mirrors; traffic lights; smartphones; wearable devices such as watches and earphones; writing implements; glass slides; and office automation equipment such as mice.

[0062] The sintering temperature (sintering temperature) can be, for example, 500°C or less, preferably 300°C or less, more preferably 250°C or less, and even more preferably room temperature (e.g., 25°C) to 150°C. A sintering temperature of 300°C or less (particularly 250°C or less) can suppress thermal deformation even when the substrate is a material that is prone to thermal deformation. In particular, when it is desired to complete sintering of the metal in a short period of time, the sintering temperature is, for example, 60 to 200°C, preferably 70 to 180°C, more preferably 80 to 150°C, and even more preferably 90 to 120°C. The sintering time can be appropriately determined taking into account the type of metal particles, the amount applied, the sintering temperature, and the like, and is, for example, within several hours (e.g., within 40 seconds to 33 hours), preferably within 1 hour, more preferably within 50 minutes, even more preferably 10 to 40 minutes, and particularly preferably 15 to 30 minutes.

[0063] Examples of the bonded body include electric and electronic devices such as electromagnetic wave control materials, circuit boards, antennas, heat sinks, liquid crystal displays, organic EL displays, field emission displays (FEDs), IC cards, IC tags, solar cells, LED elements, organic transistors, condensers (capacitors), electronic paper, flexible batteries, flexible sensors, membrane switches, touch panels, and EMI shields.

[0064] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. Furthermore, each invention according to this disclosure is not limited by the embodiments or the following examples, but is limited only by the scope of the claims.

[0065] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.

[0066] Example 1 (Preparation of Bonding Sheet) Ag powder (manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name "AGC239") was filled into an opening measuring 30 mm x 30 mm and 200 μm deep. A 30 mm x 30 mm jig was placed on top of the powder, and the powder was pressurized and heated at a pressure of 20 MPa and a temperature of 300°C. The mixture was held for 3 minutes and then molded into a sheet to obtain a metal sheet. The resulting metal sheet was then fixed to a polishing jig with wax and polished sequentially with water-resistant polishing polishers (#400, #800, #1000, #2000, and #4000) for 1 to 10 minutes each. After polishing, the wax was dissolved in an abrasive, and the opposite side was polished in the same manner. The sheet was then washed and rinsed again with acetone. In this way, a bonding sheet (metal sheet, approximately 100 μm thick) of Example 1 was prepared with polished surfaces on both sides.

[0067] (Preparation of Bonded Body) The above-mentioned bonding sheet was cut into 4 mm x 4 mm pieces, and sandwiched between an Ag-plated SiC (3 mm x 3 mm) and an Ag-plated Cu plate. The sheet was then pressurized and heated for 1, 3, and 5 minutes at a pressure of 5 MPa and a temperature of 300°C to prepare three bonded bodies with different pressurization and heating times. The die shear strength of the resulting bonded bodies was measured and found to be 40, 61, and 94 MPa after 1, 3, and 5 minutes, respectively. Furthermore, no voids were generated during bonding.

[0068] Comparative Example 1 An Ag foil sheet manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. was used as the bonding sheet in Comparative Example 1. The bonding sheet was cut to 4 mm x 4 mm, and sandwiched between an Ag-plated SiC (3 mm x 3 mm) and an Ag-plated Cu plate. Bonded bodies were produced by pressing and heating for 5 minutes under conditions of pressures of 5 and 20 MPa and a temperature of 300°C, but at 5 MPa, peeling occurred from the beginning, and at 20 MPa, the die shear strength was 5 MPa, meaning that bonding was barely achieved.

[0069] Comparative Example 2: Ag powder (manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name "AGC239") was filled into an opening measuring 30 mm x 30 mm and 200 μm deep. A 30 mm x 30 mm jig was placed on top of the powder, and the powder was pressurized and heated at a pressure of 0.05 MPa and a temperature of 300°C. The powder was held for 3 minutes and formed into a sheet to obtain a metal sheet. The resulting metal sheet was then fixed to a polishing jig with wax and polished under the same conditions as in Example 1. After polishing, the wax was dissolved with an asset, but large cracks occurred when the powder was lifted with tweezers, making it impossible to polish the back surface.

[0070] Comparative Example 3: Ag powder (manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name "AGC239") was filled into an opening measuring 30 mm x 30 mm and 200 μm deep, a 30 mm x 30 mm jig was placed on top of the powder, and the powder was pressurized and heated at a pressure of 0.2 MPa and a temperature of 300°C, held for 3 minutes, and formed into a sheet to obtain a metal sheet. This was then polished under the same conditions as in Example 1, and the resulting metal sheet was cut into 4 mm x 4 mm pieces. However, chips and cracks occurred, and the back surface could not be polished.

[0071] <Evaluation> The bonding sheets obtained in the examples and comparative examples were evaluated as follows, and the results are shown in the table.

