Production process for paper container with flattened opening folded edges

By forming an annular plane on the opening edge of the paper container and strengthening the processing, the problem of difficulty in sealing the rolled edge of the existing paper container is solved, the strength and flatness of the container are improved, and better sealing and environmental protection are achieved performance.

WO2024221431A1PCT designated stage expired Publication Date: 2024-10-31SHANTOU SAMMA PLASTIC IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/091708
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The upper surface of the rolled edge of existing paper containers is curved. When sealing, the contact area between the edge of the film and the rolled edge is small, making it difficult to ensure a firm seal.

Method used

Using the production process of flattening the paper container with the opening folded and flattened, an annular plane is formed on the opening edge of the paper container, and the annular plane is coated to increase the contact area for easier sealing, and at the same time, the overall quality of the container is improved through heat and pressure treatment Strength and flatness.

Benefits of technology

It improves the strength and flatness of the opening and folding edges of paper containers, increases the sealing and freshness preservation of the seal, is suitable for stacking and logistics transportation, reduces the waste of storage space, and complies with European and American environmental standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023091708_31102024_PF_FP_ABST
    Figure CN2023091708_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A production process for a paper container with flattened opening folded edges. The paper container uses the following paper container structure, and is formed by means of the following steps: the paper container structure comprises a bottom face (1) and a plurality of side faces (2), wherein the bottom face is polygonal, a first gap (3) is provided between every two adjacent side faces, and a connecting piece (4) is provided at each first gap; and the forming steps are as follows: 1) laminating a film on or applying an adhesive layer to a lower surface of a paperboard, and then, according to a development drawing of the paper container, die-cutting a paper container substrate out of the paperboard, and die-pressing corresponding crease lines (6); 2) folding the bottom face, each side face and each connecting piece along the corresponding crease lines to form a semi-finished paper container with opening edges; 3) performing a hot-pressing treatment between each side face and a corresponding connecting piece to shape the whole semi-finished paper container; and 4) flattening the opening edges of the semi-finished paper container to obtain the paper container. The production process can improve the strength and flatness of opening folded edges, thereby facilitating sealing.
Need to check novelty before this filing date? Find Prior Art

Description

Production process for opening, folding and flattening paper container Technical Field

[0001] The invention relates to a production process of a paper container, in particular to a production process of an opening, folding, and flattening paper container. Background Art

[0002] To improve the overall structural strength of paper containers and make them durable, the applicant has designed a foldable, rolled-edge, square-bottom, elliptical wallpaper container and has applied for an invention patent, with the authorization publication number CN216581524U. The foldable, rolled-edge, square-bottom, elliptical wallpaper container comprises a bottom and four side surfaces. The bottom surface is quadrilateral in shape, with the lower side edges of each side surface connected to the corresponding side edge of the bottom surface via corresponding first crease lines. A notch is formed between two adjacent side surfaces, with a fan-shaped connecting piece provided at the notch. The fan-shaped connecting piece has a first notch on its lower side, a second notch connected to the first notch via corresponding second crease lines, a first side of the fan-shaped connecting piece connected to the second side edge of an adjacent side surface via corresponding third crease lines, a second side of the fan-shaped connecting piece connected to the first side edge of another adjacent side surface via corresponding fourth crease lines, and two fifth crease lines provided on the fan-shaped connecting piece. The upper side edges of each side surface are each provided with a rolled-edge portion. The paper container is folded along each crease line to form an elliptical opening.

[0003] Although the side walls of the above-mentioned foldable rolled-edge square-bottom elliptical paper container fit tightly and are not easy to deform, and can improve the overall structural strength of the paper container, and improve the compressive strength of the rolled edge of the paper container opening by forming a rolled edge at the opening of the paper container, the rolled edge of the above-mentioned paper container is formed by rolling the strip edge outward, and the upper surface of the rolled edge is an arc surface. If the opening of the paper container is to be sealed with a film, the edge of the film and the upper surface of the rolled edge are only in line contact, and the contact area is small, making it difficult to ensure that the edge of the film can be firmly sealed on the edge of the opening of the paper container. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a production process for a paper container with an opening folded edge flattened. This production process for a paper container with an opening folded edge flattened can improve the strength and flatness of the opening folded edge and facilitate sealing.

