Method for preparing recycled polyolefin resin
The integration of nonionic surfactants and chitosan in the washing process effectively addresses the challenge of foreign substance and odor removal in polyolefin resin recycling, ensuring improved cleaning and maintaining resin quality by preventing re-attachment and utilizing chitosan's antibacterial properties for odor inhibition.
Patent Information
- Application Number
- PCT/KR2024/004895
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-08
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-24
AI Technical Summary
Current methods for recycling polyolefin resins often fail to effectively remove foreign substances and odors, leading to deterioration of physical properties in the final product, particularly due to the re-attachment of small floating contaminants during the washing process.
A method involving the use of a nonionic surfactant and chitosan in the washing process to separate and prevent the re-attachment of foreign substances, utilizing a washing machine with a rotating member to enhance cleaning efficiency and incorporating chitosan's antibacterial properties to inhibit microbial growth and odor removal.
The method significantly improves foreign matter and odor removal, preventing re-attachment of contaminants and maintaining the physical properties of the recycled polyolefin resin, with optimal results achieved using a nonionic surfactant at 100 to 150 ppm and a chitosan-to-surfactant ratio of 0.2:1 to 2:1.
Smart Images

Figure PCTKR2024004895-APPB-IMG-000001 
Figure PCTKR2024004895-APPB-IMG-000002 
Figure PCTKR2024004895-APPB-IMG-000003
Abstract
Description
Method for producing polyolefin recycled resin
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0051538, filed April 19, 2023, and Korean Patent Application No. 10-2024-0047361, filed April 8, 2024, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a method for producing a polyolefin (PO) recycled resin, and more particularly, to a method for producing a PO recycled resin having improved effects in removing foreign substances and odors.
[0005] The use of plastics is increasing as plastics with the properties required for various applications and purposes are developed. Generally, plastics consume significant energy from crude oil extraction to manufacturing, and the process emits significant carbon emissions. Furthermore, when the plastic contained in the final product is discarded along with it, environmental pollution and the social costs associated with its disposal are incurred. Therefore, recycling discarded plastics is essential to reduce energy consumption, carbon emissions, and environmental pollution. Plastics made by recycling plastics discarded by end consumers are called post-consumer recycled (PCR) resins, and ongoing efforts are being made to obtain PCR resins with the desired purity and properties.
[0006] Meanwhile, polyolefin resins are thermoplastic polymers manufactured by polymerizing olefins (hydrocarbons containing one double bond per molecule) such as ethylene and propylene. They exhibit different properties depending on their density, and are used as raw materials for various products based on their density. For example, high density exhibits plasticity, rigidity, and uniformity, while low density exhibits elasticity, transparency, and flexibility like liquid or rubber. Therefore, high-density polyethylene (HDPE) is used in products requiring high strength, low-density polyethylene (LDPE) is used in products requiring high transparency, and linear low-density polyethylene (LLDPE) is mainly used in film production due to its excellent formability. These polyolefin resins are widely used commercially due to their low prices, and they account for a significant portion of the waste plastic currently generated.
[0007] Generally, recycling methods for waste plastic (resin) include mechanical, chemical, and thermal recycling. Mechanical recycling involves crushing and sorting collected waste plastic, separating it by type, melting it using an extruder, and pelletizing it. This process involves mixing it with virgin plastic at a specific ratio or reinforcing it with functional additives to create resin products. Chemical recycling utilizes various chemical means to extract specific polymers from waste plastic or recover pure single molecules for repolymerization. Thermal recycling involves incinerating waste plastic to recover heat energy.
[0008] When processing waste polyolefin resin using the above mechanical recycling method, if foreign substances are included, oxidation of the foreign substances may occur during the melting process using the extruder, which may cause an unpleasant odor, and the residual foreign substances may cause a deterioration in physical properties. For example, agricultural mulching film not only contains a large amount of various foreign substances such as soil, straw, and paper, but also, due to the nature of its use, it includes a fermentation process caused by microbial growth, which may cause an unknown unpleasant odor during the pelletization process. In addition, stretch film made of LLDPE, which is widely used for packaging, may contain foreign paper substances such as delivery labels and foreign substances from other types of films (e.g., PVC, PET, etc.). In particular, the cellulose component that constitutes the paper foreign substances is difficult to completely remove, and if the residual cellulose flows into the extruder, it will be oxidized by the high temperature, which not only causes an unpleasant odor, but also may cause a color change due to carbonization.
[0009] Typically, when producing PCR (post-consumer recycled) resin by recycling waste plastic, washing is performed during the pretreatment process to prepare the raw resin, i.e. the base resin, before feeding it to the extruder. However, the effect is minimal, and the final product may contain foreign substances and have a strong odor.
