Antimicrobial glass composition, method for preparing antimicrobial glass powder therefrom, and home appliance comprising same
A novel antibacterial glass composition with a controlled component ratio and exclusion of alkali oxides addresses the challenges of long-term antibacterial efficacy and oxidation issues, achieving effective antibacterial performance and durability by creating a positive surface charge and suppressing oxidation reactions.
Patent Information
- Application Number
- PCT/KR2024/003841
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional antibacterial glass compositions face challenges in maintaining long-term antibacterial efficacy without dissolving in water, ensuring safety for parts that come into contact with drinking water, and preventing oxidation reactions, which can lead to mechanical property deterioration and transparency issues due to alkali ion elution.
A novel antibacterial glass composition excluding alkali oxides, with a controlled component ratio that forms a robust, water-insoluble glass structure, utilizing Zn ions to create a positive surface charge that attracts and kills bacteria, and suppressing oxidation reactions, thereby ensuring durability and transparency.
The solution provides permanent antibacterial activity, prevents contamination by bacteria and mold, and maintains mechanical properties, even when used in contact with drinking water, while ensuring transparency and durability.
Smart Images

Figure KR2024003841_24102024_PF_FP_ABST
Abstract
Description
Antibacterial glass composition and method for producing antibacterial glass powder thereof, and home appliances comprising the same
[0001] The present invention relates to an antibacterial glass composition and a method for producing an antibacterial glass powder thereof, and to a home appliance comprising the same.
[0002] Microorganisms such as germs, fungi, and bacteria are ubiquitous in our living spaces, including water purifiers, refrigerators, ovens, and washing machines. If these microorganisms enter the human body, they can cause life-threatening infections. Therefore, an antimicrobial glass composition capable of controlling the spread of microorganisms in home appliances such as water purifiers, refrigerators, ovens, and washing machines is in demand.
[0003] In these home appliances, bacteria and mold can grow in parts made of plastic that are exposed to moisture, causing problems with the appearance or the user environment.
[0004] The fungi that inhabit home appliances are very diverse, and the main strains may differ depending on the part, but parts exposed to moisture are generally more likely to harbor Pseudomonas aeruginosa.
[0005] Therefore, antimicrobial agents must ensure antibacterial efficacy against these strains. Furthermore, antimicrobial agents must be carefully selected from materials with low toxicity to humans and the environment and high-temperature resistance.
[0006] Antibacterial agents can be broadly categorized into inorganic and organic. Organic antibacterial agents exhibit excellent antibacterial properties because they release antibacterial materials onto the surface of the device in water, exerting their antibacterial activity against bacteria. However, their durability may be reduced when applied to washing machines. Furthermore, concerns have been raised about the human and environmental hazards of the extracted materials. Furthermore, their low decomposition temperature poses a risk of decomposition during the injection molding process.
[0007] Inorganic antibacterial agents have significantly lower solubility than organic antibacterial agents and can secure high-temperature durability, but they can cause interfacial wetting problems with plastic injection molded products and are often expensive because Ag is used as the antibacterial material, which limits their application.
[0008] Conventional non-elutable antibacterial glass does not mean that the entire glass is non-elutable, but rather, glass composed of a water-insoluble glass substrate and ionic or crystalline components that are eluted for the purpose of antibacterial properties is called non-elutable.
[0009] Consequently, to achieve antibacterial activity, the ions or crystal phases that exhibit antibacterial properties must be released. However, conventional release-type antibacterial glasses struggle to maintain long-term durability and have limited safety when applied to components that come into contact with drinking water.
[0010] Furthermore, conventional antibacterial glasses contain alkaline oxides, and alkaline ions released from these alkaline oxides gain electrons. Consequently, products using conventional antibacterial glasses can be damaged by oxidation reactions that result in electron loss. Because plastic injection moldings are susceptible to oxidation, the aforementioned oxidation reactions can degrade their mechanical properties and, in extreme cases, lead to synthesis failure.
[0011] Additionally, the alkaline ions capture OH groups, creating a weak haze. Consequently, conventional antibacterial glass faces the problem of difficulty maintaining transparency due to its increased likelihood of crystallization.
[0012] The purpose of the present invention is to provide an antibacterial glass composition that exhibits an antibacterial effect that lasts permanently even when the glass does not react with water at all, unlike the existing dissolution mechanism, and a method for producing the antibacterial glass powder, and a home appliance including the same.
