Blended polyurethane-copolymer formulation for soil resistant secure documents
The blended polyurethane-copolymer formulation addresses the challenges of soil and moisture resistance in secure documents by reducing polyurethane usage and enhancing tensile strength, ensuring effective soil resistance and maintaining optical clarity for secure documents.
Patent Information
- Application Number
- PCT/US2024/025447
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Existing secure documents face challenges in resisting soil and moisture while maintaining optical security features, as traditional polyurethane dispersions are expensive, reduce tensile strength, and obscure optically variable devices due to excessive application or limited active solids content.
A blended polyurethane-copolymer formulation incorporating copolymers like polyvinyl alcohol-polyvinyl amine, polyvinyl alcohol-polyvinyl pyrrolidone, or polyvinyl alcohol-polyvinyl coacrylamide-methyl-propane-sulfonic acid copolymers is applied within the substrate's pores and surfaces, reducing polyurethane usage and enhancing soil and moisture resistance without compromising optical effects.
The blended formulation provides increased soil resistance, improved tensile strength, and cost savings by reducing polyurethane usage, while maintaining the optical clarity and effectiveness of security features, thus enhancing the durability and authenticity verification of secure documents.
Smart Images

Figure US2024025447_24102024_PF_FP_ABST
Abstract
Description
BLENDED POLYURETHANE-COPOLYMER FORMULATION FOR SOIL RESISTANT SECURE DOCUMENTSTECHNICAL FIELD
[0001] The present disclosure relates generally to secure documents, such as banknotes, passports, and tickets. More specifically, this disclosure relates to a blended polyurethane-copolymer formulation for soil resistant secure documents.BACKGROUND
[0002] Optically variable security devices such as thin films, holograms, gratings, micro-prisms, photochromies, and microlens-based film structures (hereinafter collectively referred to as OVDs), are recognized as valued additions to secure documents such as banknotes. These devices allow for a variety of self-authenticating optical effects while rendering the secure document more resistant to counterfeiting. One of the primary requirements of banknotes and other secure documents is that the document must resist the effects of circulation. These documents must be durable (z.e., resistant to fold damage, tearing and soiling) and resistant to moisture and chemical absorption. In addition, the print applied to the document must adhere well, especially under severe conditions such as mechanical abrasion and accidental laundering.
[0003] To aid in banknote durability and resistance, pre-print and post-print treatments have been utilized. Post-print treatments can include varnishes and coating. Pre-print applications often use the general chemistry of polyurethane dispersions. A critical amount of material must be applied to the substrate in order to achieve the necessary performance for soil resistance and durability. Contributions to soil resistance can be imparted by both a physical barrier, generally measured as the porosity of the paper, and by surface energy contributions. Adding an excessive amount of any sizing material that migrates to the interior of the paper to a substantial degree will act to decrease the opacity of the paper. This is due to the solids in the solution or dispersion filling the voids in the paper and reducing the diffractive action of light traveling through the body of the paper.
[0004] Significant amounts of size added to the sheet also require the papermaker to reduce the actual paper fiber grammage, if the same basis weight specifications are to be met. The result is that tensile strength can be reduced due to a reduction in the overall fiber-fiber bonded area that contributes to sheet strength. Polyurethane dispersions are also generally expensive, and such water-borne dispersions have a limited active solids content in which they can be produced and shipped, resulting in the added expense of shipping water, in addition to freeze-thaw considerations that can require more expensive environmentally controlled conditions during transit. These issues are compounded when many applications for soil-resistant treatment are targeted towards low-denomination grades with high circulation velocity that carry a reduced premium for the manufacturer.SUMMARY
[0005] The present disclosure illustrates embodiments of a blended polyurethane-copolymer formulation for soil resistant secure documents.
[0006] In one embodiment, a secure document includes at least one porous substrate having a thickness and an amount of a soil and / or moisture resistant formulation included within pores of, and on opposing surfaces of, the at least one porous substrate. The soil and / or moisture resistant formulation is a blended formulation of a copolymer and polyurethane, and the soil and / or moisture resistant formulation is distributed throughout the thickness of the at least one porous substrate. The secure document may include one or more optically variable security devices contained on and / or partially within the at least one porous substrate.
[0007] The classes of copolymer used in the blended formulation can include (i) a polyvinyl alcohol-poly vinyl amine copolymer, (ii) a polyvinyl alcohol-polyvinyl pyrrolidone copolymer, or (iii) a polyvinyl alcohol-polyvinyl coacrylamide -methyl-propane-sulfonic acid copolymer.
[0008] In another embodiment, a method for preparing a blended polyurethane-copolymer formulation includes adding, based on a determined number of formulation batches, an amount of water and an amount of a copolymer to a mix tank. The method also includes dissolving the copolymer in the water in the mix tank using agitation and heat. The method also includes, after dissolution of the copolymer, adding an amount of polyurethane to the mix tank and combining the polyurethane with the dissolved copolymer to obtain the completed blended polyurethane-copolymer formulation.
[0009] The copolymer used in the method can include a polyvinyl alcohol (PVOH)-polyvinyl amine (PVAm) copolymer, a PVOH-polyvinyl pyrrolidone (PVP) copolymer, or a PVOH-polyvinyl co-acrylamide -methyl-propane- sulfonic acid (CoAmps) copolymer. As mentioned above, the PVOH-PVAm, PVOH-PVP, or PVOH-polyvinyl CoAmps copolymer is dissolved in the mix tank and polyurethane is added to create the blended polyurethane- copolymer formulation.
[0010] Other technical features may be readily apparent to one skilled in the art from the following figures, descriptions, and claims.
[0011] Before undertaking the DETAILED DESCRIPTION below, it may be advantageous to set forth definitions of certain words and phrases used throughout this patent document. The term “couple” and its derivatives refer to any direct or indirect communication between two or more elements, whether or not those elements are in physical contact with one another. The terms “include” and “comprise,” as well as derivatives thereof, mean inclusion without limitation. The term “or” is inclusive, meaning and / or. The phrase “associated with,” as well as derivatives thereof, means to include, be included within, interconnect with, contain, be contained within, connect to or with, couple to or with, be communicable with, cooperate with, interleave, juxtapose, be proximate to, be bound to or with, have, have a property of, have a relationship to or with, or the like. The phrase “at least one of,” when used with a list of items, means that different combinations of one or more of the listed items may be used, and only one item in the list may be needed. For example, “at least one of: A, B, and C” includes any of the following combinations: A, B, C, A and B, A and C, B and C, and A and B and C.
[0012] Definitions for other certain words and phrases are provided throughout this patent document. Those of ordinary skill in the art should understand that in many if not most instances, such definitions apply to prior as well as future uses of such defined words and phrases.BRIEF DESCRIPTION OF THE DRAWINGS
[0013] For a more complete understanding of the present disclosure and its advantages, reference is now made to the following description taken in conjunction with the accompanying drawings, in which like reference numerals represent like parts:
[0014] FIGURE 1 illustrates an example secure document in accordance with this disclosure;
[0015] FIGURE 2 illustrates constructional aspects of a secure document comprising a security device and a substrate having a blended polyurethane-copolymer formulation applied thereto in accordance with this disclosure; and
[0016] FIGURE 3 illustrates an example method for preparing a blended polyurethane-copolymer formulation in accordance with this disclosure.DETAILED DESCRIPTION
[0017] FIGURES 1 through 3, discussed below, and the various embodiments used to describe the principles of the present disclosure are by way of illustration only and should not be construed in any way to limit the scope of the disclosure. Those skilled in the art will understand that the principles of the present disclosure may be implemented in any suitably arranged secure document.
