Polyester film, laminate polyester film, and foldable display

A specially formulated polyester film with controlled refractive index and UV absorption properties, integrated into a laminated structure with a hard coat layer, addresses the limitations of existing materials by providing excellent bending resistance and UV absorption for flexible displays, ensuring image quality and portability.

WO2024219475A1PCT designated stage expired Publication Date: 2024-10-24TOYOBO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015510
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current materials for flexible displays, such as acrylic and polyimide films, lack sufficient bending resistance and UV absorption, while polyester films offer impact resistance but insufficient bending resistance, and existing solutions with high hardness and flexibility are expensive and difficult to produce in mass quantities.

Method used

A polyester film with specific thickness, refractive index, and UV absorption properties, combined with a laminated structure for enhanced adhesion and a hard coat layer, providing excellent bending resistance and UV absorption without increasing layer complexity.

Benefits of technology

The solution achieves good bending resistance and UV absorption performance while maintaining mass productivity, suitable for flexible displays like foldable organic EL displays, ensuring image quality and portability without the drawbacks of existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015510_24102024_PF_FP_ABST
    Figure JP2024015510_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a polyester film, a laminate polyester film, and a display which have good flex resistance and preferably UV absorption performance. A polyester film according the present invention is used for, for example, a surface protective film, a cover window film, or the like of a foldable display, wherein: when the length direction or the width direction of the polyester film having a thickness of 25-100 μm is defined as a direction A and a direction orthogonal to the direction A is defined as a direction B, tan δ in the direction A at 25°C is 0.008-0.030. The light transmittance of this polyester film at a wavelength of 380 nm may be not more than 15%.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester film, laminated polyester film, foldable display

[0001] The present invention relates to a polyester film, a laminated polyester film, and a foldable display that have excellent bending resistance and / or UV absorption properties.

[0002] Mobile terminal devices such as tablets and smartphones are becoming thinner and lighter. Currently, mobile terminal devices use rigid housings, so tempered glass is generally used to protect the displays installed in mobile terminal devices. However, in recent years, displays that emphasize design have become popular. For example, displays with unusual shapes such as circular shapes are preferred. In particular, in recent years, there has been a demand for bendable displays (hereinafter sometimes referred to as flexible displays) for installation on curved surfaces.

[0003] However, since glass materials cannot be used in flexible displays, acrylic sheets and the like have been used, but thin acrylic sheets have problems such as being vulnerable to scratches and impacts and having poor bending resistance.On the other hand, polyester films (hereinafter sometimes referred to as base films) are inexpensive and have excellent impact resistance, but have problems with insufficient bending resistance.

[0004] To achieve these goals, Patent Document 1 proposes a material that is highly hard and flexible as a hard coat material, but the material is expensive and has problems with versatility, as well as low scratch resistance on the surface.

[0005] In addition, as in Patent Document 2, it has been reported that a polyimide film having excellent transparency, flexibility, and folding resistance while maintaining conventional physical properties can be obtained from a polyimide resin composition in which finely divided silica is dispersed. However, this material is very expensive and has problems in terms of mass production.

[0006] In addition, as organic EL displays have become more widespread in recent years, it has become necessary to protect the organic EL from ultraviolet rays, and UV absorption performance is required on the front surface of the panel. Although UV absorbers may be applied, it is preferable to impart UV absorption performance to the polyester substrate, as this does not increase the number of layers and allows the visible light transmittance to be maintained.

[0007] JP 2017-008148 A JP 2009-215412 A

[0008] The present invention aims to solve the above-mentioned problems, and an object of the present invention is to provide a polyester film, a laminated polyester film, and a foldable display having good flex resistance.

[0009] The present invention has the following configurations, for example. (Item 1) A polyester film having a thickness of 25 to 100 μm, wherein direction A is either the longitudinal direction or the width direction of the polyester film, and direction B is the direction perpendicular to direction A, and the polyester film has a tan δ in direction A at 25°C of 0.008 to 0.030. (Item 2) The polyester film according to item 1, wherein N(AB), the refractive index in direction A minus the refractive index in direction B, is -0.12 to -0.075. (Item 3) The polyester film according to item 1 or 2, wherein tan δ in direction A at -30°C is 0.020 to 0.065. (Item 4) The polyester film according to any one of items 1 to 3, wherein the light transmittance at a wavelength of 380 nm is 15% or less. (Item 5) The polyester film according to any one of items 1 to 4, wherein the thickness unevenness in the longitudinal direction of the polyester film is 15% or less. (Item 6) The polyester film according to any one of items 1 to 5, characterized in that it has a total light transmittance of 85% or more and a haze of 3% or less. (Item 7) The polyester film according to any one of items 1 to 6, characterized in that it is used as a surface protection film or a cover window film for a foldable display. (Item 8) A laminated polyester film having an easy-adhesion layer on at least one surface of the polyester film according to any one of items 1 to 7. (Item 9) The laminated polyester film according to item 8, having a hard coat layer via the easy-adhesion layer. (Item 10) A foldable display comprising the polyester film according to any one of items 1 to 7 or the laminated polyester film according to item 8 or 9. (Item 11) The foldable display according to item 10, further comprising an organic EL panel. (Item 12) A surface protection film for a foldable display comprising the polyester film according to any one of items 1 to 7 or the laminated polyester film according to item 8 or 9. (Item 13) A cover window film for a foldable display comprising the polyester film according to any one of items 1 to 7 or the laminated polyester film according to item 8 or 9.

[0010] The polyester film of the present invention has good flex resistance while maintaining mass productivity, and preferably also has UV absorption properties.

[0011] 1 is a schematic diagram showing the bending radius when the foldable display of the present invention is folded, and FIG. 2 is a schematic diagram showing the bending direction (reference numeral 22) of the polyester film for a foldable display of the present invention.

[0012] As used herein, the phrase "comprising" is intended to encompass the phrases "consisting essentially of" and "consisting of."

[0013] In the numerical ranges described in stages in this specification, the upper or lower limit of a numerical range in a certain stage can be arbitrarily combined with the upper or lower limit of a numerical range in the same stage or in another stage. In addition, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in an example or a value that can be unambiguously derived from an example.

[0014] In this specification, numerical values ​​connected with "to" mean a numerical range including the numerical values ​​before and after "to" as the lower and upper limits. For example, "1 to 10% by mass" is equivalent to "1% by mass or more and 10% by mass or less."

[0015] Furthermore, with regard to numerical ranges, "equal to or greater than" means "equal to or greater than," and "equal to or less than" means "equal to or less than."

[0016] (Display) The term "display" as used in the present invention refers to a display device. Types of displays include LCD, organic EL display, inorganic EL display, LED, FED, etc., but LCD, organic EL, and inorganic EL, which have a bendable structure, are preferred. In particular, organic EL, which has a small number of layers and a wide color gamut, is more preferred.

[0017] The display may be in any form, including a large screen, a display, digital signage, a bendable mobile terminal device, a PC, etc. In particular, it is preferable to use it in a touch panel display that has a touch panel function that allows operation by direct touch, a digital signage, a bendable mobile terminal device, a PC, etc. It is more preferable that the display is a flexible display as described below, and a foldable display is even more preferable.

[0018] (Flexible Display) A flexible display is a single continuous display that can be bent according to the application, and is preferably thin and lightweight at the same time. Examples of flexible displays include foldable displays, which are bendable displays, and displays that can be used with a paper-like texture.

[0019] A foldable display is a single continuous display that can be folded in half or otherwise when carried. Folding reduces the size by half, improving portability. The bending radius of a foldable display is preferably 5 mm or less, and more preferably 3 mm or less. A bending radius of 5 mm or less allows for a thinner display when folded. A smaller bending radius is preferable, but the smaller the bending radius, the more likely it is that creases will form. The bending radius is preferably 0.1 mm or more, but may be 0.5 mm or more, or even 1 mm or more. Even a bending radius of 1 mm can achieve a practically thin display when carried. The bending radius when folded is measured at the location indicated by the symbol 11 in the schematic diagram of FIG. 1 and refers to the radius of the inside of the folded portion when folded. The surface protection film, described below, may be located on either the outside or inside of the folded display.

[0020] Furthermore, the foldable display may be two-fold, three-fold, four-fold, or may be a rollable display, all of which are considered to fall within the scope of the foldable display of the present invention. A foldable display may not include a rollable display.

[0021] The polyester film of the present invention may be used in any part of a folding display as long as it is a component of the display. Hereinafter, a typical configuration of a folding display and the parts in which the polyester film of the present invention can be used will be described using an organic EL display as an example.

[0022] (Foldable Organic EL Display) A foldable organic EL display essentially comprises an organic EL panel. If necessary, a touch panel, a circular polarizer, a cover window film, a surface protection film, and the like may be laminated on the organic EL panel in this order toward the viewing side. A back protection film may also be laminated on the surface of the organic EL panel opposite the viewing side.