[0013] In addition, the purpose of the present invention is to provide an antibacterial glass composition and a method for producing an antibacterial glass powder thereof, which exhibit antibacterial properties without being dissolved in water by strictly controlling each component of the glass composition and its component ratio to allow Zn ions, which are components exhibiting antibacterial properties, to participate in a network-forming structure, thereby forming a robust glass structure that does not dissolve in water, thereby controlling the surface charge of the glass, and a home appliance including the same.
[0014] In addition, the purpose of the present invention is to provide an antibacterial glass composition and a method for producing the antibacterial glass powder, which exhibits non-dissolution characteristics by strictly controlling each component of the glass composition and its component ratio, and thus can exhibit an excellent effect in preventing contamination by bacteria, mold, etc. when used as a coating agent for a group of parts that come into contact with drinking water, and a home appliance including the same.
[0015] In addition, an object of the present invention is to provide a novel antimicrobial glass composition capable of suppressing unintended oxidation reactions while providing transparent glass, a method for producing the antimicrobial glass powder, and a home appliance including the same.
[0016] The objectives of the present invention are not limited to those mentioned above. Other objectives and advantages of the present invention not mentioned above can be understood through the following description and will be more clearly understood through the embodiments of the present invention. Furthermore, it will be readily apparent that the objectives and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims.
[0017] The antibacterial glass composition and the method for producing the antibacterial glass powder according to the present invention, and the home appliance including the same, simultaneously secure antibacterial power, water resistance, and oxidation prevention by proposing a novel composition ratio that excludes alkaline oxides.
[0018] In addition, the antibacterial glass composition and the method for producing the antibacterial glass powder according to the present invention, and the home appliance including the same, cause the metal ions in the glass to have a positive surface charge, i.e., zeta potential, thereby attracting bacteria that normally have a negative charge and creating a charge atmosphere in which bacteria cannot grow, thereby killing the bacteria.
[0019] As a result, the antibacterial glass composition according to the present invention is an antibacterial agent exhibiting non-dissolution characteristics, and therefore, when used as a coating agent for a group of components that come into contact with drinking water, it exhibits an excellent effect in preventing contamination by bacteria, mold, etc.
[0020] In addition, the antibacterial glass composition according to the present invention excludes alkaline oxides and thus prevents oxidation by alkaline ions, while still having excellent antibacterial properties and durability.
[0021] To this end, the antibacterial glass composition according to the present invention contains 15 to 32 wt% of SiO2, 12 to 32 wt% of B2O3, 42 to 69 wt% of ZnO, 1 to 10 wt% of at least one of CaO, BaO, and SnO, and 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2, and GeO2, and does not contain alkali oxides.
[0022] In addition, the antibacterial glass composition according to the present invention may further include at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3, and preferably may further include at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 in an amount of 0.2 to 4 wt%, and may include at least 1 wt% of CaO.
[0023] According to the present invention, by strictly controlling each component of the glass composition and its component ratio, the Zn ion, which is a component that exhibits antibacterial performance, participates in a network-forming structure to form a robust glass structure that does not dissolve in water, thereby controlling the surface charge of the glass, thereby enabling the antibacterial performance to be exhibited without dissolving in water.
[0024] In addition, according to the present invention, since it is a water-insoluble antibacterial agent composed of a multipurpose antibacterial ingredient, it can be used permanently when used as a coating material for glass shelves and an additive for plastic injection molded products.
[0025] In addition, according to the present invention, since it is an antibacterial agent exhibiting non-dissolving properties, when used as a coating agent for a group of parts that come into contact with drinking water, it exhibits an excellent effect in preventing contamination by bacteria, mold, etc.
[0026] In particular, according to the present invention, it is possible to provide an antibacterial glass powder having excellent durability by suppressing unintended oxidation reactions, and at the same time, transparent glass can be provided.
[0027] In addition to the effects described above, specific effects of the present invention are described below while explaining specific details for carrying out the invention.
[0028] Figure 1 is a process flow diagram showing a method for manufacturing antibacterial glass powder according to an embodiment of the present invention.
[0029]
[0030] The above-described objects, features, and advantages will be described in detail below with reference to the accompanying drawings, so that those skilled in the art can easily practice the technical idea of the present invention. In describing the present invention, if it is determined that a detailed description of known technologies related to the present invention may unnecessarily obscure the gist of the present invention, a detailed description thereof will be omitted. Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the drawings, the same reference numerals are used to indicate the same or similar components.