[0010] To produce high-value-added recycled resin, additional wet washing of the raw resin is necessary. The washing effect can be enhanced by using additives that remove various contaminants through chemical reactions. These additives can be selected based on factors such as washing performance, action on impurities, rinsability, and price. Surfactants are representative washing additives.
[0011] The above surfactants, through their chemical structure comprising hydrophobic and hydrophilic groups, soften the interface boundary, and the hydrophobic groups effectively penetrate the contaminants and separate them from the surface. These surfactants can be classified as anionic, cationic, amphoteric, and nonionic depending on the charge of the hydrophilic portion when dissociated in water. Among these, nonionic surfactants facilitate oil / water separation by not generating ionic repulsion, and thus may be suitable for removing organic contaminants remaining in resins used as agricultural mulching films.
[0012] In addition, the above surfactants may have different characteristics depending on the modification of their chemical structure. Among nonionic surfactants, the EO / PO type, which is composed of ethylene oxide (EO) and propylene oxide (PO) as a block copolymer, has the advantage of being able to control the cleaning effect, rinsing property, and foaming rate depending on the temperature depending on the ratio of EO and PO as repeating units.
[0013] When the base resin is placed in water containing the aforementioned nonionic surfactant and washed by high-speed rotation of the rotating member, foreign matter separated from the resin floats in the water. Most of the separated foreign matter is composed of cellulose components. While relatively large floating foreign matter can naturally settle, small floating foreign matter can remain suspended in the water and reattach to the resin. This can result in odor and deterioration of physical properties during the extrusion stage.
[0014] Therefore, a technology is needed to improve the washing effect by inducing sedimentation of small floating foreign substances separated in the wet washing step of the above-described resin and preventing re-attachment on the resin.
[0015] The present invention is intended to solve the problems mentioned in the background technology of the above invention, and provides a method for producing a regenerated polyolefin resin that can prevent re-attachment of foreign substances separated in the washing step of a raw resin prepared by pretreating waste polyolefin, thereby improving the effect of removing foreign substances and odors and suppressing deterioration of physical properties.
[0016] According to one embodiment of the present invention for solving the above problem, a method for producing a regenerated polyolefin resin is provided, comprising the steps of: introducing a base resin containing polyolefin and washing water into a washing machine equipped with a rotating member, and washing the base resin by a wet friction method through high-speed rotation of the rotating member; and supplying the washed base resin to an extruder and extruding it, wherein the washing water contains water, a nonionic surfactant, and chitosan.
[0017] Additionally, the present invention provides a regenerated polyolefin resin comprising at least one selected from a nonionic surfactant, chitosan, and a degradation product thereof.
[0018] According to the present invention, in the washing step of a base resin obtained by pretreating waste polyolefin resin, the separation of foreign substances is promoted by using a nonionic surfactant, and the combined use of chitosan prevents the separated foreign substances from being reattached to the base resin, thereby improving the effect of removing foreign substances, and at the same time, a regenerated polyolefin resin with no odor can be manufactured through the antibacterial action, such as inhibition of microbial growth, inherent to chitosan.
[0019] In particular, by using the nonionic surfactant at 100 to 150 ppm based on the total weight of the washing water and adjusting the weight ratio of the nonionic surfactant and chitosan to a range of 0.2:1 to 2:1, the effect of removing foreign substances and odors can be maximized.
[0020] The terms or words used in the description and claims of the present invention should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0021] In the present invention, polyolefin resin is a concept that collectively refers to a homopolymer, copolymer and / or block (co)polymer containing units of ethylene and / or propylene, as well as a composition containing these polymers.
[0022] Meanwhile, in the present invention, the base resin is a polyolefin resin that has been separated and recovered from a discarded product and then pretreated, and may contain impurities or foreign substances. The resin manufactured from the base resin by the method for manufacturing a recycled resin of the present invention is defined as a recycled polyolefin resin. Furthermore, in order to apply the recycled polyolefin resin to a product, a resin in which the recycled resin and a new material are mixed or an additive is added to impart desired properties is called a PCR (post-consumer recycled) polyolefin resin.
[0023] Hereinafter, the present invention will be described in more detail to help understand the present invention.
[0024] A method for producing a regenerated polyolefin resin according to one embodiment of the present invention may include a step of washing a base resin, and a step of supplying the washed base resin to an extruder and extruding it.
[0025] The above-described resin may include a polyolefin resin that has been separated and recovered from a discarded product and then subjected to pretreatment.
