Method for manufacturing high-chromium (CR) molten steel, method for manufacturing cast piece, and method for manufacturing press roll
The converter process with controlled oxygen and chromium management, along with magnetic field-assisted casting and forging, addresses segregation and hardness issues in high chromium (Cr) molten steel and rolling rolls, resulting in a more efficient and cost-effective production of high-quality rolling rolls.
Patent Information
- Application Number
- PCT/KR2024/001910
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-02-08
- Publication Date
- 2024-10-24
AI Technical Summary
The existing methods for manufacturing high chromium (Cr) molten steel and rolling rolls face challenges such as uneven texture, cracking, and low hardness due to segregation issues, which are costly and time-consuming to address, particularly in the ESR method.
A method involving a converter process that includes oxygen blowing, deoxidation, and chromium oxide reduction to control chromium content, combined with magnetic field-assisted casting and controlled heating and forging to produce high chromium (Cr) molten steel and rolling rolls with uniform structure and high hardness.
This method effectively suppresses segregation, prevents cracking, and achieves high hardness in rolling rolls while simplifying the process and reducing costs compared to traditional methods.
Smart Images

Figure KR2024001910_24102024_PF_FP_ABST
Abstract
Description
Method for manufacturing high chromium (CR) molten steel, method for manufacturing cast steel, and method for manufacturing rolling rolls
[0001] The present invention relates to a method for manufacturing high chromium (Cr) molten steel, a method for manufacturing cast steel, and a method for manufacturing rolling rolls, and more particularly, to a method for manufacturing high chromium (Cr) molten steel, a method for manufacturing cast steel, and a method for manufacturing rolling rolls, which can efficiently manufacture high chromium (Cr) molten steel and suppress or prevent segregation in a simple and low-cost manner.
[0002] Rolling rolls are a type of steel with a high chromium (Cr) content. They are manufactured by solidifying molten steel to produce ingots and forging the ingots. More specifically, molten steel with a high chromium (Cr) content is first manufactured, solidified, and then ingots are manufactured. Then, the ingots are forged and shaped to produce rolling rolls. However, when the ingots are forged as is, there are problems such as uneven rolling roll structure, cracks, and low hardness due to segregation within the ingot. Therefore, before forging the ingot, the segregation contained in the ingot is removed using the Electro Slag Remelting (ESR) method. The ESR method involves first manufacturing an electrode using the manufactured ingot. Then, an arc is generated using the manufactured electrode to remelt the electrode. At this time, the molten steel formed by remelting the electrode rod is dropped in the form of droplets and solidified to form an ingot again. At this time, by dropping the molten steel formed by remelting in the form of droplets, an ingot with minimal segregation can be produced.
[0003] However, the ESR method requires the steps of manufacturing the ingots as described above into electrode rods, remelting the electrode rods, and then loading the remelted molten steel into the ingots for resolidification. In other words, the process requires multiple steps. Consequently, the time and cost involved in suppressing segregation pose significant challenges.
[0004] (Prior art document) (Patent document 1) Korean registered patent KR 10-1346636
[0005] The present invention provides a method for producing high chromium (Cr) molten steel using a furnace, which can produce high chromium (Cr) molten steel without contaminating the furnace.
[0006] The present invention provides a method for manufacturing a cast iron and a method for manufacturing a rolling roll, which can simplify a process for suppressing or preventing segregation and reduce costs.
[0007] The present invention provides a method for manufacturing a cast steel having high hardness and a method for manufacturing a rolling roll, which can suppress or prevent the occurrence of cracks, can uniformize the structure, and has high hardness.
[0008] An embodiment of the present invention is a method for manufacturing high chromium (Cr) molten steel having a chromium (Cr) content of 4.5 wt% to 5.5 wt%, the method including: a process of charging molten steel into a converter used in a stainless steel manufacturing process; and a process of charging a chromium alloy containing chromium (Cr) into the converter so that the chromium (Cr) content in the molten steel becomes 4.5 wt% to 5.5 wt%.
[0009] A method for manufacturing high chromium (Cr) molten steel according to an embodiment of the present invention may include an oxygen blowing process for removing carbon (C) from molten steel by introducing oxygen into the inside of the converter into which chromium alloy iron is introduced; a process for removing oxygen (O) from the molten steel by introducing a deoxidizer into the converter; and a process for reducing chromium oxide contained in slag floating on the surface of the molten steel to chromium (Cr) by introducing a reducing agent into the converter.
[0010] A method for manufacturing high chromium (Cr) molten steel according to an embodiment of the present invention may include a process of drawing molten steel from the above furnace into a ladle; and a temperature control process of heating the molten steel drawn into the ladle using a ladle furnace (LF), which is a heating device used in a carbon steelmaking process.
[0011] In the above temperature control process, it is preferable to control the temperature of the molten steel to 1560°C to 1600°C.
[0012] A method for manufacturing high chromium (Cr) molten steel according to an embodiment of the present invention includes a degassing process for removing hydrogen (H2) and nitrogen (N2) from molten steel received in the ladle using a RH (Rheinstaal Huttenwerke und Heraus) device, which is a vacuum treatment device used in a carbon steelmaking process, and the degassing process can be performed after the temperature control process is completed.
[0013] When discharging the molten steel from the above furnace into a ladle, it is preferable to dischar it into a ladle used in a carbon steelmaking process.
[0014] A method for manufacturing a cast steel according to an embodiment of the present invention may include a process for preparing molten steel containing 4.5 wt% to 5.5 wt% of chromium (Cr); a casting process for supplying the molten steel to a mold of a casting device and solidifying the molten steel inside the mold to manufacture a cast steel including unsolidified molten steel; a process for drawing the cast steel produced in the casting process to the lower side of the mold; and a solidification process for applying a magnetic field to the cast steel drawn to the lower side of the mold to cause the unsolidified molten steel contained in the cast steel to flow and solidify, thereby manufacturing the cast steel.
[0015] The above solidification process may include a process of heating the end portion of the cast piece drawn toward the lower side of the mold.
[0016] The above casting process may include a process of applying a magnetic field to the mold to cause molten steel inside the mold to flow.
[0017]
[0018] When drawing the cast iron to the lower side of the mold, it is preferable to draw it at a speed of 0.04 m / min or less.
[0019] The above solidification process includes a process of spraying cooling water onto the cast piece drawn from the lower side of the mold, and when spraying the cooling water onto the cast piece, it is preferable to spray the cooling water so that the surface temperature of the cast piece becomes 800°C to 900°C.
[0020] In the above drawing process, it is preferable to draw the cast from the mold so that it is perpendicular to the ground, and in the solidification process, it is preferable to solidify the cast so that it is positioned so that it is perpendicular to the ground.
[0021] A method for manufacturing a rolling roll according to an embodiment of the present invention includes a process of heating a cast iron; a process of forging the heated cast iron into a shape of a rolling roll; a process of heating the rolling roll manufactured in the forming process to remove hydrogen (H2) from the rolling roll; and the process of heating the cast iron may include a process of heating the cast iron by increasing the temperature of the cast iron in a plurality of stages to a target temperature.
[0022] The process of heating the cast to the target temperature may include a process of heating the cast to a first temperature of 250°C to 350°C; a process of heating the cast to a second temperature of 450°C to 550°C; a process of heating the cast to a third temperature of 650°C to 750°C; and a process of heating the cast to the target temperature of 1100°C to 1250°C.
[0023] In heating the cast to the first to third temperatures and the target temperature, the cast may be maintained at the first temperature for 3 to 5 hours, the cast may be maintained at the second temperature for 5 to 7 hours, the cast may be maintained at the third temperature for 3 to 5 hours, and the cast may be maintained at the target temperature for 14 to 18 hours.
[0024] In forging the above cast iron, the cast iron heated to a temperature of 1100°C to 1250°C is pressed and forged, and the cast iron can be pressed so that the thickness of the cast iron is reduced by 250 mm to 350 mm each time the cast iron is pressed using a pressing device.
[0025] In removing hydrogen (H2) from the above rolling roll, a process of heating the rolling roll to a temperature of 200°C to 400°C may be included.
[0026] When heating the rolling roll to a temperature of 200°C to 400°C, it is preferable to heat for 48 hours or more.
[0027] According to embodiments of the present invention, high-chromium (Cr) molten steel can be produced using a converter used for steelmaking other types of steel without contaminating the converter used for steelmaking other types of steel. Furthermore, when heating the high-chromium (Cr) molten steel or performing degassing to discharge gas, the temperature of the molten steel can be effectively increased, and the degassing efficiency can be improved.
[0028] In addition, compared to conventional methods, it is possible to suppress or prevent the occurrence of segregation within a cast steel in a simpler and less costly manner. Furthermore, when manufacturing a rolling roll by forging a cast steel, it is possible to manufacture a rolling roll in which the occurrence of cracks is suppressed or prevented, and which has a uniform structure and high hardness.
[0029] Figure 1 is a flowchart showing a method for manufacturing a rolling roll according to an embodiment of the present invention.
[0030] Figures 2 (a) to (g) are process diagrams sequentially showing the molten steel preparation process according to an embodiment of the present invention.
[0031] Figures 3 (a) to (d) are drawings sequentially showing the operation of a casting device according to an embodiment of the present invention.
[0032] Figures 4 (a) to (c) are process diagrams sequentially showing a method for manufacturing a rolling roll using a cast iron manufactured by a method according to an embodiment of the present invention.
[0033] Figures 5 (a) and (b) show the results of cutting a cross-section of a rolling roll and etching the cross-section to check whether or not coarse segregation occurred.
[0034] Hereinafter, embodiments of the present invention will be described in more detail with reference to the attached drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. To illustrate the embodiments of the present invention, the drawings may be exaggerated, and like reference numerals in the drawings represent like components.
[0035]
[0036] Figure 1 is a flowchart showing a method for manufacturing a rolling roll according to an embodiment of the present invention.
[0037] Referring to Fig. 1, a method for manufacturing a rolling roll includes a process of preparing molten steel (S100), a process of solidifying the molten steel to manufacture a cast steel sheet (S200), a process of heating the cast steel (S300), a process of forging the heated cast steel to manufacture a rolling roll (S400), and a process of heating the rolling roll (S500).
[0038] The rolling roll is a ferroalloy containing a high content of chromium (Cr). More specifically, the rolling roll is a high chromium (Cr) alloy containing a high content of chromium (Cr) of 4.5 wt% to 5.5 wt% throughout the entire rolling roll. To be more specific, the rolling roll contains, in its entirety, 4.5 wt% to 5.5 wt% of chromium (Cr), 0.75 wt% to 0.95 wt% of carbon (C), 0.2 wt% to 0.5 wt% of silicon (Si), 0.2 wt% to 0.5 wt% of manganese (Mn), 0.4 wt% to 0.65 wt% of molybdenum (Mo), 0.5 wt% or less (0 wt% or more) of nickel (Ni), 0.2 wt% or less (0 wt% or more) of copper (Cu), 0.0025 wt% or less (0 wt% or more) of phosphorus (P), 0.015 wt% or less (0 wt% or more) of sulfur (S), and iron (Fe) as the remainder content (91.16 wt% to It is an alloy iron containing 93.15 wt%).
[0039] The purpose of controlling the chromium (Cr) content of the entire rolling roll to 4.5 wt% to 5.5 wt% and the carbon (C) content to 0.75 wt% to 0.95 wt% is to secure hardness and processability. For example, if the chromium (Cr) content of the rolling roll is less than 4.5 wt% or the carbon (C) content is less than 0.75 wt%, the hardness of the rolling roll may be low. Conversely, if the chromium (Cr) content of the rolling roll exceeds 5.5 wt% or the carbon (C) content exceeds 0.95 wt%, the processability of the rolling roll is low, and processing the manufactured rolling roll may be difficult when processing it as needed.
[0040] In addition, the purpose of controlling the phosphorus (P) content in the rolling rolls to 0.025 wt% or less and the sulfur (S) content to 0.015 wt% or less is to make the structure of the rolling rolls uniform and to suppress or prevent the occurrence of cracks. That is, when the phosphorus (P) content in the rolling rolls exceeds 0.025 wt% or the sulfur (S) content exceeds 0.015 wt%, the structure may become uneven due to segregation, etc., within the rolling rolls. Accordingly, when pressing a rolling object using the rolling rolls, a problem of cracks occurring in the rolling rolls may occur. Therefore, the phosphorus (P) content in the rolling rolls is controlled to 0.025 wt% or less, and the sulfur (S) content is controlled to 0.015 wt% or less.
[0041] In an embodiment of the present invention, the rolling roll to be manufactured may be a roll applied to a rolling device that applies force to a rolling object, such as a cast iron or steel plate, and rolls it.