[0031] As used herein, singular expressions include plural expressions unless the context clearly dictates otherwise. In this application, terms such as "consisting of" or "comprising" should not necessarily be construed to include all of the components or steps described in the specification, and should be construed to mean that some of the components or steps may not be included, or that additional components or steps may be included.
[0032] Hereinafter, an antimicrobial glass composition and a method for producing an antimicrobial glass powder according to some embodiments of the present invention, and a home appliance including the same will be described.
[0033]
[0034] Antibacterial glass composition
[0035]
[0036] The antibacterial glass composition according to an embodiment of the present invention has an antibacterial effect that lasts permanently even when the glass does not react with water at all, unlike the existing dissolution mechanism.
[0037] To this end, the antibacterial glass composition according to an embodiment of the present invention controls each component and its component ratio to utilize the fact that the intermediate oxide can act as both a modified oxide and a network-forming oxide during glass formation, thereby forming a robust glass structure that does not dissolve in water by allowing the Zn ion, which is a component that exhibits antibacterial performance, to participate in the network-forming structure, and by controlling the surface charge of the glass, it is possible to exhibit antibacterial properties without dissolving in water.
[0038] In this way, the antibacterial glass composition according to the embodiment of the present invention simultaneously secures antibacterial power and water resistance by controlling the content ratio of the modified oxide and the network-forming oxide to form a network by dissolving the Zn ions to implement the antibacterial function.
[0039] In addition, the mechanism by which the antibacterial property is expressed in the present invention is that the metal ions in the glass make the surface charge of the glass, i.e., the zeta potential, positive, thereby attracting bacteria that normally have a negative charge and creating a charge atmosphere in which bacteria cannot grow, thereby killing the bacteria.
[0040] At this time, the elements for manufacturing an antibacterial glass composition with excellent durability can be broadly divided into two.
[0041] First, there is the glass matrix, which forms a glassy structure and determines chemical durability. This plays a role similar to that of the carrier of existing inorganic antibacterial agents: dispersing materials that exhibit antibacterial properties on the surface.
[0042] The difference is that while existing carriers have antibacterial ingredients loaded onto the surface of inorganic antibacterial agents, the present invention allows a metal material exhibiting antibacterial properties to exist in the form of ions within a glass substrate. In order to create such a durable glass substrate, not only is the content ratio of glass-forming agents such as SiO2 and B2O3 important, but the combination ratio of alkaline components (mixed alkali effect in glass: the mechanical properties of glass can change nonlinearly depending on the ratio of alkaline components) is also a very important factor.
[0043] Second, the effect of the metal components contained within the glass is crucial. While metal components are a key factor in exerting antibacterial properties, their antibacterial properties vary significantly across components. Furthermore, durability can vary depending on the state of ionic and covalent bonds, resulting from interactions with components within the glass matrix. Therefore, optimizing the composition of the antibacterial glass is crucial.
[0044] In addition, the present invention provides a novel antibacterial maintenance composition that can satisfy both the above-described antibacterial properties and water resistance while completely excluding alkaline oxides, in order to prevent the problem of deterioration of the durability of the product due to an oxidation reaction caused by alkali ions extracted from alkaline oxides.
[0045]
[0046] To this end, the antimicrobial glass composition according to an embodiment of the present invention contains 15 to 32 wt% of SiO2, 12 to 32 wt% of B2O3, 42 to 69 wt% of ZnO, 1 to 10 wt% of at least one of CaO, BaO, and SnO, and 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2, and GeO2, and does not contain an alkaline oxide.
[0047]
[0048] The antimicrobial glass composition according to the embodiment of the present invention described above is a water-insoluble antimicrobial agent composed of a multipurpose antimicrobial component, and therefore, when used as a coating material for glass shelves and an additive for plastic injection molded products, it can be used permanently.
[0049] In addition, since the antimicrobial glass composition according to an embodiment of the present invention is an antimicrobial agent exhibiting non-dissolution characteristics, when used as a coating agent for a group of parts that come into contact with drinking water, it exhibits an excellent effect in preventing contamination by bacteria, mold, etc.
[0050] In particular, the antimicrobial glass composition according to an embodiment of the present invention can provide an antimicrobial glass powder with excellent durability by suppressing unintended oxidation reactions.
[0051]
[0052] Hereinafter, the role and content of each component of the antibacterial glass composition according to an embodiment of the present invention will be described in detail.
[0053]
[0054] SiO2 and B2O3 are network-forming oxides that form the skeletal structure of glass and are key components that enable vitrification through covalent bonding.
