Non-conductive film, semiconductor device and manufacturing method thereof

The use of a non-conductive film with a tailored adhesive layer composition addresses the void formation issue in semiconductor devices during thermocompression bonding, ensuring reliable adhesion and stress distribution, thus enhancing the reliability of the semiconductor device.

WO2024219577A1PCT designated stage expired Publication Date: 2024-10-24LG CHEM LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/017806
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2023-11-08
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The capillary underfilling method for semiconductor devices faces challenges in uniformly injecting underfill material between fine electrodes, leading to voids in the sealing layer, which affects the reliability of the semiconductor device, especially with narrower pitches and thinner chips.

Method used

A non-conductive film with a specific adhesive layer composition, including thermoplastic and thermosetting resins, a curing agent, and inorganic filler, is used to prevent voids during the thermocompression bonding process, where the adhesive layer's properties are optimized to ensure effective sealing and stress distribution.

Benefits of technology

The non-conductive film effectively prevents voids in the sealing layer, enhancing the reliability of semiconductor devices by ensuring proper adhesion and stress distribution, even during thermocompression bonding, thereby improving the reliability of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to a non-conductive film, a semiconductor device and a manufacturing method thereof. The non-conductive film effectively prevents the generation of voids during a semiconductor manufacturing process and sufficiently adheres to a semiconductor device, so as to provide a semiconductor device having excellent reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Non-conductive film, semiconductor device and method for manufacturing the same

[0001] [Cross-reference with related application(s)]

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0050688, filed April 18, 2023, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a non-conductive film, a semiconductor device and a method for manufacturing the same.

[0004] As the trend toward miniaturization, high functionality, and large capacity of electronic devices expands, the need for high-density and high-integration semiconductor packages is rapidly increasing.

[0005] To meet these demands, flip-chip mounting, which directly connects semiconductor devices such as semiconductor chips to a substrate, has been introduced. In flip-chip mounting, semiconductor chips are electrically connected to other semiconductor chips or the wiring substrate through bumps formed on the semiconductor chips, typically made of solder. At this time, an underfill material is applied between the bonding surfaces to reinforce the bonding location and improve bonding reliability.

[0006] Capillary underfilling is a well-known underfilling method. However, this method suffers from the fundamental problem of difficulty in uniformly injecting the underfill material into the microscopic spaces between electrodes within a short period of time. Furthermore, with the recent narrowing of the electrode pitch and the thinning of semiconductor chips, the capillary underfilling method has been limited in providing a sealing layer of uniform thickness.

[0007] Accordingly, a method using a non-conductive film is being developed. According to the method, a non-conductive film is formed or attached to the element formation surface of a semiconductor wafer, the semiconductor wafer is diced to individualize semiconductor chips, and the individualized semiconductor chips are then mounted on a substrate, and metal bonding and sealing are performed simultaneously.

[0008] These metal bonding and sealing methods are primarily performed using thermocompression bonding (TCB). Thermocompression bonding can be performed by applying pressure for a short period of time, typically 2 to 10 seconds, at temperatures ranging from approximately 200°C to 300°C. Because thermocompression bonding involves rapid temperature and pressure changes, it can easily generate voids in the sealing layer, which is formed from a non-conductive film. However, if these voids are not removed and remain in the sealing layer, they can adversely affect the reliability of semiconductor devices.

[0009] The present invention provides a non-conductive film that prevents voids from occurring in a semiconductor manufacturing process.

[0010] The present invention also provides a semiconductor device including the non-conductive film.

[0011] The present invention also provides a method for manufacturing a semiconductor device using the non-conductive film.

[0012] Hereinafter, a non-conductive film, a semiconductor device, and a method for manufacturing a semiconductor device according to specific embodiments of the invention will be described.

[0013] According to one embodiment of the invention, a non-conductive film is provided, which includes a thermoplastic resin, a thermosetting resin, a curing agent, and an inorganic filler, and an adhesive layer in which Y of the following formula 1 is greater than 0 and less than or equal to 3.

[0014] [Formula 1]

[0015] Y = (△T * G) 2 / (5.88 * η)

[0016] In the above equation 1,

[0017] △T is the difference between the onset temperature of exotherm and the maximum temperature of exotherm of the adhesive layer measured at a heating rate of 10 ℃ / min and from 30 ℃ to 300 ℃ using differential scanning calorimetry, G is the gelation time at 200 ℃ measured in seconds for the adhesive layer, and η is the minimum melting viscosity measured in units of Pa·s for the adhesive layer.

[0018] The non-conductive film of the above embodiment may be a non-conductive film before being used in a semiconductor manufacturing process, a non-conductive film applied during a semiconductor manufacturing process, or a non-conductive film included in a final semiconductor device.

[0019] A non-conductive film prior to use in a semiconductor manufacturing process may refer to a film including a B-staged adhesive layer applied on a substrate. For example, a non-conductive film prior to use in a semiconductor manufacturing process may be a die-bonding film in which a substrate and an adhesive layer are laminated, or a dicing die-bonding film in which a substrate, an adhesive layer, and an adhesive layer are sequentially laminated.