[0026] The above polyolefin resin includes a homopolymer, copolymer and / or block (co)polymer containing units of ethylene and / or propylene, and a representative example thereof is polyethylene. The polyethylene is classified into HDPE (high-density polyethylene), MDPE (medium-density polyethylene), LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), VLDPE (ultra-low-density polyethylene), etc. depending on the density, and is appropriately selected and used depending on the characteristics of the product. In particular, low-density polyethylene resin (LDPE), linear low-density polyethylene resin (LLDPE), or a mixture thereof, which have excellent transparency and moldability, are used as agricultural mulching films because they are effective in managing weeds, moisture, and temperature in the soil.
[0027] Polyolefin resins used in various products, including the aforementioned agricultural mulching films, can be recovered from discarded products and recycled as raw materials for post-consumer recycled (PCR) resins. To use the recovered waste polyolefin resin as a base resin for PCR resins, it must undergo pretreatment processes such as sorting, crushing, washing, and drying before being fed to an extruder.
[0028] The above sorting is the process of separating waste polyolefin resin from waste products and then classifying it by material, size, etc., and can be done by various methods such as a classification method using wet or dry specific gravity, a classification method using a near-infrared spectrometer, and an electrostatic separation method using electrostatic properties. In this sorting process, foreign substances other than resin, such as metal components or fiber components, can be separated first, and as large foreign substances in the waste resin are removed, the overall foreign substance content is reduced.
[0029] The above-mentioned selected waste polyolefin resin can be crushed into small pieces to facilitate the smooth operation of subsequent processes. For example, the waste polyolefin resin can be fed into a large-capacity shredder equipped with a knife and cut into a uniform and consistent size, for example, 60 mm or less. Additionally, wet crushing can be performed by supplying washing water during the crushing of the waste polyolefin resin.
[0030] The shredded waste polyolefin resin is often contaminated or mixed with foreign substances such as chemicals, organic matter, sand, and stones. Therefore, removal of these foreign substances is necessary for subsequent processing. For example, the shredded waste polyolefin resin is fed into a washing machine and pre-washed with water.
[0031] The above pre-washing can be performed using a centrifugal method in a water-filled washing machine, which removes heavy substances by allowing them to settle to the bottom and recovers those that float to the surface. This method removes large foreign substances from the wastewater, thereby reducing the overall foreign substance content.
[0032] Thereafter, the waste polyolefin resin, from which foreign substances have been removed through the above-described pre-washing, can be pulverized for granulation suitable for feeding into an extruder. For example, the waste polyolefin resin can be pulverized into appropriately sized flakes or particles (pellets or fine powder) using a device such as a jaw crusher, an impact crusher, a cross jet mill, a roller mill, or a rod mill.
[0033] Through this crushing, the waste polyolefin resin can be in the form of flakes or particles having an average particle size of 4 to 10 mm, specifically 5 to 8 mm, and when the average particle size range is satisfied, the feed to the extruder can proceed smoothly in the subsequent process.
[0034] The waste polyolefin resin after the above-mentioned grinding may still contain some foreign matter. Therefore, to remove the fine foreign matter contained in the ground waste resin, equipment utilizing magnetic force, wind power, centrifugal force, gravity, etc. can be used to separate and remove the fine foreign matter. In this case, a wet method that supplies washing water may be applied.
[0035] The above pretreatment process can be appropriately selected and modified as needed, and is not particularly limited as long as it is a means capable of providing a base resin in a state suitable for being supplied to an extruder.
[0036] The waste polyolefin resin that has undergone the above pretreatment can be used as a base resin for producing a PCR resin.
[0037] Meanwhile, the above-described resin may still contain trace amounts of foreign substances even after pretreatment, and in particular, in the case of resin recovered from agricultural mulching films, a fermentation process may be included due to the nature of the use, which may cause an unpleasant odor.
[0038] Accordingly, the present invention additionally performs wet friction washing on the base resin that has undergone the above-described pretreatment. Specifically, the base resin and washing water are introduced into a washing machine equipped with a rotating member, and washing is performed by rotating the rotating member at high speed.
[0039] The above washing solution may contain a nonionic surfactant and chitosan used as a washing promoter together with water.
[0040] Surfactants generally soften the interface barrier through their chemical structure, which includes hydrophobic and hydrophilic groups. These hydrophobic groups effectively penetrate contaminants and separate them from the surface. Nonionic surfactants, in particular, do not generate ionic repulsion, facilitating oil / water separation. Therefore, they can be advantageously used to remove organic contaminants remaining in resins used as agricultural mulching films.
[0041] In one embodiment of the present invention, the nonionic surfactant may include a propylene oxide-ethylene oxide block copolymer.
[0042] More specifically, the propylene oxide (PO)-ethylene oxide (EO) block copolymer is (EO) x (PO) y (EO) x It can be expressed by the chemical formula (EO), wherein the polyoxyethylene on both sides constitutes a hydrophilic chain and the polyoxypropylene in the center constitutes a hydrophobic chain, which may be a nonionic triblock copolymer. The chemical formula (EO) x (PO) y (EO) x Depending on the x and y values of the copolymer, the molecular weight and PO ratio of the copolymer may vary, and in particular, the PO ratio is a factor that determines the toxicity and solubility in the application of the copolymer.