[0055] SiO2 is a glass-forming agent that enables vitrification, and it is a key component that plays a role as a framework in the structural aspect of glass. If SiO2 is included in an amount exceeding an appropriate amount, the viscosity of the glass increases when melted, which reduces workability and yield during the cooling process. In addition, SiO2 does not act as a direct component that exerts antibacterial activity, but it forms OH groups on the glass surface compared to P2O5, a representative network-forming oxide. - It is advantageous in forming less charge and making the glass surface positively charged by the metal ions in the glass.
[0056] Therefore, it is preferable that SiO2 be added in a content ratio of 15 to 32 wt% of the total weight of the antibacterial glass composition according to the present invention. When the amount of SiO2 added is less than 15 wt%, the network-forming oxide may be insufficient, which may cause the glass to go beyond the vitrification region, resulting in opalescence or heterogeneity in which transparent glass is mixed. On the other hand, when the amount of SiO2 added exceeds 32 wt%, it may be difficult to control the surface charge of the glass to a positive value, resulting in a decrease in antibacterial power.
[0057]
[0058] B2O3 is a representative network-forming oxide and, along with SiO2, is a key component that enables sufficient vitrification. Because B2O3 has a low melting point, it is used to lower the eutectic point of the melt. Furthermore, B2O3 helps to create a homogeneous glass by increasing the solubility of rigid components (such as TiO2) during melting for vitrification. However, if B2O3 is added beyond a certain level, it can weaken the bonding structure of the glass, which can lead to problems such as reduced water resistance.
[0059] Conventional antibacterial glass compositions controlled the elution of metal ions that exhibit antibacterial performance by adjusting the B2O3 content. In the present invention, since alkali oxides are excluded from the composition to impart antioxidation properties as described below, B2O3 becomes a key component that supports ZnO in the glass and controls the structure. B2O3 exists in two coordination numbers of [BO3] / [BO4] in the glass. When ZnO is present with B2O3, O-Zn-O covalent bonds are possible depending on the coordination number of B2O3, and Zn 2+ Ionic bonds are also present in a mixed manner. In the present invention, antibacterial properties are realized through the local charge of Zn.
[0060] For this purpose, it is preferable that B2O3 be added in a content ratio of 12 to 32 wt% of the total weight of the antibacterial glass composition according to the present invention. If B2O3 is added in an amount less than 12 wt%, the glass may go beyond the vitrification region due to insufficient flux, resulting in non-melting. Conversely, if B2O3 exceeds 32 wt%, the durability and water resistance of the glass may deteriorate due to the inherent properties of the element, resulting from structural problems of B within the network-forming structure.
[0061]
[0062] ZnO is a component that acts as both a network-forming oxide and a modifying oxide by covalently bonding with and substituting for some of the network-forming oxides. Furthermore, ZnO is a component that significantly contributes to the development of antibacterial effects.
[0063] This ZnO is an intermediate oxide, and in order to participate in the network-forming structure in glass, the atomic radius must be small and the electronegativity must be high so that the difference with oxygen is small. This intermediate oxide is a component that has a larger atomic radius and lower electronegativity than the typical network-forming oxides, Si, P, and B, so it is difficult to form glass on its own, but it plays that role by substituting for the network-forming oxide in the presence of the network-forming oxide. Below a certain content, this ZnO only functions as a modifier oxide, but above a certain content, it forms a covalent bond, radically improving durability. Here, the certain content is determined by the content of the network-forming oxide and the modifier oxide.
[0064] Therefore, it is preferable that ZnO be added in a content ratio of 42 to 69 wt% of the total weight of the antibacterial glass composition according to the present invention. If ZnO is added in an amount less than 42 wt%, there is a problem in that sufficient antibacterial activity is not exhibited because the absolute amount of the substance exhibiting antibacterial activity is insufficient. On the other hand, if ZnO is added in excess of 69 wt%, it cannot exist in an ionic state within the glass in a homogeneous manner, but partially forms crystals and goes beyond the vitrification region, resulting in opalescence and a heterogeneous phenomenon in which transparent glass is mixed.
[0065]
[0066] In the present invention, CaO, BaO, and SnO are used to lower the melting point of the antibacterial glass. The addition of specific amounts of these components to the antibacterial glass composition results in a decrease in the viscosity of the antibacterial glass. Since the antibacterial glass composition of the present invention contains a high content of ZnO and does not contain alkaline oxides, it is important to lower the melting point by adding trace amounts of these components.