[0042] In the process of preparing molten steel (S100), molten steel for manufacturing rolling rolls is prepared. That is, in the process of preparing molten steel (S100), molten steel having the component contents required for rolling rolls is prepared. That is, high chromium (Cr) molten steel having a chromium (Cr) content of 4.5 wt% to 5.5 wt% is prepared. To be more specific, in preparing molten steel, chromium (Cr) is contained in an amount of 4.5 wt% to 5.5 wt%, carbon (C) is contained in an amount of 0.75 wt% to 0.95 wt%, silicon (Si) is contained in an amount of 0.2 wt% to 0.5 wt%, manganese (Mn) is contained in an amount of 0.2 wt% to 0.5 wt%, molybdenum (Mo) is contained in an amount of 0.4 wt% to 0.65 wt%, nickel (Ni) is contained in an amount of 0.5 wt% or less (0 wt% or more), copper (Cu) is contained in an amount of 0.2 wt% or less (0 wt% or more), phosphorus (P) is contained in an amount of 0.0025 wt% or less (0 wt% or more), sulfur (S) is contained in an amount of 0.015 wt% or less (0 wt% or more), and iron (Fe) is contained in an amount of the remainder (91.16 wt% to 91.16 wt%). 93.15 wt%). This can be achieved by sequentially performing each step of the molten steel preparation process described below.
[0043]
[0044] Figures 2 (a) to (g) are process diagrams sequentially showing the molten steel preparation process according to an embodiment of the present invention.
[0045] Referring to FIG. 2, the process (S100) of preparing molten steel (M) may include a process of processing molten steel (M) using a furnace (11) (hereinafter, a furnace processing process (S110)), a process (S120) of expelling molten steel (M) inside the furnace (11) into a ladle (20), a temperature control process (S130) of controlling the temperature of the molten steel (M) expelled into the ladle (20) using a temperature control device (30), and a degassing process (S140) of removing gas from the molten steel (M) using a vacuum treatment device (40).
[0046] The converter treatment process (S110) is a process for adjusting the components of molten steel (M) by charging it into the converter (11). The converter (11) used in the converter treatment process (S110) is a converter used in a steelmaking process (hereinafter, stainless steel steelmaking process) that prepares molten steel for manufacturing stainless steel (hereinafter, molten steel for manufacturing stainless steel). That is, the converter (11) used in the stainless steel steelmaking process is utilized in preparing molten steel according to the embodiment.
[0047] For a more specific explanation, a steelmaking process using a converter among stainless steel manufacturing processes will be briefly described. The stainless steel manufacturing process includes a process of charging molten steel into a converter, a process of introducing a ferroalloy containing chromium (Cr) and a ferroalloy containing nickel (Ni) into the converter, and an oxygen blowing process of removing carbon (C), phosphorus (P), etc. by injecting oxygen into the converter using a lance. When introducing a chromium (Cr) alloy ferroalloy into the converter, the chromium (Cr) content in the molten steel is introduced so as to be 10.5 wt% to 11 wt%. Therefore, the molten steel prepared in the steelmaking process using a converter among stainless steel manufacturing processes contains 10.5 wt% to 11 wt% of chromium.
[0048] For comparison, a steelmaking process using a converter in a steelmaking process (hereinafter, “carbon steel steelmaking process”) that prepares molten steel for manufacturing carbon steel (hereinafter, “molten steel for manufacturing carbon steel”) will be briefly described. The carbon steel steelmaking process includes a process of charging molten steel into a converter and an oxygen annealing process of removing carbon (C) and phosphorus (P) by injecting oxygen into the converter using a lance. Carbon steel is steel with a low chromium (Cr) content. Therefore, in the carbon steel steelmaking process, chromium (Cr) is not introduced into the converter, and the chromium (Cr) content in the molten steel is controlled to be low at 0.1 wt% to 1.0 wt%.
[0049] As described above, in the converter for the stainless steel manufacturing process, molten steel having a high chromium (Cr) content of 10.5 wt% to 11 wt% is prepared. In other words, the inside of the converter used in the stainless steel manufacturing process is filled with molten steel having a high chromium (Cr) content of 10.5 wt% to 11 wt%. However, the inside of the converter used in the carbon steel manufacturing process is filled with molten steel having a low chromium (Cr) content of 0.1 wt% to 1.0 wt%.
[0050] Accordingly, when preparing molten steel for manufacturing rolling rolls having a high chromium (Cr) content of 4.5 wt% to 5.5 wt%, if a converter used in a carbon steelmaking process is used, the converter for manufacturing carbon steel may become contaminated. That is, if molten steel having a high chromium (Cr) content of 4.5 wt% to 5.5 wt% is placed in the converter for manufacturing carbon steel, even if the molten steel is tapped, a large amount of chromium (Cr) may remain inside the converter for manufacturing carbon steel. For example, a large amount of chromium (Cr) may adhere or adhere to the inner wall of the converter for manufacturing carbon steel. As a result, the converter for manufacturing carbon steel becomes contaminated with chromium (Cr). And when a furnace for manufacturing carbon steel containing a large amount of chromium (Cr) is used in a carbon steelmaking process, the molten steel contains a large amount of chromium (Cr), and the chromium (Cr) acts as an impurity that lowers the quality of the carbon steel.
[0051] However, when preparing high chromium (Cr) molten steel having a high chromium (Cr) content of 4.5 wt% to 5.5 wt%, if a converter used in stainless steel manufacturing is used, the converter for manufacturing stainless steel is not contaminated. That is, even if molten steel having a high chromium (Cr) content of 4.5 wt% to 5.5 wt% is put into the converter (11) for manufacturing stainless steel and then tapped, and a large amount of chromium (Cr) remains inside the converter for manufacturing stainless steel, the chromium remaining inside the converter does not act as an impurity. This is because the converter for manufacturing stainless steel is already a means for putting molten steel having a high chromium content of 10.5 wt% to 11 wt%. In addition, the chromium content of the molten steel put into the converter for manufacturing stainless steel is higher than that of the molten steel to be manufactured in the embodiment. Accordingly, even if molten steel for rolling roll manufacturing is placed in a furnace for manufacturing stainless steel, the furnace for manufacturing stainless steel is not contaminated. Accordingly, when molten steel for manufacturing stainless steel is again produced using the furnace for manufacturing stainless steel that was previously placed therein, no problem occurs due to the chromium (Cr) in the molten steel previously placed therein.
[0052] Therefore, in the embodiment, in processing molten steel using a converter (11) (S110), a converter (11) used in a stainless steel manufacturing process as described above is used. Accordingly, the converter can be used without causing contamination of the converter (11) due to chromium (Cr). In addition, the converter used to prepare molten steel according to the embodiment containing 4.5 wt% to 5.5 wt% of chromium (Cr) can be used to prepare molten steel for manufacturing stainless steel. That is, the converter for manufacturing stainless steel can be used interchangeably in the operation for preparing molten steel for manufacturing stainless steel and the operation for preparing molten steel according to the embodiment containing 4.5 wt% to 5.5 wt% of chromium (Cr).
[0053] The temperature control device (30) used in the temperature control process and the vacuum treatment device (40) used in the degassing process use a ladle furnace (LF: Ladle Furnace) and a RH (Rheinstaal Huttenwerke und Heraus) device used in the steelmaking process (hereinafter, carbon steelmaking process) for preparing molten steel for manufacturing carbon steel (hereinafter, molten steel for manufacturing carbon steel). The reason for using the ladle furnace and the RH device used in the carbon steelmaking process will be explained later.
[0054]
[0055] Hereinafter, with reference to FIG. 2, the molten steel preparation process according to an embodiment of the present invention will be described in more detail.
[0056] As described above, the molten steel preparation process (S100) includes a process (S110) of processing molten steel (M) using a furnace (11), a process (S120) of discharging the molten steel (M) inside the furnace (11) into a ladle, a process (S130) of controlling the temperature of the molten steel (M) using a temperature control device (30), and a degassing process (S140) of removing gas from the molten steel (M) using a vacuum treatment device (40).
[0057] Referring to (a) to (d) of FIG. 2, the process (S110) of processing molten steel (M) using a furnace (11) may include a process (S111) ((a) of FIG. 2) of injecting an alloy iron containing chromium (Cr) (hereinafter, chromium (Cr) alloy iron) into the furnace (11), an oxygen blowing process (S112) ((b) of FIG. 2) of injecting oxygen into the molten steel inside the furnace (11), a deoxidation process (S113) ((c) of FIG. 2) of removing oxygen (O) contained in the molten steel (M), and a process (S114) ((d) of FIG. 2) of reducing chromium oxide contained in slag floating on the surface of the molten steel (M) to chromium (Cr).
[0058] In addition, although not shown, the molten steel preparation process may include a preliminary refining process for removing sulfur (S), phosphorus (P), and silicon (Si) contained in the molten steel before charging the molten steel into the converter. First, the preliminary refining process will be briefly described. The preliminary refining process may include a first preliminary refining process for removing sulfur (S) from the molten steel, and a second preliminary refining process for removing phosphorus (P) and silicon (Si) from the molten steel. In the first preliminary refining process, the content of sulfur (S) in the molten steel is controlled to be 0.04 wt% or less. In the second preliminary refining process, the content of silicon (Si) in the molten steel is controlled to be 0.05 wt% or more, and the content of phosphorus (P) is controlled to be 0.03 wt% or less. In carrying out these first and second preliminary refining processes, quicklime (CaO) and fluorite (CaF2) are added to the ladle containing the molten steel to remove sulfur (S), silicon (Si), and phosphorus (P) from the molten steel. In addition, the first and second preliminary refining processes can be carried out in a Hot Metal Pretreatment Station (HMPS).
[0059] After the first and second preliminary refining processes are completed, the molten steel (M) is charged into a converter (11). Here, the converter (11) into which the molten steel (M) is charged is a converter (11) used in a stainless steel manufacturing process as described above.
[0060] When molten steel (M) is charged into the converter (11), chromium (Cr) alloy iron is injected into the inside of the converter (11) as shown in (a) of Fig. 2. Accordingly, the chromium (Cr) alloy iron injected into the converter (11) is melted by the heat of the molten steel (M). At this time, the amount of chromium (Cr) alloy iron injected is adjusted so that the content of chromium (Cr) in the entire molten steel (M) becomes 4.5 wt% to 5.5 wt%. Accordingly, molten steel (M) having a high chromium (Cr) content of 4.5 wt% to 5.5 wt% is manufactured.
[0061] Next, as shown in (b) of Fig. 2, oxygen blowing is performed by blowing or spraying oxygen into the molten steel (M) inside the furnace (11). That is, after a part of the lance is inserted into the inside of the furnace (11), oxygen (O) is supplied into the inside of the lance (12). Accordingly, oxygen (O) is blown or sprayed from the lance (12). The oxygen (O) blown into the inside of the furnace (11) using the lance (12) reacts with the carbon (O) contained in the molten steel (M) (C + O --> CO (gas)). At this time, the carbon (O) in the molten steel (M) reacts with the oxygen (O) to become carbon monoxide (CO) gas, and the generated carbon monoxide (CO) gas is discharged outside the furnace (11). Accordingly, the content of carbon (C) contained in the molten steel (M) decreases. That is, decarburization occurs, in which the content of carbon (C) decreases from the molten steel (M). At this time, at least one of the oxygen injection flow rate and time is adjusted so that the carbon (C) content in the molten steel (M) becomes 0.75 wt% to 0.95 wt%.
[0062] In this way, when decarburization is performed by introducing oxygen into the furnace (11), reaction by-products composed of metal oxides in addition to carbon monoxide (CO) gas are generated. Then, the generated reaction by-products rise toward the upper surface of the molten steel (M), that is, the molten steel (M) bath surface, and float on the upper portion of the molten steel (M) bath surface. The reaction by-product that floats on the molten steel bath surface in this way is slag (SL).
[0063] When the carbon (C) content in the molten steel (M) reaches 0.75 wt% to 0.95 wt% and decarburization is completed, or when the carbon (C) content in the molten steel (M) decreases and approaches 0.95 wt% and reaches the final stage of decarburization, a dephosphorization agent is injected into the converter (11). At this time, the dephosphorization agent is injected while blowing oxygen into the converter (11) using a lance (12), and the dephosphorization agent may be a material containing, for example, quicklime (CaO). Accordingly, phosphorus (P) in the molten steel (M) reacts with the dephosphorization agent and oxygen (O) (3CaO + 2P + 5O --> 3CaO·P2O5). Then, the reaction by-product 3CaO·P2O5 rises and is absorbed into the slag (SL) floating on the molten steel (M) surface. That is, phosphorus (P) separated from molten steel (M) is absorbed into slag (SL) floating on the molten steel (M) surface. As a result, the content of phosphorus (P) contained in the molten steel (M) decreases. That is, dephosphorization occurs, which reduces the content of phosphorus (P) from the molten steel (M). At this time, at least one of the dephosphorization agent input amount, the oxygen injection flow rate, and the slag injection time is adjusted so that the content of phosphorus (P) in the molten steel (M) becomes 0.025 wt% or less.