[0043] For example, the nonionic PO / EO block copolymer used in the present invention has a polystyrene-equivalent weight average molecular weight (hereinafter referred to as “weight average molecular weight (Mw)”) of 9,000 to 15,000, specifically 11,000 to 13,000, as measured by gel permeation chromatography (GPC; using tetrahydrofuran as an eluting solvent), and the proportion of propylene oxide (PO) in the copolymer may be 20% to 40%, specifically 25% to 35% of the total molecular weight. When the above range is satisfied, it exhibits low toxicity and high solubility, thereby being effective in controlling the cleaning effect, rinsability, and bubble generation rate of a polyolefin base film. When the PO proportion in the PO / EO block copolymer is too high, it exhibits high hydrophobicity, resulting in poor solubility in water, making it difficult to obtain a sufficient cleaning effect.
[0044] A nonionic surfactant having these characteristics can effectively induce the separation of foreign substances from a polyolefin-based resin during wet friction washing of the resin even when used in a very small amount. For example, the nonionic surfactant can exhibit excellent washing effects when used in an amount of 50 to 200 ppm, preferably 100 to 150 ppm, based on the total weight of the wash water. If the content of the nonionic surfactant is less than 50 ppm, the washing promotion effect may be insufficient. If the content exceeds 200 ppm, excessive foaming may occur, which may cause difficulties in the process, and the possibility of generating an unpleasant odor due to self-oxidation may increase, and the effect of other additives used together may be interfered with.
[0045] When the base resin is placed in water containing the above-described nonionic surfactant and washed by high-speed rotation of a rotating member, foreign matter separated from the resin floats in the water. Most of the separated foreign matter is composed of cellulose components. While relatively large floating foreign matter can naturally settle, small floating foreign matter can remain suspended in the water and reattach to the resin. This can result in the generation of unpleasant odors and deterioration of physical properties during the extrusion stage.
[0046] Accordingly, in the present invention, in order to prevent foreign substances separated in the washing step from floating in water and reattaching to the polyolefin base resin, and to enhance the odor removal effect, chitosan, a natural polymer, is used in combination with the nonionic surfactant.
[0047] Chitosan is a natural biopolymer with a linear polysaccharide structure composed of D-glucosamine and N-acetylglucosamine. It contains functional groups such as hydroxyl and amine groups, and is known to exhibit antibacterial and bactericidal effects by binding to microbial cell membranes and inhibiting microbial growth. When chitosan is used to wash waste polyolefin resin recovered from agricultural mulching films, it will be effective in eliminating odors caused by microbial fermentation.
[0048] Furthermore, because chitosan is structurally similar to cellulose, it can aggregate with foreign matter separated from the resin during the washing process. Specifically, most foreign matter separated in the wash water is composed of cellulose, which possesses numerous hydroxyl groups on its surface. These hydroxyl groups bind to the various functional groups of chitosan, resulting in aggregates that settle to the bottom of the water rather than floating. This sedimentation effect of chitosan can also be beneficial in removing paper foreign matter during the washing of waste polyolefin resin recovered from stretch film used for packaging.
[0049] Meanwhile, chitosan exhibits hydrophilic properties due to the numerous hydroxyl groups present on its surface. However, it forms strong hydrogen bonds with neighboring molecules, making it insoluble in water. However, it is soluble in dilute organic and inorganic acids. Chitosan's solubility is inversely proportional to its molecular weight. Therefore, when adding chitosan to wash water, it is advantageous to select a molecular weight range that ensures water solubility.
[0050] In this respect, the weight average molecular weight (Mw) of chitosan suitable for use in the present invention may be in the range of 4,000 to 700,000, preferably 5,000 to 500,000, and more preferably 10,000 to 200,000. If the molecular weight of the chitosan exceeds 700,000, its water solubility is very low, making it difficult to function as an additive for removing odors and foreign substances, and if it is less than 4,000, the degree of aggregation and sedimentation of foreign substances may decrease.
[0051] As previously explained, the chitosan used in the present invention is structurally similar to cellulose, and thus can aggregate with foreign substances separated from the resin during the washing process. Specifically, the foreign substances separated within the wash water are mostly cellulose components, which possess numerous hydroxyl groups on their surfaces. These hydroxyl groups are then bonded to various functional groups of chitosan, resulting in aggregates that do not float in the water but instead settle downward. Therefore, in a washing machine equipped with a rotating member, aggregated foreign substances can be easily removed by settling to the bottom, while the clean wash water in the upper layer can be recovered and reused.