[0023] (Organic EL Panel) An organic EL panel generally comprises an electrode / electron transport layer / light-emitting layer / hole transport layer / transparent electrode. The polyester film of the present invention can be used as a substrate on which an electrode is provided, and further an electron transport layer, a light-emitting layer, a hole transport layer, and a transparent electrode are provided. In particular, the polyester film of the present invention can be preferably used as a substrate for a transparent electrode. In this case, since the substrate film is required to have high barrier properties against water vapor and oxygen, it is preferable that the polyester film of the present invention be provided with a barrier layer such as a metal oxide layer. To improve the barrier properties, multiple barrier layers may be provided, or multiple polyester films each provided with a barrier layer may be used.

[0024] (Touch Panel) The mobile terminal device preferably has a touch panel. When an organic EL display is used, the touch panel is preferably disposed above the organic EL display or between the organic EL panel and the circular polarizer. The touch panel has a transparent substrate such as a film and a transparent electrode disposed thereon. The polyester film of the present invention can be used as this transparent substrate. When used as a transparent substrate for a touch panel, the polyester film is preferably provided with a hard coat layer or a refractive index adjusting layer.

[0025] (Circular Polarizing Plate) A circular polarizing plate prevents deterioration of image quality due to reflection of external light by components inside a display. A circular polarizing plate has a linear polarizing plate and a retardation plate. The linear polarizing plate has a protective film on at least the viewing side of the polarizer. A protective film may also be provided on the side of the polarizer opposite the viewing side, or a retardation plate may be directly laminated on the polarizer. The retardation plate may be a resin film having a retardation, such as a polycarbonate or cyclic olefin, or a resin film provided with a retardation layer made of a liquid crystal compound. The polyester film of the present invention can also be used as a polarizer protective film or a resin film for a retardation plate. In these cases, the slow axis direction of the polyester film of the present invention is preferably parallel or perpendicular to the absorption axis direction of the polarizer. A deviation of up to 10 degrees, preferably 5 degrees, from this parallel or perpendicular orientation is permitted.

[0026] (Cover window film and surface protective film) When an impact is applied to a display from above, there is a risk of disconnection of the circuits of an organic EL panel or a touch panel. For this reason, in many displays, a cover window film or a surface protective film is provided on the viewing side of the organic EL panel or the touch panel. It is preferable that the polyester film of the present invention is used as a cover window film or a surface protective film. In the case of a surface protective film, it is preferable to use a laminated polyester film in which a hard coat layer is laminated on at least the surface side of the polyester film. The hard coat layer is provided on the surface of a foldable display with the hard coat layer on the viewing side. The hard coat layer may be provided on both sides of the polyester film.

[0027] The polyester film of the present invention contains a polyester as a constituent component, and examples of the polyester that can be used include those composed of a polymer having an acid component, such as an aromatic dicarboxylic acid, an alicyclic dicarboxylic acid, or an aliphatic dicarboxylic acid, and a diol component as constituent units (polymerization units).

[0028] Examples of aromatic dicarboxylic acid components include terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid. Among these, terephthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid are particularly preferred. Examples of alicyclic dicarboxylic acid components include cyclohexanedicarboxylic acid. Examples of aliphatic dicarboxylic acid components include adipic acid, suberic acid, sebacic acid, and dodecanedioic acid. These acid components may be used singly or in combination.

[0029] Examples of diol components include ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, and 2,2'-bis(4'-β-hydroxyethoxyphenyl)propane. Among these, ethylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, and diethylene glycol are particularly preferred. Ethylene glycol is particularly preferred as a diol component. These diol components may be used alone or in combination.

[0030] The polyester may be copolymerized with a monofunctional compound. Furthermore, the polyester may be copolymerized with a trifunctional compound or the like, provided that the polymer is substantially linear without excessive branching or crosslinking. Examples of monofunctional compounds include lauryl alcohol and phenyl isocyanate. Examples of trifunctional compounds include trimellitic acid, pyromellitic acid, glycerol, pentaerythritol, and 2,4-dihydroxybenzoic acid. In addition to the acid component and diol component, the polyester may also be copolymerized with aromatic hydroxycarboxylic acids such as p-hydroxybenzoic acid, m-hydroxybenzoic acid, and 2,6-hydroxynaphthoic acid, as well as p-aminophenol and p-aminobenzoic acid, in small amounts sufficient to avoid impairing the effects of the present invention.

[0031] The copolymerization ratio of the polymer can be determined by NMR (nuclear magnetic resonance) or microscopic FT-IR (Fourier transform microscopic infrared spectroscopy).

[0032] Polyesters with a glass transition temperature of less than 150°C are preferably used because they can be biaxially stretched and exhibit the effects of the present invention, such as flex resistance. Polyesters used in the present invention are preferably polyethylene terephthalate or polyethylene naphthalate (e.g., polyethylene-2,6-naphthalate). Copolymers or modified products of these may also be used, as well as polymer alloys with other thermoplastic resins. The term "polymer alloy" as used herein refers to a multicomponent polymer system, and may be a block copolymer obtained by copolymerization or a polymer blend obtained by mixing. It is particularly preferable for the polyester of the present invention to be primarily composed of polyethylene terephthalate, as this facilitates the application of processes to increase crystallite size and crystalline orientation. Here, "primary component" refers to at least 80% by mass of the film composition.

[0033] When polyethylene terephthalate is used in the polymer alloy of the present invention, the other thermoplastic resin is preferably a polymer compatible with polyester, and more preferably a polyetherimide resin. Any polyetherimide resin may be used as long as it is compatible with polyester, but the following is preferred from the viewpoints of affinity with polyester, cost, melt moldability, etc. That is, in the present invention, the polyetherimide resin is preferably a polymer having a repeating unit represented by the following formula, which is a condensation product of 2,2-bis[4-(2,3-dicarboxyphenoxy)phenyl]propane dianhydride and m-phenylenediamine or p-phenylenediamine:

[0034]

[0035] This polyetherimide is available from SABIC Innovative Plastics under the trade name "Ultem" and is known by trade names such as the "Ultem® 1000," "Ultem® 1010," "Ultem® 1040," "Ultem® 5000," "Ultem® 6000," and "Ultem® XH6050" series, as well as "Extem® XH" and "Extem® UH."

[0036] (Additives) The polyester used in the present invention as a material for the polyester film may contain particles, primarily for the purpose of imparting lubricity to the film. The type of particles is not particularly limited as long as they are capable of imparting lubricity. Specific examples of such particles include silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide.

[0037] Heat-resistant organic particles such as those described in JP-B No. 59-5216 and JP-A No. 59-217755 may also be used. Other examples of heat-resistant organic particles include particles made of silicone resin, thermosetting urea resin, thermosetting phenolic resin, thermosetting epoxy resin, benzoguanamine resin, etc. Furthermore, precipitated particles obtained by precipitating and finely dispersing a portion of a metal compound such as a catalyst during the polyester production process may also be used.

[0038] The shape of the particles for imparting the above-mentioned lubricity is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. Furthermore, the hardness, specific gravity, color, etc., of the particles are also not particularly limited. Furthermore, two or more types of these particles can be used in combination as needed.

[0039] The average particle size is preferably 0.05 μm or more and 3.0 μm or less, and more preferably 0.1 μm or more and 2.0 μm or less. When the average particle size is 0.05 μm or more, the particles are less likely to aggregate and have sufficient dispersibility. On the other hand, when the average particle size is 3.0 μm or less, the surface roughness of the resulting polyester film is not increased and the haze is low, which is preferable for optical applications. Furthermore, when using secondary aggregated particles with primary particles of less than 0.05 μm, such as aggregated silica, it is preferable to disperse them in an ethylene glycol slurry and filter them to remove particles larger than 3.0 μm. As the secondary aggregated particles, in addition to aggregated silica, fumed silica and the like are preferably used. When secondary aggregated particles are used, the particles easily deform and follow the deformation of the resin due to stretching, which makes it less likely that voids will form at the interface between the resin and the particles, preventing high haze.

[0040] The content of particles blended to impart slipperiness to the polyester film is preferably 0.01% by mass or more and 2% by mass or less, more preferably 0.01% by mass or more and 1% by mass or less. When the particle content is 0.01% by mass or more, the film has sufficient slipperiness. On the other hand, when the particle content is 2% by mass or less, the film surface has sufficient smoothness.

[0041] In addition, additives such as compatibilizers, plasticizers, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, brighteners, colorants, conductive agents, crystal nucleating agents, ultraviolet absorbers, flame retardants, flame retardant assistants, pigments, and dyes may be added within a range that does not impair light transmittance or haze.

[0042] Furthermore, in order to suppress deterioration of optically functional dyes such as iodine-based dyes, the polyester film of the present invention preferably has a light transmittance of 15% or less at a wavelength of 380 nm. The light transmittance of 380 nm is preferably 0% or more, and more preferably 0.1% or more. A light transmittance of 15% or less can suppress deterioration of the optically functional dye due to ultraviolet light. This light transmittance can be achieved, for example, by incorporating an ultraviolet absorber into the polyester film. Note that the light transmittance in the present invention is measured in a direction perpendicular to the plane of the polyester film. The light transmittance can be measured, for example, using a spectrophotometer (e.g., UV1800 manufactured by Shimadzu Corporation). Examples of ultraviolet absorbers include triazine-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, benzoxazinone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, and salicylate-based ultraviolet absorbers. Triazine-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers are preferred. As an ultraviolet absorber that is not adversely affected by heat during the production of the polyester film, for example, the following ultraviolet absorbers can be used.That is, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, octyl-3-[3-tert-butyl-4-hydroxy-5-( 5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, 2-(2H-benzotriazol-2-yl)4,6-bis(1-ethyl-1-phenylethyl)phenol, phenol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)4-methyl, 2,2'-methylenebi bis(6-(2H-benzotriazol-2-yl)-4-1,1,3,3-tetramethylbutyl)phenol), 2-(4,6,-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)roxy]phenol, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenicyl)-1,3,5-triazine, benzenepropanoic acid, 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-, C7- 9 Branched and linear alkyl esters such as 2-(2-hydroxy-5-tert-methylphenyl)-2H-benzotriazole, 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol, 2,2'-dihydroxy-4-methoxybenzophenone, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol, and 2-(2'-hydroxy-5'-octylphenyl)benzotriazole can be used.