[0020] The non-conductive film applied during the semiconductor manufacturing process may refer to a B-staged adhesive layer applied on a semiconductor element. In other words, the non-conductive film may be applied on a substrate, manufactured in the form of a film, and then attached to a semiconductor element, or it may be manufactured in the form of a film by applying an adhesive composition to a semiconductor element.

[0021] The non-conductive film included in the final semiconductor device may refer to a cured adhesive layer found in the final semiconductor device manufactured through the semiconductor manufacturing process. The cured adhesive layer may be a sealing layer that seals the semiconductor element.

[0022] In the above equation 1, a value calculated in units of ℃ is substituted for △T, a value measured in units of seconds (sec) is substituted for G, and a value measured in units of Pa·s is substituted for η. However, by omitting the units and only substituting the numerical values, Y in equation 1 can be calculated as a unitless value.

[0023] When a non-conductive film including an adhesive layer in which Y, calculated by the above formula 1, is 3 or less is used in a semiconductor manufacturing process, voids are not easily generated, thereby providing a semiconductor device with excellent reliability. In particular, a non-conductive film including an adhesive layer in which Y, calculated by the above formula 1, is 3 or less can effectively prevent void generation even in a thermocompression bonding process of a flip-chip mounting method in which voids are likely to be generated, thereby providing a semiconductor device with excellent reliability.

[0024] An adhesive layer used to bond components of a semiconductor device (e.g., a wiring board and a semiconductor chip or different semiconductor chips) having different coefficients of thermal expansion, etc., needs to sufficiently protrude around the bonded components to form a fillet in order to disperse stress of the components due to temperature changes and improve reliability. A non-conductive film including an adhesive layer in which Y calculated by Equation 1 is 3 or less can form a fillet in an appropriate amount to ensure the reliability of the semiconductor device, and in particular, can effectively prevent voids from occurring in the fillet.

[0025] △T in the above equation 1 is the difference between the onset temperature of heating and the maximum heating temperature of the adhesive layer. The specific method of measuring △T can be referred to the details described in the test examples described below.

[0026] The above △T may be a value determined according to the gel time and the lowest melting viscosity so that Y in Equation 1 is 3 or less. As an example, △T may be 1°C to 20°C. More specifically, △T may be 1°C or more, 2°C or more, 3°C or more, 4°C or more, 5°C or more, 6°C or more, or 7°C or more, and 20°C or less, 15°C or less, 14°C or less, 13°C or less, 12°C or less, 11°C or less, or 10°C or less. Within this range, it is possible to prevent additional voids from being created inside while securing sufficient time for the voids to escape as the adhesive layer is cured at an appropriate rate in the thermocompression bonding process.

[0027] In the above formula 1, G is the gelation time of the adhesive layer at 200°C. G is the gelation time of the B-phase adhesive layer, and the specific measurement method can be referred to the details described in the test examples described below.

[0028] The above G may be a value determined based on the above △T and the lowest melting viscosity such that Y in Equation 1 is 3 or less. As an example, G may be 5 seconds to 30 seconds. More specifically, G may be 5 seconds or more, 6 seconds or more, or 7 seconds or more, and 30 seconds or less, 20 seconds or less, 10 seconds or less, 9 seconds or less, 8.5 seconds or less, 8.3 seconds or less, 8.2 seconds or less, or 8.14 seconds or less. Within this range, it is possible to prevent additional voids from being created inside while securing sufficient time for voids to escape as the adhesive layer is cured at an appropriate rate in the thermocompression bonding process.

[0029] η in the above equation 1 is the lowest melting viscosity of the adhesive layer. For a specific method of measuring η, refer to the details described in the test examples described below.

[0030] The above η may be a value determined according to the above △T and gel time such that Y in Equation 1 is 3 or less. As an example, η may be 10 Pa·s to 5000 Pa·s. More specifically, η may be 10 Pa·s or more, 50 Pa·s or more, 100 Pa·s or more, 150 Pa·s or more, 200 Pa·s or more, 250 Pa·s or more, 300 Pa·s or more, 350 Pa·s or more, or 400 Pa·s or more, and 5000 Pa·s or less, 4000 Pa·s or less, 3000 Pa·s or less, 2000 Pa·s or less, 1000 Pa·s or less, 900 Pa·s or less, 800 Pa·s or less, or 700 Pa·s or less. Within this range, the adhesive layer can exhibit adequate fluidity to sufficiently fill the semiconductor element without causing voids.

[0031] Y of the above formula 1 is a factor related to the occurrence of voids due to an adhesive layer during a semiconductor manufacturing process, and when it has a value of 3 or less, void occurrence can be effectively suppressed. More specifically, Y of the above formula 1 may be 3 or less, 2.5 or less, 2 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, or 1.5 or less. Y of the above formula 1 is a value greater than 0, and may be, for example, 0.00001 or more, 0.001 or more, 0.001 or more, 0.1 or more, 0.5 or more, 0.8 or more, or 1 or more.

[0032] An adhesive layer according to one embodiment may include a thermoplastic resin, a thermosetting resin, a curing agent, and an inorganic filler.

[0033] An adhesive layer according to one embodiment may include two or more types of thermoplastic resins having different glass transition temperatures. In this case, it is advantageous to provide an adhesive layer in which Y in the above formula 1 is 3 or less.