[0067] The antibacterial glass composition of the present invention contains 1 to 10 wt% of at least one of CaO, BaO, and SnO.
[0068] If the content of the above components is less than 1 wt%, the melting point lowering function is not fully developed, which can lead to the problem of unmelted products. In addition, if the content of the above components exceeds 10 wt%, immiscibility may occur, resulting in phase separation into zinc borate and alkaline earth silicate.
[0069] Preferably, the present invention may include 1 wt% or more of CaO within the above content range to obtain a more excellent melting point lowering effect.
[0070]
[0071] Conventional antibacterial glass compositions contain alkaline oxides. Representative examples of alkaline oxides include Na2O and K2O. Alkali oxides are oxides that essentially function as modifiers that form non-crosslinking bonds within glass. While alkaline oxides alone cannot vitrify, vitrification becomes possible when mixed with network-forming agents such as SiO2 and B2O3 in a certain ratio. Furthermore, when alkaline oxides are incorporated into glass as a single component, the durability of the glass continually deteriorates within the vitrifiable range. However, when two or more alkaline oxides are incorporated into glass, the durability of the glass can be improved again, depending on the ratio. This is called the mixed alkali effect.
[0072] However, the present invention is characterized by the exclusion of alkali oxides. While alkali oxides have the advantage of lowering the melting point of glass, the present invention excludes them to prevent problems caused by the dissolution of alkali ions. During the corrosion / dissolution process of glass, the sizes of H3O+ present in moisture and alkali ions are similar, leading to easy substitution. In particular, alkali ions are weakly bonded within the glass, so they are the first to be dissolved. These dissolved ions have the following two problems. First, since the alkali ions dissolved from the antibacterial glass gain electrons, products containing antibacterial glass as an additive lose electrons. Consequently, the products are damaged by the oxidation reaction caused by the loss of electrons. For example, plastic injection molding products are critically susceptible to oxidation, resulting in deterioration of the mechanical properties of the manufactured product or, in extreme cases, failure of the synthesis process. Second, trace amounts of dissolved alkali ions can bind OH ions to the surface, creating a slight haze. Consequently, dissolved alkali ions can reduce the transparency of the glass and, in some cases, increase the likelihood of crystallization.
[0073] The present invention proposes a novel composition system that can satisfy all properties such as antibacterial properties, durability, and longevity while excluding alkaline oxides.
[0074]
[0075] In addition, the antibacterial glass composition of the present invention contains 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2, and GeO2. These components have the function of enhancing the durability of the antibacterial glass while assisting in the vitrification of the antibacterial glass. If the above components are used in an amount of less than 1 wt%, the durability of the antibacterial glass is not sufficiently enhanced, and thus continuous use is not possible. In addition, if these components are used in an amount exceeding 11 wt%, the alkaline earth component, which is a substance that melts at high temperatures, does not sufficiently melt, so it goes beyond the vitrification range, and a phenomenon of unmelted matter being formed occurs.
[0076]
[0077] Next, the antibacterial glass composition of the present invention may further include at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 in order to realize a color with high transparency, and preferably, at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 may be included in an amount of 0.4 to 4 wt%. If the content is outside the above range, the color may fail to be realized or the durability and antibacterial performance of the antibacterial glass may be reduced.
[0078]
[0079] Conventional antibacterial glasses exhibit antibacterial properties through the release of ions, which exert their antibacterial properties. This performance is determined by the design of the skeletal structure and the selection of antibacterial-active substances. This means that while the amount of ions released varies depending on the strength of the skeletal structure, they are ultimately consumable.
[0080]
[0081] The antibacterial glass composition of the present invention is characterized by being water-insoluble and not exhibiting antibacterial properties through ion leaching. It is difficult to directly correlate the individual components released upon exposure to water with antibacterial activity on a ppb basis. It is understood that the antibacterial properties exhibited on their own, without ion leaching, are due to the presence of ions and electron transfer within the solid glass, depending on the ratio of the components, resulting in surface charge (ZetaPotential) and the formation of reactive oxygen species (ROS).
[0082] Injection moldings and window glass have a surface charge of -100 mV. Regardless of whether they are Gram-negative or Gram-positive, the cell membrane surface exhibits a negative charge. The antibacterial glass composition of the present invention has a surface charge of -10 to +10 mV, and this difference in charge causes bacteria to be adsorbed to the antibacterial glass surface. The adsorbed strains enter a state of charge disturbance due to the relatively positive charge of the antibacterial glass, which leads to a severe stress state and a weakening of the cell membrane.