[0043] The content of the ultraviolet absorber in the polyester film of the present invention is, for example, 0.17% by weight or more, preferably 1 to 80% by weight, based on the weight of the polyester film.

[0044] (Layer Structure) The structure of the polyester film of the present invention is not particularly limited and may be a single-layer structure or a laminate structure. Furthermore, in the case of a laminate structure, in addition to a two-layer or three-layer structure, it may also be a four-layer or more multilayer structure as long as it does not deviate from the gist of the present invention. The laminate structure is also not particularly limited and examples thereof include A / B, A / B / A, A / B / C, and A / B / A'. The polyester film of the present invention is produced, for example, as follows. Hereinafter, an example using polyethylene terephthalate (PET) as the polyester will be described as a representative example, but the present invention is not particularly limited thereto.

[0045] One method for incorporating inert particles into polyester is, for example, dispersing the inert particles in a predetermined ratio in the form of a slurry in ethylene glycol, a diol component, and adding this ethylene glycol slurry at any stage before the completion of polyester polymerization. When adding particles, for example, adding the aqueous sol or alcohol sol obtained during particle synthesis without drying it at any stage before the completion of polyester polymerization can improve the particle dispersibility and the film's slipperiness, transmittance, and haze. Another effective method is to mix the aqueous slurry of particles with predetermined polyester pellets, feed them into a vented twin-screw kneading extruder, and knead them into the polyester. These methods are used to prepare polyester pellets containing inert particles. Furthermore, the number of protrusions on the film surface can be further reduced by, for example, kneading and extruding the pellets with pellets not containing particles (masterbatch method), after obtaining a polyester containing particles in advance.

[0046] One method for preparing polymer alloys involves mixing substantially particle-free polyester pellets with, for example, polyetherimide pellets in a predetermined ratio, feeding the mixture into a vented twin-screw kneading extruder heated to 270-300°C, and melt-extruding. Polyetherimide-containing polyester pellets can be prepared using this method. Furthermore, in the production of polyester films, the intrinsic viscosity of at least one polyester resin pellet is preferably in the range of 0.50-1.0 dl / g. More preferably, it is 0.55-0.68 dl / g. An intrinsic viscosity of 0.50 dl / g or higher is preferred because it allows for entanglement of molecular chains, making it less likely to crack when bent. Furthermore, the resulting film has improved impact resistance, making it less likely to break internal display circuits due to external impact. On the other hand, an intrinsic viscosity of 1.00 dl / g or lower is preferred because it prevents excessive increases in the filtration pressure of the molten fluid, facilitating stable film production.

[0047] For the same reason, the intrinsic viscosity of the polyester film is preferably 0.50 to 1.00 dl / g.

[0048] The thickness of the polyester film is preferably 25 to 100 μm, more preferably 40 to 75 μm. A thickness of 25 μm or more is preferable because it improves handling properties and impact resistance, while a thickness of 100 μm or less is advantageous for weight reduction and is excellent in flexibility, processability, handling properties, etc.

[0049] The thickness unevenness of the polyester film in the longitudinal direction is preferably 15% or less, and more preferably 12% or less, and is calculated by the formula: Thickness unevenness (%) = (maximum thickness - minimum thickness) / average thickness x 100.

[0050] (Regarding tan δ) The tan δ at -30°C obtained by dynamic viscoelasticity measurement by tensioning the polyester film in the width direction or length direction is preferably 0.020 to 0.065. It is more preferably 0.025 to 0.060. The tan δ at 25°C is preferably 0.008 to 0.030, and more preferably 0.008 to 0.028. In dynamic viscoelasticity measurement, tan δ is determined from the ratio of the loss modulus to the storage modulus, and a smaller tan δ indicates a smaller loss modulus or a larger storage modulus. In the present invention, by setting the balance between the loss modulus and the storage modulus within a specific tan δ range at a low temperature such as -30°C and at an ordinary temperature of 25°C, a structure that is resistant to creases and cracks can be achieved.

[0051] (Regarding Refractive Index) The refractive index of a polyester film used, for example, as a surface protection film or cover window film for a foldable display will be described. When at least one of the longitudinal direction (machine flow direction) and width direction of the polyester film is designated as A, the value N(A-B), obtained by subtracting the refractive index in direction B perpendicular to direction A from the refractive index in direction A, is preferably −0.12 to −0.075, more preferably −0.11 to −0.078. It is preferable that direction A is the longitudinal direction (machine flow direction) of the polyester film, and direction B is the width direction of the polyester film. When a polyester film is used in a foldable display, it is preferable that the longitudinal direction (machine flow direction) of the film is the bending direction. When the longitudinal direction (machine flow direction) of the film is the bending direction and the width direction is the folding direction, it is preferable that N(A-B) be determined by taking direction A as the bending direction and direction B as the folding direction. In the case of a foldable display, the bending direction is the direction perpendicular to the folding portion of the foldable display. When a polyester film is repeatedly folded, fatigue accumulates, resulting in cracks or, in the worst case, breakage or deformation. It is believed that this is because the oriented molecules in the folding direction act as a resistance to fatigue caused by molecular elongation during folding, making the film less susceptible to cracking, while the moderate deformation of unoriented molecules in the folding direction makes it less susceptible to crease marks during compression. The present invention can suppress fracture and deformation due to fatigue by controlling the refractive index in the folding direction or in the direction perpendicular to the folding direction. Here, a negative N(A-B) indicates low orientation in the folding direction. If the N(A-B) is -0.12 or greater, cracks in the folding direction or, in the worst case, breakage can be suppressed after a bending test. If the N(A-B) is -0.075 or less, crease marks are less likely to form, and the visibility of the display is less likely to be impaired.

[0052] In the present invention, the refractive index of the polyester film in at least one of the longitudinal direction (machine flow direction) and width direction is preferably 1.590 to 1.620, more preferably 1.590 to 1.606, and even more preferably 1.591 to 1.600. The refractive index in the other direction (e.g., the direction perpendicular to the direction in which the refractive index is 1.590 to 1.620) is preferably 1.670 to 1.700, more preferably 1.670 to 1.695, and even more preferably 1.680 to 1.695. By setting the refractive index to 1.700 or less, cracks and breaks in the direction of the folded portion can be suppressed. By setting the refractive index to 1.670 or more, flexibility in the bending direction and surface hardness can be improved.

[0053] A refractive index of 1.590 to 1.620 in at least one of the longitudinal direction and the width direction and the bending direction is preferable because deformation during repeated folding is small and there is little risk of degradation of the image quality of the foldable display. If the refractive index is 1.590 or more, there is no risk of cracks occurring in the folding direction after the bending test described below, and of course no breakage occurs, so the visibility of the display can be maintained good.

[0054] The refractive index of the polyester film can be effectively adjusted by adjusting the stretching ratio and stretching temperature. A relaxation step in the stretching direction and multi-stage stretching may also be used to adjust the refractive index. When multi-stage stretching is performed, it is preferable to set the stretching ratios in the second and subsequent stages higher than the stretching ratio in the first stage.

[0055] (Regarding the refractive index in the bending direction) The bending direction is the direction indicated by reference numeral 22 on the polyester film (reference numeral 2) in Figure 2, and refers to the direction perpendicular to the folding portion (reference numeral 21) assumed in the use of a foldable display. The refractive index in the bending direction is preferably 1.590 to 1.620, more preferably 1.590 to 1.606, and even more preferably 1.591 to 1.600.

[0056] By controlling the refractive index in at least one of the longitudinal direction (machine flow direction) and width direction of the polyester film within the above range, and more preferably by controlling the refractive index in the bending direction within the above range, fatigue due to compressive stress applied to the inside of the fold when folded can be reduced. Fatigue due to compressive stress is thought to occur mainly in crystalline parts, and the fewer crystals there are in the bending direction, the less fatigue there is. Therefore, by making the refractive index in the bending direction smaller than the refractive index in the direction perpendicular to the bending direction, the amount of oriented crystals in the bending direction is reduced, and fatigue due to compressive stress is suppressed.

[0057] Furthermore, the creep phenomenon caused by tensile stress applied to the outside of the fold when folded can be suppressed by reducing the refractive index. Fatigue due to tensile stress is thought to occur mainly in the amorphous portion, and repeated stress causes molecular chains to align, resulting in deformation. It can be assumed that the fewer molecular chains aligned in the bending direction, the less deformation due to alignment. Furthermore, since fatigue due to tension can be suppressed with fewer amorphous portions, a higher degree of crystallinity, i.e., a higher density, is preferable.