[0064] After oxygen annealing of molten steel (M) to perform decarburization and dephosphorization, the oxygen (O) content in the molten steel (M) increases. Oxygen (O) in the molten steel (M) causes pin holes in the cast steel. In addition, oxygen (O) in the molten steel reacts with the metal contained in the molten steel, causing metal oxide inclusions to form. Inclusions contained in the molten steel cause defects such as cracks in the cast steel.
[0065] Therefore, after the oxygen annealing is completed, deoxidation is performed to remove oxygen (O) from the molten steel (M). To this end, a deoxidizer containing at least one of silicon (Si) and aluminum (Al) is injected into the furnace (11). The deoxidizer may use at least one of an alloy containing silicon (Si) and an alloy containing aluminum (Al). At this time, the alloy containing silicon (Si) may be an Fe-Si alloy containing silicon (Si) and iron (Fe), and may contain 70 wt% to 80 wt% of silicon (Si) and 20 wt% to 30 wt% of iron (Fe). In addition, the alloy containing aluminum (Al) may be an alloy close to pure aluminum (Al) containing 90 wt% to 95 wt% of aluminum (Al).
[0066] When a deoxidizer is injected, oxygen (O) contained in molten steel (M) reacts with at least one of silicon (Si) and aluminum (Al) contained in the deoxidizer. As a result, at least one of silicon oxide such as SiO2 and aluminum oxide such as Al2O3 is generated. Then, at least one of the reaction byproducts of silicon oxide and aluminum oxide is absorbed into slag (SL) floating on the molten steel (M) surface. Accordingly, the content of oxygen (O) contained in the molten steel (M) decreases (deoxidation). At this time, the amount of deoxidizer injected is adjusted so that the content of oxygen (O) in the molten steel (M) becomes 0.001 wt% or less.
[0067] As described above, at least one of an alloy containing silicon (Si) and an alloy containing aluminum (Al) is used as a deoxidizer. In this case, it is preferable to use both an alloy containing silicon (Si) and an alloy containing aluminum (Al) as a deoxidizer, compared to using an alloy containing silicon (Si) or an alloy containing aluminum (Al) as a deoxidizer.
[0068] Meanwhile, if the content of oxygen (O) in molten steel exceeds 0.001 wt%, pinhole defects may occur in the cast steel due to oxygen (O), and cracks may occur due to a large amount of inclusions. Therefore, during the deoxidation process, the content of oxygen (O) in the molten steel (M) is adjusted to 0.001 wt% or less.
[0069] As described above, when oxygen annealing is performed to remove carbon (C) and phosphorus (P) in molten steel (M), chromium (Cr) that was introduced into the molten steel (M) (S110) is oxidized and becomes chromium oxide. The generated chromium oxide is absorbed into the slag (SL) floating on the surface of the molten steel (M). As a result, the content of chromium (Cr) in the molten steel decreases. Therefore, it is necessary to reduce the chromium oxide contained in the slag (SL) to chromium and supply it back to the molten steel (M). To this end, a reducing agent is introduced into the converter (11) where deoxidation is completed. More specifically, the reducing agent is introduced into the slag (SL). At this time, the reducing agent may be a material containing silicon (Si), and more specifically, may be a ferroalloy containing silicon (Si). As a more specific example, the reducing agent may contain 70 wt% to 80 wt% of silicon (Si) and 20 wt% to 30 wt% of iron (Fe).
[0070] When a reducing agent is introduced into the furnace (11), the chromium oxide contained in the slag (SL) reacts with the silicon (Si) contained in the reducing agent. As a result, the chromium oxide contained in the slag (SL) is reduced to chromium (Cr), and the produced chromium (Cr) is absorbed or supplied to the molten steel. As a result, the content of chromium (Cr) in the molten steel increases. At this time, the amount of reducing agent introduced is adjusted so that the content of chromium (Cr) in the molten steel becomes 4.5 wt% to 5.5 wt%.
[0071] After chromium reduction is completed, the component content and temperature of the molten steel (M) are checked. For example, the molten steel (M) inside the furnace (11) is collected or sampled, and the component content and temperature of the collected molten steel are measured. Then, it is checked whether the measured component content of the molten steel (M) is included in the target component content, and it is checked whether the measured temperature of the molten steel (M) is included in the target temperature. Here, the target temperature may be, for example, 1650°C to 1750°C.
[0072] To give a more specific example, it is checked whether the contents of chromium (Cr), carbon (C), phosphorus (P), sulfur (S), and oxygen (O) are each included in the target contents. At this time, if the contents of chromium (Cr), carbon (C), phosphorus (P), sulfur (S), and oxygen (O) are each included in the target contents and the temperature of the molten steel is included in the target temperature, the slag floating on the upper part of the molten steel bath surface is excluded (not shown). That is, the slag is removed from the molten steel bath surface. However, if the contents of chromium (Cr), carbon (C), phosphorus (P), sulfur (S), and oxygen (O) are not included in the target contents or the temperature of the molten steel is not included in the target temperature, the process for adjusting the component contents or controlling the temperature is re-performed. That is, if the contents of chromium (Cr), carbon (C), phosphorus (P), sulfur (S), and oxygen (O) contained in the molten steel are not within the target contents, at least one of the processes of adding chromium (Cr) alloy steel, decarburization, dephosphorization, desulfurization, deoxidation, and chromium reduction is performed. In addition, if the temperature of the molten steel (M) is lower than 1650℃, the molten steel (M) is heated so that the temperature of the molten steel is higher than 1650℃. Conversely, if the temperature of the molten steel exceeds 1750℃, the temperature of the molten steel is reduced.
[0073] Meanwhile, if the content of each component included in the molten steel deviates from the target content, a problem of deterioration in the quality of the cast steel (S) may occur. That is, if at least one of the contents of chromium (Cr), carbon (C), phosphorus (P), sulfur (S), and oxygen (O) deviates from the target content, the hardness of the manufactured cast steel may be low, or pinholes and cracks may occur on the surface or inside of the cast steel. In addition, this may lower the hardness of the rolling roll and become a factor in generating pinholes and cracks on the surface or inside.
[0074] In addition, if the temperature of the molten steel (M) is lower than 1650℃, it may be difficult to raise the temperature of the molten steel (M) to the target temperature (LF starting target temperature) in the subsequent temperature control process. Therefore, when the molten steel (M) is supplied to the tundish, the temperature of the molten steel (M) may not reach the casting target temperature. In this case, the nozzle supplying the molten steel from the tundish to the mold may become clogged. Conversely, if the temperature of the molten steel (M) exceeds 1750℃, the refractory material constituting the converter may be damaged by erosion due to high heat. Therefore, the temperature of the molten steel (M) is controlled to be between 1650℃ and 1750℃ in the converter treatment process.
[0075] When the content of each component in the molten steel (M) is within the target content and the temperature of the molten steel (M) is within the target temperature, the slag floating on the upper surface of the molten steel (M) is excluded (not shown).
[0076] After removing the slag (SL) inside the converter (11), the molten steel (M) inside the converter (11) is tapped into a ladle (20). At this time, it is preferable to tap the molten steel (M) into a ladle (20) used in a carbon steelmaking process. This is because the device used in the process performed later uses the ladle (20) used in the carbon steelmaking process. That is, in the temperature control process, a ladle furnace (LF) is used as a temperature control device (30), and in the degassing process, a RH (Rheinstaal Huttenwerke und Heraus) device is used as a vacuum treatment device (40). At this time, the ladle furnace (LF) and the RH device are each devices used in the carbon steelmaking process, and are devices combined with the ladle used in the carbon steelmaking process.
[0077] Furthermore, the stainless steel manufacturing process does not use a ladle furnace (LF). Furthermore, while a vacuum treatment device is used in the stainless steel manufacturing process, this is a VTD (Vacuum Tank Degasser), which is different from the RH device used in the carbon steel manufacturing process.
[0078] In the embodiment, molten steel inside the furnace (11) is discharged into a ladle (20) used in a carbon steelmaking process. That is, in order to use the device used in the carbon steelmaking process in the subsequent temperature control process and degassing process, the molten steel is discharged into a ladle (20) used in the carbon steelmaking process.
[0079] As described above, in the embodiment, a ladle furnace is used as a temperature control device (30), and an RH device is used as a vacuum treatment device (40). Accordingly, for convenience of explanation, the temperature control device and the ladle furnace are described below by referring to them with the same drawing reference numeral '30', and the vacuum treatment device and the RH device are described by referring to them with the same drawing reference numeral '40'.
[0080] When the discharge of molten steel (M) into the ladle (20) is completed, the ladle (20) containing the molten steel (M) is moved to a temperature control device (30) as shown in (f) of FIG. 2, and the ladle (20) is coupled to the temperature control device (30). That is, the ladle (20) is moved to a ladle furnace (30), which is a temperature control device (30) used in a carbon steelmaking process, and the ladle (20) is coupled to the ladle furnace (30). The ladle furnace may include a cover (32) that can cover the upper opening of the ladle (20), as shown in (f) of FIG. 2, and an electrode rod (31) that can be inserted into the interior of the ladle (20) by penetrating the cover (32). And in this ladle furnace (30), desulfurization is performed to remove sulfur (S) from the molten steel, and the content of carbon (C) and chromium (Cr) is adjusted, and then the temperature of the molten steel is controlled.
[0081] First, the desulfurization process using a ladle furnace (30) will be described. When the ladle (20) arrives at the ladle furnace (30), the cover (32) of the ladle furnace (30) is attached to the upper part of the ladle (20). Then, a desulfurization agent is injected into the interior of the ladle (20). At this time, the desulfurization agent can be injected into the interior of the ladle (20) by passing it through an opening provided in the cover (32). It is preferable that the desulfurization agent use at least one of a first material including quicklime (CaO) and alumina (Al2O3) and a second material including fluorite (CaF2), for example. When the desulfurization agent is injected into the interior of the ladle (20), the desulfurization agent reacts with sulfur (S) in the molten steel to generate a reaction byproduct including sulfur (S), and the generated reaction byproduct is absorbed into the slag (SL) of the molten steel (M) surface. As a result, the content of sulfur (S) in the molten steel decreases (desulfurization). At this time, the content of sulfur (S) in the molten steel is set to 0.015 wt% or less, and this can be controlled by controlling the amount of desulfurizing agent added.
[0082] When desulfurization is completed, the molten steel (M) contained in the ladle (20) is sampled to measure the carbon (C) and chromium (Cr) content. Then, the carbon (C) and chromium (Cr) content in the molten steel (M) is adjusted according to the carbon (C) and chromium (Cr) content. For example, when the carbon (C) content is low, less than 0.75 wt%, a carbon (C)-containing accumulator is injected into the ladle (20). Then, the amount of accumulator is adjusted so that the carbon (C) content in the molten steel (M) is 0.75 wt% or more. Conversely, when the measured carbon (C) content exceeds 0.95 wt%, solid oxygen, for example, iron ore such as FeO, is injected into the ladle (20). At this time, the amount of solid oxygen is adjusted so that the carbon (C) content in the molten steel (M) is 0.95 wt% or less.
[0083] As another example, if the measured chromium (Cr) content is low, less than 4.5 wt%, an alloy ferroalloy containing chromium (Cr) is introduced into the ladle (20). Conversely, if the measured chromium (Cr) content exceeds 5.5 wt%, solid oxygen, for example, iron ore such as FeO, is introduced into the ladle (20). At this time, the amount of solid oxygen introduced is adjusted so that the chromium (Cr) content in the molten steel is 5.5 wt% or less.
[0084] In the above, when the carbon (C) content exceeds 0.95 wt% or the chromium (Cr) content exceeds 5.5 wt%, it was described that solid oxygen is introduced into the ladle (20) coupled to the ladle furnace (30). However, this is not limited thereto, and oxygen may be introduced into the molten steel (M) in a vacuum treatment device (40) to control the carbon (C) content to 0.95 wt% or less, or the chromium (Cr) content to 5.5 wt% or less.
[0085] When molten steel (M) is discharged into the ladle (20), the ladle (20) is moved for the next process. However, the temperature of the molten steel (M) gradually decreases while the ladle (20) is moving. That is, even if the temperature of the molten steel (M) is adjusted to a temperature of 1650°C to 1750°C before the molten steel from the converter (11) is discharged into the ladle (20), the temperature of the molten steel (M) decreases while the ladle (20) is moved to the next process.
[0086] Accordingly, before moving the ladle (20) to the vacuum treatment device (40), which is the next process, it is necessary to heat the molten steel (M) inside the ladle (20). To this end, power is supplied to the electrode (31) to generate an arc and heat from the electrode (31), and the molten steel is heated by the generated arc and heat. At this time, the molten steel (M) is heated so that the temperature becomes a starting target temperature, and the starting target temperature may be 1560°C to 1600°C. Here, the starting target temperature means the target temperature of the molten steel (M) accommodated in the ladle (20) when the ladle (20) separated from the ladle furnace (30) starts for the next process. Adjusting the temperature of the molten steel (M) to become the starting target temperature can be controlled by controlling at least one of the amount of power supplied to the electrode (31) and the heating time of the molten steel using the electrode (31).