[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0006] A production process for an open, folded, and flattened paper container, characterized by adopting the following paper container structure and forming it through the following steps:

[0007] The paper container structure includes a bottom surface and multiple side surfaces. The bottom surface is polygonal in shape, with a first notch between two adjacent side surfaces, a connecting piece provided at the first notch, a first notch portion provided on the lower side of the connecting piece, and a second notch portion connected to the first notch portion at each corner of the bottom surface; a first strip folding piece is provided on the upper side edge of each side surface, a second strip folding piece is provided on the upper side edge of each first strip folding piece, an arc-shaped folding piece is provided on the upper side edge of each connecting piece, and an arc-shaped folding strip is provided on the upper side edge of each arc-shaped folding piece, each first strip folding piece and each arc-shaped folding piece are folded outward and connected in sequence to form an annular plane, and the annular plane is parallel to the bottom surface; each second strip folding piece and each arc-shaped folding strip are bent downward, and each second strip folding piece is bonded to the lower surface of the corresponding first strip folding piece through an adhesive layer, and each arc-shaped folding strip is bonded to the lower surface of the corresponding arc-shaped folding piece through an adhesive layer;

[0008] The molding steps are as follows:

[0009] (1) Laminating or coating the lower surface of the paperboard with a glue layer, then die-cutting the paper container base sheet on the paperboard according to the unfolded drawing of the paper container and embossing the corresponding crease lines, so that the corresponding positions on the paper container base sheet form the corresponding contours of the bottom surface, each side surface, each connecting piece, each first strip fold piece, each second strip fold piece, each arc-shaped fold piece, and each arc-shaped fold strip;

[0010] (2) folding the bottom surface, each side surface, and each connecting piece along the corresponding crease lines into a semi-finished paper container with an open edge;

[0011] (3) performing hot pressing treatment between each side surface and the corresponding connecting piece to finalize the shape of the entire paper container semi-finished product;

[0012] (4) Flatten the opening edge of the semi-finished paper container:

[0013] (4-1) Folding each first strip fold piece and each arc-shaped fold piece outward to form a folded edge;

[0014] (4-2) Connecting the folded edges in sequence to form a circular plane, and applying a coating on the upper surface of the circular plane;

[0015] (4-3) Bend each second strip fold and each arc-shaped fold downward;

[0016] (4-4) Flattening each first strip folding piece and the corresponding second strip folding piece so that the upper surface of each second strip folding piece fits with the lower surface of the corresponding first strip folding piece; flattening each arcuate folding piece and the corresponding arcuate folding strip so that the upper surface of each arcuate folding strip fits with the lower surface of the corresponding arcuate folding piece, thereby obtaining the paper container.

[0017] When the paper container is folded into a semi-finished product with an open edge, the lower surface of the paperboard becomes the outer surface of the paper container. In step (1), before the paperboard is die-cut, a film or glue layer is applied to the lower surface of the paperboard, that is, the outer surface of the paper container is laminated or coated on one side, so that the outer surface of the paper container is composited with a film layer or glue layer, which can make the outer surface of the paper container waterproof and facilitate hot pressing and laminating the outer surface of the paper container.

[0018] In the above-mentioned paper container structure, the arc-shaped folding pieces on each connecting piece are folded outwardly and connected to the first strip folding pieces on each side surface, which can increase the stiffness of each corner of the opening of the paper container; the above-mentioned annular plane parallel to the bottom surface constitutes a flat opening folding edge of the paper container, which improves the strength and flatness of the opening folding edge and facilitates sealing. If the opening of the paper container needs to be sealed with a film, the contact area between the edge of the film and the annular plane is increased, ensuring that the edge of the film can be firmly sealed on the edge of the opening of the paper container.