[0018] As noted above, optically variable security devices such as thin films, holograms, gratings, micro-prisms, photochromies, and microlens-based film structures (OVDs), are recognized as valued additions to secure documents such as banknotes. These devices allow for a variety of self-authenticating optical effects while rendering the secure document more resistant to counterfeiting.
[0019] Microlens-based OVDs, such as those are described in U.S. Patent Application Publication No. 2005 / 0180020 Al to Steenblik et al, incorporated by reference herein in its entirety, can have a film material or structure employing a regular two-dimensional array of non-cylindrical lenses to enlarge micro-images and can comprise (a) an optical spacer, (b) a regular periodic planar array of image icons positioned on one surface of the optical spacer, and (c) a regular periodic array of lenses positioned on an opposing surface of the optical spacer. The images projected by this film structure show a number of visual effects including orthoparallactic movement. OVDs in the form of security patches can be mounted on one or both surfaces of a security document (e.g., banknote), while OVDs in the form of security strips or threads can be partially embedded within the document, with the OVDs being visible in one or more clearly defined windows on one or both surfaces of the document.
[0020] One of the primary requirements of banknotes and other secure documents is that the document must resist the effects of circulation. These documents must be durable (z.e., resistant to fold damage, tearing and soiling) and resistant to moisture and chemical absorption. In addition, the print applied to the document must adhere well, especially under severe conditions such as mechanical abrasion and accidental laundering.
[0021] In order to render banknotes and other secure documents more resistant to the effects of circulation, manufacturers and printers have coated the documents with certain varnishes and polymeric coatings. These varnishes and coatings, which can consist of ultraviolet (UV) radiation-crosslinkable prepolymers (100% solids) or resin mixtures with different host solvents (resin solids content ranging from 30% to 50% by weight), serve to seal the surface of the document, increasing its resistance to soiling and moisture. Typically applied in a final, or near-final step in the document’s production using standard coating techniques (e.g., roller coating, gravure coating, air knife coating, roll coating, or blade coating), these surface coatings are generally referred to as post-print varnishes. Coat weights applied to each side of the document surface range from 0.5 grams per square meter (g / m2) to 5.0 g / m2.
[0022] A more recent trend has been to apply a coating to substrates used in the production of secure documents either during or immediately following manufacture. These surface coatings, commonly referred to as pre-print coatings, may be described as aqueous resin binder systems that serve to render the document resistant to moisture and soiling. Pre-print coatings may constitute or make up 1% to 15% of the document’s finished mass.
[0023] Unfortunately, OVDs in secure documents subjected to one or both of these prior art techniques are at least partially obscured or otherwise adversely affected as a result of the overlying varnish or coating. As will be readily appreciated by those skilled in the art, OVDs rely on unique surface topographies in order to produce novel and specifically engineered visual and machine verifiable effects. Covering these surfaces with coatings and varnishes can cloud, mute, distort or otherwise diminish the features’ effect.
[0024] As the requirement for resistance to soiling and moisture increases, generally the amount of pre-print coatings and / or post-print varnishes applied to the substrate is likewise increased. A trade-off then occurs in the form of increased substrate durability in exchange for reduced performance and effectiveness of some security features. Inaddition, some types of varnishes contain light scattering or light diffusing additives to reduce an appearance of glossiness on the finished, varnished documents. These additives can further decrease the effects of some security features.
[0025] In an effort to avoid these detrimental effects on the optically variable effects generated by OVDs, certain manufacturers (i) use very light coat weights of pre-print coatings or post-print varnishes, which reduces the document’s ability to resist moisture and soiling, (ii) avoid the combination of pre-print coatings or post-print varnishes with certain OVD security features, or (iii) block the areas on the document surface prior to applying the pre-print coating or post-print varnish, which leaves significant areas of the document surface unprotected and unduly complicates the application process.
[0026] The optical effect of OVDs can be preserved by applying a soil and / or moisture resistant formulation by way of a size press or other similar device instead of by way of standard coating techniques. Thin layers of fibers (e.g., papermaking fibers) overlying and thus embedding portions of security devices in windowed secure documents rendered soil and / or moisture resistant in this way demonstrate increased durability. U.S. Patent No. 8,366,879, incorporated by reference herein in its entirety, provides a soil and / or moisture resistant secure document and methods and techniques for imparting soil and / or moisture resistance to a porous substrate used in the manufacture of secure documents. These techniques include (a) applying a soil and / or moisture resistant formulation to opposing surfaces of the porous substrate, (b) forcing the soil and / or moisture resistant formulation into the pores of the substrate, the formulation thereby penetrating and extending throughout at least a portion of the thickness of the substrate, and (c) removing excess formulation from opposing surfaces of the substrate. Preferably, a size press (e.g. , puddle or metering) or other similar device is used to force the soil and / or moisture resistant formulation into the pores of the substrate and to remove excess formulation from opposing surfaces thereof.
[0027] Techniques for imparting soil and / or moisture resistance to a porous substrate without obscuring optically variable effects generated by non-porous OVDs contained (or exposed) on a surface thereof can also include (a) applying a soil and / or moisture resistant formulation to opposing surfaces of the porous substrate, the substrate supporting one or more non-porous OVDs, and (b) employing a size press or other similar device to force the soil and / or moisture resistant formulation into the pores of the substrate and to remove excess formulation from opposing surfaces thereof, thereby leaving exposed surfaces of the non-porous OVDs substantially free of the soil and / or moisture resistant formulation. As used herein, the term “non-porous OVDs” includes OVDs having substantially or essentially non-porous surfaces and OVDs having surfaces that are substantially or essentially non-porous only in areas contained (or exposed) on a surface of the porous substrate.
[0028] Techniques for imparting soil and / or moisture resistance to a windowed porous substrate supporting one or more security devices while increasing the durability of the substrate in areas overlying the security device(s), those areas of the substrate framing the device(s) and forming at least one window through which the security device(s) is exposed, can include (a) applying a soil and / or moisture resistant formulation to opposing surfaces of the porous substrate having the one or more security devices partially embedded therein and visible in one or more windows on at least one surface thereof and (b) employing a size press or other similar device to force the soil and / or moisture resistant formulation into the pores of the porous substrate and to remove excess formulation from opposing surfaces thereof.
[0029] A soil and / or moisture resistant secure document, which comprises at least one porous substrate having a thickness, can have an effective amount of a soil and / or moisture resistant formulation contained within the pores and on opposing surfaces of the porous substrate(s), wherein the soil and / or moisture resistant formulation is distributed throughout at least a portion of the thickness of the porous substrate(s).
[0030] For example, a soil and / or moisture resistant secure document can include one or more non-porous OVDs contained on and / or partially within the substrate(s), wherein the one or more non-porous OVDs have exposed surfaces that are substantially free of the soil and / or moisture resistant formulation. As used herein, the phrase “substantially free” means that the non-porous OVDs have only residual or trace amounts of formulation on exposed surfaces thereof.
[0031] As another example, a soil and / or moisture resistant secure document can be a windowed secure document having one or more security devices partially embedded therein and exposed in one or more windows, those areas of the secure document overlying the one or more security devices demonstrating increased durability. Preferably, the one or more security devices are non-porous, optically variable, security strips or threads having surfaces that are substantially free of the soil and / or moisture resistant formulation.
[0032] As also noted above, pre-print applications can use the general chemistry of polyurethane dispersions, which can cover an array of different specific chemistries and functional groups. Such pre-print applications can be utilized on-machine, or post paper-machine coated. For on-machine pre-print applications, the polyurethane dispersion is applied via a traditional coating operation such as a tub sizer, or via a rod or roll sizer, or other metered coating operation. A critical amount of material is applied to the substrate in order to achieve the necessary performance for soil resistance and durability. Contributions to soil resistance can be imparted by both a physical barrier, generally measured as the porosity of the paper, and by surface energy contributions.