[0058] In the present invention, the unstretched polyester sheet is preferably stretched at a ratio of 1.2 to 2.0 times in at least one of the longitudinal direction (machine flow direction) and the width direction, with 1.7 to 2.0 times being more preferred. Furthermore, the stretching direction at this ratio is preferably the bending direction when the polyester film is used in a folding display. A stretching ratio of 2.0 times or less is preferred because it does not cause thickness unevenness in the film. The preheating temperature for stretching is preferably 75 to 100°C, and the stretching temperature is preferably 75 to 120°C, with 75 to 105°C being more preferred. Heating methods during stretching can be conventionally known, such as hot air heating, roll heating, and infrared heating. By setting the stretching temperature to 75 to 120°C, significant thickness unevenness due to stretching at the above stretching ratio can be prevented. Furthermore, by stretching at a temperature as low as possible within a range that does not cause significant thickness unevenness, the refractive index in the thickness direction can be reduced.

[0059] (Regarding the refractive index in the direction of the folded portion) The refractive index in the direction perpendicular to the bending direction (direction of the folded portion) is preferably 1.670 to 1.700, more preferably 1.670 to 1.695, and even more preferably 1.680 to 1.695. By setting the refractive index in this direction to 1.670 to 1.700, deformation when folded in the bending direction can be reduced. By setting the refractive index to 1.700 or less, cracks and breakage in the direction of the folded portion can be suppressed. By setting the refractive index to 1.670 or more, flexibility in the bending direction and surface hardness can be improved. Methods for adjusting the refractive index in the direction perpendicular to the bending direction include stretching ratio, stretching preheating temperature, stretching temperature, multi-stage stretching, and film relaxation. The stretching ratio is preferably 4.0 to 6.0 times, and more preferably 4.4 to 6.0 times. Furthermore, the stretching preheating temperature in the direction perpendicular to the bending direction is preferably 70 to 110°C, and the stretching temperature is preferably 80 to 130°C. When multistage stretching is performed in the direction perpendicular to the bending direction, it is preferable to set the stretching ratio in the second stage and thereafter higher than that in the first stage. The film may be relaxed by 1 to 10% in either the machine direction (longitudinal direction) or the perpendicular direction (width direction).

[0060] (Regarding the refractive index in the thickness direction) The refractive index in the thickness direction is preferably 1.520 or less. By setting the refractive index to 1.520 or less, even if the refractive index in the bending direction is designed to be low, a decrease in the hardness of the film surface can be suppressed, thereby achieving both flexibility and surface hardness. By setting the refractive index to 1.520 or less, the indentation depth after unloading the test force in the thickness direction is reduced, and the hardness of the film surface, particularly the pencil hardness of the laminated polyester film after lamination of a hard coat layer, can be improved. The refractive index is more preferably 1.515 or less, even more preferably 1.510 or less, particularly preferably 1.505 or less, and most preferably 1.500 or less. A low refractive index in the thickness direction is preferable, but from the perspective of stable production, it is preferably 1.3 or more, and even 1.4 or more. It is particularly preferably 1.410 or more. It can be said that the above range can be achieved by increasing the stretch ratio in both the bending direction and the folding direction. However, in order to control the refractive index in the thickness direction after controlling the refractive index in the bending direction and the width direction within preferred ranges, it is preferable to set the conditions while checking the balance of the conditions for each process in the film formation process.

[0061] Methods for controlling the refractive index in the thickness direction within the above range include the preheating temperature, stretching temperature, and stretching ratio in the bending direction, the preheating temperature, stretching temperature, multi-stage stretching, high-strength stretching, or heat setting temperature in the folding direction. The preheating temperature for stretching in the bending direction is preferably 70°C to 110°C. The stretching temperature in the bending direction is preferably 75°C to 120°C. The stretching ratio in the bending direction is preferably 1.2 to 2.0 times, more preferably 1.7 to 2.0 times. By lowering the stretching temperature and stretching at a low stretching ratio, the refractive index in the thickness direction can be effectively reduced while maintaining the flexibility in the bending direction. The preheating temperature for stretching in the folding direction is also preferably 75°C to 110°C. The stretching temperature is preferably 75°C to 120°C. The stretching ratio in the folding direction is preferably 4.0 to 6.0 times, more preferably 4.4 to 6.0 times. The refractive index in the thickness direction can be effectively reduced while maintaining or reducing the refractive index in the bending direction. Multistage stretching may be used as a method for high-ratio stretching. In this case, it is preferable to set the stretching ratio in the second stage higher than that in the first stage, as this allows for more effective control of the refractive index. A method of stretching again after the crystallization step may also be used. Accelerated stretching, in which the stretching speed is increased from the initial stage to the latter stage of stretching, may also be used. The heat setting temperature is preferably 180 to 240°C. Heat setting promotes oriented crystallization in the stretching direction, thereby reducing the refractive index in the thickness direction. While the reason why reducing the refractive index in the thickness direction improves the hardness of the film surface is not entirely clear, it is thought that this is due to the effect of aromatic groups such as benzene rings in the molecular chain being oriented in the plane direction, thereby suppressing deformation due to stress applied in the thickness direction.

[0062] (Regarding density of polyester film) The density of polyester film is 1.380 g / cm 3 It is preferable that the density is 1.383 g / cm or more. It is more preferable that the density is 1.380 g / cm or more. 3 By setting the density to 1.40 g / cm or more, it is possible to improve the flexibility and the film surface hardness, particularly the pencil hardness of the laminated polyester film after laminating the hard coat layer. The higher the density, the better. Although it depends somewhat on the presence or absence of particles in the film, it is preferable to set the density to 1.40 g / cm or more. 3 It is preferable that the density is 1.395 g / cm or less, and more preferably 1.395 g / cm 3The following is more preferable. By setting the heat setting temperature during film formation to 180 to 240°C, crystallization can be promoted and the density can be effectively increased. 3 If the temperature is lower than this, the crystallization will be insufficient, which will lead to deformation due to bending, and the thermal shrinkage will be high, which will result in poor processability when applying a hard coat.

[0063] The bending direction of the polyester film preferably corresponds to the longitudinal direction (machine flow direction). This facilitates lowering the refractive index in the bending direction during biaxial stretching, thereby improving flexibility. That is, a polyester film is preferably obtained by stretching an unstretched polyester sheet in the longitudinal direction at a stretching ratio of 1.2 to 2.0, more preferably 1.7 to 2.0. It can be said that a preferred embodiment is to stretch the polyester sheet in the width direction at a stretching ratio of 4.0 to 6.0, more preferably 4.4 to 6.0.

[0064] The surface of the polyester film of the present invention may be smooth or uneven, but since it is used as a surface cover for a display, deterioration of optical properties due to unevenness is undesirable. The haze is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. A haze of 3% or less can improve image visibility. The lower limit of the haze is the better, but it can be 0.1% or more, or even 0.3% or more. The haze can be 0.1 to 3%, 0.1 to 2%, 0.1 to 1%, 0.3 to 3%, 0.3 to 2%, or 0.3 to 1%.

[0065] As mentioned above, in order to reduce haze, it is preferable that the film surface roughness is not too large. On the other hand, from the viewpoint of handling, there is a method of forming roughness to provide a certain degree of slipperiness. In this method, roughness is formed by blending a filler into the polyester resin layer of the surface layer or by coating a filler-containing coating layer during film formation. The most preferred method for reducing haze is to not include a filler in the polyester resin layer, and to coat at least one surface with a filler-containing coating layer during film formation.

[0066] The method of incorporating particles into the base film can be a known method. For example, they can be added at any stage of polyester production, but preferably they can be added as a slurry dispersed in ethylene glycol or the like at the stage of esterification, or after the completion of the transesterification reaction and before the start of the polycondensation reaction, to proceed with the polycondensation reaction. Alternatively, they can be added by a method of blending a slurry of particles dispersed in ethylene glycol or water with polyester raw materials using a vented kneading extruder, or a method of blending dried particles with polyester raw materials using a kneading extruder.

[0067] Among these, a method in which aggregate inorganic particles are homogeneously dispersed in a monomer liquid that will become a part of the polyester raw material, and then the filtered product is added to the remainder of the polyester raw material before, during, or after the esterification reaction is preferred. This method facilitates homogeneous dispersion of the particles and high-precision filtration of the slurry, since the monomer liquid has a low viscosity. Furthermore, when the monomer liquid is added to the remainder of the raw material, the particles are well dispersible and new aggregates are unlikely to form. From this perspective, it is particularly preferred to add the monomer liquid to the remainder of the raw material at a low temperature before the esterification reaction.

[0068] Furthermore, the number of protrusions on the film surface can be further reduced by a method (masterbatch method) in which a polyester containing particles is prepared in advance and then the pellets are kneaded and extruded with pellets containing no particles.