[0034] Specifically, the thermoplastic resin may include a first thermoplastic resin having a glass transition temperature of -10°C to 50°C and a second thermoplastic resin having a glass transition temperature of more than 50°C and less than or equal to 100°C.

[0035] The type of the above first thermoplastic resin is not particularly limited, but may include, for example, one or more resins selected from the group consisting of polyimide-based resins, polyether imide-based resins, polyester imide-based resins, polyamide-based resins, polyether sulfone-based resins, polyether ketone-based resins, polyolefin-based resins, polyvinyl chloride-based resins, phenoxy-based resins, butadiene-based rubbers, styrene-butadiene-based rubbers, modified butadiene-based rubbers, reactive butadiene acrylonitrile copolymer rubbers, and (meth)acrylate-based resins.

[0036] As an example, the first thermoplastic resin may include a (meth)acrylate-based resin. The (meth)acrylate-based resin may be a (co)polymer generated from at least one monomer selected from the group consisting of alkyl (meth)acrylates having 1 to 12 carbon atoms, (meth)acrylates containing a reactive functional group, acrylonitrile, and vinyl monomers polymerizable therewith. Examples of the alkyl (meth)acrylates having 1 to 12 carbon atoms include ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, or octyl (meth)acrylate (ethylhexyl (meth)acrylate). Examples of (meth)acrylates containing the above reactive functional group include monomers containing at least one of an epoxy group, a hydroxyl group, and a carboxyl group. Specifically, examples of (meth)acrylates containing the above reactive functional group include glycidyl (meth)acrylate, etc. Examples of the above vinyl monomer include styrene, etc.

[0037] For example, the first thermoplastic resin may be a first copolymer produced from an alkyl (meth)acrylate having 1 to 12 carbon atoms, a (meth)acrylate containing an epoxy group, and acrylonitrile.

[0038] The first copolymer may comprise, for example, 30 to 99 wt%, 50 to 97 wt%, or 60 to 95 wt% of repeating units of an alkyl (meth)acrylate having 1 to 12 carbon atoms, based on the total repeating units. The first copolymer may comprise, for example, 0.1 to 30 wt%, 0.1 to 20 wt%, 0.1 to 10 wt%, or 0.1 to 7 wt% of repeating units containing an epoxy group, based on the total repeating units. The first copolymer may comprise, for example, 1 to 60 wt%, 5 to 50 wt%, or 7 to 35 wt% of repeating units of acrylonitrile, based on the total repeating units.

[0039] The weight average molecular weight of the first thermoplastic resin may be 50,000 to 1,000,000 g / mol.

[0040] The glass transition temperature of the first thermoplastic resin may be -10°C or higher, -8°C or higher, or -6°C or higher, and 50°C or lower, 45°C or lower, or 42°C or lower. Within this range, it may be combined with the second thermoplastic resin to make Y in the above formula 1 have a lower value.

[0041] The type of the second thermoplastic resin is not particularly limited, but may include, for example, one or more resins selected from the group consisting of polyimide-based resins, polyether imide-based resins, polyester imide-based resins, polyamide-based resins, polyether sulfone-based resins, polyether ketone-based resins, polyolefin-based resins, polyvinyl chloride-based resins, phenoxy-based resins, butadiene-based rubbers, styrene-butadiene-based rubbers, modified butadiene-based rubbers, reactive butadiene acrylonitrile copolymer rubbers, and (meth)acrylate-based resins.

[0042] As an example, the second thermoplastic resin may include at least one type of resin selected from the group consisting of (meth)acrylate-based resins and phenoxy-based resins.

[0043] The above (meth)acrylate-based resin may be a (co)polymer produced from at least one monomer selected from the group consisting of alkyl (meth)acrylates having 1 to 12 carbon atoms, (meth)acrylates containing a reactive functional group, acrylonitrile, and vinyl monomers polymerizable therewith. Examples of the above alkyl (meth)acrylates having 1 to 12 carbon atoms include ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, or octyl (meth)acrylate (ethylhexyl (meth)acrylate). Examples of the above (meth)acrylate containing a reactive functional group include monomers containing at least one of an epoxy group, a hydroxyl group, and a carboxyl group. Specifically, examples of the (meth)acrylate containing the reactive functional group include glycidyl (meth)acrylate, etc. Examples of the vinyl monomer include styrene, etc.

[0044] For example, the second thermoplastic resin may be a second copolymer produced from an alkyl (meth)acrylate having 1 to 12 carbon atoms, a (meth)acrylate containing an epoxy group, acrylonitrile, and styrene.

[0045] The second copolymer may comprise, for example, 20 to 60 wt% or 30 to 50 wt% of repeating units of an alkyl (meth)acrylate having 1 to 12 carbon atoms based on the total repeating units. The second copolymer may comprise, for example, 0.1 to 30 wt%, 0.1 to 20 wt%, 0.1 to 10 wt% or 0.1 to 7 wt% of repeating units containing an epoxy group based on the total repeating units. The second copolymer may comprise, for example, 5 to 60 wt%, 10 to 50 wt% or 20 to 40 wt% of repeating units of acrylonitrile based on the total repeating units. The second copolymer may comprise 5 to 50 wt%, 10 to 40 wt% or 20 to 30 wt% of repeating units of styrene.