[0019] In the above step (3), the folded side surfaces are connected together with the corresponding connecting pieces by heat pressing, which can improve the strength of the entire paper container and prevent leakage even if liquid is placed in the paper container.

[0020] In the above step (4-2), the annular plane is formed by each first strip folding piece, each second strip folding piece, each arc-shaped folding piece, and each arc-shaped folding strip. Applying a coating on the upper surface of the annular plane can enhance the toughness and strength of the annular plane and make the processing smoother.

[0021] In step (4-4), the upper surfaces of the second strip-shaped folds are flattened to fit the lower surfaces of the corresponding first strip-shaped folds, and the upper surfaces of the arcuate folds are flattened to fit the lower surfaces of the corresponding arcuate folds. This increases the thickness of the annular plane and makes the annular plane flatter. This provides support and reinforcement for the bottom of the annular plane, improves the strength and flatness of the opening edge of the paper container, and facilitates subsequent processing. The above-mentioned paper container can be made into lunch boxes, trays, etc.

[0022] In a preferred embodiment, after folding in step (4-1) and before flattening in step (4-4), the folded edge in step (4-1) can be rolled up, and after rolling up, the coating in step (4-2) is applied to the surface of the rolled folded edge, and after applying the coating, the rolled folded edge is flattened.

[0023] In a further preferred embodiment, the curling specifically comprises the following steps:

[0024] (4-1-1) Humidifying the folded edges of semi-finished paper containers;

[0025] (4-1-2) Apply a layer of lubricating oil on the edge of the folded edge of the semi-finished paper container;

[0026] (4-1-3) Roll the folded edge after applying lubricating oil.

[0027] In the above step (4-1-1), the folded edge of the semi-finished paper container is subjected to a humidification pretreatment, which can increase the moisture content of the opening edge of the semi-finished paper container, thereby increasing its toughness and reducing the risk of cracking.

[0028] In the above step (4-1-2), a layer of lubricating oil is applied to the edge of the folded edge of the semi-finished paper container in order to reduce the friction of the paperboard during the subsequent rolling process.

[0029] In a further preferred embodiment, the humidification treatment in step (4-1-1) specifically includes the following steps:

[0030] (4-1-1-1) Control the air humidity in the steam room between 70%RH and 90%RH, and then place the semi-finished paper container in the steam room for 1 hour to 4 hours;

[0031] (4-1-1-2) In the steam room, spray or brush the folded edges with water every 15 to 30 minutes. The number of spraying or brushing is 2 to 4 times.

[0032] During the humidification process, the semi-finished paper container is completely placed in a steam room. The folded edge is wetted by spraying or brushing water, moistening the surface of the folded edge. This changes the moisture distribution on the surface of the folded edge, causing the surface structure of the folded edge to change. The folded edge of the semi-finished paper container can better maintain its toughness and strength, reducing damage during subsequent processing. Finally, the folded edge of the semi-finished paper container is rounded, achieving a better forming effect. The semi-finished paper container is placed in a steam room with constant temperature and humidity, which can prevent the moisture from drying out too quickly after humidification in an environment with unstable humidity. If a steam room is not available, the folded edge can be covered with a wet towel after wetting to prevent the moisture from drying out too quickly after humidification.

[0033] In a further preferred embodiment, the lubricating oil in step (4-1-2) is a food-grade lubricating oil. Using food-grade lubricating oil can ensure the safety of the entire paper container production process.

[0034] In a further preferred embodiment, the food-grade lubricant is of the type DOWCORNING, MOLYKOTE or KLUBER.

[0035] In a preferred embodiment, the coating in step (4-2) is a water-based coating. The water-based coating is a coating with water as the main solvent. Compared with traditional organic solvent-based coatings, it has the characteristics of being environmentally friendly, pollution-free, and non-toxic.

[0036] In a further preferred embodiment, the water-based coating in step (4-2) is a chitosan coating or an acrylate polymer coating. Chitosan coatings are primarily used as interior coatings for food containers, significantly improving their oxidation and moisture resistance. Acrylate polymer coatings are primarily used for coating surfaces of materials such as paper. They offer high light transmittance, flexibility, and shock absorption, meeting diverse product design and functionality requirements.