[0069] The total light transmittance of the polyester film is preferably 85% or more, more preferably 87% or more. Similarly, the total light transmittance of a laminated polyester film having an easy-adhesion layer and a hard coat layer provided on the surface of the polyester film is preferably 85% or more, more preferably 87% or more. A transmittance of 85% or more can ensure sufficient visibility. Although a higher total light transmittance is considered better, it may be 99% or less, or even 97% or less. The total light transmittance of the polyester film and laminated polyester film may be 85 to 99%, 85 to 97%, 87 to 99%, or 87 to 97%.

[0070] The surface of the polyester film of the present invention may be subjected to a treatment to improve adhesion to a resin forming a hard coat layer or the like.

[0071] Examples of surface treatment methods include roughening treatments such as sandblasting and solvent treatment, and oxidation treatments such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromic acid treatment, and hot air treatment, and any of these methods can be used without particular limitation.

[0072] The polyester film can be produced, for example, by homogeneously dispersing inorganic particles in a monomer solution that forms part of the polyester raw material, filtering the solution, and then carrying out a polymerization step and a film-forming step. The polymerization step involves adding the inorganic particles to the remainder of the polyester raw material to polymerize the polyester. The film-forming step involves melt-extruding the polyester through a filter into a sheet, cooling it, and stretching it to form a substrate film.

[0073] Next, a method for producing a biaxially stretched polyester film will be described in detail using an example in which polyethylene terephthalate (hereinafter sometimes referred to as PET) pellets are used as the raw material for the base film, but the method is not limited to this. Furthermore, the number of layers, such as a single layer or a multilayer structure, is not limited.

[0074] PET pellets are mixed in a predetermined ratio, dried, and then fed into a known melt lamination extruder, extruded through a slit die into a sheet, and cooled and solidified on a casting roll to form an unstretched film. A single extruder is used for a single-layer film. On the other hand, two or more extruders, two or more layer manifolds, or merging blocks are used for producing multilayer films. When producing a multilayer film, multiple film layers constituting the outermost layers are laminated, and a two or more layer sheet is extruded through a die and cooled on a casting roll to form an unstretched film. This merging block is, for example, a merging block having a rectangular merging portion.

[0075] In this case, it is preferable to perform high-precision filtration to remove foreign matter contained in the resin during melt extrusion at any location where the molten resin is maintained at approximately 280°C. The filter material used for high-precision filtration of the molten resin is not particularly limited, but various metals or alloys such as stainless steel, nickel, chromium, aluminum, and copper can be used. Among these, stainless steel filters are preferred in terms of heat resistance and durability, and high-precision sintered-fiber stainless steel filters are particularly preferred. However, while sintered-fiber stainless steel filters are effective in capturing regular inorganic foreign matter, they are prone to generating irregular organic foreign matter (modified polymers) during long-term film production. To suppress this, for example, sintered-powder stainless steel filters are preferred. When using these two types of filters in combination, it is preferable to use a sintered-fiber stainless steel filter upstream (first) and a sintered-powder stainless steel filter downstream (second). The second filter is preferably located after the extruder, or if a gear pump is used to ensure uniform extrusion volume, after the gear pump and near the die, as this allows for the capture of degraded materials generated in piping dead zones, etc.

[0076] In the present invention, the filtration accuracy (the particle diameter at which a collection efficiency of 95% or more can be achieved) of the sintered fiber stainless steel filter, which is the benchmark for capturing inorganic contaminants, is preferably 3 to 50 times, more preferably 3.5 to 45 times, and most preferably 4 to 40 times, the average particle size of the inert particles used. When particles are not included, a filtration accuracy of 30 μm or less is preferred, and a filtration accuracy greater than the filtration accuracy of the downstream sintered powder filter is preferable to extend the life of the sintered powder filter. The mesh size of the sintered powder filter is smaller than 30 μm, preferably 20 μm or less, and even more preferably 10 μm or less, because it allows for efficient capture of organic contaminants. Furthermore, a mesh size of 5 μm or less increases the efficiency of capturing organic contaminants, but is undesirable because it increases the filter's pressure rise rate, increases the frequency of filter replacement, and reduces production efficiency.

[0077] Specifically, for example, PET pellets are thoroughly vacuum-dried and then fed into an extruder. The extruder temperature is preferably higher than the melting point of PET (258°C) and not higher than 295°C, from the viewpoints of pellet melting, kneading stability, and preventing a decrease in intrinsic viscosity. It is more preferably 265 to 290°C. Furthermore, it is preferable that the inlet side of the extruder be in the range of 265 to 275°C, with the middle and outlet sides being higher than the inlet side and 280 to 290°C. The film is then extruded into a sheet form through a die, cooled, and solidified to form an unstretched PET sheet. The die temperature is preferably 285 to 290°C, with a widthwise difference of 2°C or less, to prevent thickness variations in the widthwise direction. Subsequently, the unstretched film is biaxially stretched in the longitudinal direction and in the width direction perpendicular to the longitudinal direction, followed by heat treatment. The stretching process is not particularly limited, but stretching in each direction may be performed in two or more stages. Performing longitudinal stretching in two stages is particularly preferable, as it effectively suppresses thickness variations in the longitudinal direction.

[0078] The stretching method may be simultaneous biaxial stretching or sequential biaxial stretching. Simultaneous biaxial stretching is preferred because it does not involve stretching with rolls, so localized heating of the film surface does not occur and surface properties are easily controlled. Sequential biaxial stretching is preferred because it is easier to control orientation by combining the stretching ratio and stretching pattern and it is easy to adopt conditions that are less likely to leave creases at low temperatures. In sequential biaxial stretching, an unstretched film is stretched in the longitudinal direction using a longitudinal stretching machine equipped with several rolls, utilizing the difference in peripheral speed between the rolls, and then transversely stretched in the width direction using a stenter. In the longitudinal stretching step, the unstretched polyester film obtained in the above-mentioned unstretched polyester film forming step is stretched in the longitudinal direction (hereinafter sometimes referred to as longitudinal stretching) to obtain a longitudinally uniaxially stretched polyester film. In this case, it is preferable to preheat the film at a temperature of (Tg-10)°C or higher (Tg-2)°C or lower prior to the primary stretching step in order to obtain a biaxially oriented polyester film having a uniform thickness and the desired N(AB). Here, Tg indicates the glass transition temperature (unit: °C) of the unstretched polyester film. In the case of PET, it is 78°C.

[0079] In the primary stretching step, it is preferable to stretch an optionally preheated unstretched polyester film in the longitudinal direction at a stretching ratio of 1.2 to 1.9 times under a temperature condition of (Tg + 2)°C or higher and (Tg + 40)°C or lower. When the longitudinal stretching temperature is (Tg + 2)°C or higher, film breakage is prevented and productivity is improved. On the other hand, when the longitudinal stretching temperature is (Tg + 40)°C or lower, the film has sufficient strength, making it easy to obtain the desired N(AB), and the film does not stick to the longitudinal stretching rolls, thereby suppressing stretching unevenness. Next, when the stretching ratio is 1.2 times or higher, N(AB) is reduced and tan δ at room temperature and low temperature is prevented from becoming too small. That is, crazes in the bending direction can be prevented, and the crystalline modulus is reduced, thereby preventing cracking when bent at low temperatures. Furthermore, when the stretching ratio is 1.9 times or lower, N(AB) is increased and tan δ at room temperature and low temperature is not too large, making it difficult to leave creases. Stretching may be performed in one stage or two stages. Performing it in two stages is preferred because it allows for uniform orientation and reduces thickness unevenness. When performing it in two stages, it is preferred to set the stretching ratio in the first stage high. It is preferred to keep the stretching ratio in the second stage to a slight degree, and a ratio of 1.01 to 1.1 is preferred because it allows for uniform longitudinal stretching stress across the entire width in the width direction and reduces thickness unevenness.