[0033] Adding an excessive amount of any sizing material, including polyurethane, will act to decrease the opacity of the paper. This is due to the solids entrained and / or dissolved in the solution or dispersion filling the voids in the paper and reducing the diffractive action of light traveling through the body of the paper. Significant amounts of size added to the sheet also require the papermaker to reduce the actual paper fiber grammage, if the same basis weight specifications are to be met. This can result in reduced tensile strength of the substrate due to a reduction in the overall fiber-fiber bonded area that contributes to sheet strength.
[0034] Polyurethane dispersions are also generally expensive, and such water-borne dispersions have a limited active solids content that they can be produced and shipped in, resulting in the added expense of shipping water, in addition to freeze-thaw considerations that can require more expensive environmentally controlled conditions during transit. These issues are compounded when many applications for soil-resistant treatment are targeted towards low- denomination grades with high circulation velocity, which carry a reduced premium for the manufacturer.
[0035] To address the above problems, this disclosure provides a blended formulation that includes a copolymer that is blended with a polyurethane dispersion. In various embodiments, the copolymer can be a class of copolymer such as (i) a polyvinyl alcohol (PVOH)-polyvinyl amine (PVAm) copolymer, (ii) a polyvinyl alcohol (PVOH)-polyvinyl pyrrolidone (PVP) copolymer, or (iii) a polyvinyl alcohol (PVOH)-polyvinyl co-acrylamide -methyl-propane-sulfonic acid (e.g., co-2-acrylamide-2-methyl-l -propane sulfonic acid) (CoAmps) copolymer. In some embodiments, the copolymer can be a linear copolymer such as polyvinyl alcohol (PVOH) at a low degree of hydrolysis. Linear copolymers consist of a single main chain and include alternating copolymers, statistical copolymers, and block copolymers. PVOH generally is a hydrophilic linear copolymer synthesized from vinyl acetate and vinyl alcohol. PVOH is produced by polymerizing polyvinyl acetate to achieve a certain molecular weight. Then the acetate functional groups are replaced with alcohol groups (OH) via a methanolysis reaction. The greater the degree of replacement, the greater the degree of hydrolysis. However, while PVOH has been used in paper sizing, such prior uses include fully hydrolyzed PVOH, i.e., PVOH with a level of hydrolysis of 98% or more.
[0036] The low or partially hydrolyzed PVOH of this disclosure has a degree of hydrolysis at only about 80%, such as a degree of hydrolysis ranging from 78.5% to 82%. One example commercially available partially hydrolyzed polyvinyl alcohol is SELVOL E 605 manufactured by SEKISUI SPECIALTY CHEMICALS AMERICA, LLC, whichis a low viscosity partially hydrolyzed polyvinyl alcohol that is stored as a granular solid and has a degree of hydrolysis Mol percentage at 78.5-82%. Other example commercially available partially hydrolyzed polyvinyl alcohol include KURARAY POVAL 5-82 (having a degree of hydrolysis of 82% and lower molecular weight) and KURARAY POVAL 32-80 (having a degree of hydrolysis of 80% and having a higher molecular weight similar to fully hydrolyzed PVOH) both manufactured by KURARAY CO., LTD. The low or partially hydrolyzed PVOH of this disclosure can be mixed with polyurethane to provide a blended formulation that is resistant to soil and moisture.
[0037] Surprisingly, it has been discovered and verified by way of this disclosure that such classes of copolymers are compatible with polyurethane formulations used in production, and that a determined solids level of copolymer can be used on current process equipment to avoid viscosity process limitations. The blended polyurethane-copolymer formulations of this disclosure provide increased soil resistance at a level comparable to standard polyurethane dispersions. Additionally, tests using the blended polyurethane-copolymer formulations of this disclosure have shown promising chemical resistance as well.
[0038] The blended polyurethane-copolymer formulations of this disclosure act as an extender for the traditional polyurethane. The copolymer acts to seal the surface of the substrate as a physical barrier to soil resistance significantly more efficiently than the polyurethane, for example because it is a much more efficient film-former. This allows a reduction in the use of the polyurethane at a ratio of up to 2.5: 1, by reducing the polyurethane solids from approximately 30% to 15% by weight and replacing the polyurethane solids with an equal volumetric solution of the copolymer having a solids concentration of approximately 5% by weight. Additionally, the blended polyurethane- copolymer formulations of this disclosure have been found compatible for use with sized paper on the same equipment used for polyurethane dispersions, as the viscosity of the final solution remains in the range of the original polyurethane formulation, allowing for the copolymer formulations of this disclosure to be adopted into current papermaking processes without altering the sizing equipment.
[0039] The reduction in overall solids concentration of the blended polyurethane-copolymer formulations of this disclosure reduces the impact on opacity and enables a lower filler content in the size recipe. The lower overall solids content delivering the same soil resistance also results in a greater fiber content at equivalent basis weight, reducing the impact on tensile strength, and thus providing a banknote with a higher tensile strength than those that include a traditional polyurethane formulation. The polyurethane remaining in blended polyurethane-copolymer formulations of this disclosure also continues to contribute to the surface energy holdout for soil resistance, to a greater degree than a pure copolymer solution could provide.
[0040] Additionally, the copolymer (whether using a PVOH-PVAm copolymer, a PVOH-PVP copolymer, a PVOH- poly vinyl CoAmps copolymer, or low or partially hydrolyzed PVOH) can be a 100% solids material in granular form that can be shipped and stored without the constraints of potential freeze / thaw damage typical of polyurethane formulations. In addition, the copolymer material can be shipped in 100% active solids form, unlike polyurethane formulations that are typically in the range of 25% to 40% solids, such as 42% solids in water, resulting in the user having to ship the majority of the product as water, which is both burdensome and costly. Once such polyurethane formulations are mixed with filler and polyethylene glycol, total solids in a size tub can amount to about 28%. The blended formulation of this disclosure, however, can use half the polyurethane, while only including 5% copolymer solids, significantly reducing the total solids, even in embodiments in which filler and polyethylene glycol are still added to the blended formulation. The blended formulation of this disclosure provides for a reduction in usage of the polyurethane dispersion of approximately 50%, resulting in significant material cost savings, while maintaining performance for soil resistance and other durability parameters as a full polyurethane dispersion would possess.
[0041] Blended formulations of low or partially hydrolyzed P VOH and polyurethane have shown unexpectedly high levels of soil and moisture resistance. The blended formulation of low or partially hydrolyzed P VOH and polyurethane of this disclosure has high soil resistance, performs well in printed ink durability, and is an economical extender material (by a factor of about two times). The blended formulation of low or partially hydrolyzed PVOH and polyurethane of this disclosure also has exceeded porosity targets on paper machines, which is a measure of how impermeable the sheet is to air flow.
[0042] In some embodiments, the blended formulation of low or partially hydrolyzed PVOH and polyurethane of this disclosure also includes a defoamer or defoaming agent. This is because the blended partially hydrolyzed PVOH- polyurethan formulation can tend to foam. One example of a defoaming agent is 880815 FLEXO ANTI-FOAMING AGENT from SICPA. As indicated herein, the low or partially hydrolyzed PVOH of this disclosure can be in a dry powder form. This provides a long shelf life and low transportation costs until the partially hydrolyzed PVOH is used in creating the blended formulation.
[0043] Other features and advantages of this disclosure will be apparent to one of ordinary skill from the following detailed description. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. All publications, patent applications, patents and other references mentioned herein are incorporated by reference in their entirety. In case of conflict, the present specification, including definitions, will control. In addition, the materials, methods, and examples are illustrative only and not intended to be limiting.