[0052] In one embodiment of the present invention, the chitosan may be used in an amount of 50 to 1,000 ppm or 100 to 1,000 mm based on the total weight of the wash water. In addition, the chitosan may be added directly to the wash water in a powdered form, or may be added to the wash water in a dissolved form in an acid solution such as acetic acid to increase water solubility.
[0053] Meanwhile, the chitosan can effectively induce coagulation and sedimentation of foreign substances when used in an appropriate mixing ratio with a nonionic surfactant added together. If chitosan is used alone as an additive in the washing step of the base resin, even if the chitosan combines with the cellulose component of the foreign substance to form coagulation, the tendency to settle is reduced, and it is highly likely that it will remain in a suspended state throughout the wash water. As a result, it is difficult for the chitosan and foreign substance coagulation to be separated from the base resin, and they may be introduced together into the extrusion process.
[0054] For example, the weight ratio of the nonionic surfactant and chitosan may be in the range of 0.05:1 to 4:1, preferably 0.2:1 to 2:1, and more preferably 1:1 to 2:1. In particular, when the nonionic surfactant is included in an amount of 100 to 150 ppm based on the total weight of the wash water, and the weight ratio of the nonionic surfactant and chitosan is 0.2:1 to 2:1, the effect of removing foreign substances and removing odors can be maximized.
[0055] If the nonionic surfactant is used in an excess of more than 4 times that of the chitosan, it may cause difficulties in the process due to foaming, and the residue of the nonionic surfactant may cause an unpleasant odor due to oxidation during the extrusion process, and may inhibit the sedimentation of foreign substances in the chitosan. In particular, if the sedimentation of foreign substances is reduced, the possibility of re-contamination by foreign substances that have not settled may increase if the wash water is continuously used. On the other hand, if the content of the chitosan is excessively increased compared to the nonionic surfactant, the chitosan itself may act as a foreign substance, inhibiting the properties of the final manufactured regenerated resin and causing an unpleasant odor.
[0056] The combined use of such nonionic surfactants and chitosan can be applied not only to the above-mentioned washing step, but also to cases where water is added during the pretreatment process of waste polyolefin resin.
[0057] In one embodiment of the present invention, the temperature of the washing water is adjusted to 30 to 50°C, for example, 40 to 45°C, and the rotating member provided in the washing machine is rotated at 1000 to 2000 rpm, for example, 1200 to 1500 rpm, for 1 to 5 minutes, for example, 2 to 3 minutes, to perform the washing step. When the temperature and rotation speed ranges are satisfied, the effect of removing foreign substances / odors can be implemented while preventing damage to the polyolefin base resin.
[0058] If necessary, the washing water may further include a bleach, a sterilizer, an antibacterial agent, a disinfectant, a dispersant, an oxidizer, a pH adjuster, an antifoaming agent, etc. to further enhance the washing effect of the base resin. In particular, the antifoaming agent is intended to remove foam that may be generated from a nonionic surfactant, and an antifoaming agent such as silicone, mineral oil, or a polymer may be used.
[0059] Thereafter, the polyolefin base resin washed through the above process can be manufactured into a regenerated polyolefin resin by supplying it to an extruder and going through an extrusion step.
[0060] The extruder has a function of melting and kneading a base resin and extruding it, and may be, for example, a twin-screw extruder. In addition, the extruder may include a supply port into which the base resin is fed, an outlet located at the other end of the supply port and through which the extrudate is discharged, a cylinder in which the extrusion feed is extruded within the housing of the extruder, a screw located inside the cylinder and rotating to push the extrusion feed or the extrudate toward the outlet, and a heating device provided on the outside of the cylinder to heat the cylinder.
[0061] The temperature inside the extruder may be 150 to 260°C, specifically 190 to 230°C. In the case of an extruder having a cylinder inside the extruder housing, the temperature inside the extruder may refer to the internal temperature of the cylinder. The temperature range inside the extruder as described above is above the melting point and below the deterioration temperature of the polyolefin base resin. However, the temperature range is higher than the extrusion temperature for producing a conventional polyolefin recycled resin. If the polyolefin base resin remains inside the extruder within the above temperature range for a long time, the resin is likely to deteriorate and discolor due to heat, which directly leads to a deterioration in the physical properties of the recycled resin. Therefore, when maintaining the temperature inside the extruder within the range of 150 to 260°C, it is important to minimize adverse effects due to heat by shortening the residence time of the extrusion feed inside the extruder. For example, in the present invention, the residence time of the polyolefin base resin in the extruder may be 0.5 to 10 minutes, and specifically, 1 to 5 minutes.