[0080] In the secondary stretching step, the film is stretched in the width direction (hereinafter sometimes referred to as transverse stretching) to obtain a biaxially stretched polyester film. Prior to the secondary stretching step, preheating at a temperature of (Tg + 10)°C to (Tg + 30)°C is preferred to ensure uniform stretching in the subsequent secondary stretching step. In the secondary stretching step, the film is stretched in the width direction at a temperature of (Tg + 5)°C to (Tg + 80)°C, preferably below the auxiliary heating temperature and between (Tg + 5)°C and (Tg + 50)°C, at a magnification of 3.0 to 6.0 times. The magnification is preferably 4 to 5 times. Stretching is performed in separate zones, allowing the temperature to be gradually increased in each zone, making it easier to control the orientation state, achieving the desired tan δ at room temperature and low temperature, and achieving the desired refractive index difference N(AB). Three or more zones are preferred, with four or more being more preferred. The temperature in the first stretching zone is preferably set low, between (Tg + 5)°C and (Tg + 20)°C. This is because the longitudinal stretching ratio is low, allowing for high stretching stress in both the longitudinal and transverse directions at a lower temperature. Setting the final zone higher, between (Tg + 20)°C and (Tg + 50)°C, is preferred because it reduces the temperature difference with the subsequent heat-setting zone and reduces bowing. The relationship between the stretching ratio in the first stretching step (hereinafter sometimes referred to as the longitudinal stretching ratio) and the stretching ratio in the second stretching step (hereinafter sometimes referred to as the transverse stretching ratio) is preferably longitudinal stretching ratio < transverse stretching ratio. A longitudinal stretching ratio < transverse stretching ratio relationship is preferred because it allows for a smaller molecular orientation in the longitudinal direction than in the transverse direction, and allows for N(AB) and tan δ to fall within the desired range, resulting in a film that is resistant to crease marks even at room temperature or low temperatures. Thereafter, heat setting is carried out to stabilize the dimensions, and the maximum temperature is (Tg + 100) ° C. to (Tg + 160) ° C., preferably (Tg + 110) ° C. to (Tg + 150) ° C., and more preferably (Tg + 120) ° C. to (Tg + 140) ° C. Heat setting is preferably carried out in several zones, preferably three or more zones.The heat setting temperature in the first zone is preferably (Tg + 100) ° C to (Tg + 120) ° C, which allows for the gradual relaxation of molecular chains strained by stretching and allows for control of crystal size. The maximum heat setting temperature is then preferably used in the second and subsequent zones. The final heat setting zone is preferably lower than the maximum heat setting temperature, preferably (Tg + 50) ° C to (Tg + 130) ° C. A temperature too high in the final zone is undesirable because subsequent cooling proceeds too quickly, resulting in the formation of wrinkles and other problems. Furthermore, setting the heat setting temperature below the maximum value is preferable because it prevents the excessive increase in crystallinity that occurs as the polyester amorphous chain portion relaxes, thereby reducing cracking when bent. The heat setting time is preferably 0.5 to 20 seconds, preferably 1 to 15 seconds. A cooling zone may then be provided in the range of (Tg - 20) ° C to (Tg + 80) ° C. In the latter half of the heat setting zone or in the cooling zone, relaxation treatment of, for example, 0.5 to 7.0%, preferably 0.5 to 6.5%, in the longitudinal direction and / or width direction is preferred from the viewpoint of improving the planar stability of the film or preventing shrinkage during storage or processing. The molecular orientation state in the bending direction obtained by the above-mentioned preferred first stretching, second stretching, heat setting, and relaxation treatment can be in the range of N(AB).

[0081] (Regarding the density of polyester film) The density of polyester film is 1.380 to 1.395 g / cm 3 It is preferable that the density is 1.381 to 1.390 g / cm 3 It is more preferable that the density is 1.380 g / cm 3 By setting the density at 1.390 g / cm or more, the polyester film can be sufficiently crystallized to form a film with excellent thermal dimensional stability, and dimensional changes in the polyester film due to heat generation in the device can be suppressed. 3 If it is less than this, crazes are less likely to occur when the film is bent, which is preferable.

[0082] (Easy-Adhesion Layer) Furthermore, adhesion can be improved by an adhesion-improving layer such as an easy-adhesion layer. The easy-adhesion layer can be obtained by applying a coating liquid described below to one or both sides of an unstretched or uniaxially stretched film in the machine direction, drying the film at 75 to 150°C, and then stretching the film in one or two directions. The final coating amount of the easy-adhesion layer is 0.05 to 0.20 g / m 2 It is preferable to control the coating amount to 0.05 g / m 2 On the other hand, when the coating amount is 0.20 g / m or more, the adhesiveness is satisfied, which is preferable. 2 If it is less than this, blocking resistance can be obtained, which is preferable.

[0083] Resins used in the adhesion layer include, without particular limitation, polyester resins, polyurethane resins, polyester polyurethane resins, polycarbonate polyurethane resins, acrylic resins, etc. Crosslinking agents for the adhesion layer include melamine-based, isocyanate-based, oxazoline-based, and epoxy-based crosslinking agents. Two or more types can also be used in combination. Due to the nature of inline coating, these are preferably applied using an aqueous coating liquid, and the resins and crosslinking agents are preferably water-soluble or water-dispersible resins or compounds.

[0084] It is preferable to add particles to the adhesion layer to impart lubricity. The average particle size of the fine particles is preferably 1.1 to 5.0 times the thickness of the coating layer. If the particle size is smaller than this, it is difficult to impart lubricity, and if it exceeds 5.0 times, the filler may fall off during handling, which is undesirable. The thickness of the coating layer is preferably 10 nm to 1,000 nm, more preferably 20 nm to 500 nm, and even more preferably 50 nm to 200 nm. The average particle size of the filler is preferably 11 nm to 2,000 nm. Examples of particles contained in the adhesion layer include inorganic particles and organic polymer particles. These particles may be added to the adhesion layer alone or in combination of two or more types. Examples of inorganic particles include titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride. Examples of organic polymer particles include styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles.

[0085] The coating solution can be applied by any known method, similar to that used for the coating layer, such as reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire bar coating, and pipe doctor coating, which can be used alone or in combination.

[0086] (Hard Coating Layer) The resin forming the hard coating layer can be any of (meth)acrylic acid ester, siloxane, inorganic hybrid, urethane acrylate, polyester acrylate, epoxy, etc., without any particular limitation. Two or more materials can be mixed and used, or particles of inorganic filler or organic filler can be added. Among them, (meth)acrylic acid ester and acrylate resins are preferred, and resins having three or more reactive groups in the molecule as an essential component are preferred.

[0087] (Resin Having Three or More Reactive Groups) Examples of resins having three or more reactive groups include tris[(meth)acryloyloxyalkyl]isocyanurates such as tris(2-acryloyloxyethyl)isocyanurate, tris(3-acryloyloxypropyl)isocyanurate, tris(2-methacryloyloxyethyl)isocyanurate, and tris(3-methacryloyloxypropyl)isocyanurate, as well as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propane tri(meth)acrylate, and the like. (Meth)acrylates such as propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate may be used alone or in combination of two or more.

[0088] Other commercially available hard coating agents may also be used, such as the Beamset (registered trademark) series manufactured by Arakawa Chemical Industries, Ltd., the AICA Itron (registered trademark) series manufactured by Aica Kogyo Co., Ltd., and the Lioduras (registered trademark) series manufactured by Toyo Ink Co., Ltd., which may be used in combination with other (meth)acrylic acid ester compounds.

[0089] (Photopolymerization Initiator) When the hard coat layer of the present invention is cured using ultraviolet light, it is necessary to add a photopolymerization initiator. Examples of the photopolymerization initiator include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, β-chloroanthraquinone, (2,4,6-trimethylbenzyldiphenyl)phosphine oxide, and 2-benzothiazole-N,N-diethyldithiocarbamate. In particular, from the viewpoint of excellent surface curing properties, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methylpropan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one are preferred, and of these, 2-hydroxy-2-methyl-1-phenyl-propan-1-one and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one are preferred. These may be used alone or in combination of two or more.

[0090] The amount of photopolymerization initiator added is not particularly limited. For example, it is preferable to use about 1 to 10% by mass of the resin used. Adding 1% by mass or more can provide sufficient curability, while adding 10% by mass or less can provide a high content of resin having three or more reactive groups, resulting in a hard coat film with high crosslink density and high hardness.

[0091] (Film Thickness) The film thickness of the hard coat layer is preferably 1 to 55 μm. If the film thickness is greater than 1 μm, sufficient curing occurs and good pencil hardness is obtained. Furthermore, by making the thickness 55 μm or less, curling due to cure shrinkage of the hard coat can be suppressed, and the handling properties of the film can be improved.

[0092] (Coating Method) The hard coat layer can be coated by any method, including but not limited to a Mayer bar, gravure coater, die coater, knife coater, etc., and can be appropriately selected depending on the viscosity and film thickness. The drying temperature is preferably 60 to 100°C, more preferably 60 to 90°C. A temperature of 60°C or higher allows for sufficient drying in a short time, and a temperature of 100°C or lower is preferred because deformation of the polyester film does not occur.

[0093] (Curing Conditions) The hard coat layer can be cured by energy rays such as ultraviolet rays and electron beams, or by heat, but ultraviolet rays and electron beams are preferred in order to reduce damage to the film.

[0094] (Ultraviolet Rays) Ultraviolet lamps include high-pressure mercury lamps and electrodeless lamps, and can be appropriately selected and used. The cumulative light dose of ultraviolet rays is preferably 50 to 500 mJ / cm2, and more preferably 100 to 200 mJ / cm2. Sufficient pencil hardness can be obtained by irradiating with an cumulative light dose of 50 mJ / cm2 or more, while an cumulative light dose of 500 mJ / cm2 or less can increase the processing speed and is therefore preferable as it improves economy. Curability can also be improved by irradiating with ultraviolet rays in an inert gas such as nitrogen, argon, or carbon dioxide, and this can be selected appropriately.

[0095] (Electron beam) Electron beam irradiation devices include area type and scanning type, and can be appropriately selected and used. The cumulative dose of electron beam is preferably 25 to 500 kGy, and more preferably 50 to 300 kGy. A cumulative dose of 25 kGy or more can provide sufficient pencil hardness, while a dose of 500 kGy or less can increase the processing speed and is preferable for improving economy. It is preferable to irradiate in an inert gas such as nitrogen or argon, with an oxygen concentration of 500 ppm or less. By keeping the oxygen concentration at 500 ppm or less, ozone generation can be suppressed, improving safety during work.