[0087] Meanwhile, when the temperature of the molten steel (M) (hereinafter, starting temperature) is less than 1560°C or more than 1600°C when the ladle (20) separated from the ladle furnace (30) starts for the next process, the temperature of the molten steel (M) may exceed the casting target temperature when the ladle (20) reaches the tundish of the casting device. Here, the casting target temperature refers to the target temperature of the molten steel received in the tundish, and the casting target temperature may be 1520°C to 1550°C. When the starting temperature is less than 1560°C, the temperature of the molten steel (M) may be less than 1520°C when the ladle reaches the tundish. In addition, when the starting temperature is less than 1600°C, the temperature of the molten steel may exceed 1550°C when the ladle reaches the tundish.
[0088] When the temperature of the molten steel (M) is lower than 1520°C when the ladle (20) reaches the tundish, the nozzle supplying the molten steel (M) in the tundish to the mold may become clogged. In addition, when the temperature of the molten steel exceeds 1600°C when the ladle (20) reaches the tundish, a breakout may occur in which the solidification shell bursts and the molten steel inside flows out when the molten steel solidifies in the casting device. Therefore, the starting temperature of the molten steel (M) in the ladle furnace (30) is adjusted to be 1560°C to 1600°C so that the temperature of the molten steel becomes 1520°C to 1550°C when the ladle (20) reaches the tundish.
[0089] In performing the temperature control process (S130), the reason why a ladle furnace (LF) used in a carbon steelmaking process is used is because it can effectively increase the temperature without contaminating the molten steel (M). That is, in a stainless steelmaking process, when increasing the temperature of the molten steel, a metal such as aluminum (Al) is added to the molten steel to cause an exothermic reaction and increase the temperature. That is, in a stainless steelmaking process, a separate heating device is not used when increasing the temperature of the molten steel. Therefore, in the embodiment, the temperature of the molten steel (M) is controlled using a ladle furnace (30) used to increase the temperature of the molten steel in a carbon steelmaking process. Therefore, the temperature of the molten steel (M) can be increased without adding other materials to the molten steel (M). That is, the temperature of the molten steel can be increased without changing the composition of the molten steel (M).
[0090] When the component and temperature control in the ladle furnace (30) is completed, the ladle (20) is separated from the ladle furnace (30). Next, the ladle (20) separated from the ladle furnace (30) is moved to a vacuum treatment device (40). Then, degassing is performed using the vacuum treatment device (40) to remove nitrogen (N2) and hydrogen (H2) contained in the molten steel (M) (S140).
[0091] The vacuum treatment device (40) is a RH (Rheinstaal Huttenwerke und Heraus) device (40), and is an RH device (40) used in a carbon steelmaking process. Referring to (g) of FIG. 2, the RH device (40) may include a vessel (41) having an internal space, a pump (not shown) connected to the vessel (41) so as to control the pressure inside the vessel (41), a pair of reflux tubes (42a, 42b) arranged in parallel left and right so as to be inserted into the interior of the ladle (20) and connected to the lower part of the vessel (41), and a lance (43) inserted into the upper part of the vessel (41) to inject oxygen. Here, one (42a) of a pair of reflux tubes (42a, 42b) is a rising tube through which the molten steel inside the ladle (20) rises, and the other reflux tube (42b) is a descending tube through which the molten steel rising from the rising tube descends toward the ladle (20).
[0092] A process for removing gas from molten steel (M) using an RH device (40) as described above will be described. First, a ladle (20) is positioned below a pair of reflux tubes (42a, 42b), and these are joined together to seal them. Then, the inside of the vessel (41) is decompressed to a vacuum pressure of, for example, 0.2 torr or less, and the ladle (20) is raised so that the pair of reflux tubes (42a, 42b) are immersed in the molten steel in the ladle (20). Thereafter, an inert gas, for example, argon (Ar), is blown into the pair of reflux tubes (42a, 42b) to circulate the molten steel (M) into the vessel (41). The circulated molten steel is exposed to a vacuum atmosphere in the vessel (41), and thus nitrogen (N2) and hydrogen (H2) gases in the molten steel are discharged to the outside of the vessel (41). Accordingly, the contents of nitrogen (N) and hydrogen (H2) in molten steel (M) are reduced, and at this time, the content of nitrogen (N2) is set to 0.015 wt% or less, and the content of hydrogen (H2) is set to 0.0005 wt% or less.
[0093] Below, the reason why the content of hydrogen (H2) is controlled to 0.0005 wt% or less in the degassing process (S140) is explained.
[0094] In manufacturing a rolling roll, it is necessary to control the content of hydrogen (H2) contained in the rolling roll to 0.0002 wt% or less. This is because hydrogen (H2) contained inside the rolling roll is easily accumulated as inclusions and segregation contained in the rolling roll, which may cause internal cracks in the rolling roll when the rolling roll is actually used. Here, actual use of the rolling roll may mean that the manufactured rolling roll is used to roll a rolling object, such as a cast steel. Accordingly, the content of hydrogen (H2) contained in the rolling roll is controlled to 0.0002 wt% or less. At this time, when the content of hydrogen (H2) contained in the rolling roll is 0.0002 wt% or less, cracks do not occur or are almost non-existent inside the rolling roll due to hydrogen (H2). And, since it is realistically difficult to completely remove hydrogen from the rolling roll, the hydrogen content is controlled to be 0.0002 wt% or less.
[0095] In this way, in order for the hydrogen (H2) content of the rolling roll to be 0.0002 wt% or less, it is desirable to reduce the hydrogen (H2) content in the molten steel to 0.0005 wt% or less in the degassing process (S140). That is, if the hydrogen (H2) content in the molten steel (M) is not controlled to 0.0005 wt% or less in the degassing process (S140), it is difficult to control the hydrogen (H2) content to 0.0002 wt% or less in the subsequent process of heating the rolling roll to remove hydrogen (Fig. 4 (c)). In other words, it is difficult to manufacture a rolling roll in which the hydrogen (H2) content is controlled to 0.0002 wt% or less. Therefore, the hydrogen (H2) content in the molten steel is controlled to 0.0005 wt% or less in the degassing process (S140).
[0096] In addition, in the degassing treatment process (S140), the content of nitrogen (N2) in the molten steel (M) is controlled to be 0.015 wt% or less. If the content of nitrogen (N2) in the molten steel (M) exceeds 0.015 wt%, precipitates due to nitrogen (N2) are generated when the cast steel is manufactured, which may cause a large number of cracks in the cast steel. Therefore, the content of nitrogen (N2) in the molten steel (M) is controlled to 0.015 wt% or less through the degassing treatment process (S130).
[0097] In this way, the content of hydrogen (H2) in molten steel (M) can be adjusted to 0.0005 wt% or less and the content of nitrogen (N2) to 0.015 wt% or less by controlling the pressure and treatment time of the vessel (41) of the RH device (40). That is, by adjusting the pressure of the vessel (41) to 0.2 torr or less and maintaining the pressure for 20 minutes or more to treat the molten steel, molten steel having a content of hydrogen (H2) of 0.0005 wt% or less and a content of nitrogen (N2) of 0.015 wt% or less can be manufactured.
[0098] When performing degassing treatment using a vacuum treatment device (40), the reason why an RH device (40) is used as the vacuum treatment device (40) is because other types of vacuum treatment devices have relatively low pressure control capabilities. That is, an RH device (40) used in a carbon steelmaking process can control the pressure inside a vessel (41) to 2 torr or less, but a VOD (Vacuum Oxygen Decarburization) device, which is a vacuum treatment device used in a stainless steelmaking process, can only lower the maximum pressure to 3 torr to 4 torr. In addition, in removing hydrogen (H2) and nitrogen (N2) from molten steel, a lower pressure, that is, a higher vacuum, is advantageous. Therefore, an RH device (40) used for degassing in a carbon steelmaking process is used. Therefore, hydrogen (H2) and nitrogen (N2) can be easily removed from molten steel (M), and hydrogen (H2) and nitrogen (N2) can be removed more effectively than when using other vacuum processing devices, such as VOD.
[0099]
[0100] In this way, in the embodiment, the converter treatment process (S110) uses the converter (11) used in the stainless steel manufacturing process. That is, in preparing molten steel for manufacturing rolling rolls having a high chromium (Cr) content, the converter (11) used in the stainless steel manufacturing process is used. Accordingly, molten steel for manufacturing rolling rolls having a high chromium (Cr) content can be prepared without contaminating the converter for other steel types. In addition, when preparing molten steel for manufacturing stainless steel again using the converter for manufacturing stainless steel used to prepare molten steel for manufacturing rolling rolls, the chromium remaining in the converter for manufacturing stainless steel does not act as an impurity.
[0101] In addition, a ladle furnace (30) used in a carbon steelmaking process is used as a device for adjusting the composition and raising the temperature of molten steel (M) discharged from a furnace (11). In other words, the temperature of the molten steel (M) can be raised without adding other materials to the molten steel. Accordingly, the temperature of the molten steel can be raised without changing the composition of the molten steel.
[0102] In addition, when performing degassing using a vacuum treatment device (40), an RH device (40) used in a carbon steelmaking process is used. That is, degassing is performed using an RH device (40) capable of controlling the pressure of the vessel to a low level of 0.2 torr or less. Therefore, nitrogen (N2) and hydrogen (H2) can be effectively removed from the molten steel.
[0103] In addition, in preparing molten steel (M) for manufacturing rolling rolls, a new electric furnace, heating device, and vacuum treatment device are not separately provided, but a stainless steel-making electric furnace (11), a carbon steel-making ladle furnace (30), and an RH device (40) are used. Accordingly, there is no need to prepare a separate device for preparing molten steel for manufacturing rolling rolls, which has the effect of reducing costs.
[0104]
[0105] Figures 3 (a) to (d) are drawings sequentially showing the operation of a casting device according to an embodiment of the present invention.
[0106] First, the casting device (100) will be described with reference to (a) to (d) of FIG. 3.
[0107] Referring to (a) to (d) of FIG. 3, the casting device (100) is a vertical casting device (100) that draws the cast slab (S) vertically with respect to the ground when drawing the cast slab from the mold (120). The casting device according to the embodiment may be a device capable of manufacturing a thick cast slab (i.e., a thick plate) having a thickness of about 700 mm, for example.
[0108] Referring to (a) to (d) of FIG. 3, a casting device (100) includes a mold (120) capable of solidifying molten steel (M) supplied therein, a support member (171) that can be inserted into the interior of the mold (120) and can be raised and lowered, a driving member (172) connected to the support member (171) so as to provide raising and lowering power, a first magnetic field generating member (150a) located laterally outside the mold (120), a second magnetic field generating member (150b) located laterally outside the mold (120) at the lower side of the mold (120), and a heating member (160) located laterally outside the mold (120) between the mold (120) and the second magnetic field generating member (150b).
[0109] In addition, the casting device (100) is formed to extend in a direction perpendicular to the ground from the lower side of the mold (120), and includes a cooling unit (140) that can solidify the cast slab (S) drawn from the lower side of the mold (120) by spraying cooling water, a rotating unit (190) arranged on the lower side of the second magnetic field generating unit (150b) so as to receive and rotate the cast slab (S) supported on the support unit (171), and a moving unit (180) arranged on the lower side of the second magnetic field generating unit (150b) so as to face the rotating unit (190) so as to push and move the cast slab (S) supported on the support unit (171) toward the rotating unit (190).
[0110] In addition, the casting device (100) may include a tundish (110) positioned above the mold (120) to supply molten steel (M) to the mold (120) and a nozzle (130) connected to the lower part of the tundish (110) to supply molten steel (M) to the mold (120).
[0111] In Fig. 3, for the convenience of explanation, the rotating part (190) is only illustrated in (d) of Fig. 3, and is omitted in (a) to (c) of Fig. 3. However, even in cases like (a) to (c) of Fig. 3, the rotating part (190) is positioned facing the moving part (180) at the lower side of the cooling part.
[0112] The mold (120) is a means for receiving liquid molten steel (M) from the tundish (110) and solidifying it into a predetermined shape. This mold (120) may have a cooling water pipe (not shown) provided inside through which cooling water circulates. When molten steel is supplied to the mold (120) and solidified for the first time, the molten steel (M) enters a semi-solid state in which a solidified region (A) and a non-solidified region (B) coexist.