[0046] As another example, the second thermoplastic resin may be a phenoxy resin such as a bisphenol A type phenoxy resin, a bisphenol F type phenoxy resin, a bisphenol A / F type phenoxy resin, or a fluorene type phenoxy resin. Commercially available phenoxy resins include YP-50 (Kukdo Chemical).

[0047] The weight average molecular weight of the second thermoplastic resin may be 10,000 to 1,000,000 g / mol.

[0048] The glass transition temperature of the second thermoplastic resin may be greater than 50°C, greater than 55°C, or greater than 60°C, but less than or equal to 100°C, less than or equal to 90°C, less than or equal to 85°C, less than or equal to 80°C, less than or equal to 75°C, or less than or equal to 70°C. Within this range, it may be combined with the first thermoplastic resin to make Y in the above formula 1 have a lower value.

[0049] The thermoplastic resin may be included in an amount of 1 to 30 wt% based on the total solid content of the adhesive layer. Specifically, the thermoplastic resin may be included in an amount of 1 wt% or more, 3 wt% or more, 5 wt% or more, or 7 wt% or more, and 30 wt% or less, 20 wt% or less, 15 wt% or less, or 12 wt% or less based on the total solid content of the adhesive layer. Within this range, it is advantageous to provide an adhesive layer capable of embedding a semiconductor element without generating voids in a semiconductor manufacturing process.

[0050] The first and second thermoplastic resins may be included in a weight ratio of 1:10 to 1:0.1, 1:5 to 1:0.2, 1:2 to 1:0.5, or 1:1.2 to 1:0.8. Within this range, it is advantageous to provide an adhesive layer in which Y in the above formula 1 is 3 or less.

[0051] The above thermosetting resin can exhibit heat resistance or mechanical strength by reacting with a curing agent.

[0052] The thermosetting resin may include an epoxy resin. The type of the epoxy resin is not particularly limited, but may include at least one resin selected from the group consisting of cresol novolac epoxy resin, bisphenol F-type epoxy resin, bisphenol F-type novolac epoxy resin, bisphenol A-type epoxy resin, bisphenol A-type novolac epoxy resin, phenol novolac epoxy resin, tetrafunctional epoxy resin, biphenyl-type epoxy resin, biphenyl-type novolac epoxy resin, triphenol methane-type epoxy resin, alkyl-modified triphenol methane-type epoxy resin, naphthalene-type epoxy resin, dicyclopentadiene-type epoxy resin, dicyclopentadiene-modified phenol-type epoxy resin, glycidylamine-type epoxy resin, and cycloaliphatic epoxy resin.

[0053] The above thermosetting resin may include a liquid epoxy resin and a solid epoxy resin. In this case, the degree of curing of the adhesive layer can be easily controlled, thereby further improving adhesive performance. In addition, it is advantageous for the resin to have appropriate fluidity, such that Y in the above formula 1 has a value of 3 or less.

[0054] The properties of the above liquid epoxy resin are not particularly limited, but for example, it may have a viscosity of 500 mPa·s to 20,000 mPa·s at 25°C. The above liquid epoxy resin may have an epoxy equivalent of 100 to 1000 g / eq.

[0055] The above-mentioned solid epoxy resin has no particular limitations in its physical properties, but may have, for example, a softening point of 50°C to 120°C. The above-mentioned solid epoxy resin may have an epoxy equivalent of 100 to 1000 g / eq.

[0056] The thermosetting resin may be included in an amount of 5 to 50 wt% based on the total solid content of the adhesive layer. Specifically, the thermosetting resin may be included in an amount of 5 wt% or more, 10 wt% or more, or 15 wt% or more, and 50 wt% or less, 40 wt% or less, or 35 wt% or less based on the total solid content of the adhesive layer. Within this range, it is advantageous to provide an adhesive layer capable of embedding a semiconductor element without generating voids in a semiconductor manufacturing process.

[0057] The above liquid epoxy resin and solid epoxy resin may be included in a weight ratio of 1:10 to 1:0.1, 1:5 to 1:0.2, 1:2 to 1:0.5, or 1:2 to 1:1.2. Within this range, the adhesive layer has sufficient adhesion to the semiconductor element, and it is advantageous to provide an adhesive layer in which Y in the above formula 1 is 3 or less.

[0058] The type of the above-mentioned curing agent is not particularly limited, but may include, for example, at least one of an amine compound, an acid anhydride compound, an amide compound, and a phenol compound. Specifically, the amine compound may be at least one selected from the group consisting of diaminodiphenylmethane, diethylenetriamine, triethylenetriamine, diaminodiphenylsulfone, and isophoronediamine. The acid anhydride compound may be at least one selected from the group consisting of phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride. The amide compound may be a polyamide resin synthesized from dicyandiamide, a dimer of linolenic acid, and ethylenediamine. The above phenolic compound may be a polyhydric phenol such as bisphenol A, bisphenol F, bisphenol S, fluorenebisphenol, terpene diphenol, etc.; a phenol resin obtained by condensation of a phenol and an aldehyde, ketone, diene, etc.; a phenol and / or a modified product of a phenol resin; a halogenated phenol such as tetrabromobisphenol A, a brominated phenol resin, etc.; other imidazoles, BF3-amine complexes, guanidine derivatives. By selecting the curing agent from the above, the degree of curing of the thermosetting resin can be controlled while improving the mechanical properties of the adhesive.