[0044] FIGURE 1 illustrates an example secure document 100 in accordance with this disclosure. In this illustrative example, secure document 100 is a currency note, though other embodiments (for example, tickets, identification papers, etc.) are within the contemplated scope of this disclosure. Secure document 100 comprises a substrate 105. Substrates suitable for use in the secure document 100 and in this disclosure can include paper or paper-like sheet materials.
[0045] In various embodiments, the substrate 105 can be a fibrous substrate formed from a wet web of fibrous material (for example, wood pulp, cotton fiber, linen fiber, flax fiber, sisal fiber, hemp fiber, Abaca fiber, Kozo fiber, Mitsumata fiber, bamboo fiber, Kenaf fiber, and / or synthetic fiber), which is laid down (for example, in a Fourdrinier process) at a first, baseline fiber density. Regions of the web in which the first fiber density is not altered while the web is wet (for example, through the use of wire rolls, electrotypes, or other watermarking tools) prior to pressing, drying and in some embodiments, calendaring, form bulk regions 110 of secure document 100. As used in this disclosure, the expression “bulk region” encompasses a portion of a fibrous substrate embodying one or more of a baseline fiber density, baseline light absorption, or baseline caliper thickness. Put differently, as used in this disclosure, the expression “bulk region” encompasses portions of a finished fibrous substrate in which the locations of the constituent fibers are not deliberately altered (for example, through the use of wire cloths or electrotypes) as part of the papermaking process. In the various embodiments of this disclosure, a blended polyurethane-copolymer soil and / or moisture resistant formulation can be applied to the substrate 105 such that the formulation is contained within the pores and on opposing surfaces of the substrate 105, wherein the soil and / or moisture resistant formulation is distributed throughout at least a portion of the thickness of the substrate 105.
[0046] As shown in the explanatory example of FIGURE 1, secure document 100 further comprises one or more security features 115 adhered to the surface of secure document 100. In this example, security feature(s) 115 comprises a thin section of material with one or more optical structures that can be cast-cured and provide an optically variable effect. Examples of optical structures provided on security feature 115 include, without limitation, micro-lenses, diffractive structures, and micro-optic icons. Examples of optically variable effects provided by the optical structuresof security feature 115 include, without limitation, holograms, color shift effects, and synthetic images, characterized by the synthetic projection of portions of image icons across an array of image icons by focusing elements of an array of focusing elements. In some embodiments, the scale ratio (z.e., the ratio of the repeat period of the focusing elements to the repeat period of the image icons) is approximately 1.000. In some embodiments, the security features 115 can include embossed portions.
[0047] In some embodiments, secure document 100 further comprises one or more functional watermarks 120. According to various embodiments, functional watermarks 120 comprise one or more regions in which the fiber density of fibrous substrate 105 is deliberately altered (either increased or decreased) from the fiber density in bulk region 110 to form a visible pattern of light (z.e., allowing more light to pass in transmission through the fibrous substrate than bulk region 110) and / or dark (z.e., less light to pass in transmission through the fibrous substrate than bulk region 110) elements. Additionally, at least a portion of functional watermark 120 is covered by part of security feature 115, wherein security feature 115 is maintained in contact with functional watermark 120 by an adhesive bond.
[0048] Although FIGURE 1 illustrates one example of a secure document 100, various changes may be made to FIGURE 1. For example, the secure document 100 can be any type of document such as tickets, identification papers, etc. Also, the watermark 120 can be of any shape, image, or other design, or the secure document may not include the watermark 120. The security device 115 can also be placed in differing areas or portions of the secure document 100. Secure documents can come in a variety of configurations, and FIGURE 1 does not limit this disclosure to any particular configuration of a secure document.
[0049] As described above, embodiments of this disclosure provide a soil and / or moisture resistant blended polyurethane-copolymer formulation that addresses issues with traditional polyurethane formulations. Embodiments of the soil and / or moisture resistant blended polyurethane-copolymer formulation can include (i) a polyvinyl alcohol (PVOH) and polyvinyl amine (PVAm) copolymer, (ii) a PVOH-polyvinyl pyrrolidone (PVP) copolymer, (iii) a PVOH-polyvinyl CoAmps copolymer, or (iv) partially hydrolyzed PVOH, that is blended with polyurethane. In some embodiments, the blended formulation can also include an amount of opacifying filler and an amount of polyethylene glycol or an amount of glycerin. In some embodiments, the blended formulation can also include a defoamer. As also described above, the blended polyurethane -formulations of this disclosure provide increased soil resistance at a level comparable to standard polyurethane dispersions, increased surface energy holdout compared to pure copolymer solutions, lower overall solids concentration than polyurethane dispersions, and chemical resistance.
[0050] Polyurethane dispersions can contain particles or solids of polyurethane resins, polyether-urethane resins, and / or urethane-acrylic resins, which have resin solids content ranging from 25% to 50% by dry weight. The copolymer of the blended formulation of this disclosure acts to seal the surface of the substrate as a physical barrier to soil resistance significantly more efficiently than the polyurethane, for example because it is a much more efficient film -former. This allows a reduction in the use of the polyurethane at a ratio of up to 2.5: 1, such as by reducing the polyurethane solids from approximately 30% to 15% by dry weight. The polyurethane solids are replaced by using a solution of the copolymer (e.g., a 10.4% solution of the copolymer), and adding an equal volume of the copolymer solution with the polyurethane, achieved a final solids concentration for the blended formulation of approximately 17% to 21%, with about 5% being the copolymer.
[0051] For example, the blended formulation can be made by mixing the components (including the polyurethane and the copolymer (e.g., PVOH-PVAm, PVOH-PVP, or PVOH-polyvinyl CoAmps copolymers, or partially hydrolyzed PVOH) with water so as to obtain an aqueous formulation having a final solids content of 12% to 15% polyurethane and about 5% copolymer, such as 4% to 6% copolymer, by dry weight, based on the total dry weight of the formulation. In some embodiments, the blended formulation can have an average particle size of the dispersedparticles found in the polymer dispersion ranging from about 50 to about 150 nanometers (nm) (such as from about 70 to about 140 nm). The pH of the aqueous of such formulations is between 5.5 and 9.5, such as between 6.0 and 8.0.
[0052] The reduction in overall solids concentration of the blended polyurethane -copolymer formulations of this disclosure reduces the impact on opacity and enables a lower filler content in the size recipe, thus retaining opacity and the diffractive properties of the substrate for the secure document. Since less formulation is used to fill the voids of the paper, the blended formulation of this disclosure having lower overall solids content delivers the same soil resistance while also resulting in a greater fiber content at equivalent basis weight, providing secure documents that include the blended formulation with a higher tensile strength than those that include a traditional polyurethane formulation. This is due to the solids in the solution or dispersion filling the voids in the paper and reducing the diffractive action of light traveling through the body of the paper.
[0053] In addition to the above components, in some embodiments, the soil and / or moisture resistant formulation of this disclosure may advantageously contain other solvents, cosolvents or diluents as well as additives including (but not limited to) antimicrobial agents, catalysts, crosslinking agents (e.g., silane crosslinking agents), defoaming agents, pigments (e.g., titanium dioxide), plasticizers, stabilizers, surfactants or wetting agents, and viscosity modifiers, provided any such solvent, cosolvent, diluent, or additive does not adversely impact upon the desirable properties of the resulting secure document.
[0054] FIGURE 2 illustrates constructional aspects 200 of a secure document 201 comprising a security device 260 and a substrate 206 having a blended polyurethane -copolymer formulation applied thereto in accordance with this disclosure.