[0083] Strains produce small amounts of ROS during their basal metabolic processes. However, when ROS generated by antibacterial glass are added, external factors cause a rapid increase in ROS concentration, resulting in oxidative stress. This can lead to the destruction of cell membranes, DNA, and proteins.
[0084] Consequently, the antibacterial glass composition of the present invention exhibits antibacterial properties non-consumptively, as ions are released and do not directly affect bacteria, but rather exert their antibacterial effects through charge and oxidative stress. Accordingly, even if the content of components such as Ag, Mn, Ga, Te, La, and Cu, which typically exhibit strong antibacterial properties, is absent or very small, sufficient antibacterial activity is exhibited.
[0085] In addition, as described above, the antibacterial glass composition of the present invention does not contain alkaline oxides, and thus it can be seen that the oxidation prevention performance of the applied product is also excellent.
[0086]
[0087] Method for producing antibacterial glass powder
[0088]
[0089] Hereinafter, a method for manufacturing an antibacterial glass powder according to an embodiment of the present invention will be described with reference to the attached drawings.
[0090] Figure 1 is a process flow diagram showing a method for manufacturing antibacterial glass powder according to an embodiment of the present invention.
[0091] As illustrated in FIG. 1, the method for manufacturing antibacterial glass powder according to an embodiment of the present invention includes a mixing step (S110), a melting step (S120), a cooling step (S130), and a crushing step (S140).
[0092]
[0093] mix
[0094] In the mixing step (S110), a composition including 15 to 32 wt% of SiO2, 12 to 32 wt% of B2O3, 42 to 69 wt% of ZnO, 1 to 10 wt% of at least one of CaO, BaO, and SnO, and 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2, and GeO2 and not including an alkaline oxide is mixed and stirred to form an antibacterial glass composition.
[0095] The characteristics of the above antibacterial glass composition are as described above.
[0096]
[0097] melting
[0098] In the melting step (S120), the antibacterial glass composition is melted.
[0099] In this step, melting is preferably performed at 1,100 to 1,400°C for 1 to 60 minutes. If the melting temperature is lower than 1,100°C or the melting time is lower than 1 minute, the antimicrobial glass composition may not be completely melted, which may cause incompatibility of the glass melt. Conversely, if the melting temperature exceeds 1,400°C or the melting time exceeds 60 minutes, excessive energy and time are required, which is not economical.
[0100]
[0101] cooling
[0102] In the cooling step (S130), the molten antibacterial glass composition is cooled to room temperature.
[0103] At this stage, cooling is preferably performed in a furnace. If air or water cooling is used, the antibacterial glass may experience severe internal stress, which may lead to cracks in some cases. Therefore, furnace cooling is preferred.
[0104]
[0105] smash
[0106] In the crushing step (S140), the cooled antibacterial glass is crushed. At this time, any of the commonly known ball mills, jet mills, and planetary mills can be used for crushing.
[0107] By this crushing, the antibacterial glass is finely crushed to produce antibacterial glass powder. The antibacterial glass powder preferably has an average diameter of 30 μm or less, and a more preferred range is 2 to 12 μm.
[0108]
[0109] Meanwhile, a home appliance according to an embodiment of the present invention comprises a resin material and a plastic injection molded product to which antibacterial glass powder manufactured by the method described above has been added. The home appliance used in the present invention may include, but is not limited to, a water purifier, a washing machine, a stand air conditioner, a system air conditioner, a refrigerator, and the like.
[0110]
[0111] Here, the plastic injection molding comprises 95.0 to 99.0 wt% of resin material and 1.0 to 5.0 wt% of antibacterial glass powder.
[0112] If the amount of antibacterial glass powder added is less than 1.0 wt% of the total weight of the plastic injection molded product, the antibacterial activity against Pseudomonas aeruginosa may not be sufficient. Conversely, if the amount of antibacterial glass powder added is excessive, exceeding 5.0 wt% of the total weight of the plastic injection molded product, the mechanical properties may deteriorate.
[0113] The resin material includes at least one of PP (polypropylene), PC (polycarbonate), EPDM (ethylene propylene rubber), ABS (acrylonitrile-buradiene-styrene), and HIPS (high impact polystyrene).
[0114] At this time, the antibacterial glass powder has the same components as the antibacterial glass composition described above.
[0115]
[0116] Additionally, the plastic injection molded product may contain functional additives in addition to the antibacterial glass powder. The functional additives may include one or more selected from the group consisting of antioxidants, foaming agents, impact modifiers, nucleating agents, and coupling agents.