[0062] Meanwhile, the pressure inside the extruder according to one embodiment of the present invention may be from atmospheric pressure to 100 bar or less. Within the above pressure range, the temperature inside the extruder is easily controlled, and melting and kneading of the polyolefin base resin can be preferably performed.
[0063] In one embodiment of the present invention, the extruded composition discharged from the extruder may be supplied to a pelletizer and pelletized. For example, the extruded composition discharged through the outlet of the extruder may be formed into a desired size through an underwater pelletizer and cooled, thereby ultimately producing a polyolefin recycled resin.
[0064] As described above, according to the present invention, in the washing step of the base resin obtained by pretreating waste polyolefin resin, the separation of foreign substances is promoted by using a nonionic surfactant, and the mixed use of chitosan induces sedimentation by coagulation of the separated foreign substances, thereby preventing the foreign substances from reattaching to the resin, thereby improving the effect of removing foreign substances, and at the same time, a regenerated polyolefin resin with no odor can be manufactured through the antibacterial action, such as inhibition of microbial growth, inherent to chitosan.
[0065] In particular, by using the nonionic surfactant at 100 to 150 ppm based on the total weight of the washing water and adjusting the weight ratio of the nonionic surfactant and chitosan to a range of 0.2:1 to 2:1, the effect of removing foreign substances and odors can be maximized.
[0066] The regenerated polyolefin resin manufactured by the above method may contain at least one selected from the nonionic surfactant used in the washing step, chitosan, and their decomposition products.
[0067] For example, in the case where 50 to 200 ppm of a nonionic surfactant and 50 to 1,000 ppm of chitosan based on the weight of the wash water are used in the washing step of the base resin in the present invention, the final manufactured regenerated resin may contain less than 25 ppm, for example, 4 to 21 ppm, of the nonionic surfactant or its decomposition product and less than 100 ppm, for example, 4 to 99 ppm, of the chitosan or its decomposition product as residues based on the weight thereof.
[0068] Hereinafter, the present invention will be described in more detail by way of examples. However, the following examples are intended to illustrate the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present invention, and the scope of the present invention is not limited to these examples alone.
[0069] Example 1
[0070] Waste linear low density polyethylene (LLDPE) resin recovered from agricultural mulching films was pretreated through a process including sorting, crushing, pre-washing, granulating and classifying, and in the process, large foreign substances were separated and removed, and then crushed to prepare a pellet-shaped LLDPE base resin having an average particle diameter (D50) of 8 mm or less.
[0071] 400g of the above resin, Pluronic with a PO-EO block copolymer structure as a nonionic surfactant in water TM 23 L of washing water (45°C) containing 100 ppm of F127 (PF-127, Mw approximately 12,500) and 100 ppm of chitosan (Mw 120,000) was introduced into a washing machine equipped with a rotating member, and the rotating member was rotated at 1,200 rpm to wash the base resin for 2 minutes. After washing was completed, the base resin and washing water were recovered.
[0072] The washed base resin was supplied to a twin-screw extruder having a cylinder with an inner diameter of 25 mm and a screw length of 800 mm, and melt mixing was performed. At this time, the internal temperature of the extruder was sequentially increased from 150°C at the hopper to 190°C at the die, and the rotation speed of the screw was controlled to 300 rpm and the residence time was controlled to 120 seconds. Thereafter, the composition discharged from the extruder was supplied to a pelletizer to produce a LLDPE recycled resin having an average diameter of 2 mm.
[0073] Comparative Example 1
[0074] LLDPE recycled resin was prepared in the same manner as in Example 1, except that washing of the above-described resin was not performed.
[0075] Examples 2 to 23 and Comparative Examples 2 to 10
[0076] LLDPE recycled resin was manufactured in the same manner as in Example 1, except that the types and contents of additives used in the washing water of the above-described resin were changed to those shown in Table 1 below.
[0077] [Table 1a]
[0078]
[0079] [Table 1b]
[0080]
[0081] Experimental Example 1: Evaluation of Foreign Matter and Odor
[0082] The foreign matter and odor evaluation of the regenerated resin manufactured in the above examples and comparative examples was performed in the following manner, and the results are shown in Table 2 below.
[0083] <Foreign Matter Assessment - Measurement of the Number of Film Gels>
[0084] The manufactured LLDPE recycled resin was extruded using a separate extruder to produce a film specimen with a thickness of 0.04 mm, and then the number of gels in the film was counted using optical equipment (Q-film software, COLLIN). At this time, gels and fibers with a diameter of 100 ㎛ or more in the prepared film specimen were judged as gels and counted, and 0.3 points were added for gels with a diameter of 100 to 300 ㎛, 0.5 points for gels with a diameter of 300 to 500 ㎛, and 1 point for gels with a diameter of 500 ㎛ or more, thereby calculating the foreign matter score of the film.