[0055] Referring to the non-limiting example of FIGURE 2, imparting the blended polyurethane-copolymer formulations of this disclosure to a porous substrate 202 comprises (a) applying the above-described soil and / or moisture resistant formulation to opposing surfaces of the porous substrate, (b) forcing the soil and / or moisture resistant formulation into the pores of the substrate, the formulation thereby penetrating and extending throughout at least a portion of the thickness of the substrate, and (c) removing excess formulation from opposing surfaces of the substrate.
[0056] It has been discovered and verified by way of this disclosure that copolymers such as PVOH-PVAm, PVOH- PVP, PVOH-polyvinyl CoAmps and partially hydrolyzed PVOH are compatible with polyurethane formulations used in production, and that a determined solids level of copolymer can be used on current process equipment to avoid viscosity limitations. Thus, the blended polyurethane-copolymer formulations of this disclosure have been found compatible for use with sized paper on the same equipment used for polyurethane dispersions, as the viscosity of the final solution remains in the range of the original polyurethane formulation, allowing for the copolymer formulations of this disclosure to be adopted into current papermaking processes without altering the sizing equipment.
[0057] For example, as shown in FIGURE 2, a size press 204 or other similar device is used to force the blended soil and / or moisture resistant formulation 203 into the pores of the substrate 202 and to remove excess formulation 203 from opposing surfaces thereof. The resultant soil resistant substrate 206, or a portion thereof, can then be used as the substrate for a security device, such as the example security device 260 illustrated in FIGURE 2. It will be understood that the size press 204 shown in FIGURE 2 is simplified for illustrative purposes, and that size presses can include various additional components and come in various configurations. For example, the blended formulation 203 can be supplied to the applicator rolls shown in FIGURE 2 by one or more liquid supply heads that receive the blended formulation 203 from a run tank in which the prepared blended formulation is stored.
[0058] For instance, upon leaving the “wet-end” of a papermaking machine, a fibrous web containing a considerable amount of water is directed toward a press section (e.g. , a series of heavy rotating cylinders), which serves to pressthe water from the web, further compacting it and reducing its water content, typically to about 60% by weight. Following pressing, the paper web is dried in the main dryer section of the papermaking machine. In the drying section, which is typically the longest section of the papermaking machine, hot air or steam -heated cylinders contact both sides of the web, substantially drying the web by evaporating the water, such as to a level of approximately 1% or less by weight of the paper.
[0059] These sheet materials, which are single or multi-ply sheet materials, may be made from a variety of fibers such as abaca, cotton, linen, wood pulp, and blends thereof. As is well known to those skilled in the art, cotton and cotton / linen blends are preferred for banknotes, while wood pulp is commonly used in non-banknote security documents. For example, in various embodiments, the substrate 202 can be a fibrous substrate formed from a wet web of fibrous material (for example, wood pulp, cotton fiber, linen fiber, flax fiber, sisal fiber, hemp fiber, Abaca fiber, Kozo fiber, Mitsumata fiber, bamboo fiber, Kenaf fiber, and / or synthetic fiber), which is laid down (for example, in a Fourdrinier process) at a first, baseline fiber density.
[0060] The dried web or substrate 202 is then surface sized using the size press 204. By way of the present disclosure, the size press 204 is used to force an effective amount (z.e., from about 5% to about 20% by dry weight, preferably from about 7.5% to about 12.5% by dry weight, based on the total dry weight of the size press-treated substrate) of the blended soil and / or moisture resistant formulation 203 into the interstices of the substrate from both sides of the substrate. The size press 204 is also used to remove excess blended formulation 203 from opposing surfaces of the substrate. Penetration and distribution of the blended formulation 203 is thus achieved throughout at least a portion of the thickness of the substrate. The size press-treated substrate 206 is then dried in a secondary dryer section of the papermaking machine to a moisture level of from about 4% to about 6%.
[0061] The Gurley porosity of the resulting secure document 201 can range from about 15,000 to about 300,000 seconds, and more preferably ranges from about 25,000 to about 60,000 seconds. Gurley porosity values are determined using TAPPI Test Method No. T-460 om-06 (2006). The blended soil and / or moisture resistant formulation 203 provides the resulting secure document 201 with superior durability. Moreover, the printability of the secure document 201 is not adversely affected and in fact may be improved.
[0062] With respect to blended formulations of partially hydrolyzed PVOH and polyurethane, the high performance of the low or partially hydrolyzed PVOH and polyurethane is at least due in part to that partially hydrolyzed PVOH tends to be a highly efficient film-former in such a way that tests have shown significant advantages over prior formulations used in the industry. For example, prior formulations have been known to achieve a Gurley value of about 50,000 seconds (PVOH paper is only in the hundreds of seconds). However, blended formulations of partially hydrolyzed PVOH and polyurethane of this disclosure, tested on a paper machine, achieved a Gurley porosity from 250,000 to 300,000 seconds.
[0063] Additionally, in some embodiments, pigment is added to the blended formulation 203 just prior to applying it to the porous substrate. Pigment is used to counteract the transparentizing effect of resin pickup and incorporation into the porous substrate or base sheet. Adding pigment to the formulation just prior to its application to the base sheet obviates the need for stabilizers to assure homogeneity. It also allows for these formulations to be customized for different paper grades with different requirements, and even allows for batch-to-batch adjustments during production of a particular grade.
[0064] For secure documents employing one or more non-porous OVDs, the soil and / or moisture resistant formulation provides the resulting secure document with superior durability without diminishing the optically variable effects generated by the OVDs. More specifically, in those areas of the substrate in which a non-porous OVD is present, the OVD causes the formulation to be rejected from the surface of the OVD as the hydraulic pressure of thesize press increases. The surface of the OVD is left substantially free of the formulation that now resides within the pores and on opposing surfaces of the substrate. For windowed secure documents, those portions of the secure document overlying partially embedded security devices demonstrate increased durability in the form of a reduced tendency to tear and crack.
[0065] The example security device 260, as illustrated in FIGURE 2, can be a micro-optic security device, and can comprise a plurality of focusing elements 205 (including, for example, focusing element 207), and an arrangement of image icons 220 (including, for example, image icon 221). According to various embodiments, each focusing element of the plurality of focusing elements 205 has a footprint, in which one or more image icons of the arrangement of image icons 220 is positioned. Collectively, the focusing elements of the plurality of focusing elements 205 magnify portions of image icons 220 to produce a synthetic magnification effect (also referred to as “synthetic image”) wherein the individually microscopic image icons are collectively magnified by the plurality of focusing elements 205 to produce an image which dynamically reacts (for example, by appearing to move or change colors) in response to shifts in viewing angle. Given the small scale and tight manufacturing tolerances of the constituent structures of optical security devices providing moire magnification effects, many malicious actors are not able to produce counterfeit versions of optical security device 260. Accordingly, optical security device 260 is, in many cases, a trusted visual indicium of a secure document’s (for example, secure document 201) authenticity.
[0066] According to certain embodiments, the plurality of focusing elements 205 comprises a planar array of microoptic focusing elements. In some embodiments, the focusing elements of plurality of focusing elements 205 comprise micro-optic refractive focusing elements (for example, plano-convex or GRIN lenses). Refractive focusing elements of plurality of focusing elements 205 are, in some embodiments, produced from light cured resins with indices of refraction ranging from 1.35 to 1.7, and have diameters ranging from 5|im to 200pm. In various embodiments, the focusing elements of plurality of focusing elements 205 comprise reflective focusing elements (for example, very small concave mirrors), with diameters ranging from 5pm to 50pm.