[0059] As an example, the curing agent may include a phenolic compound. The phenolic compound may have a softening point of 60°C or higher, 80°C or higher, or 100°C or higher, but 160°C or lower or 150°C or lower. A phenolic compound having a softening point within this range can enable the adhesive layer to have a higher tensile modulus at room temperature and provide flow characteristics advantageous for embedding semiconductor devices.

[0060] The curing agent may be included in an amount of 1 to 30 wt% based on the total solid content of the adhesive layer. Specifically, the curing agent may be included in an amount of 1 wt% or more, 5 wt% or more, or 10 wt% or more, and 30 wt% or less, 25 wt% or less, or 20 wt% or less based on the total solid content of the adhesive layer. Within this range, the phenomenon of the adhesive layer flowing away during the semiconductor manufacturing process can be prevented, and the occurrence of voids can be effectively prevented.

[0061] The type of the above-mentioned inorganic filler is not particularly limited, but may include, for example, one or more selected from the group consisting of silica, titanium dioxide, aluminum hydroxide, calcium carbonate, magnesium hydroxide, aluminum oxide, talc, and aluminum nitride. By using the above-mentioned type of inorganic filler, the adhesive strength of the adhesive layer can be improved and cracks in the semiconductor package can be prevented.

[0062] The average particle diameter of the above-mentioned inorganic filler may be 0.03 ㎛ to 3 ㎛. Specifically, the average particle diameter of the above-mentioned inorganic filler may be 0.04 ㎛ or more or 0.05 ㎛ or more and 2.5 ㎛ or less or 2 ㎛ or less. When the average particle diameter of the above-mentioned inorganic filler is within the above-mentioned range, the dispersion degree of the inorganic filler within the adhesive layer can be improved.

[0063] The above-mentioned inorganic filler may be included in an amount of 20 to 60 wt% based on the total solid content of the adhesive layer. Specifically, the above-mentioned inorganic filler may be included in an amount of 20 wt% or more, 30 wt% or more, or 35 wt% or more, and 60 wt% or less, 55 wt% or less, or 50 wt% or less based on the total solid content of the adhesive layer. Within this range, the mechanical properties of the adhesive layer can be improved, and the mismatch in thermal expansion coefficient with the semiconductor chip can be reduced, thereby improving reliability.

[0064] The above adhesive layer may additionally include a curing catalyst. Specifically, the curing catalyst may be one selected from the group consisting of phosphorus compounds, boron compounds, phosphorus-boron compounds, imidazole compounds, and combinations thereof, but is not limited thereto. By using the curing catalyst, the action of the curing agent or the curing of the adhesive layer can be promoted. In addition, the amount of the curing catalyst used may be appropriately selected in consideration of the physical properties of the adhesive layer to be finally manufactured.

[0065] The adhesive layer may further include known additives as needed. For example, the adhesive layer may further include a coupling agent, a leveling agent, a dispersing agent, or a combination thereof.

[0066] The thickness of the adhesive layer may vary depending on the height of the semiconductor device to which the non-conductive film is to be applied. As a non-limiting example, the thickness of the adhesive layer may be controlled to be 1 μm or more or 5 μm or more and 500 μm or less, 100 μm or less or 50 μm or less.

[0067] Meanwhile, according to another embodiment of the invention, a semiconductor device is provided, comprising a non-conductive film and a semiconductor element, wherein the semiconductor element is embedded by the adhesive layer. The non-conductive film may be a non-conductive film according to the embodiment.

[0068] The semiconductor device is not particularly limited in type, but may include, for example, a bump that can be used in a flip chip mounting method.

[0069] The semiconductor device of the above-described other embodiment can be manufactured by forming an adhesive layer on a bump formation surface of a semiconductor element or attaching an adhesive layer, performing a dicing process as needed, mounting the semiconductor element at a location to be connected, and simultaneously performing metal bonding and sealing using a thermocompression bonding method.

[0070] As described above, the adhesive layer can effectively fill fine-pitch electrodes without easily generating voids even when applied to a thermocompression bonding method since Y calculated by the above formula 1 has a value of 3 or less, thereby providing a semiconductor device with excellent reliability.

[0071] Meanwhile, according to another embodiment of the invention, a method for manufacturing a semiconductor device is provided, comprising: a step of calculating Y of the above formula 1 for a non-conductive film including an adhesive layer and selecting an adhesive layer in which Y is greater than 0 and less than or equal to 3; and a step of applying the selected non-conductive film to a device formation surface of a semiconductor device.

[0072] As described above, when a non-conductive film including an adhesive layer in which Y calculated by the above formula 1 is 3 or less is used in a semiconductor manufacturing process, a semiconductor device having excellent reliability can be provided by effectively filling fine-pitch electrodes without easily generating voids.