[0085] <Odor Evaluation>
[0086] The recycled resin was provided to 50 panelists, and scores were given on a scale of 0 to 5, with "3" being the most odorless and "0" being the closest to it. The average score of the 50 panelists was calculated.
[0087] [Table 2a]
[0088]
[0089] [Table 2b]
[0090]
[0091] From the above Table 2, it can be confirmed that Examples 1 to 23 have superior foreign substance removal effects compared to Comparative Example 1, which did not perform a washing step, and Comparative Examples 2 to 10, which used washing water containing no additives or other types of additives, by using washing water containing 50 to 200 ppm of PF-127 as a nonionic surfactant and 50 to 1000 ppm of chitosan having a molecular weight of 4,000 to 700,000 when washing a base resin obtained by pretreating a waste polyolefin resin.
[0092] More specifically, Examples 1 to 5 showed a significantly improved foreign substance removal effect compared to Comparative Example 8, which used PF-127 alone, and Comparative Example 10, which used chitosan (Mw 120,000) alone, when PF-127 was used at 100 to 150 ppm in the wash water and the mixing ratio with chitosan (Mw 10,000 to 200,000) was adjusted to 0.2:1 to 2:1, and the odor evaluation was also equal to excellent. In particular, Examples 1 and 5 showed the lowest foreign substance / odor evaluation scores by adjusting the mixing ratio of PF-127 and chitosan (Mw 120,000) to 1:1 or 2:1.
[0093] Examples 11 and 13 showed similar foreign matter scores to Examples 1 to 4 when the content of chitosan (Mw 120,000) was increased while using PF-127 at 100 to 150 ppm and the acid mixing ratio was adjusted to 0.1:1 to 0.15:1, but the odor evaluation scores were somewhat higher. This is thought to be due to the generation of an unpleasant odor by oxidation of chitosan itself as a result of using an excess of 1,000 ppm of chitosan. Meanwhile, Example 12, in which the content of chitosan (Mw 120,000) was reduced, also showed a somewhat higher odor evaluation score.
[0094] Examples 6, 8 to 10 showed that the foreign matter score and odor evaluation score increased compared to Examples 1 to 4 when the mixing ratio of chitosan (Mw 120,000) was changed from 0.05:1 to 1:1 while reducing PF-127 to 50 ppm. This is because the amount of PF-127 added was small, which reduced the foreign matter separation effect. It is thought that due to the use of insufficient PF-127, even if chitosan coagulates foreign matters, it does not induce sedimentation and remains suspended in the wash water, ultimately worsening the separation of the base resin and foreign matters.
[0095] In Examples 7, 14 to 16, even when the mixing ratio with chitosan (Mw 120,000) was changed from 0.2:1 to 1:4 while increasing PF-127 to 200 ppm, the foreign matter score and odor evaluation score were higher than in Examples 1 to 4. This is thought to be because the excessive amount of PF-127 acts as a foreign matter and self-oxidation occurs, causing an unpleasant odor.
[0096] Meanwhile, Examples 17 to 23 were used under conditions where the mixing ratio of PF-127 and chitosan was 1:1, and the molecular weight of chitosan was changed. It was confirmed that the effect of removing foreign substances and odors was excellent when the molecular weight of chitosan was in the range of 10,000 to 200,000.
[0097] As described above, the combined use of PF-127 and chitosan for polyolefin-based resin improved the foreign substance removal effect compared to the use of PF-127 alone, and when such a combination was used, the odor removal effect was additionally excellent when the concentration of PF-127 in the wash water was 100 to 150 ppm and the mixing ratio of PF-127 and chitosan was 0.2:1 to 2:1.
[0098] Experimental Example 2: Measurement of the Residual Content of Additives in Regenerated Resin
[0099] The residual content of components used as cleaning additives in the recycled resin manufactured in the above example was analyzed by LC-MS (liquid chromatography-mass spectrometry).
[0100] <Preparation of sample solution>
[0101] A sample solution was prepared by dissolving 1 g of regenerated resin in xylene, adding it to ethanol, immersing it, and then filtering the supernatant obtained through centrifugation.
[0102] <Preparation of standard solution>
[0103] - Standard solutions were prepared by completely dissolving PE-64 standard and PF-127 standard as nonionic surfactants in acetonitrile or water, respectively.
[0104] - A standard solution was prepared by dissolving the chitosan standard in a 0.5% acetic acid aqueous solution.