[0067] As shown in the illustrative example of FIGURE 2, the arrangement of image icons 220 comprises a set of image icons (including image icon 221), positioned at predetermined locations within the footprints of the focusing elements of plurality of focusing elements 205. According to various embodiments, the individual image icons of the arrangement of image icons 220 comprise regions of light cured material associated with the focal path of structured light (for example, collimated UV light) passing through the plurality of focusing elements 205 from a projection point associated with one or more predetermined ranges of viewing angles. In some embodiments, the individual image icons of the arrangement of image icons 220 are not provided within a structured image icon layer.
[0068] As used in this disclosure, the term “structured image layer” encompasses a layer of material (for example, a light-curable resin) which has been embossed, or otherwise formed to comprise structures (for example, recesses, posts, grooves, or mesas) for positioning and retaining image icon material. According to various embodiments, the individual image icons of the arrangement of image icons 220 are provided within a structured image layer, the structured image layer comprising one or more of voids, mesas, or posts, which act as retaining structures to hold micro- and nano-scale volumes of colored material.
[0069] As shown in the illustrative example of FIGURE 2, in certain embodiments, optical security device 260 includes an optical spacer 210. According to various embodiments, the optical spacer 210 comprises a film of substantially transparent material (for example, polyethylene terephthalate (“PET”) or Biaxially-Oriented Polypropylene (“BOPP”)) which operates to position image icons of the arrangement of image icons 220 in or around the focal plane of focusing elements of the plurality of focusing elements 205. In certain embodiments according to this disclosure, the optical spacer 210 comprises a manufacturing substrate upon which one or more layers of lightcurable material can be applied, to form one or more of the arrangement of image icons 220 or the plurality of focusing elements 205.
[0070] According to various embodiments, the optical security device 260 comprises one or more regions of light- cured protective material which occupy the spaces between the image icons of the arrangement of image icons 220. In some embodiments, the arrangement of image icons 220 is first formed (for example, by selectively curing and removing liquid light-curable material on the optical spacer 210), and then a layer of clear, light-curable material is applied to fill spaces between the image icons of the arrangement of image icons 220 and then flood-cured to create a protective layer, which protects the image icons from being moved from their positions within the footprints of focusing elements of the plurality of focusing elements 205. In certain embodiments, the light-curable material used to form the arrangement of image icons 220 is a pigmented, ultraviolet (UV)-curable polymer.
[0071] In accordance with this disclosure, the arrangement of image icons 220 is affixed or bonded to a second substrate or adhesive layer 230. The second substrate 230 provides an adhesive interface for attaching optical security device 260 to a substrate 206 as part of secure document 201. Thus, according to embodiments of this disclosure, the optical security device 260 is affixed to substrate 206 by the adhesive layer 230.
[0072] In certain embodiments according to this disclosure, optical security device 260 comprises a seal layer 240. According to certain embodiments, the seal layer 240 comprises a thin (for example, a 2|im to 50|im thick layer) of substantially clear material which interfaces on a lower surface with focusing elements of the plurality of focusing elements 205 and comprises an upper surface with less variation in curvature (for example, by being smooth, or by having a surface whose local undulations are of a larger radius of curvature than the focusing elements) than the plurality of focusing elements 205. It will be understood that other types of security devices can also be used and applied to substrates including the blended formulations of this disclosure without departing from the scope of this disclosure.
[0073] As is well known to those skilled in the art, a security strip or thread that is partially embedded within and partially exposed on the surface of a banknote or other secure document is commonly referred to as a windowed thread. The embedded areas of the thread are covered with a thin layer of paper that serves to frame the thread and form at least one window through which the thread is exposed. This thin layer of paper can be the result of any technique employed in the paper -making industry. By way of example, the thread may be fed into a cylinder mold papermaking machine, cylinder vat machine, Fourdrinier papermaking machine, or similar machine of known type, upon which a suspension of papermaking fibers or papermaking stock is deposited (or selectively deposited) onto the security thread, is formed around it, or is displaced from an already formed web. By way of further example, laminating or wet laminating techniques, as well as techniques involving spraying of fibrous suspensions over select areas of the thread, can be employed to achieve partial embedment. The overlying borders and bridges that result not only cover a portion of the security thread but are an integrated, rather than separately attached, part of the paper structure.
[0074] One method of simulating the degradation effects that a secure document or banknote endures in circulation is described in the publication: Bartz, W. J., and Crane, T. T, “The Circulation Simulator Method for Evaluating Bank Note and Optical Feature Durability,” SPIE Vol. 6075, San Jose, Calif., January 2006. This publication describes a test method developed by Crane & Co., Inc. that simulates the deterioration observed in actual circulated banknotes( / .e., soiling, creasing, tearing, edge tatteredness, and limpness). The test method described, which is hereinafter referred to as “the Circulation Simulator Method,” utilizes a tumbler mounted on a lathe. Banknote specimens are weighted on each comer and are tumbled in a medium of glass beads, metal discs, and a synthetic soil mixture for three, 30-minute cycles, during which physical degradation of the note specimens occurs. Durability isjudged by how well a note retains its initial optical and physical properties after being subjected to the conditions of the Circulation Simulator Method.
[0075] Banknotes containing security threads that have been subjected to the described conditions of the Circulation Simulator Method can in some circumstances display weakness in the thin paper layer that covers the security thread. This weakness is exemplified by cracking or tearing of this paper layer. One observation that has been made about windowed banknotes containing non-porous, microlens-based, optically variable security threads that have been produced in accordance with this disclosure is that the thin paper layer that covers the security thread better resists the degradation effects imposed by way of the Circulation Simulator Method. This improved strength or increased durability is visually apparent, exemplified by the thin paper layer remaining intact and free from tearing and cracking.
[0076] Further, the soil and / or moisture resistant materials of this disclosure, when applied by way of a size press or other similar device instead of by way of standard coating techniques, do not obscure the optically variable effects generated by OVDs employed on or within banknotes and other secure documents. Additionally, the durability of thin fibrous layers overlying a security strip or thread embedded in a windowed banknote or other secure document is increased when soil and / or moisture resistant materials are applied during manufacture by way of a size press or other similar device.
[0077] Use of the blended formulation and processes of this disclosure thus allows for improved process economics where the method represents a more time-efficient, streamlined pathway to providing soil and / or moisture resistance to secure documents by obviating the need for pre-print coating and post-print varnishing processes and the concomitant capital investment in the necessary coating and varnishing equipment.
[0078] Although the soil and / or moisture resistant secure document of this disclosure will be described herein mainly for use in the manufacture of banknotes, this disclosure is not so limited. The inventive secure document can be used to prepare a variety of different items including checks, identity cards, lottery tickets, passports, postage stamps, stock certificates, and the like.
[0079] As noted above, the soil and / or moisture resistant secure document of this disclosure comprises at least one porous substrate having a thickness, and an effective amount of a soil and / or moisture resistant formulation contained within the pores and on opposing surfaces of the substrate(s), wherein the soil and / or moisture resistant formulation is distributed throughout at least a portion of the thickness of the porous substrate(s).
[0080] While FIGURE 2 provides one example of constructional aspects 200 of a secure document 201, various changes may be made to FIGURE 2. For example, other optical security devices include hard-to-reproduce micro- and nano-scale optical structures (for example, holograms, devices providing thin-film effects, devices producing diffraction-based optical effects, etc.) are within the contemplated scope of this disclosure. Additionally, while in this illustrative example the focusing elements of the plurality of focusing elements 205 are shown as comprising circular plano-convex lenses, other refractive lens geometries, for example, lenticular lenses, are possible and within the contemplated scope of this disclosure. Also, the optical security device 260 could include any suitable number of each component in any suitable arrangement, such as including a plurality of layers of image icon arrangements. In general, this disclosure is not limited to any particular security device.