[0113] The support member (171) is inserted into the inside of the mold (120) to close the lower opening of the mold (120) before supplying molten steel (M) to the mold (120). Then, when molten steel is supplied into the inside of the mold (120) with the support member (171) closing the lower opening of the mold (120), the molten steel (M) begins to solidify on the support member (171). Accordingly, the cast slab (S) in a semi-solid state is supported on the support member (171). Then, when the driving member (172) is operated to lower the support member (171), the support member (171) is lowered to the lower side of the mold (120) while supporting the cast slab (S) in a semi-solid state. That is, the cast slab (S) inside the mold (120) is drawn to the lower side of the mold (120) by lowering the support member (171). These supports may be plate-shaped.
[0114] The driving unit (172) is a means for raising and lowering the support unit (171), and can be connected to the lower part of the support unit (171). The driving unit (172) can include a power source (172-1) that provides raising and lowering driving force, and a driving member (172-2) that connects the power source (172-1) and the support unit (171) so that raising and lowering is possible by the driving force transmitted from the power source (172-1).
[0115] The power source (172-1) may be a device including a hydraulic piston. Of course, the power source (172-1) is not limited to the above-described example, and any means capable of raising and lowering the driving member (172-2) may be used.
[0116] The driving member (172-2) has one end connected to the power source (172-1) and the other end connected to the support member (171). This driving member (172-2) may have, for example, a shape extending vertically. In addition, the driving member (172-2) may be arranged so that the height of the one end connected to the power source (172-1) is fixed, and the height of the other end connected to the support member (171) can be raised or lowered by the operation of the power source (172-1).
[0117] As described above, the driving unit (172) is a means for raising and lowering the support unit (171), and can control the speed at which the support unit (171) is raised and lowered. In particular, by controlling the speed at which the support unit (171) is lowered, the speed at which the cast slab (S) supported on the support unit (171) is pulled downwards from the mold (120) can be controlled. At this time, the speed at which the cast slab (S) is pulled downwards from the mold (120) may refer to the casting speed. When the driving unit (172) controls the lowering speed of the support unit (171), its operation is controlled so as to lower at a speed of 0.04 m / min or less. More specifically, its operation is controlled so as to lower at a speed of 0.01 m / min to 0.04 m / min. In other words, the driving unit (172) controls the lowering speed of the support unit so that the casting speed is 0.04 m / min or less, more specifically, 0.01 m / min to 0.04 m / min.
[0118] In this way, the purpose of controlling the casting speed to 0.04 m / min or less is to suppress or prevent segregation in the cast steel (S) and to suppress or prevent a decrease in the production rate. That is, if the casting speed exceeds 0.04 m / min, the unsolidified molten steel (M) inside the cast steel (S) may not be sufficiently solidified, which may cause segregation. In addition, if the casting speed is less than 0.01 m / min, there is a problem that the production rate of the cast steel (S) decreases. Therefore, it is preferable to control the casting speed to 0.01 m / min to 0.04 m / min.
[0119] The cooling unit (140) includes a plurality of rolls (141) arranged in a row in the direction in which the support unit (171) is raised and lowered at the lower side of the mold (120), and a nozzle (not shown) positioned between the plurality of rolls (141) to spray cooling water onto the cast piece drawn to the lower side of the mold.
[0120] A plurality of rolls (141) may be arranged in a vertical direction relative to the ground. In addition, each of the plurality of rolls (141) is provided so that the cast iron (S) can be rotated by the downward force of the cast iron (S) when the cast iron (S) is lowered downward by the support member (171). Accordingly, the cast iron (S) pulled downward from the mold (120) is lowered in a vertical direction relative to the ground by the lowering of the support member (171) and the plurality of rolls (141).
[0121] A nozzle that sprays cooling water is placed between a plurality of rolls (141). Accordingly, the cast piece (S) drawn to the lower side of the mold (120) is lowered by the support member (171) and is secondarily cooled by the cooling water sprayed from the nozzle.
[0122] In the case of secondary solidification of the cast slab (S) by spraying cooling water onto the cast slab (S) drawn from the lower side of the mold (120), the spray amount of the cooling water is adjusted so that the surface temperature of the cast slab (S) becomes 800°C to 900°C. That is, the spray amount of the cooling water is adjusted so that the entire surface of the cast slab (S) at the lower side of the mold (120) becomes 800°C to 900°C. More specifically, the spray amount of the cooling water is adjusted so that the surface temperature from the upper to the lower side of the cast slab (S) becomes uniformly 800°C to 900°C. To this end, among the plurality of nozzles arranged in the vertical direction, the spray amount of the cooling water may be adjusted so that the lower the nozzle is arranged, the less the nozzle is sprayed.
[0123] The purpose of controlling the surface temperature of the cast slab (S) to 800°C to 900°C is to suppress or prevent the occurrence of surface cracks in the cast slab (S) and to prevent the occurrence of bulging. That is, when the temperature of the surface of the cast slab (S) is lower than 800°C, cracks may occur on the surface of the cast slab (S) due to overcooling. Conversely, when the temperature of the surface of the cast slab exceeds 900°C, the strength of the solidification shell, which is the surface portion of the cast slab (S), may be low, resulting in bulging, in which the solidification shell swells. Therefore, the surface temperature of the cast slab (S) drawn out of the mold (120) is controlled to 800°C to 900°C.
[0124]
[0125] If the temperature of the molten steel (M) supplied to the mold (120) is low, the molten steel (M) solidifies and stagnates, which causes segregation in the cast steel (S). Therefore, in order to suppress the drop in the molten steel temperature, a mold flux, which is an insulating agent, is applied on the surface of the molten steel bath supplied to the mold (120). However, the mold flux alone is not enough to suppress the drop in the molten steel temperature.
[0126] Therefore, in order to suppress the temperature drop of the molten steel (M) by causing the molten steel (M) inside the mold (120) to flow, a first magnetic field generating unit (150a) is installed on the outside of the mold (120). The first magnetic field generating unit (150a) is located on the lateral outer side of the mold (120) and generates a magnetic field. Here, the lateral outer side of the mold (120) may mean the outside of the outer surface, which is the opposite side of the inner surface of the mold (120) with which the molten steel (M) comes into contact. That is, the first magnetic field generating unit (150a) is installed on the outside of the mold (120) to face the outer surface of the mold (120). In other words, the first magnetic field generating unit (150a) may be installed on the lateral outer side of the mold (120) to surround the mold (120). To this end, the first magnetic field generating unit (150a) may be provided in a hollow shape extending along the outer surface of the mold (120). This first magnetic field generating unit (150a) may include a coil that is installed in the body and inside the body and generates a magnetic field by applied power.
[0127] When a magnetic field is generated from the first magnetic field generating unit (150a), the generated magnetic field causes the molten steel (M) inside the mold (120) to flow. Accordingly, the molten steel (M) inside the mold (120) flows due to the magnetic field, and a temperature drop due to the flow of the molten steel (M) can be suppressed or prevented. When the molten steel (M) flows, the components contained in the molten steel (M) are mixed evenly or uniformly. As a result, the occurrence of segregation, in which specific components are accumulated or gathered in a predetermined area inside the cast iron, can be suppressed or prevented.
[0128] The magnetic field generated from the first magnetic field generating unit (150a) may vary depending on the magnitude of the current according to the power or voltage applied to the first magnetic field generating unit (150a). Accordingly, the power or voltage supplied to the first magnetic field generating unit (150a) is adjusted so that a current of a target magnitude flows through the coil of the first magnetic field generating unit (150a). In this way, by allowing the current to flow in the first magnetic field generating unit (150a), a magnetic field can be generated in the first magnetic field generating unit (150a). In addition, the molten steel (M) inside the mold (120) can be made to flow by the magnetic field generated from the first magnetic field generating unit (150a), thereby suppressing or preventing a drop in the temperature of the molten steel (M), and suppressing or preventing the mold flux on the molten steel (M) surface from being mixed into the molten steel.
[0129] Meanwhile, if the current flowing in the first magnetic field generating unit (150a) is too small, the molten steel (M) inside the mold (120) may not flow, and thus the temperature of the molten steel (M) may drop, causing segregation in the cast slab (S). Conversely, if the current flowing in the first magnetic field generating unit (150a) is too large, the molten steel flow rate inside the mold (120) may be very fast, causing mold flux to be mixed into the molten steel. The mold flux mixed into the molten steel (M) may cause cracks in the cast slab as an impurity. Therefore, the size of the current flowing in the first magnetic field generating unit (150a) is controlled by adjusting the size of the power or voltage supplied to the first magnetic field generating unit (150a) so that a magnetic field capable of causing the molten steel inside the mold (120) to flow at an appropriate flow rate is generated.
[0130]
[0131] When molten steel (M) solidifies inside the mold (120), the molten steel (M) supplied into the mold (120) is not solidified all at the same time. That is, it solidifies sequentially from the edge in the width and length direction of the mold (120) toward the center region. Accordingly, the molten steel solidifies at the edge in the width and length direction inside the mold (120) to become a solidified shell or solid state, but the molten steel (M) exists in a non-solidified state in the center region in the width and length direction of the mold (120) in a liquid state. In other words, a cast iron manufactured by partially solidifying molten steel inside the mold (120) is in a semi-solid state in which a solidified region (A) and a non-solidified region (B) exist.
[0132] In addition, when the cast slab (S) in a reaction solid state is drawn from the lower side of the mold (120), the cast slab (S) is secondarily cooled by cooling water sprayed from the nozzle of the cooling unit (140). At this time, since the cooling unit (140) is located in the lateral direction of the cast slab (S), the cast slab (S) is sequentially solidified from the edge in the width and length direction toward the center region. Accordingly, the cast slab (S) drawn from the lower side of the mold (120) may be in a reaction solid state in which a solidification region (A) and a non-solidification region (B) exist. And, as the molten steel (M) in the non-solidification region (B) solidifies over time, a completely solidified cast slab without a non-solidification region (B) is manufactured.
[0133] And, in the cast piece (S) drawn to the lower part of the mold (120), the accumulated solidification time becomes shorter toward the upper part closer to the mold (120), and the accumulated solidification time becomes longer toward the lower part. Accordingly, in the cast piece (S) drawn to the lower part of the mold (120), the area of the non-solidification region (B) becomes wider toward the upper part closer to the mold (120), and the area of the non-solidification region (B) becomes smaller toward the lower part. In other words, in the cast piece (S) drawn to the lower part of the mold (120), the area of the solidification region (A) becomes smaller toward the upper part closer to the mold (120), and the area of the solidification region (A) becomes larger toward the lower part.
[0134] As described above, there is a non-solidified region (B) in which the molten steel (M) is not solidified at the upper portion of the cast slab (S) drawn downward from the mold (120). That is, the cast slab (S) includes unsolidified molten steel (M). When the cast slab (S) is drawn downward from the mold (120), the cast slab (S) is solidified by the cooling water sprayed from the cooling unit (140). However, if the unsolidified molten steel (M) present in the cast slab (S) solidifies without stagnating, segregation may occur within the cast slab (S).
[0135] Therefore, a second magnetic field generating unit (150b) is installed on the lower side of the mold (120) so as to cause the unsolidified molten steel (M) inside the cast slab (S) drawn to the lower side of the mold (120) to flow. The second magnetic field generating unit (150b) is positioned on the lateral outer side of the mold (120) at the lower side of the mold (120) to generate a magnetic field. More specifically, the second magnetic field generating unit (150b) may be positioned to face the first magnetic field generating unit (150a) in the vertical direction at the lower side of the mold (120). More specifically, the second magnetic field generating unit (150b) may be positioned on the lateral outer side of the cooling unit (140) at the lower side of the mold (120). To this end, the second magnetic field generating unit (150b) may be provided in a hollow shape. In addition, the second magnetic field generating unit (150b) may be provided with the same configuration as the first magnetic field generating unit (150a). That is, the second magnetic field generating unit (150b) may include a coil that is installed in the body and inside the body and generates a magnetic field by applied power.
[0136] When a magnetic field is generated from the second magnetic field generating unit (150b), the generated magnetic field is applied to the cast iron. Accordingly, the liquid molten steel inside the cast iron (S) flows due to the magnetic field. Accordingly, the molten steel (M) inside the cast iron (S) can flow and solidify, thereby suppressing or preventing segregation from occurring inside the cast iron (S).
[0137] The magnetic field generated from the second magnetic field generating unit (150b) may vary depending on the magnitude of the current according to the power or voltage applied to the second magnetic field generating unit (150b). Accordingly, the power or voltage supplied to the second magnetic field generating unit (150b) is adjusted so that a current of a target magnitude flows through the coil of the second magnetic field generating unit (150b). In this way, by allowing the current to flow in the second magnetic field generating unit (150b), a magnetic field can be generated in the second magnetic field generating unit (150b). In addition, the molten steel inside the cast iron (S) can be made to flow by the magnetic field generated from the second magnetic field generating unit (150b), and the mold flux can be suppressed or prevented from being mixed into the molten steel (M).