[0096] (Pencil hardness) The pencil hardness of the hard coat layer is preferably 2H or more, more preferably 3H or more, and particularly preferably 4H or more. If the hard coat layer has a pencil hardness of 2H or more, it will not be easily deformed and will not reduce visibility. Generally, the higher the pencil hardness of the hard coat layer, the better, but it may be 10H or less, or 8H or less, or even 6H or less, and it can be used without any practical problems.

[0097] (Type of hard coat layer) The hard coat layer in the present invention may have other functions added thereto, as long as it can be used for the purpose of increasing the pencil hardness of the surface and protecting the display as described above. For example, hard coat layers having the above-mentioned certain pencil hardness and added functionality such as an antiglare layer, an antiglare antireflection layer, an antireflection layer, a low reflection layer, and an antistatic layer are also preferably used in the present invention.

[0098] Next, the effects of the present invention will be described using examples and comparative examples. First, the evaluation methods of the characteristic values ​​used in the present invention will be described below.

[0099] (1) Intrinsic Viscosity Polyester resin (polyethylene terephthalate pellets) was pulverized and dried, and then dissolved in a phenol / tetrachloroethane (60 / 40 mass ratio) mixed solvent. After centrifuging the solution to remove inorganic particles, the flow time of a 0.4 (g / dl) solution and the flow time of the solvent alone were measured at 30°C using an Ubbelohde viscometer. From the ratio of these times, the intrinsic viscosity was calculated using the Huggins equation, assuming a Huggins constant of 0.38. The intrinsic viscosity of a polyester film was determined by scraping the polyester layer of a laminated polyester film, dissolving the polyester obtained in the mixed solvent, and then calculating the intrinsic viscosity in the same manner.

[0100] (2) Refractive Index Five polyester film samples were taken, and the refractive indexes in the longitudinal direction (Nx), width direction (Ny), and thickness direction (Nz) of the film were measured using an Abbe refractometer with sodium D-line as a light source in accordance with JIS K7142. Direction A was defined as the longitudinal direction, and the value (N(AB)) obtained by subtracting the refractive index in the direction perpendicular to direction A (direction B) from the refractive index in direction A was calculated from Nx - Ny. When direction A is the width direction, the value (N(AB)) obtained by subtracting the refractive index in the direction perpendicular to direction A (direction B) is calculated from Ny - Nx. The value calculated by Nx - ((Ny + Nz) / 2) is shown in the table as ΔNx.

[0101] (3) Dynamic Viscoelasticity Measurement of Polyester Film Measurements were performed using a dynamic viscoelasticity measuring device "DMA7100" (manufactured by Hitachi High-Tech Science Corporation) in tensile mode with a sample size of 8 mm wide x 20 mm between chucks. The frequency was 1 Hz, and the measurement temperature was increased at 10°C / min from -40°C to 100°C. Tan δ was calculated from the equation "loss modulus / storage modulus," and tan δ in direction A at -30°C and 25°C was read from the graph of tan δ values.

[0102] (4) Bending Resistance of Polyester Film (Bending Radius 1.5 mm) A polyester film sample measuring 20 mm in the transverse direction (TD) and 110 mm in the machine direction (MD) was prepared. Using a no-load U-shaped stretch tester (Yuasa System Co., Ltd., DLDMLH-FS), the sample was bent 200,000 times at a bending radius of 1.5 mm and a speed of 1 bending / second. The sample was fixed at 10 mm positions on both ends of the long side, and the bending area was 20 mm x 90 mm. Measurements were performed at temperatures of -30°C and / or 25°C. This test simulated the folding display shown in Figure 1, in which a polypropylene film was placed on the inner folded surface, the display bending radius was set to 1.5 mm, and the display was repeatedly folded. After the predetermined number of bending cycles, the sample was placed on a flat surface with the inner folded surface facing down, and visually inspected and observed under a digital microscope (HIROX RH8800) at 700x magnification. ○: The sample has no cracks or folds, and when placed on a horizontal surface, the maximum lift is less than 3 mm. △: The sample has no cracks, and when placed on a horizontal surface, the maximum lift is less than 5 mm. ×: The sample has cracks or folds, and when placed on a horizontal surface, the maximum lift is 5 mm or more.

[0103] (5) Resistance to cracking and bending of polyester film (bending radius 0.75 mm) The test was carried out in the same manner as described above for the resistance to bending and breaking of polyester film, except that the bending radius was set to 0.75 mm and the test device was a small tabletop planar clamshell durability tester (DLDMLP-CS, manufactured by Yuasa System Co., Ltd.). The evaluation was as follows: ◯: No holes were found in the film after the test ×: Holes were found in the film after the test

[0104] (6) Thickness Unevenness The thickness unevenness of the polyester film in the longitudinal direction was calculated using the following formula: Thickness Unevenness (%) = ((Maximum Thickness - Minimum Thickness) / Average Thickness) x 100

[0105] (7) Average particle size of inactive particles in polyester film A polyester film was cut in a direction perpendicular to the film-forming direction to obtain ultrathin sections with a thickness of 0.2 μm, and the ultrathin sections were observed with a transmission electron microscope (JEM2010 manufactured by JEOL Ltd.). From this observation, the area-equivalent circle diameters (μm) of 100 particles in the polyester film forming each surface of the ultrathin sections were calculated, and the average value thereof was taken as the average particle size (μm).

[0106] (8) Average particle size of inactive particles in adhesive layer A platinum thin film vapor-deposited layer with a thickness of 2 to 3 nm was formed on the surface of the coating layer (adhesion layer) of a polyester film using a platinum sputtering device, and the layer was observed at a magnification of about 100,000 times using a scanning electron microscope (Hitachi High-Technologies S-4700). From this observation, the area-equivalent circle diameters of at least 100 particles in the adhesion layer were calculated, and the average value thereof was taken as the average particle size.

[0107] (9) Thickness of the Adhesion Layer The laminated polyester film was cut in a direction perpendicular to the film formation direction to obtain ultrathin sections with a thickness of 0.2 μm, which were then stained with osmium tetroxide (OsO). The ultrathin sections were observed using a transmission electron microscope (JEM2010, manufactured by JEOL Ltd.). The thickness of the adhesion layer was measured by this observation.

[0108] (10) Pencil Hardness According to JIS K 5600-5-4:1999, the laminated polyester film was measured at a load of 750 g and a speed of 1.0 mm / s, and the presence or absence of deformation was visually confirmed. Those without deformation were rated as OK. The measurement was carried out five times, and the pencil hardness of four or more evaluations of OK was taken as the measured value.

[0109] (11) Haze According to JIS-7136, the haze of a polyester film sample was measured using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0110] (12) UV absorption performance A polyester film sample measuring 8 mm in the transverse direction (TD) and 40 mm in the machine direction (MD) was prepared. The sample was placed so that the machine direction (MD) was parallel to the direction of gravity, and the transmittance at a wavelength of 380 nm was measured using a spectrophotometer (Shimadzu Corporation, UV1800).

[0111] (Polymerization of Urethane Resin) A four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer was prepared. 72.96 parts by mass of 1,3-bis(isocyanatomethyl)cyclohexane, 12.60 parts by mass of dimethylolpropionic acid, 11.74 parts by mass of neopentyl glycol, 112.70 parts by mass of polycarbonate diol having a number average molecular weight of 2000, and 85.00 parts by mass of acetonitrile and 5.00 parts by mass of N-methylpyrrolidone as solvents were added to the four-neck flask. These were then stirred in a nitrogen atmosphere at 75°C for 3 hours, and it was confirmed that the reaction solution in the four-neck flask had reached the predetermined amine equivalent. Next, the reaction solution was cooled to 40°C, and 9.03 parts by mass of triethylamine was added to obtain a polyurethane prepolymer D solution. Next, 450 g of water was added to a reaction vessel equipped with a homodisper capable of high-speed stirring, and the temperature was adjusted to 25°C. While stirring and mixing, the isocyanate group-terminated prepolymer was added and dispersed in water. Thereafter, acetonitrile and a portion of the water were removed under reduced pressure to prepare a water-soluble polyurethane resin (A) with a solids content of 35% by mass.

[0112] (Polymerization of Water-Soluble Carbodiimide Compound) A flask equipped with a thermometer, nitrogen gas inlet tube, reflux condenser, dropping funnel, and stirrer was prepared. 200 parts by mass of isophorone diisocyanate and 4 parts by mass of 3-methyl-1-phenyl-2-phospholene-1-oxide as a carbodiimidization catalyst were added to the flask, and the mixture was stirred at 180°C for 10 hours under a nitrogen atmosphere to obtain an isocyanate-terminated isophorone carbodiimide (degree of polymerization = 5). Next, 111.2 g of the resulting carbodiimide and 80 g of polyethylene glycol monomethyl ether (molecular weight 400) were reacted at 100°C for 24 hours. Water was gradually added to the mixture at 50°C to obtain a yellow, transparent, water-soluble carbodiimide compound (B) with a solids content of 40% by mass.