[0081] FIGURE 3 illustrates an example method 300 for preparing a blended polyurethane-copolymer formulation in accordance with this disclosure. At block 302, an amount of solids to be used for the formulation is determined based on a number of batches to be prepared. For example, for ease of preparation, as high a solids as possible can be prepared to minimize the number of copolymer batches that have to be prepared for continuous substrate production operations. At block 304, formulation of the polyurethane-copolymer blend begins with adding, based on the determined number of batches to be prepared, water and the copolymer to a mix tank. In various embodiments, thecopolymer is a formulation of approximately 85% polyvinyl alcohol (PVOH) and 15% polyvinyl amine (PVAm), but could be adjusted based on desired properties. In some embodiments, the copolymer is approximately 95% to 96% PVOH and 4% to 5% polyvinyl pyrrolidone (PVP) (e.g., 4% to 5 mol% PVP), but could be adjusted based on desired properties. In some embodiments, the copolymer is approximately 95% to 97% PVOH and 3% to 5% polyvinyl CoAmps (e.g., 3% to 5% mol AMPS), but could be adjusted based on desired properties. In some embodiments, the copolymer is partially hydrolyzed polyvinyl alcohol (PVOH) having a degree of hydrolysis around a molecular percent of 80%, such as 78.5-82%.
[0082] At block 306, the copolymer is dissolved in the water in the mix tank. As indicated, the method 300 can be carried out in equipment, such as a mix tank and eventually a run tank, typically used for sizing in papermaking operations. Once the water is added to the mix tank, followed by the copolymer, dissolution of the copolymer in the water is achieved using agitation to promote blending uniformity, as well as heat. The temperature in the mix tank is raised to a predetermined or prescribed level for the copolymer to allow the copolymer to dissolve, which is typically around 85°C, but different temperatures could be used if needed for the copolymer.
[0083] At decision block 308, it is determined whether dissolution of the copolymer in the water in the mix tank is complete. For example, agitation with the applied heat can continue for a period of 45 minutes to one hour, at which point the copolymer should be completely dissolved in the water. In various embodiments, an amount of water used is sufficient to dissolve the copolymer such that the mix tank contains 10% solids, i. e. , the copolymer is cooked to a 10% solids concentration. If, at decision block 308, it is determined that dissolution of the copolymer is not yet complete, dissolution continues at block 306. If, at decision block 308, it is determined that dissolution of the copolymer is complete, the method 300 moves to block 310.
[0084] At block 310, the polyurethane is added to the mix tank at an amount that will result in the desired concentration and the polyurethane is combined with the copolymer (such as to bring the copolymer solids to 5%) by continuing to apply heat and agitation to the mix in the mix tank. Prior to adding the polyurethane, an amount of additional water can be added to the mix tank, to cook the copolymer as concentrated as possible, based on the batches to be sent to the run tank. Then, an amount of polyurethane to add is determined based on a desired solids level. For example, a mass balance can be performed to determine the amount of water to add before adding the polyurethane. In some embodiments, the final solids of the blended formulation can be 12% to 15% polyurethane and approximately 5% copolymer, as opposed to a pure polyurethane recipe of approximately 25% polyurethane or more.
[0085] At decision block 312, it is determined whether to add additional components to the mixture and, if so, the additional components are added to the mix tank and combined at block 314. The method 300 then moves to block 316. If, at decision block 312, it is determined not to add additional components to the mix the method moves from decision block 312 to block 316. Various additional components could be added to the formulation at block 314. For example, polyethylene glycol or glycerin may still be added for increased fold strength. Additionally or alternatively, other solvents, cosolvents or diluents as well as additives including (but not limited to) antimicrobial agents, catalysts, crosslinking agents (e.g., silane crosslinking agents), defoaming agents, pigments (e.g., titanium dioxide), plasticizers, stabilizers, surfactants or wetting agents, and viscosity modifiers.
[0086] At block 316, the blended formulation is pumped to a run tank, allowing the mix tank to be used for the next batch, as required during production, and allowing the blended formulation in the run tank to be used in papermaking / substrate production. The blended formulation, when applied to secure documents as described in this disclosure, performs exceptionally well at blocking foreign materials from getting into the pores of a substrate of a secure document, is optically clear, can promote surface energy to increase resistance to liquids, and has increasedtensile strength compared to pure polyurethane dispersions. At block 318, the blended formulation is applied to a substrate(s) using a size press.
[0087] Although FIGURE 3 illustrates one example method 300 for preparing a blending polyurethane-copolymer formulation, various changes may be made to FIGURE 3. For example, while shown as a series of steps, various steps in FIGURE 3 could overlap, occur in parallel, occur in a different order, or occur any number of times. As a particular example, block 314 could occur at a same time or near in time to block 310, such as if the polyurethane and the additional components are added to the mix tank together.
[0088] In one example embodiment, a secure document comprises at least one porous substrate having a thickness and an amount of a soil and / or moisture resistant formulation included within pores of, and on opposing surfaces of, the at least one porous substrate, wherein the soil and / or moisture resistant formulation is a blended formulation of a copolymer and polyurethane, wherein the soil and / or moisture resistant formulation is distributed throughout the thickness of the at least one porous substrate.
[0089] In one or more of the above examples, the copolymer is a partially hydrolyzed polyvinyl alcohol.
[0090] In one or more of the above examples, the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage of approximately 80%.
[0091] In one or more of the above examples, the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage in a range of 78.5-82%.
[0092] In one or more of the above examples, the blended formulation of the partially hydrolyzed polyvinyl alcohol and the polyurethane further includes a defoaming agent.
[0093] In one or more of the above examples, the copolymer is one of a polyvinyl alcohol-polyvinyl amine copolymer, a polyvinyl alcohol-polyvinyl pyrrolidone copolymer, or a polyvinyl alcohol-polyvinyl CoAmps copolymer.
[0094] In one or more of the above examples, the PVOH-PVAm copolymer is approximately 85% PVOH and approximately 15% P VAm.
[0095] In one or more of the above examples, a final solids concentration of the blended formulation includes 12% to 15% of the polyurethane and approximately 5% of the copolymer by dry weight.
[0096] In one or more of the above examples, the secure document also includes one or more optically variable security devices contained on and / or partially within the at least one porous substrate.
[0097] In one or more of the above examples, the one or more optically variable security devices have exposed surfaces that are substantially free of the soil and / or moisture resistant formulation.
[0098] In one or more of the above examples, the one or more the optically variable security devices is non-porous.
[0099] In one or more of the above examples, the secure document is a windowed secure document including the one or more optically variable security devices partially embedded therein and exposed in one or more windows, wherein areas of the secure document overlying the one or more optically variable security devices demonstrate increased durability in the form of reduced cracking or tearing as compared to a secure document that does not contain the soil and / or moisture resistant formulation.
[0100] In one or more of the above examples, the one or more optically variable security devices is one or more non- porous, optically variable security strips or threads having surfaces that are substantially free of the soil and / or moisture resistant formulation.
[0101] In one or more of the above examples, the secure document has a porosity ranging from about 15,000 to about 300,000 seconds, determined in accordance with TAPPI Test Method No. T-460 om-06 (2006).
[0102] In one or more of the above examples, the porosity of the secure document ranges from about 25,000 to about 60,000 seconds.
[0103] In one or more of the above examples, the soil and / or moisture resistant formulation further includes an amount of polyethylene glycol or an amount of glycerin.
[0104] In one or more of the above examples, the soil and / or moisture resistant formulation further includes at least one of an amount of one or more solvents, cosolvents, or diluents, and an amount of one or more additives including at least one of an antimicrobial agent, a catalyst, a crosslinking agent, a defoaming agent, a plasticizer, a stabilizer, a surfactant, a wetting agent, and a viscosity modifier.