[0138] Meanwhile, if the current flowing to the second magnetic field generating unit (150b) is too small, the molten steel (M) inside the cast slab (S) may not flow or may flow insufficiently, which may cause segregation inside the cast slab (S). Conversely, if the current flowing to the first magnetic field generating unit (150a) is too large, the flow rate of the molten steel (M) may be very fast, causing mold flux to be mixed into the molten steel. The mold flux mixed into the molten steel (M) may cause cracks in the cast slab (S) as an impurity. Therefore, in generating a magnetic field using the second magnetic field generating unit (150b), the current flowing to the second magnetic field generating unit (150b) is controlled by adjusting the magnitude of the power or voltage supplied to the second magnetic field generating unit (150b) so that a magnetic field capable of causing the molten steel (M) inside the cast slab (S) to flow at an appropriate flow rate is generated.
[0139] And, if the time for generating a magnetic field by operating the second magnetic field generating unit (150b) is too short, the cast slab (S) may not be sufficiently solidified. In other words, casting may be terminated with unsolidified molten steel remaining inside the cast slab (S). Conversely, if the time for generating a magnetic field by operating the second magnetic field generating unit (150b) is too long, the magnetic field may be applied to an area where there is no unsolidified molten steel, that is, to the lower part of the cast slab. In other words, the magnetic field may be applied to an area where application of the magnetic field is unnecessary. Therefore, in generating a magnetic field using the second magnetic field generating unit (150b), the time for applying the magnetic field to the cast slab is controlled so that the unsolidified molten steel inside the cast slab (S) can be sufficiently solidified, while the magnetic field is not unnecessarily applied to the solidified area.
[0140]
[0141] As previously explained, the cast piece drawn from the lower side of the mold (120) has a larger non-solidified area toward the upper side. Here, the lowermost part of the cast piece (S) is the area drawn first from the mold (120), and the uppermost part of the cast piece (S) is the area drawn last from the mold (120). Accordingly, in the cast piece drawn from the lower side of the mold (120), the uppermost part of the cast piece (S) is called the end part of the cast piece (S).
[0142] When the cast steel (S) drawn to the lower side of the mold (120) solidifies, the unsolidified molten steel at the end of the cast steel solidifies before the molten steel (M) at the lower side of the end of the cast steel. As the molten steel (M) at the end of the cast steel solidifies before the molten steel (M) at the lower side of the end of the cast steel, a pipe defect occurs due to solidification shrinkage at the end of the cast steel. In addition, since the end of the cast steel where the pipe defect occurs cannot be used as a product, the end of the cast steel where the pipe defect occurs is cut off after casting is completed. Therefore, there is a problem that the yield of the cast steel decreases by the length of the cut end part, and since the cut end part is discarded, there is a problem that material equivalent to the cut length is consumed in each operation, which is also a waste in terms of cost.
[0143] Therefore, in order to suppress or prevent solidification shrinkage of the end portion of the cast, a heating unit (160) capable of heating the end portion of the cast is installed on the lower side of the mold (120). The heating unit (160) is arranged on the lateral outer side of the mold (120) between the mold (120) and the second magnetic field generating unit (150b). More specifically, the heating unit (160) may be arranged to face the first magnetic field generating unit (150a) and the second magnetic field generating unit (150b) in the vertical direction on the lower side of the mold (120). In addition, the heating unit (160) may be arranged to be positioned on the lateral outer side of the cooling unit (140). For this purpose, the heating unit (160) may be provided in a hollow shape. The heating unit (160) may include a heating element that is installed on the body and the inside of the body and generates heat by the applied power.
[0144] When the heating unit (160) operates and heat is generated, this heat heats or induces the molten steel (M) inside the cast end portion. This can delay the solidification of the molten steel (M) at the cast end portion. In other words, the molten steel at the cast end portion can be controlled to solidify later than the molten steel at the lower portion of the molten steel. Accordingly, the occurrence of pipe defects at the cast end portion can be suppressed or prevented.
[0145] The heat generated in the heating unit (160) may vary depending on the power or voltage applied to the heating unit (160). Accordingly, the power applied to the heating unit (160) is adjusted so that heat of a target temperature can be generated in the heating unit (160). By supplying power to the heating unit (160) in this way to generate heat, the end portion of the cast piece can be heated. Accordingly, solidification shrinkage of the end portion of the cast piece can be suppressed or prevented.
[0146] Meanwhile, if the power supplied to the heating unit (160) is too small, the temperature of the heat generated from the heating unit (160) is low, so that the molten steel (M) at the end of the cast piece cannot be sufficiently heated, which may cause solidification shrinkage at the end of the cast piece, resulting in pipe defects. Conversely, if the power supplied to the heating unit (160) is too large, the temperature of the heat generated from the heating unit (160) is too high, so that not only the end of the cast piece but also the lower part of the end of the cast piece is heated, causing a problem of remelting. Therefore, when heating the end of the cast piece using the heating unit (160), the power supplied to the heating unit (160) is adjusted so that the end of the cast piece can be sufficiently heated, while preventing the lower part of the end of the cast piece from being heated and remelted.
[0147] In addition, if the time for heating the end of the cast piece using the heating unit (160) is too short, the end of the cast piece may not be sufficiently heated. As a result, the molten steel (M) at the end of the cast piece may solidify earlier than the molten steel (M) below the end of the cast piece, which may cause solidification shrinkage at the end of the cast piece, resulting in pipe defects. Conversely, if the time for heating the end of the cast piece using the heating unit (160) is too long, there is no need to heat the end of the cast piece using the heating unit because the molten steel at the end of the cast piece has already completed solidification. Therefore, when heating the end of the cast piece using the heating unit (160), the time for heating the end of the cast piece is adjusted so that the end of the cast piece can be sufficiently heated while not heating the end of the cast piece that has already completed solidification.
[0148]
[0149] In this embodiment, when solidifying molten steel inside the mold (120), the first magnetic field generating unit (150a) is used to cause the molten steel inside the mold (120) to flow. Accordingly, a decrease in the temperature of the molten steel (M) inside the mold (120) can be suppressed or prevented, and thus segregation in the cast steel (S) can be suppressed or prevented.
[0150] In addition, when the cast slab pulled to the lower side of the mold (120) solidifies, the unsolidified molten steel inside the cast slab (S) is caused to flow using the second magnetic field generating unit (150b) arranged on the lower side of the mold (120). Accordingly, when the cast slab solidifies outside the mold (120), the unsolidified molten steel inside the cast slab (S) can solidify while flowing without stagnation. Accordingly, it is possible to suppress or prevent segregation in the cast slab (S) due to stagnation of the unsolidified molten steel.
[0151] Meanwhile, in the past, in order to prevent segregation in ingots for manufacturing rolling rolls, the ESR (Electro Slag Remelting) method was used. Hereinafter, the ESR (Electro Slag Remelting) method will be briefly described. First, molten steel adjusted to the upper part for manufacturing rolling rolls is solidified and manufactured into an electrode rod. Then, an arc is generated with the manufactured electrode rod to remelt the electrode rod, and the remelted molten steel is solidified while dripping downward in the shape of droplets to manufacture the ingot again. Although this process can suppress or prevent segregation in the ingot, it requires a complex process of manufacturing the manufactured ingot into an electrode rod, remelting the electrode rod, and resolidifying the remelted molten steel as described above. Therefore, the time and cost consumed in the process for suppressing segregation are significant.
[0152] On the other hand, in the embodiment, the first and second magnetic field generating units (M) provided in the casting device (100) are used to flow the molten steel in the mold (120) and the unsolidified molten steel (M) in the slab (S), thereby suppressing or preventing segregation from occurring inside the slab (S). Therefore, compared to manufacturing an ingot through the conventional ESR (Electro Slag Remelting) method, when manufacturing a slab through the method according to the embodiment, the process is simple and time and cost are shortened. In addition, compared to the magnitude of the power applied to generate an arc in the electrode rod in the conventional ESR (Electro Slag Remelting) method, the magnitude of the power applied to operate the first and second magnetic field generating units in the embodiment is small. Therefore, compared to manufacturing an ingot through the conventional ESR (Electro Slag Remelting) method, when manufacturing a slab through the method according to the embodiment, there is an effect of reducing the electric energy consumption.
[0153] In addition, in the embodiment, by heating the heating part (160) using the cast end, the solidification of the molten steel (M) at the cast end can be delayed. As a result, the occurrence of solidification shrinkage at the cast end can be suppressed or prevented, and thus the occurrence of pipe defects at the cast end can be suppressed.
[0154]
[0155] Returning to Figure 3, the moving part (180) and the rotating part (190) will be described.
[0156] The moving unit (180) is a means for pushing the cast (S) drawn from the lower side of the mold (120) from one side and moving it toward the rotating unit (190). That is, the moving unit (180) is drawn from the lower side of the mold (120) and is vertically supported on the support unit (171), and pushes the cast (S) that has completed solidification and transfers it to the rotating unit (190). This moving unit (180) may be, for example, a means driven horizontally with respect to the ground, and for example, the moving unit may include a hydraulic or pneumatic cylinder.
[0157] The rotating part (190) receives the cast iron (S) separated from the support part (171) by the moving part (180) and rotates the received cast iron (S). That is, the rotating part (190) receives the cast iron supported in a direction perpendicular to the ground on the support part (171) and rotates the received cast iron parallel to the ground.
[0158] The rotating part (190) is arranged to face the moving part (180) in a horizontal direction. The rotating part (190) can receive and support a cast iron (S) separated from the support part (171), and includes a rotating table (191) that can rotate, and a rotating member (192) connected to the rotating table (191) so that the rotating table (191) can rotate.
[0159] The rotary table (191) includes a first table (191-1) extended in one direction and a second table (191-2) extended in a direction intersecting the extension direction of the first table (191-1) and having one end connected to the first table (191-1).
[0160] Based on the cast iron (S) vertically supported on the support member (171), the first table (191-1) is a means for supporting the side surface of the cast iron (S), and the second table (191-2) is a means for supporting the lower surface of the cast iron (S). The first table (191-1) may be provided with a longer extension length than the second table (191-2). In addition, it is preferable that the second table (191-2) be provided with an area equal to or larger than the area of the lower surface of the cast iron (S). A plurality of rotatable rollers (191-3) may be installed on the first table (191-1), and the plurality of rollers (191-3) are arranged in the direction in which the first table (191-1) extends.
[0161] One end of the first table (191-1) and one end of the second table (191-2) can be interconnected by a rotary member (192). And the rotary table (191) can be rotated or tilted by the rotary member (192) as shown in (d) of FIG. 3. That is, when the cast iron (S) is vertically supported on the support member (171), the first table (191-1) of the rotary member is arranged perpendicular to the ground, and the second table (191-2) is arranged parallel to the ground. And, when the cast iron (S) supported on the support member (171) is transferred to the rotary member (190), the rotary member (190) is rotated or tilted. That is, the first table (191-1) of the rotary member (190) is rotated so that it is parallel to the ground, and the second table (191-2) is rotated so that it is perpendicular to the ground.
[0162] The above describes manufacturing a cast slab using a vertical casting device. However, the present invention is not limited thereto, and a cast slab (S) may be manufactured using various types of casting devices including a first magnetic field generating unit (150a) installed on the lateral outer side of a mold (120), a second magnetic field generating unit (150b) installed on the lower side of the mold (120), and a heating unit (160).
[0163]
[0164] Figures 4 (a) to (c) are process diagrams sequentially showing a method for manufacturing a rolling roll using a cast iron manufactured by a method according to an embodiment of the present invention.
[0165] When the cast slab (S) is manufactured, the manufactured cast slab (S) is heated and softened (S300). To this end, the cast slab (S) is loaded into a first heating device (200). The first heating device (200) may include a furnace having an internal space and a heater for heating the furnace. Here, the heater may be installed, for example, inside or outside a wall constituting the furnace, and may include a heating element capable of generating heat by applied electric power. As another example, the heater may include a burner that generates heat by burning fuel.
[0166] In heating the slab (S) in the first heating device (200), the slab is heated to a temperature of 1100°C to 1250°C, preferably 1140°C to 1240°C. At this time, the slab is not charged into the furnace heated to 1100°C to 1250°C, but rather into the furnace controlled to a lower temperature, and then the temperature inside the furnace is gradually increased to 1140°C to 1240°C.
[0167] To be more specific, first, the inside of the furnace is heated to 250°C to 350°C (first temperature) and maintained at the first temperature for 3 to 5 hours, preferably 3 hours 30 minutes to 4 hours 30 minutes. Thereafter, the inside of the furnace is heated to 450°C to 550°C (second temperature) and maintained at the second temperature for 5 to 7 hours, preferably 5 hours 30 minutes to 6 hours 30 minutes. Next, the inside of the furnace is heated to 650°C to 750°C (third temperature) and maintained at the third temperature for 3 to 5 hours, preferably 3 hours 30 minutes to 4 hours 30 minutes. Next, the inside of the furnace is heated to 1100℃ to 1250℃ (fourth temperature) and maintained at the fourth temperature for 14 hours to 18 hours, preferably 15 hours and 30 minutes to 17 hours and 30 minutes. In addition, the time for raising the temperature of the inside of the furnace from the first temperature to the second temperature (first heating time) and the time for raising the temperature of the inside of the furnace from the second temperature to the third temperature are each preferably 3 hours to 4 hours, and the time for raising the temperature of the inside of the furnace from the third temperature to the fourth temperature is preferably 9 to 10 hours. Heating the inside of the furnace to the first to fourth temperatures and maintaining the inside of the furnace at the first to fourth temperatures in this way means that the temperature of the cast iron charged into the furnace is heated to the first to fourth temperatures, and the temperature of the cast iron is maintained at the first to fourth temperatures.