[0073] In the above method for manufacturing a semiconductor device, Y of the above formula 1 is calculated before the manufacturing process of the semiconductor device to predict in advance whether a void will occur in the non-conductive film, and a non-conductive film that is unlikely to cause voids can be selected and applied to the semiconductor manufacturing process.

[0074] In one example, in the method for manufacturing the semiconductor device, a non-conductive film may be prepared in the form of a die-bonding film in which an adhesive layer is laminated on a substrate, or a dicing die-bonding film in which an adhesive layer and an adhesive layer are sequentially laminated on a substrate. Then, an adhesive layer is attached to the element formation surface of a semiconductor element, and if the non-conductive film is a dicing die-bonding film, after a dicing process, it is mounted at a location where a semiconductor element is to be connected, and metal bonding and sealing are simultaneously performed by a thermocompression bonding method, thereby manufacturing a semiconductor device.

[0075] In another example, in the method for manufacturing the semiconductor device, the aforementioned adhesive layer may be formed on the element formation surface of the semiconductor element to form a non-conductive film. Then, after a dicing process as needed, the semiconductor element may be mounted at the location to be connected, and metal bonding and sealing may be performed simultaneously using a thermocompression bonding method to manufacture the semiconductor device.

[0076] The conditions of the above thermocompression bonding process are not particularly limited. As an example, the thermocompression bonding process may be performed by applying a pressure of 30 to 150 N for 2 to 10 seconds at a temperature of about 50°C to 150°C, and then heating for 2 to 10 seconds at a temperature of about 200°C to 300°C.

[0077] The non-conductive film used in the method for manufacturing the above semiconductor device is selected as one that does not easily generate voids through the above formula 1, so even if it undergoes a thermocompression bonding process under the above conditions, voids are not easily generated, and thus a semiconductor device with excellent reliability can be provided.

[0078] A non-conductive film according to an embodiment can effectively prevent void generation during a semiconductor manufacturing process and sufficiently adhere to a semiconductor element to provide a semiconductor device with excellent reliability.

[0079] The following specific examples of the invention will further illustrate its functions and effects. However, these examples are presented as illustrative examples and do not limit the scope of the invention in any way.

[0080]

[0081] Manufacturing Example 1: Manufacturing of thermoplastic resin

[0082] 59 g of n-butyl acrylate, 10 g of acrylonitrile, 3 g of glycidyl methacrylate, and 28 g of isobutyl methacrylate were added to 100 g of toluene. Thereafter, the obtained reactants were reacted at 80°C for approximately 12 hours to synthesize an acrylate resin (weight average molecular weight of approximately 500,000, glass transition temperature of -5°C) having a glycidyl group introduced therein.

[0083]

[0084] Manufacturing Example 2: Manufacturing of thermoplastic resin

[0085] 40 g of n-butyl acrylate, 25 g of ethyl acrylate, 30 g of acrylonitrile, and 5 g of glycidyl methacrylate were added to 100 g of toluene. Thereafter, the resulting reactants were reacted at 80°C for approximately 12 hours to synthesize an acrylate resin (weight average molecular weight of approximately 500,000, glass transition temperature of 40°C) to which a glycidyl group was introduced.

[0086]

[0087] Manufacturing Example 3: Manufacturing of thermoplastic resin

[0088] 40 g of butyl acrylate, 30 g of acrylonitrile, 5 g of glycidyl methacrylate, and 25 g of styrene were added to 100 g of toluene. Afterwards, the resulting reactants were reacted at 80°C for approximately 12 hours to synthesize an acrylate resin (weight average molecular weight of approximately 700,000, glass transition temperature of 63°C) to which a glycidyl group was introduced.

[0089]

[0090] Manufacturing Example 4: Manufacturing of thermoplastic resin

[0091] A thermoplastic resin was prepared by dissolving 35 g of phenoxy resin (Kukdo Chemical YP-50, weight average molecular weight approximately 55,000, glass transition temperature 80-83 ℃) in 65 g of toluene.

[0092]

[0093] Example 1: Fabrication of non-conductive films and semiconductor devices

[0094] (1) Preparation of adhesive composition

[0095] The components listed in Table 1 below were added to methyl ethyl ketone in the amounts listed in Table 1 below and mixed to prepare an adhesive composition (solid content 50 wt%).

[0096]

[0097] (2) Manufacturing of non-conductive film

[0098] The above adhesive composition was applied onto a polyethylene terephthalate film (thickness 38 ㎛) that had been released using a comma coater, and then dried at 110°C for 3 minutes to form a B-phase adhesive layer having a thickness of about 20 ㎛.

[0099]

[0100] (3) Manufacturing of semiconductor devices

[0101] A semiconductor device was prepared in which a plurality of silicon through-hole electrodes were formed with lead-free solder (SnAgCu) to a height of 3 ㎛ on a copper pillar having a height of 15 ㎛ and a pitch of 50 ㎛ as bumps.

[0102] After positioning the adhesive layer of the non-conductive film so that it touches the surface where the bump of the semiconductor element is formed, vacuum lamination was performed at 80°C. Then, the polyethylene terephthalate film was peeled off from the adhesive layer.