[0105] In one or more of the above examples, the soil and / or moisture resistant formulation further includes one or more pigments.
[0106] In one or more of the above examples, the one or more optically variable security devices is selected from a group of thin films, holograms, gratings, micro-prisms, photochromies, and microlens-based film structures.
[0107] In one or more of the above examples, the one or more optically variable security devices is a microlensbased film structure in the form of a security strip or thread that is partially embedded within the secure document, with the microlens-based film structure being visible in one or more clearly defined windows on one or both surfaces of the secure document.
[0108] In one or more of the above examples, the optically variable security devices include a microstructured surface contained on and / or partially within the at least one porous substrate, wherein the one or more optically variable security devices have exposed surfaces that are substantially free of the soil and / or moisture resistant formulation.
[0109] In another example embodiment, a method for preparing a blended polyurethane-copolymer formulation comprises adding, based on a determined number of formulation batches, an amount of water and an amount of a copolymer to a mix tank, dissolving the copolymer in the water in the mix tank using agitation and heat, after dissolution of the copolymer, adding an amount of polyurethane to the mix tank and combining the polyurethane with the dissolved the copolymer, and obtaining the completed blended polyurethane-copolymer formulation.
[0110] In one or more of the above examples, the copolymer is a partially hydrolyzed polyvinyl alcohol.
[0111] In one or more of the above examples, the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage of approximately 80%.
[0112] In one or more of the above examples, the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage in a range of 78.5-82%.
[0113] In one or more of the above examples, the method further includes adding a defoaming agent to the blended formulation of the partially hydrolyzed polyvinyl alcohol and the polyurethane.
[0114] In one or more of the above examples, the method further comprises pumping the completed blended polyurethane-copolymer formulation to a run tank and applying the completed blended polyurethane-copolymer formulation to at least one porous substrate using a size press.
[0115] In one or more of the above examples, the method further comprises combining, in the mix tank with the polyurethane and the copolymer, at least one of an amount of polyethylene glycol, an amount of glycerin, an amount of one or more solvents, cosolvents, or diluents, and an amount of one or more additives including at least one of an antimicrobial agent, a catalyst, a crosslinking agent, a defoaming agent, a pigment, a plasticizer, a stabilizer, a surfactant, a wetting agent, and a viscosity modifier.
[0116] In one or more of the above examples, the copolymer is one of a polyvinyl alcohol-polyvinyl amine copolymer, a polyvinyl alcohol-polyvinyl pyrrolidone copolymer, or a polyvinyl alcohol-polyvinyl CoAmps copolymer.
[0117] In one or more of the above examples, the PVOH-PVAm copolymer is approximately 85% PVOH and approximately 15% PVAm.
[0118] In one or more of the above examples, a final solids concentration of the completed blended polyurethanecopolymer formulation is 12% to 15% of the polyurethane and approximately 5% of the copolymer.
[0119] Although the present disclosure has been described with various embodiments, various changes and modifications may be suggested to one skilled in the art. It is intended that the present disclosure encompass such changes and modifications as falling within the scope of the claims.
Claims
WHAT IS CLAIMED IS:
1. A secure document, comprising: at least one porous substrate having a thickness and an amount of a soil and / or moisture resistant formulation included within pores of, and on opposing surfaces of, the at least one porous substrate, wherein the soil and / or moisture resistant formulation is a blended formulation of a copolymer and polyurethane, and wherein the soil and / or moisture resistant formulation is distributed throughout the thickness of the at least one porous substrate.
2. The secure document of Claim 1 , wherein the copolymer is a partially hydrolyzed polyvinyl alcohol.
3. The secure document of Claim 2, wherein the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage of approximately 80%.
4. The secure document of Claim 2, wherein the partially hydrolyzed polyvinyl alcohol has a degree of hydrolysis of a molecular percentage in a range of 78.5-82%.
5. The secure document of Claim 2, wherein the blended formulation of the partially hydrolyzed polyvinyl alcohol and the polyurethane further includes a defoaming agent.
6. The secure document of Claim 1, wherein the copolymer is one of: a polyvinyl alcohol-polyvinyl amine copolymer; a polyvinyl alcohol-polyvinyl pyrrolidone copolymer; or a polyvinyl alcohol-polyvinyl co-acrylamide-methyl-propane-sulfonic acid (CoAmps) copolymer.
7. The secure document of Claim 1, wherein a final solids concentration of the blended formulation includes 12% to 15% of the polyurethane and approximately 5% of the copolymer by dry weight.
8. The secure document of Claim 1 , further comprising one or more optically variable security devices contained on and / or partially within the at least one porous substrate.
9. The secure document of Claim 8, wherein the one or more optically variable security devices have exposed surfaces that are substantially free of the soil and / or moisture resistant formulation.
10. The secure document of Claim 8, wherein the one or more the optically variable security devices is non-porous.
11. The secure document of claim 8, wherein the one or more optically variable security devices is selected from a group of thin films, holograms, gratings, micro-prisms, photochromies, and microlens-based film structures.
12. The secure document of claim 1, wherein the secure document has a porosity ranging from about 15,000 to about 300,000 seconds, determined in accordance with TAPPI Test Method No. T-460 om-06 (2006).
13. The secure document of claim 11, wherein the porosity of the secure document ranges from about 25,000 to about 60,000 seconds.
14. The secure document of claim 1, wherein the soil and / or moisture resistant formulation further includes an amount of polyethylene glycol or an amount of glycerin.
15. The secure document of claim 1, wherein the soil and / or moisture resistant formulation further includes at least one of: an amount of one or more solvents, cosolvents, or diluents; and an amount of one or more additives including at least one of an antimicrobial agent, a catalyst, a crosslinking agent, a defoaming agent, a plasticizer, a stabilizer, a surfactant, a wetting agent, and a viscosity modifier.
16. The secure document of claim 1, wherein the soil and / or moisture resistant formulation further includes one or more pigments.
17. A method for preparing a blended polyurethane-copolymer formulation, the method comprising: adding, based on a determined number of formulation batches, an amount of water and an amount of a copolymer to a mix tank; dissolving the copolymer in the water in the mix tank using agitation and heat; after dissolution of the copolymer, adding an amount of polyurethane to the mix tank and combining the polyurethane with the dissolved the copolymer; and obtaining the completed blended polyurethane-copolymer formulation.
18. The method of Claim 17, wherein the copolymer is a partially hydrolyzed polyvinyl alcohol having a degree of hydrolysis of a molecular percentage in a range of 78.5-82%.
19. The method of Claim 17, further comprising: pumping the completed blended polyurethane-copolymer formulation to a run tank; and applying the completed blended polyurethane-copolymer formulation to at least one porous substrate using a size press.
20. The method of Claim 17, wherein the copolymer is one of: a polyvinyl alcohol-polyvinyl amine copolymer; a polyvinyl alcohol-polyvinyl pyrrolidone copolymer; or a polyvinyl alcohol-polyvinyl co-acrylamide-methyl-propane-sulfonic acid (CoAmps) copolymer.
21. The method of Claim 17, wherein a final solids concentration of the completed blended polyurethane-copolymer formulation is 12% to 15% of the polyurethane and approximately 5% of the copolymer.
Citation Information
Patent Citations
Glossy ink jet recording materials
US20040152819A1
Soil and / or moisture resistant secure document
US20100230947A1
Porous tantalum used for medical implantation and method for preparing the same
US20130011691A1
Sheet for security documents having high printability and high handling resistance
US5660919A
Porous media having biocidal properties
WO2022243189A1