[0168] The reason for gradually increasing the temperature as described above when heating the cast steel (S) to 1100°C to 1250°C is that the cast steel (S) containing a high amount of chromium of 4.5 wt% or more has high hardness and thus cracks may easily occur during heating and cooling. Therefore, by gradually increasing the temperature as described above when heating the cast steel (S) to 1100°C to 1250°C, cracks may be suppressed or prevented from occurring in the cast steel (S).
[0169] When the process of heating or heat treating the cast steel (S) in the first heating device (200) is completed, the cast steel (S) is forged using a forging device (300) to manufacture a rolling roll. The forging device (300) may include, for example, an upper pressing part and a lower pressing part spaced apart from each other in the vertical direction, and a driving part connected to the upper pressing part and the lower pressing part so as to apply a predetermined force. Here, the driving part may be a cylinder driven by hydraulic pressure or air pressure.
[0170] Hereinafter, a method for forging a cast slab (S) using a forging device (300) will be described. First, a cast slab is placed between an upper presser and a lower presser of the forging device (300). Then, a driving unit is operated to lower the upper presser and raise the lower presser, thereby reducing the distance between the upper presser and the lower presser. Next, the driving unit is operated to apply more downward force to the upper presser and more upward force to the lower presser. At this time, as time passes after the upper and lower pressers come into contact with the cast slab (S), the force with which the upper and lower pressers press the slab increases. Accordingly, the cast slab (S) placed between the upper presser and the lower presser is pressed, thereby reducing the thickness of the slab. Then, when the thickness of the slab is reduced to a target thickness, the upper and lower pressers are separated from the slab. Here, the target thickness may be 250 mm to 350 mm. And this process is repeated multiple times.
[0171] In this way, by contacting the upper and lower press members to the cast steel (S) and applying force, when the thickness of the cast steel (S) is reduced to the target thickness, the upper and lower press members are separated from the cast steel (S). This series of processes is defined as 'one pass (one pass)'. At this time, in the embodiment, the target thickness is set to 250 mm to 350 mm. And, the reduced thickness of the cast steel (S) per pass is adjusted to 250 mm to 350 mm. And, by repeating the above-described one pass multiple times, a rolling roll is manufactured.
[0172] Meanwhile, if the thickness reduction of the cast steel (S) per pass is less than 250 mm, the force may not be sufficiently applied to the center region of the thickness direction of the cast steel (S), so the pores in the center region of the cast steel may not be removed. If the pores in the center region of the thickness direction of the cast steel (S) are not removed, this may be a factor that reduces the hardness of the rolling roll. Conversely, if the thickness reduction of the cast steel (S) per pass exceeds 350 mm, cracks may occur on the surface of the cast steel, which causes defects in the rolling roll.
[0173] When forging is completed and the rolling roll (141) is manufactured, the rolling roll (141) is heated to remove hydrogen (H2). To this end, the rolling roll (141) is loaded into the second heating device (400), and the rolling roll (141) is heated using the second heating device (400). Here, the second heating device (400) may be the same as or different from the first heating device (200) described above.
[0174] In heating the rolling roll (141) using the second heating device (400), the rolling roll (141) is heated to 200°C to 400°C, more preferably 250°C to 350°C. In addition, the temperature of the rolling roll (141) is maintained at a temperature of 200°C to 400°C for 48 hours or more, more preferably 48 hours or more and 55 hours or less.
[0175] In this way, when the rolling roll (141) is heated to 200°C to 400°C, preferably 250°C to 350°C, and maintained at this temperature for 48 hours or more, hydrogen (H2) contained or remaining in the rolling roll (141) diffuses to become hydrogen gas, and the hydrogen gas is discharged to the outside. Accordingly, the hydrogen content in the rolling roll (141) decreases. At this time, it is preferable that the hydrogen content in the rolling roll (141) be 0.0002 wt% or less (0 wt% or more), and this can be controlled by controlling at least one of the temperature and heat treatment time for heating the rolling roll (141).
[0176] Meanwhile, hydrogen contained within the rolling roll (141) is easily accumulated in inclusions and segregation contained in the rolling roll (141), which may cause internal cracks in the rolling roll (141) when the rolling roll (141) is actually used. Here, actual use of the rolling roll may refer to a case where the manufactured rolling roll (141) is used to roll a rolling target, for example, a cast iron (S).
[0177] Accordingly, the manufactured rolling roll (141) is heated at 200°C to 400°C for 48 hours or more to remove hydrogen so that the content of hydrogen contained in the rolling roll (141) becomes 0.0002 wt% or less. At this time, when the content of hydrogen contained in the rolling roll (141) is 0.0002 wt% or less, cracks do not occur inside the rolling roll (141) due to hydrogen. In addition, since it is realistically difficult to completely remove hydrogen from the rolling roll (141), the content of hydrogen is made to be 0.0002 wt% or less.
[0178]
[0179] Hereinafter, a method for manufacturing a rolling roll according to an embodiment of the present invention will be described in detail with reference to FIGS. 1 to 4. In this case, any content that overlaps with the previously described content will be omitted or briefly described.
[0180] First, molten steel (M) for manufacturing rolling rolls is prepared (S100). To this end, molten steel (M) is first charged into a stainless steel-making furnace (11). Then, chromium (Cr) alloy iron is introduced into the furnace (11) as shown in (a) of Fig. 2. At this time, the amount of chromium (Cr) alloy iron introduced is adjusted so that the chromium (Cr) content of the molten steel inside the furnace (11) is 4.5 wt% to 5.5 wt%.
[0181] Next, oxygen is injected into the inside of the furnace (11) using a lance (12) as shown in (b) of Fig. 2. That is, oxygen is injected into the molten steel (M) in the furnace (11) to remove carbon (C) and phosphorus (P). At this time, the content of carbon (C) in the molten steel (M) is set to be 0.75 wt% to 0.95 wt%, and the content of phosphorus (P) is set to be 0.025 wt% or less.
[0182] Next, as shown in (c) of Fig. 2, a deoxidizer is injected into the inside of the furnace (11) to remove oxygen (O) in the molten steel (M). At this time, at least one of an alloy containing silicon (Si) and an alloy containing aluminum (Al) may be used as the deoxidizer. Then, deoxidation is performed so that the content of oxygen (O) in the molten steel (M) becomes 0.001 wt% or less.
[0183] When deoxidation is completed, a reducing agent, i.e., an alloy ferroalloy containing silicon (Si), is injected into the furnace (11) as shown in (d) of Fig. 2. Accordingly, the chromium oxide contained in the slag (SL) and the silicon (Si) contained in the reducing agent react. Accordingly, the chromium oxide contained in the slag (SL) is reduced to chromium (Cr), and the generated chromium (Cr) is absorbed or supplied to the molten steel (M). Accordingly, the content of chromium (Cr) in the molten steel (M) increases. At this time, the amount of reducing agent injected is adjusted so that the content of chromium (Cr) in the molten steel (M) becomes 4.5 wt% to 5.5 wt%.
[0184] When the chromium reduction is completed, the molten steel (M) inside the furnace (11) is discharged into a ladle (20) as shown in (e) of Fig. 2. At this time, the molten steel (M) is discharged into a ladle (20) for carbon steelmaking.
[0185] Then, the ladle (20) is moved to the temperature control device (30), i.e., the ladle furnace (30), and the ladle (20) is connected to the cover (32) of the ladle furnace (30) (Fig. 2 (f)). Next, a desulfurizing agent is injected into the ladle (20) to remove sulfur (S) in the molten steel. At this time, the content of sulfur (S) in the molten steel is made to be 0.015 wt% or less.
[0186] When degassing is completed, the molten steel (M) contained in the ladle (20) is sampled to measure the carbon (C) and chromium (Cr) content. Then, according to the measured carbon (C) and chromium (Cr) content, the carbon (C) and chromium (Cr) content in the molten steel (M) is adjusted. At this time, according to the measured carbon (C) and chromium (Cr) content, at least one of the alloy ferroalloys containing carbonaceous material and chromium (Cr) is added, or solid oxygen such as iron ore is added, so that the measured carbon (C) content of the molten steel is 0.75 wt% to 0.95 wt%, and the chromium (Cr) content is 4.45 wt% to 5.5 wt%.
[0187] Once the carbon (C) and chromium (Cr) component adjustments are completed, the molten steel (M) is heated to increase its temperature. That is, an arc and heat are generated from the electrode rod (31) to heat the molten steel contained in the ladle (20). At this time, the temperature of the molten steel is set to 1560°C to 1600°C.
[0188] When the temperature of the molten steel (M) reaches 1560°C to 1600°C, the ladle (20) is separated from the ladle furnace (30). Then, the ladle (20) is moved to a vacuum treatment device, i.e., an RH device (40), as shown in (g) of FIG. 2. Then, the ladle (20) is positioned below a pair of reflux tubes (42a, 42b), and these are mutually coupled to seal them. Next, the pump is operated to reduce the pressure inside the vessel (41) to a vacuum pressure of, for example, 0.2 torr or less, and then the ladle (20) is raised so that the pair of reflux tubes (42a, 42b) are immersed in the molten steel inside the ladle (20). Thereafter, argon (Ar) gas is blown into the pair of reflux tubes (42a, 42b) to circulate the molten steel inside the vessel (41). The circulating molten steel is exposed to a vacuum atmosphere within the vessel (41), and thus nitrogen (N2) and hydrogen (H2) gases in the molten steel are discharged outside the vessel (41). Accordingly, the contents of nitrogen (N) and hydrogen (H2) in the molten steel are reduced, and at this time, the content of nitrogen (N2) is made to be 0.015 wt% or less, and the content of hydrogen (H2) is made to be 0.0005 wt% or less.
[0189] By going through the processes (a) to (g) of the above-described Fig. 2, molten steel (M) for manufacturing rolling rolls is prepared.
[0190] When the molten steel (M) is prepared, the ladle (20) is moved to the tundish (110) of the casting device (100), and the molten steel (M) is supplied to the tundish (110) to initiate casting. To this end, the lower opening of the mold (120) is first closed using the support (171) of the casting device (100). Then, as shown in (a) of FIG. 3, the molten steel (M) of the tundish (110) is supplied to the mold (120) (S210). Accordingly, the molten steel (M) supplied to the mold (120) solidifies and begins to solidify from the upper portion of the support (171) (casting process) (S210). Then, while continuously supplying the molten steel (M) of the tundish (110) to the mold (120), the driving unit (172) is operated to lower the support (171). Accordingly, as shown in (b) of Fig. 3, the cast iron (S) inside the mold (120) is gradually drawn downward into the mold (S220).
[0191] As described above, while continuously supplying molten steel (M) to the mold (120), the first magnetic field generating unit (150a) located outside the mold (120) is operated to generate a magnetic field. Accordingly, the magnetic field generated from the first magnetic field generating unit (150a) is applied to the inside of the mold (120), and as a result, the molten steel (M) inside the mold (120) flows due to the magnetic field. Accordingly, a temperature drop of the molten steel (M) inside the mold (120) can be suppressed or prevented, and mold flux on the molten steel (M) bath surface can be suppressed or prevented from being mixed into the molten steel.
[0192] While continuously supplying molten steel into the mold (120), the driving unit (172) is operated to gradually lower the support unit (171) toward the lower side of the mold (120). At this time, the speed at which the support unit (171) descends downward is adjusted to be 0.04 m / min or less, and more specifically, to be 0.01 m / min to 0.04 m / min. That is, the casting speed is adjusted to be 0.04 m / min or less, and more specifically, to be 0.01 m / min to 0.04 m / min.
[0193] As shown in (b) of Fig. 3, when the cast is drawn to the lower side of the mold (120), the drawn cast (S) is secondarily solidified (solidification process) (S220) by cooling water sprayed from the nozzle of the cooling unit (140). Then, the tundish (110) continuously supplies molten steel (M) to the mold, and the support unit (171) continuously lowers, and accordingly, the length of the cast drawn to the lower side of the mold (120) gradually increases. When the cast of the target length is drawn to the lower side of the mold (120), the supply of molten steel to the mold (120) is stopped. Then, as shown in (c) of Fig. 3, the cast is drawn to the lower side of the mold to the uppermost part, i.e., the end part (S230). In addition, when the cast iron is pulled downwards to the end of the mold, the second magnetic field generating unit (150b) is operated to generate a magnetic field. Accordingly, the unsolidified molten steel existing inside the cast iron (S) pulled downwards of the mold (120) flows due to the magnetic field generated by the second magnetic field generating unit (150b). As a result, the mold flux can be suppressed or prevented from being mixed into the molten steel.