[0105] <LC 분석조건>
[0106] System: Waters HPLC
[0107] Column: C18 column (inner diameter 4.6 mm x length 50 mm, average silica particle size 3.0 μm)
[0108] Mobile phase: Acetonitrile / H2O (containing 0.1% TFA), gradient from 10 / 90 (v / v) to 100 / 0 (v / v)
[0109] Flow rate: 1.0 ml / min
[0110] Column temperature: 40℃
[0111] Injection volume: 10 μl
[0112] <MS 분석조건>
[0113] SIM (selective ion monitoring mode)
[0114] PE-64: m / z=694, PF-127: m / z=801, chitosan: m / z=892
[0115] In the HPLC / MS chromatogram obtained through the above analysis, the area of the peak corresponding to PF-127, chitosan, or their decomposition products, which are additive components used in washing the regenerated resin, was calculated and then substituted into the calibration curve to analyze the residual content of the additive components contained in a sample solution of 1 g of the regenerated resin, and the results are shown in Table 3 below.
[0116] [Table 3]
[0117]
[0118] From the above Table 3, it can be confirmed that in the embodiment of the present invention, when 50 to 200 ppm of PF-127 (nonionic surfactant) and 50 to 1,000 ppm of chitosan based on the weight of the wash water were used in the washing step of the base resin, 4 to 21 ppm of the PF-127 component (including decomposition products) and 4 to 99 ppm of the chitosan component (including decomposition products) remained in the final manufactured regenerated resin. That is, about 5% to 15% of the PF-127 and chitosan used in the washing step remained in the final regenerated resin.
Claims
1. A step of putting a base resin containing polyolefin and washing water into a washing machine equipped with a rotating member, and washing the base resin by wet friction through high-speed rotation of the rotating member; and It includes a step of supplying the washed base resin to an extruder and extruding it, The above washing water is a method for producing a regenerated polyolefin resin containing water, a nonionic surfactant, and chitosan.
2. In paragraph 1, A method for producing a regenerated polyolefin resin, wherein the above nonionic surfactant is a propylene oxide-ethylene oxide block copolymer.
3. In paragraph 2, A method for producing a regenerated polyolefin resin, wherein the above propylene oxide (PO)-ethylene oxide (EO) block copolymer has a weight average molecular weight (Mw) of 9,000 to 15,000, and the proportion of propylene oxide (PO) in the copolymer accounts for 20% to 40% of the total molecular weight.
4. In paragraph 1, The above chitosan is a method for producing a regenerated polyolefin resin having a weight average molecular weight (Mw) of 4,000 to 700,000.
5. In paragraph 4, The above chitosan is a method for producing a regenerated polyolefin resin having a weight average molecular weight (Mw) of 5,000 to 500,000.
6. In paragraph 5, The above chitosan is a method for producing a regenerated polyolefin resin having a weight average molecular weight (Mw) of 10,000 to 200,000.
7. In paragraph 1, A method for producing a regenerated polyolefin resin, wherein the nonionic surfactant is contained in an amount of 50 to 200 ppm based on the total weight of the washing water.
8. In paragraph 1, A method for producing a regenerated polyolefin resin, wherein the chitosan is contained in an amount of 50 to 1,000 ppm based on the total weight of the wash water.
9. In paragraph 1, A method for producing a regenerated polyolefin resin, wherein the weight ratio of the nonionic surfactant and chitosan is 0.05:1 to 4:
1.
10. In paragraph 8 or 9, The above nonionic surfactant is contained in an amount of 100 to 150 ppm based on the total weight of the washing water, A method for producing a regenerated polyolefin resin, wherein the weight ratio of the nonionic surfactant and chitosan is 0.2:1 to 2:
1.
11. In paragraph 1, The above-described resin is a method for producing a recycled polyolefin resin obtained by subjecting waste polyolefin resin to a pretreatment process including selection, crushing, and pre-washing.
12. In paragraph 1, A method for producing a regenerated polyolefin resin, wherein the above washing step is performed for 1 to 5 minutes under conditions of a temperature of 30 to 50°C and a speed of 1000 to 2000 rpm.
13. In paragraph 1, The above-described resin is a method for producing a recycled polyolefin resin selected from among low-density polyethylene resin (LDPE), linear low-density polyethylene resin (LLDPE), or a mixture thereof.
14. A regenerated polyolefin resin comprising at least one selected from nonionic surfactants, chitosan, and their decomposition products.
15. In paragraph 14, A regenerated polyolefin resin wherein the content of the non-ionic surfactant or its decomposition product is 4 to 21 ppm based on the weight of the regenerated polyolefin resin, and the content of the chitosan or its decomposition product is 4 to 99 ppm based on the weight of the regenerated polyolefin resin.
Citation Information
Patent Citations
Grinding / Cleaning device for waste plastics and grinding / cleaning method
JP2002096329A
Method and system for recycling used scrap film
JP2016522099A
The solution which contains chitosan and surfactants for soil washing and a method of preparing thereof
KR1020120022104A
New cleaning material
KR1020150036455A
Solidifying nonionic surfactants
US20200399563A1