[0103] Thereafter, the substrate and the semiconductor element were arranged so that the bumps of the semiconductor element were positioned on the connection pads of the substrate having connection pads with a pitch of 50 μm. Then, using a thermocompression bonder, the laminate of the substrate and the semiconductor element was pressed at 70°C for 3 seconds with 100 N, and then heated to 260°C for 4 seconds to perform thermocompression bonding.

[0104]

[0105] Examples 2 to 4 and Comparative Examples 1 to 3: Preparation of non-conductive films and semiconductor devices

[0106] An adhesive composition, a non-conductive film, and a semiconductor device were manufactured in the same manner as in Example 1, except that the composition of the adhesive composition of Example 1 was changed as described in Table 1 below.

[0107] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Thermoplastic resin Manufacturing Example 155105 Manufacturing Example 255105 Manufacturing Example 355 Manufacturing Example 455 Thermosetting resin RE-310S10101010101010EOCN-1020-701515151515151515 Curing agent KA-116515151515151515GPH-10315 Inorganic filler SC-205045454545454545 Curing catalyst 2P4MHZ4444444 Coupling agent KBM-4031111111

[0108] The contents (weight parts) in Table 1 above are the solid content.

[0109] RE-310S: Liquid epoxy resin (Japan Explosives, bisphenol A type epoxy resin, epoxy equivalent 180 g / eq)

[0110] EOCN-1020-70: Solid epoxy resin (Japan Explosives, cresol novolac type epoxy resin, epoxy equivalent 199 g / eq, softening point: 70℃)

[0111] KA-1165: Phenolic resin (DIC product, bisphenol A novolac resin, hydroxyl equivalent 119 g / eq, softening point: 125 ℃)

[0112] GPH-103: Phenol resin (Japanese gunpowder, hydroxyl equivalent 230 g / eq, softening point: 103 ℃)

[0113] SC-2050: Spherical silica, Admatec, average particle size approximately 400 nm

[0114] 2P4MHZ: 2-phenyl-4-methyl-5-hydroxymethylimidazole

[0115] KBM-403: Silane coupling agent (Shin-Etsu, 3,3-glycidoxypropyl trimethoxysilane)

[0116]

[0117] Test Example: Evaluation of the properties of non-conductive films and the performance of semiconductor devices.

[0118] (1) Difference between the onset temperature and maximum temperature of heating of the adhesive layer (△T)

[0119] The onset and peak exothermic temperatures of the adhesive layer were determined using differential scanning calorimetry (DSC). DSC analysis was performed at a heating rate of 10°C / min and over a temperature range from 30°C to 300°C.

[0120] The DSC analysis results yielded a thermogram, where the horizontal axis represents temperature and the vertical axis represents heat flow. The onset of the exothermic peak in the thermogram was defined as the exothermic onset temperature, and the apex of the exothermic peak was defined as the maximum exothermic temperature.

[0121]

[0122] (2) Gel time (G) of the adhesive layer

[0123] The gel time of the B-phase adhesive layer was measured on a hot plate at 200°C. Specifically, the adhesive layers were overlapped and laminated until the thickness reached 120 μm, and then pressed using a roll laminator at 60°C. The test pieces thus obtained were cut into circles with a diameter of 10 mm. The cut test pieces were placed on a 200°C hot plate and stirred with a stirring rod so that small circles were drawn on the surface of the test pieces. The stirring was continued until the viscosity of the test piece increased and it finally gelled and lost fluidity. The time from the time the test piece was placed on the hot plate until the test piece gelled and lost fluidity was measured in seconds. These measurements were performed twice, and if the difference between the two measurements was within 10% of the lower value of the measurements, the gel time was recorded as the average of the two measurements. If the difference exceeded 10%, the measurements were performed three times, and the gel time was recorded as the average of the three measurements.

[0124]

[0125] (3) Minimum melting viscosity (η) of the adhesive layer

[0126] The adhesive layers were overlapped and laminated until the thickness reached 400 ㎛, and then pressed using a roll laminator at 60 ℃. The test pieces obtained in this way were cut into circles with a diameter of 20 mm. The viscosity of the cut test pieces was measured using MARS equipment from HAKKE under the conditions of 1000 Pa and a heating rate of 10 ℃ / min. The lowest viscosity value among the measured viscosity values ​​was defined as the minimum melting viscosity.

[0127]

[0128] (4) Mold Void Test

[0129] Using IR MicroScope, a void that appears between a semiconductor element and a substrate occupies less than 3% of the area was evaluated as pass (○), and a void that exceeded 3% was evaluated as fail (×).

[0130]

[0131] (5) Overall evaluation

[0132] For semiconductor devices, those that could confirm daisy chain connection were evaluated as pass (○), and those that could not confirm daisy chain connection were evaluated as fail (×).

[0133]

[0134] (6) Connection status evaluation

[0135] The cross-section of the connection part of the semiconductor device was polished to expose it, and the cross-section of the exposed connection part was observed under an optical microscope. If no trapping of the adhesive composition was observed at the connection part and the solder was sufficiently wetted to the wiring, it was evaluated as pass (○), and if not, it was evaluated as fail (×).