[0194] In the above, it was explained that when the cast iron (S) is pulled downwards to the end of the mold, the second magnetic field generating unit (150b) is operated to generate a magnetic field. However, this is not limited to this, and when the cast iron begins to be pulled downwards to the mold (120), the second magnetic field generating unit (150b) may be operated to generate a magnetic field.
[0195] When the end of the cast (S) is pulled toward the lower side of the mold, the heating unit (160) is operated to heat the end of the cast. As a result, the solidification of the unsolidified molten steel (M) at the end of the cast (S) is delayed. As a result, solidification shrinkage at the end of the cast can be suppressed or prevented, and remelting of areas other than the end of the cast can be prevented.
[0196] When solidification is completed up to the end of the cast iron (S), the moving part (180) is operated as shown in (d) of Fig. 3 to push the cast iron (S) placed vertically on the support part (171) toward the rotating part (190). Accordingly, the cast iron (S) of the support part (171) is transferred to the rotating part (190). At this time, the side of the cast iron (S) is supported on the first table (191-1) of the rotating part (190), and the lower surface of the cast iron is supported on the second table (191-2). Next, the rotating part (190) is rotated, i.e., tilted (S240). More specifically, the rotating part (190) is rotated so that the first table (191-1) is parallel to the ground and the second table (191-2) is horizontal to the ground. Accordingly, the cast iron (S) is rotated so that it is placed horizontally with respect to the ground. The cast iron placed horizontally on the rotating part (190) is transferred to the next process.
[0197] When the cast slab (S) is manufactured, the cast slab is heated (S300) using the first heating device (200). At this time, the inside of the furnace in which the cast slab (S) is loaded is gradually increased to 1140°C to 1240°C (target temperature) to heat the cast slab. More specifically, the cast slab (S) is first heated to 250°C to 350°C (first temperature) and maintained for 3 to 5 hours. Thereafter, the cast slab (S) is heated to 450°C to 550°C (second temperature) and maintained for 5 to 7 hours. Next, the cast slab (S) is heated to 650°C to 750°C (third temperature) and maintained at the third temperature for 3 to 5 hours. Next, the cast steel (S) is heated to a target temperature of 1100°C to 1250°C (the fourth temperature) and maintained for 14 to 18 hours. In this way, by gradually increasing the temperature from the first to the fourth temperature as described above while heating the cast steel (S) to 1100°C to 1250°C (the fourth temperature), it is possible to suppress or prevent the occurrence of heat-induced cracks in the cast steel containing a large amount of chromium (Cr) of 4.5 wt% or more.
[0198] When the process of heating the cast steel (S) in the first heating device (200) is completed, the cast steel is forged using the forging device (300) to manufacture a rolling roll (S400). At this time, the reduced thickness of the cast steel (S) per pass is set to 250 mm to 350 mm, and this is repeated multiple times to manufacture a rolling roll (141).
[0199] When the rolling roll (R) is manufactured, the rolling roll (141) is heated using a second heating device (400) to remove hydrogen (H2). At this time, the rolling roll (141) is heated at a temperature of 200°C to 400°C for 48 hours or more. Accordingly, the hydrogen content in the rolling roll (141) can be adjusted to 0.0002 wt% or less (0 wt or more).
[0200]
[0201] Table 1 is an evaluation table for rolling rolls manufactured using a method according to an embodiment of the present invention. To evaluate quality, some rolling rolls manufactured using a method according to an embodiment were cut and used as test pieces.
[0202] UT (Ultrasonic testing) quality assessment is a quality assessment method used to detect internal defects such as pores and cracks. In other words, it is an assessment method that detects the presence and amount of pores and cracks inside a specimen by transmitting ultrasonic waves into the interior of the specimen and using the amount of ultrasonic energy reflected from discontinuities inside the specimen and the propagation time of the ultrasonic waves.
[0203] Macro quality assessment is designed to determine the presence and amount of coarse tissue. For evaluation, the specimen was etched using corrosion, and its internal structure was observed using an optical microscope.
[0204] Inclusion quality assessment aims to determine the quantity and size of inclusions present in a specimen. For evaluation, a portion of the specimen was polished, and the size and quantity of inclusions were detected using an optical microscope.
[0205] Hardness was measured using a Brickell hardness tester as the hardness of the specimen.
[0206] Quality evaluation items Evaluation results Evaluation criteria UT (Ultrasonic testing) quality evaluation (presence and amount of pores and cracks) Pass JIS 1st class inspection criteria Mark quality evaluation (presence and amount of coarse structure) Pass ASTM E381 S1. R1. C2 criteria Inclusion quality evaluation (inclusion content) Pass ASTM E45 inspection criteria Hardness quality evaluation Pass HB255 or less
[0207] Referring to Table 1, the specimens manufactured by the method according to the examples have acceptable UT quality, macro quality, inclusion quality, and hardness quality. In other words, the rolling rolls manufactured by the method according to the examples all pass the evaluation results for UT quality, macro quality, inclusion quality, and hardness quality. This shows that by manufacturing rolling rolls by the method according to the examples, rolling rolls with fewer pores, cracks, and inclusions, a uniform structure, and high hardness can be manufactured.
[0208]
[0209] Figures 5 (a) and (b) show the results of cutting a cross-section of a rolling roll and etching the cross-section to check whether or not coarse segregation occurred.
[0210] Here, (a) of Fig. 5 is a cross-section of a rolling roll manufactured by a method according to an embodiment, and (a) of Fig. 5 is a cross-section of a rolling roll manufactured by a method according to a comparative example. In addition, the rolling roll manufactured by a method according to a comparative example is a rolling roll manufactured by an ESR (Electro Slag Remelting) method.
[0211] Comparing (a) and (b) of Fig. 5, no coarse segregation occurred in either of the rolling rolls according to the examples and the comparative examples. That is, the rolling roll according to the examples has a uniform structure equivalent to that of the rolling roll according to the comparative examples. From this, it can be seen that even if the rolling roll is manufactured in the same manner as in the examples without using the conventional ESR (Electro Slag Remelting) method, the occurrence of segregation can be sufficiently suppressed. That is, even if the cast steel is cast by using the first and second magnetic field generating units to flow the molten steel during the casting process as in the examples, it can be seen that the occurrence of segregation can be suppressed to a level equivalent to that of the conventional ESR (Electro Slag Remelting) method.
[0212] In addition, compared to the conventional ESR (Electro Slag Remelting) method, the process of suppressing segregation by using the first and second magnetic field generating units during the casting process as in the example is simple and requires less time. That is, in the case of the example, while the occurrence of segregation can be suppressed to the same level as the conventional method, the process required for the occurrence of segregation is shorter and the process time is shorter.
[0213] According to embodiments of the present invention, high-chromium (Cr) molten steel can be produced using a converter used for steelmaking other types of steel without contaminating the converter used for steelmaking other types of steel. Furthermore, when heating the high-chromium (Cr) molten steel or performing degassing to discharge gas, the temperature of the molten steel can be effectively increased, and the degassing efficiency can be improved.
Claims
1. A method for manufacturing high chromium (Cr) molten steel having a chromium (Cr) content of 4.5 wt% to 5.5 wt%, The process of charging molten steel into the inside of a furnace used in a stainless steel manufacturing process; and A method for manufacturing high chromium (Cr) molten steel, comprising the step of injecting chromium alloy iron containing chromium (Cr) into the inside of the furnace so that the content of chromium (Cr) in the molten steel is 4.5 wt% to 5.5 wt%.
2. In claim 1, An oxygen blowing process in which oxygen is blown into the inside of the above-mentioned furnace into which chromium alloy iron is introduced to remove carbon (C) in the molten steel; The process of removing oxygen (O) from molten steel by adding a deoxidizer to the above furnace; and A method for manufacturing high chromium (Cr) molten steel, comprising the step of reducing chromium oxide contained in slag floating on the molten steel surface to chromium (Cr) by injecting a reducing agent into the above-mentioned furnace.
3. In claim 1, The process of discharging the molten steel from the above furnace into a ladle; A method for manufacturing high chromium (Cr) molten steel, comprising a temperature control process for heating molten steel received in a ladle furnace (LF), which is a heating device used in a carbon steelmaking process.
4. In claim 3, A method for manufacturing high chromium (Cr) molten steel, wherein the temperature of the molten steel is controlled to 1560°C to 1600°C in the above temperature control process.
5. In claim 3, It includes a degassing process for removing hydrogen (H2) and nitrogen (N2) from the molten steel received in the ladle using a RH (Rheinstaal Huttenwerke und Heraus) device, which is a vacuum treatment device used in the carbon steelmaking process. A method for manufacturing high chromium (Cr) molten steel, wherein the above degassing process is performed after the above temperature control process is completed.
6. In any one of claims 3 to 5, A method for producing high chromium (Cr) molten steel by discharging molten steel from the above furnace into a ladle, which is used in a carbon steelmaking process.
7. A process for preparing molten steel containing 4.5 wt% to 5.5 wt% of chromium (Cr); A casting process of supplying molten steel to a mold of a casting device, solidifying the molten steel inside the mold, and manufacturing a cast steel including unsolidified molten steel; A process of drawing the cast iron manufactured in the above casting process to the lower side of the mold; and A method for manufacturing a cast iron, including a solidification process in which a magnetic field is applied to a cast iron drawn from the lower side of the mold to cause unsolidified molten steel contained in the cast iron to flow and solidify the cast iron.
8. In claim 7, A method for manufacturing a cast iron, wherein the above solidification process includes a process of heating the end portion of the cast iron drawn toward the lower side of the mold.
9. In claim 7, The above casting process is a method for manufacturing a cast iron, which includes a process of applying a magnetic field to the mold to cause molten steel inside the mold to flow.
10. In claim 7, A method for manufacturing a cast iron, wherein the cast iron is drawn to the lower side of the mold at a speed of 0.04 m / min or less.
11. In claim 7, The above solidification process includes a process of spraying cooling water onto the cast piece drawn from the lower side of the mold, A method for manufacturing a cast iron, wherein cooling water is sprayed onto the cast iron so that the surface temperature of the cast iron becomes 800°C to 900°C.
12. In any one of claims 7 to 11, In the above drawing process, the cast piece is drawn from the mold so as to be perpendicular to the ground, A method for manufacturing a cast iron in which the cast iron is solidified in a state in which the cast iron is placed perpendicular to the ground during the above solidification process.
13. A process for heating a cast iron manufactured by the method for manufacturing a cast iron according to any one of claims 7 to 11; A process of forging a heated cast iron into the shape of a rolling roll; A process of removing hydrogen (H2) from the rolling roll by heating the rolling roll manufactured in the above forming process; A method for manufacturing a rolling roll, wherein the process of heating the above-mentioned cast steel includes a process of heating the cast steel by raising the temperature of the cast steel in multiple stages to a target temperature.
14. In claim 13, The process of heating the cast iron to the above target temperature is as follows: A process of heating the cast iron to a first temperature of 250°C to 350°C; A process of heating the cast iron to a second temperature of 450°C to 550°C; A process of heating the cast iron to a third temperature of 650°C to 750°C; and A method for manufacturing a rolling roll, comprising: a process of heating a cast iron to the target temperature of 1100°C to 1250°C.
15. In claim 14, In heating the above cast iron to the first to third temperatures and the target temperature, Maintain the cast iron at the first temperature for 3 to 5 hours, Maintain the cast iron at the second temperature for 5 to 7 hours, Maintain the cast iron at the above third temperature for 3 to 5 hours, A method for manufacturing a rolling roll by maintaining the cast iron at the above target temperature for 14 to 18 hours.
16. In claim 15, In forging the above cast iron, the cast iron heated to a temperature of 1100°C to 1250°C is pressed and forged, A method for manufacturing a rolling roll that reduces the thickness of a cast steel by 250 mm to 350 mm each time the cast steel is reduced using a pressure reducing device.
17. In claim 13, A method for manufacturing a rolling roll, comprising a process of heating the rolling roll to a temperature of 200°C to 400°C in order to remove hydrogen (H2) from the rolling roll.
18. In claim 17, A method for manufacturing a rolling roll, wherein the rolling roll is heated to a temperature of 200°C to 400°C for 48 hours or longer.
Citation Information
Patent Citations
Method for manufacturing forging rolling roll by using gradual up-setting method and diffused bonding method
KR101346636B1
HIGH Mn STEEL MATERIAL AND PRODUCTION METHOD THEREFOR
JP2016084529A
Method of continuous casting of steel
KR101168195B1
Continuous casting methods