[0072] (1) Handling Ease The bonding sheets obtained in the examples and comparative examples were cut with scissors into pieces of 4 mm x 4 mm, and the condition at that time was observed. If 90% or more of the bonding sheets after cutting maintained a size of 3 mm x 3 mm or more (i.e., there was no significant collapse after cutting), and if 80% or more of them had no chips or cracks, it was judged as "○", and if not, it was judged as "×".

[0073] (2) Porosity The bonding sheets obtained in the examples and comparative examples were cut and milled using a milling machine (trade name "ArBlade5000", manufactured by Hitachi, Ltd.). The cross section was then polished. Next, a scanning electron microscope (trade name "JEOL JSM-F100", manufactured by JEOL Ltd.) was used to observe the bonded cross section by adjusting the magnification, and the porosity was calculated. The internal porosity was measured within a 30 μm range in the center of the thickness direction of the bonding sheet, and the porosity near the surface was measured within a 2 μm range from the end face of the bonding sheet cross section.

[0074] (3) Die Shear Strength In order to examine the strength of the bond between the SiC and Cu plates in the bonded bodies obtained in the Examples and Comparative Examples, the shear strength (shear head speed: 50 μm / s) between the SiC and Cu plates was measured using a die shear tester (manufactured by DAGE Corporation, product name "XD-7500").

[0075] (4) Observation of Crystal Grains The exposed bonded cross sections in the measurement of the porosity were observed using a scanning electron microscope (trade name "JEOL JSM-F100", manufactured by JEOL Ltd.) with the magnification adjusted. A cross-sectional photograph of Example 1 before water-resistant polishing is shown in FIG. 3, a cross-sectional photograph after water-resistant polishing is shown in FIG. 4, and a cross-sectional photograph of Comparative Example 1 is shown in FIG. 5. A 50 nm × 50 nm lattice mesh was displayed in the photographs of FIGS. 3 to 5, and the area of ​​the crystal grains on the surface of the bonding sheet was 40,000 nm. 2 The area ratio of the following regions was calculated: Note that no crystal grains could be confirmed in the photograph of FIG.

[0076]

[0077] As shown in Table 1, the bonding sheet obtained in Example 1 was easy to handle, and since it was a metal sheet, no voids were generated during bonding. It was also judged to have high die shear strength and excellent bonding. On the other hand, in Comparative Example 1, the die shear strength was low, and as described above, bonding was barely possible. Furthermore, in Comparative Examples 2 and 3, the metal sheet was brittle, and no bonding sheet with excellent handleability was obtained.

[0078] Variations of the present invention are described below. [Supplementary Note 1] At least one surface has an area of ​​40,000 nm or more, and 50% or more of the surface area is 2 A metal sheet having a region composed of the following crystal grains. [Appendix 2] The metal sheet according to Appendix 1, having an internal porosity of 50% or less. [Appendix 3] The metal sheet according to Appendix 1 or 2, having a porosity of 20% or less near the surface of the region. [Appendix 4] A metal sheet having an internal porosity of 50% or less, and having a sinterable region on at least one surface, having a porosity of 20% or less near the surface. [Appendix 5] A metal sheet having a non-metallic region inside, the non-metallic region being impregnated with an organic component, and having a sinterable region on at least one surface. [Appendix 6] The metal sheet according to any one of Appendices 1 to 5, having a network structure formed of metal.

[0079] REFERENCE SIGNS LIST 1 Metal sheet 2 Internal metal portion 2a Metal network 2b Void 2c Non-metal region 31, 32 Surface metal portion 31a, 32a Surface 10 Organic component-impregnated metal sheet

Claims

1. At least one surface has a surface area of ​​40,000 nm or more. 2 A metal sheet having regions made up of the following grains:

2. The metal sheet according to claim 1, having an internal porosity of 50% or less.

3. The metal sheet according to claim 1, wherein the porosity near the surface in said region is 20% or less.

4. A metal sheet having an internal porosity of 50% or less and having a sinterable region on at least one surface having a porosity of 20% or less near the surface.

5. A metal sheet having a non-metallic region therein, said non-metallic region being impregnated with an organic component, and having a sinterable region on at least one surface.

6. The metal sheet according to any one of claims 1 to 5, having a network structure formed of a metal.

Citation Information

Patent Citations

  • Porous silver sheet, method of manufacturing metal member joined body, metal member joined body, method of manufacturing bump for connecting electric circuit, and bump for connecting electric circuit

    JP2010248617A

  • Porous silver-made sheet and metallic member conjugate using the porous silver-made sheet

    JP2016169411A

  • Copper sintered substrate nano-silver impregnated joint sheet, method therefor and joining method

    JP2021107569A

  • Method for producing metal sheet made of aggregation of metal fine particles in which the metal fine particles are metal-bonded each other or method for producing alloy sheet made of aggregation of alloy fine particles in which the alloy fine particles are metal-bonded each other

    JP2022040422A