[0113] (Preparation of easy-adhesion layer coating liquid) The following coating materials were mixed to prepare a coating liquid: Water 16.97 parts by mass Isopropanol 21.96 parts by mass Water-soluble polyurethane resin (A) 3.27 parts by mass Water-soluble carbodiimide compound (B) 1.22 parts by mass Particles 0.51 parts by mass (silica sol with an average particle size of 40 nm, solid content concentration 40% by mass) Surfactant 0.05 parts by mass (silicone-based, solid content concentration 100% by mass)

[0114] (Preparation of hard coat coating liquid) 95 parts by weight of pentaerythritol triacrylate (A-TMM-3, manufactured by Shin-Nakamura Chemical Co., Ltd., solid content concentration 100%), 5 parts by weight of photopolymerization initiator (Irgacure (registered trademark) 907, manufactured by BASF Japan, solid content concentration 100%), and 0.1 parts by weight of leveling agent (BYK Japan, BYK307, solid content concentration 100%) were mixed and diluted with a solvent of toluene / MEK = 1 / 1. This prepared a hard coat coating liquid with a concentration of 40%.

[0115] (Preparation of polyethylene terephthalate pellets) A continuous esterification reactor consisting of a three-stage complete mixing vessel equipped with a stirrer, a partial condenser, a raw material inlet, and a product outlet was used as the esterification reactor. The TPA rate was 2 ton / hr, the EG was 2 moles per mole of TPA, and antimony trioxide was added in an amount that would result in an Sb atom concentration of 160 ppm relative to the PET produced. These slurries were continuously fed to the first esterification reactor of the esterification reactor and reacted at atmospheric pressure for an average residence time of 4 hours at 255°C. The reaction product in the first esterification reactor was then continuously removed from the system and fed to the second esterification reactor. In addition, EG distilled from the first esterification reactor was supplied to the second esterification reactor at 8% by mass relative to the produced polymer (produced PET). Furthermore, an EG solution containing magnesium acetate in an amount equivalent to 65 ppm of Mg atoms relative to the produced PET and an EG solution containing TMPA in an amount equivalent to 20 ppm of P atoms relative to the produced PET were added. These solutions were then reacted at 260°C for an average residence time of 1.5 hours at atmospheric pressure. The reaction product in the second esterification reactor was then continuously removed from the system and supplied to a third esterification reactor. An EG solution containing TMPA in an amount equivalent to 20 ppm of P atoms relative to the produced PET was then added, and the reaction was continued at 260°C for an average residence time of 0.5 hours at atmospheric pressure. The esterification reaction product produced in the third esterification reactor was continuously supplied to a three-stage continuous polycondensation reactor for polycondensation, and then filtered through a stainless steel sintered filter medium (filtration accuracy: 90% cutoff of 5 μm particles). This gave polyethylene terephthalate pellets with an intrinsic viscosity of 0.60 dl / g.

[0116] Example 1: First, the polyethylene terephthalate pellets were dried under reduced pressure (3 Torr) at 180°C for 8 hours. The polyethylene terephthalate pellets (hereinafter sometimes referred to as PET pellets) were then mixed with UV-absorbing pellets, fed into an extruder, and melted at 285°C. The UV-absorbing pellets were primarily composed of polyethylene terephthalate and contained an organic UV absorber. The UV-absorbing pellets were UN101 (manufactured by Nippon Pigment Co., Ltd.). The molten polymer was filtered through a stainless steel nonwoven sintered filter medium (nominal filtration accuracy: 95% cutoff for 20 μm particles) and then further filtered through a stainless steel granular sintered filter medium (nominal filtration accuracy: 95% cutoff for 10 μm particles) immediately before the die. The filtered polymer was then extruded into a sheet from the die and cooled and solidified by contacting it with a casting drum at a surface temperature of 30°C using an electrostatic casting method, producing an unstretched film. This unstretched film was preheated to 77°C in the machine direction and stretched 1.7 times at 85°C. The adhesive layer coating solution was applied to one side of the PET film by roll coating, and then dried at 80°C for 20 seconds. The final coating amount after drying (after biaxial stretching) was 0.06 g / m 2 The uniaxially stretched film was preheated to 100°C using a tenter in a preheating zone. It was then uniformly stretched 4.5 times in the width direction using three zones at 90°C, 95°C, and 120°C. Heat setting was then performed in four zones at 180°C, 210°C, 210°C, and 140°C for a total of 5 seconds. In the fourth zone, a 0.5% relaxation treatment was performed in the width direction. Cooling was then performed in two zones at 100°C and 85°C, respectively, and the film was wound up to obtain a biaxially oriented polyester film and a roll thereof. The content of the organic UV absorber was 2% by mass based on 100% by mass of the biaxially oriented polyester film.

[0117] The hard coat coating solution was applied onto the easy-adhesion layer of the polyethylene terephthalate film using a Mayer bar so that the film thickness after drying would be 5.0 μm, and the film was dried at 80° C. for 1 minute, and then irradiated with ultraviolet light (cumulative light amount 200 mJ / cm2) to obtain a laminated polyester film.

[0118] Examples 2 and 3 Polyethylene terephthalate films and laminated polyester films were obtained in the same manner as in Example 1, except that the feed rate of the extruder was adjusted to suit the film thickness shown in Table 1 and the film thickness was changed.

[0119] Examples 4 and 5 A polyethylene terephthalate film and a laminated polyester film were obtained in the same manner as in Example 1, except that the film thickness and stretching ratio were changed to those shown in Table 1.

[0120] Example 6 A polyethylene terephthalate film and a laminated polyester film were obtained in the same manner as in Example 1, except that the mixing ratio of the ultraviolet absorbing pellets to the PET pellets was changed to that shown in Table 1.

[0121] The films of Examples 1 to 6 had a total light transmittance of 85% or more and a haze of 3% or less, and are therefore suitable for use in displays.

[0122] The polyethylene terephthalate films of Examples 1 to 6 had an intrinsic viscosity of 0.56 dl / g.

[0123] Comparative Example 1 A polyethylene terephthalate film and a laminated polyester film were obtained in the same manner as in Example 1, except that the feed rate of the extruder was adjusted to suit the film thickness shown in Table 1 and the film thickness was changed.

[0124] Comparative Examples 2 and 3 Stretching was performed in the same manner as in Example 1 except that the stretching ratio was changed as shown in Table 1, and a polyethylene terephthalate film and a laminated polyester film were obtained in the same manner as in Example 1 except that the stretching ratio was changed.

[0125] Example 7 A biaxially oriented polyester film and a laminated polyester film were obtained in the same manner as in Example 1, except that no ultraviolet absorbing pellets were used and the stretching ratios shown in Table 2 were used.

[0126] Examples 8 to 9, Comparative Examples 4 to 6 Biaxially oriented polyester films and laminated polyester films were obtained in the same manner as in Example 7, except that the stretching ratios shown in Table 2 were used.

[0127] The intrinsic viscosity of the polyethylene terephthalate films of Examples 8 and 9 was 0.56 dl / g.

[0128] (Foldable display) In all of the above examples, the prepared laminated polyester film was attached to an organic EL panel via a 25 μm thick adhesive layer to prepare a foldable display. In each example, the laminated polyester film was able to protect the organic EL panel from external impacts and provide good visibility.

[0129]

[0130]

[0131] According to a foldable display using the polyester film or laminated polyester film of the present invention, the polyester film or laminated polyester film located on the surface of the foldable display does not deform after repeated folding while maintaining mass productivity. Therefore, this foldable display can prevent image distortion at the folded portion of the display. Mobile terminal devices or image display devices equipped with this foldable display provide beautiful images, are highly functional, and are convenient in terms of portability and other factors.

Claims

1. A polyester film having a thickness of 25 to 100 μm, wherein either the longitudinal direction or the width direction of the polyester film is defined as direction A, and the direction perpendicular to direction A is defined as direction B, and the tan δ in direction A at 25°C is 0.008 to 0.

030.

2. The polyester film according to claim 1, characterized in that the refractive index in direction A minus the refractive index in direction B, N(A-B), is -0.12 to -0.

075.

3. The polyester film according to claim 1, wherein tan δ in direction A at -30°C is 0.020 to 0.

065.

4. The polyester film according to any one of claims 1 to 3, characterized in that the light transmittance at a wavelength of 380 nm is 15% or less.

5. The polyester film according to any one of claims 1 to 4, characterized in that the thickness unevenness in the longitudinal direction of the polyester film is 15% or less.

6. The polyester film according to any one of claims 1 to 5, characterized in that the total light transmittance is 85% or more and the haze is 3% or less.

7. The polyester film according to any one of claims 1 to 6, which is used as a surface protection film or a cover window film for a folding display.

8. A laminated polyester film having an easy-adhesion layer on at least one surface of the polyester film according to any one of claims 1 to 7.

9. The laminated polyester film according to claim 8, which has a hard coat layer via an easy-adhesion layer.

10. A folding display comprising the polyester film according to any one of claims 1 to 7, or the laminated polyester film according to claim 8 or 9.

11. The foldable display of claim 10, further comprising an organic electroluminescence panel.

12. A surface protection film for a folding display, comprising the polyester film according to any one of claims 1 to 7, or the laminated polyester film according to claim 8 or 9.

13. A cover window film for a folding display, comprising the polyester film according to any one of claims 1 to 7, or the laminated polyester film according to claim 8 or 9.

Citation Information

Patent Citations

  • Polyester film and applications thereof

    WO2018150940A1

  • Polyester film and use thereof

    WO2020162119A1

  • Multilayer film and use of same

    WO2020241278A1