[0117] Accordingly, the home appliance according to the embodiment of the present invention is applied to the surface of a part that is vulnerable to bacterial growth and has a lot of contact with moisture, and has an antibacterial effect that can prevent the inhabitation and growth of various microorganisms.
[0118]
[0119] In addition, the antibacterial glass powder of the present invention can be used not only as an injection molded product but also as a coating material for glass shelves, or as an additive for paint or powder coating.
[0120]
[0121] Example
[0122] Hereinafter, the structure and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.
[0123] Anything not described here will be omitted as it is technically feasible for those skilled in this field to infer.
[0124]
[0125] 1. Preparation of antibacterial glass powder samples
[0126]
[0127] Table 1 shows the composition and composition ratio of the antibacterial glass compositions of the examples and comparative examples.
[0128] The antimicrobial glass compositions having the compositions described in the above examples and comparative examples were each melted in an electric furnace at a temperature of 1,200°C, and then cooled in the form of glass bulk on a stainless steel plate by air cooling. Thereafter, the obtained glass was pulverized using a dry grinder (ball mill), and an antimicrobial glass powder sample having a D50 particle size of 2 to 12 μm was prepared.
[0129] Here, the raw materials for the components CaO and BaO were used by calculating the stoichiometry of CaCO3 and BaCO3, respectively, and the remaining components were the same as those described in Tables 1 and 2. In addition, vitrification was classified based on the case where a homogeneous glassy state was observed and the phenomenon of opalescence and unmelted matter occurring.
[0130]
[0131] Classification Implementation Preliminary Comparative Example 1 2 3 4 5 1 2 3 4 SiO 2 2 0 1 6 8 1 5 1 1 7 6 3 1 8 2 5 4 5 2 0 3 5 7 B 2 O 3 1 9 5 1 2 4 3 1 4 1 8 4 1 4 2 8 4 4 0 2 0 5 8 ZnO 5 4 1 6 8 4 2 2 5 1 9 4 7 1 3 3 6 5 2 5 4 9 8 CaO 4 5 1 4 4 1 2 1 6 2 4 1 5 0 0 BaO 0 0 2 8 0 4 0 5 4 0 1 SnO 0 0 1 1 0 2 1 0 7 0 0 Al 2 O 3 1 0 7 0 4 9 0 ... 3.10.80000TiO2000.300.80050GeO2000.32.100000CuO0000.21.20000.5F e2O300.100.20.80000MoO30.30.10000000Co3O4001.1000000MnO20.40.20 0000.800Bi2O3000.801.53.8000Total100100100100100100100100100
[0132]
[0133] 2. Evaluation of antibacterial glass powder properties
[0134] Table 2 shows the results of property evaluation for samples manufactured according to examples and comparative examples.
[0135]
[0136] 1) Measurement of antibacterial power
[0137] For the examples and comparative examples in which vitrification was performed homogeneously, an antibacterial evaluation was performed on four bacteria (Staphylococcus aureus, Escherichia coil, Klebsiella pneumoniae, Pseudomonas aeruginosa) according to the shaking flask method (ASTM E2149-13a).
[0138]
[0139] 2) Antibacterial power measurement after durability evaluation
[0140] In order to evaluate the durability of the homogeneously vitrified examples and comparative examples, the antibacterial activity test was additionally conducted after exposure to moisture using the ASTM C1285-14 (glass and glass ceramic durability evaluation method) test method (50℃, 32 hours).
[0141]
[0142] Classification Preliminary Comparative Example 123451234 Vitrification (O, X) OOOOOOOXX Antibacterial activity Staphylococcus aureus 99.9% 99.9% 99.9% 99.9% 99.9% 94.6% 99.9% -- Escherichia coli 99.9% 99.9% 99.9% 99.9% 99.9% 80.6% 99.9% -- Klebsiella pneumoniae 99.9% 99.9% 99.9% 99.9% 99.9% 74.4% 99.9% -- Pseudomonas aeruginosa 99.9% 99.9% 99.9% 99.9% 99.9% 43.8% 99.9% -- (After durability evaluation) Antibacterial activity Staphylococcus aureus99.9%99.9%99.9%99.9%99.9%26.8%54.4%--Escherichia coil99.9%99.9%99.9%99.9%99.9%32.8%57.6%--Klebsiella pneumoniae99.9%99.9%99.9%99.9%99.9%43.8%65.4%--Pseudomonas aeruginosa99.9%99.9%99.9%99.9%99.9%11.7%32.8%--
[0143]
[0144] As shown in Table 2, the samples manufactured according to Examples 1 to 5 exhibited antibacterial activity of 99% or more against all four strains of bacteria. Furthermore, the samples manufactured according to Examples 1 to 5 all exhibited antibacterial activity of 99% or more when measured for antibacterial activity after exposure to moisture according to a durability evaluation method.