[0136]

[0137] (7) Fillet void evaluation

[0138] After connecting a semiconductor device using a thermocompression bonding process, the fillet formed at the edge of the semiconductor element was checked using an IR Microscope. If there was no void with a diameter of 1 ㎛ or more in the fillet, it was evaluated as pass (○), and if there was a void with a diameter of 1 ㎛ or more, it was evaluated as fail (×).

[0139]

[0140] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Non-conductive film △T (℃) 8888888 G (sec) 7.5 8.17 88.08 28.7 8.4 η (Pa·s) 480 4106 10450 180 240 210 Y 1.28 1.74 1.09 1.55 4.07 3.43 3.66 Semiconductor device Void evaluation ○○○○××× Conductivity evaluation ○○○○××× Connection status evaluation ○○○○××× Fillet void evaluation ○○○○×××

[0141] In the above Table 2, Y is a value calculated by the above-described Equation 1.

[0142]

[0143] Referring to Table 2 above, in the cases of Examples 1 to 4 where Y calculated by Equation 1 is 3 or less, it is confirmed that voids are prevented from being formed between the substrate and the semiconductor element or in the fillet formed at the edge of the semiconductor element, thereby providing a semiconductor device having excellent metal connection. In contrast, in the cases of Comparative Examples 1 to 3 where Y calculated by Equation 1 exceeds 3, it is confirmed that voids are formed between the substrate and the semiconductor element and in the fillet formed at the edge of the semiconductor element, resulting in poor metal connection.

Claims

1. Contains thermoplastic resin, thermosetting resin, curing agent and inorganic filler, A non-conductive film comprising an adhesive layer in which Y of the following formula 1 is greater than 0 and less than or equal to 3: [Formula 1] Y = (△T * G) 2 / (5.88 * h) In the above equation 1, △T is the difference between the onset temperature of exotherm and the maximum temperature of exotherm of the adhesive layer measured at a heating rate of 10 ℃ / min and from 30 ℃ to 300 ℃ using differential scanning calorimetry, G is the gelation time at 200 ℃ measured in seconds for the adhesive layer, and η is the minimum melting viscosity measured in units of Pa·s for the adhesive layer.

2. A non-conductive film in the first paragraph, wherein △T of the above formula 1 is 1°C to 20°C.

3. A non-conductive film in the first paragraph, wherein G in the above formula 1 is 5 seconds to 30 seconds.

4. A non-conductive film in the first paragraph, wherein η in the above formula 1 is 10 Pa·s to 5000 Pa·s.

5. A non-conductive film according to claim 1, wherein the thermoplastic resin comprises two or more types of thermoplastic resins having different glass transition temperatures.

6. A non-conductive film according to claim 1, wherein the thermoplastic resin comprises a first thermoplastic resin having a glass transition temperature of -10°C to 50°C and a second thermoplastic resin having a glass transition temperature of more than 50°C and less than or equal to 100°C.

7. A non-conductive film according to claim 6, wherein the first thermoplastic resin comprises a first copolymer produced from an alkyl (meth)acrylate having 1 to 12 carbon atoms, a (meth)acrylate containing an epoxy group, and acrylonitrile.

8. A non-conductive film according to claim 6, wherein the second thermoplastic resin comprises a second copolymer produced from an alkyl (meth)acrylate having 1 to 12 carbon atoms, a (meth)acrylate containing an epoxy group, acrylonitrile, and styrene; or at least one phenoxy resin selected from the group consisting of a bisphenol A type phenoxy resin, a bisphenol F type phenoxy resin, a bisphenol A / F type phenoxy resin, and a fluorene type phenoxy resin.

9. A non-conductive film according to claim 6, wherein the first and second thermoplastic resins are included in a weight ratio of 1:10 to 1:0.

1.

10. A non-conductive film according to claim 1, wherein the thermosetting resin comprises a liquid epoxy resin and a solid epoxy resin.

11. Including the non-conductive film and semiconductor element of Article 1, A semiconductor device, wherein the semiconductor element is embedded by the adhesive layer.

12. A semiconductor device according to claim 11, wherein the semiconductor element includes a bump.

13. A step of calculating Y of the following formula 1 for a non-conductive film including an adhesive layer and selecting one including an adhesive layer in which Y is greater than 0 and less than or equal to 3; and A method for manufacturing a semiconductor device, comprising the step of applying a selected non-conductive film to a device formation surface of a semiconductor device: [Formula 1] Y = (△T * G) 2 / (5.88 * h) In the above equation 1, △T is the difference between the onset temperature of exotherm and the maximum temperature of exotherm of the adhesive layer measured at a heating rate of 10 ℃ / min and from 30 ℃ to 300 ℃ using differential scanning calorimetry, G is the gelation time at 200 ℃ measured in seconds for the adhesive layer, and η is the minimum melting viscosity measured in units of Pa·s for the adhesive layer.

Citation Information

Patent Citations

  • Adhesive film, adhesive sheet, semiconductor device and method of producing semiconductor device

    JP2010001453A

  • Composition for non-conductive adhesive film and non-conductive adhesive film comprising same

    KR101435758B1

  • Submersible pump with automatic desorption device

    KR102345833B1

  • Acrylic copolymer composition and adhesive coatings therefrom

    US4975484A

  • KR20200020666A