[0145] On the other hand, in the case of comparative examples 3 and 4, vitrification did not proceed homogeneously.
[0146] In addition, none of the samples manufactured according to Comparative Examples 1 and 2 exhibited good antibacterial activity against all four strains.
[0147]
[0148] Although the present invention has been described with reference to the drawings exemplified above, it is to be understood that the present invention is not limited to the embodiments and drawings disclosed herein, and that various modifications may be made by those skilled in the art within the scope of the technical idea of the present invention. Furthermore, even if the operational effects according to the configuration of the present invention have not been explicitly described while describing the embodiments of the present invention, it is natural that the effects predictable by the corresponding configuration should also be acknowledged.
Claims
1. SiO2 15 ~ 32 wt%; B2O312 ~ 32 wt%; ZnO 42 to 69 wt%; 1 to 10 wt% of at least one of CaO, BaO and SnO and Contains 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2 and GeO2 Does not contain alkaline oxides Antibacterial glass composition.
2. In paragraph 1, Containing at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Antibacterial glass composition.
3. In paragraph 2, Further containing 0.2 to 4 wt% of at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Antibacterial glass composition.
4. In paragraph 1, Containing 1 wt% or more of the above CaO Antibacterial glass composition. 5.(a) SiO2 15 ~ 32 wt%; B2O312 ~ 32 wt%; ZnO 42 to 69 wt%; 1 to 10 wt% of at least one of CaO, BaO and SnO and A step of forming an antibacterial glass composition by mixing and stirring a composition containing 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2 and GeO2 and not containing an alkali oxide; (b) a step of melting the antibacterial glass composition; (c) a step of cooling the molten antibacterial glass composition; and (d) a step of crushing the cooled antibacterial glass; Method for manufacturing antibacterial glass powder.
6. In paragraph 5, In step (a) above, The above antibacterial glass composition Containing at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Method for manufacturing antibacterial glass powder.
7. In paragraph 6, In step (a) above, The above antibacterial glass composition Further containing 0.2 to 4 wt% of at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Method for manufacturing antibacterial glass powder.
8. In paragraph 5, Containing 1 wt% or more of the above CaO Method for manufacturing antibacterial glass powder.
9. In paragraph 5, In step (b) above, The above melting is Performed at 1,100 to 1,400℃ for 1 to 60 minutes Method for manufacturing antibacterial glass powder.
10. A home appliance including a plastic injection molded product with antibacterial glass powder added to the resin material, The above plastic injection molded product 95.0 to 99.0 wt% of the above resin material; and Contains 1.0 to 5.0 wt% of the above antibacterial glass powder; The above antibacterial glass powder SiO2 15 ~ 32 wt%; B2O312 ~ 32 wt%; ZnO 42 to 69 wt%; 1 to 10 wt% of at least one of CaO, BaO and SnO and Contains 1 to 11 wt% of at least one of Al2O3, ZrO2, CeO2, TiO2 and GeO2 and does not contain alkali oxides Home appliances.
11. In paragraph 10, The above resin material Containing at least one of PP (polypropylene), PC (polycarbonate), EPDM (ethylene propylene rubber), ABS (acrylonitrile-buradiene-styrene), and HIPS (high impact polystyrene). Home appliances.
12. In paragraph 10, The above antibacterial glass powder Containing at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Home appliances.
13. In paragraph 10, The above antibacterial glass powder Further containing 0.2 to 4 wt% of at least one of CuO, Fe2O3, MoO3, Co3O4, MnO2, and Bi2O3 Home appliances.
14. In paragraph 10, The above antibacterial glass powder Containing 1 wt% or more of the above CaO Home appliances.
Citation Information
Patent Citations
Antimicrobial water-insoluble silicate glass powder and glass powder mixture
JP2005525985A
Antibacterial glass powder and antibacterial fiber
JP2009023877A
Antibiotic container and product method thereof
KR1020160069052A
machine carrying handle
KR1020220168730A
Micro-needle patch manufacturing method
KR1020230012358A