[0037] In a preferred embodiment, in step (1), the upper surface of the paperboard is coated with a film or a glue layer before the paperboard is die-cut. When the paper container is folded into a semi-finished product with an open edge, the upper surface of the paperboard becomes the inner surface of the paper container, and the lower surface of the paperboard becomes the outer surface of the paper container. Double-sided coating or double-sided coating of the inner and outer surfaces of the paper container can make both the inner and outer surfaces of the paper container waterproof and facilitate hot pressing and bonding the inner and outer surfaces of the paper container. When the inner surface of each side surface is hot pressed with the inner surface of the corresponding connecting piece in step (3), the side surface of the paper container and the connecting piece are bonded more tightly.

[0038] In a further preferred embodiment, the connecting piece is divided into a first fan-shaped folding piece, a central trapezoidal folding piece and a second fan-shaped folding piece by two crease lines, the lower side of the central trapezoidal folding piece is provided with the first notched portion, and the lower side edge of the arc-shaped folding piece is connected to the upper side edge of the central trapezoidal folding piece through the corresponding crease line; in the step (2), the outer surface of the first fan-shaped folding piece is bonded to the outer surface of the central trapezoidal folding piece through the adhesive layer along the corresponding crease line, the inner surface of the first fan-shaped folding piece is bonded to the inner surface of the adjacent side surface through the adhesive layer, the outer surface of the second fan-shaped folding piece is bonded to the outer surface of the central trapezoidal folding piece through the adhesive layer, and the inner surface of the second fan-shaped folding piece is bonded to the inner surface of the adjacent side surface through the adhesive layer; in the step (4-4), the upper surface of the end portion of the first strip folding piece is bonded to the lower surface of the end portion of the adjacent arc-shaped folding piece through the adhesive layer, and the upper surface of the end portion of the second strip folding piece is bonded to the lower surface of the end portion of the adjacent arc-shaped folding strip through the adhesive layer. Arranging the connecting piece as an integrally connected first fan-shaped folded piece, a central trapezoidal folded piece, and a second fan-shaped folded piece can increase the crease when the paper container is folded. The lower side of the arc-shaped folded piece is connected only to the upper side of the central trapezoidal folded piece via corresponding crease lines, and is not connected to the first fan-shaped folded piece or the upper side of the first fan-shaped folded piece. This allows the two ends of the arc-shaped folded piece to have a larger area to cross-fit with the ends of the first strip-shaped folded piece, thereby strengthening the connection between the ends of the arc-shaped folded piece and the ends of the first strip-shaped folded piece and improving the strength of the annular surface.

[0039] In a further preferred embodiment, the first and second fan-shaped folded sheets are each separated by a crease line into two third fan-shaped folded sheets; in step (2), the inner surfaces of the two third fan-shaped folded sheets are bonded together along the corresponding crease line using an adhesive layer, and then the outer surface of the third fan-shaped folded sheet adjacent to the central trapezoidal folded sheet is bonded together with the outer surface of the central trapezoidal folded sheet using an adhesive layer. The thickness of this combined third fan-shaped folded sheet is thicker than that of the original first and second fan-shaped folded sheets, which can better improve the strength of each corner of the side wall of the paper container.

[0040] In a further preferred embodiment, a reinforcing connecting piece integrally connected to the third fan-shaped folded piece is provided on the upper side of the third fan-shaped folded piece adjacent to the corresponding side surface; in step (4-4), the reinforcing connecting piece is bent outward, and the upper surface of the reinforcing connecting piece is bonded to the lower surface of the corresponding arc-shaped folded piece via an adhesive layer. This bonding of the reinforcing connecting piece to the lower surface of the arc-shaped folded piece can further enhance the strength of the annular plane.

[0041] In a preferred embodiment, in step (4-4), a plurality of second notches or tangent lines are provided on the upper side of each of the arcuate folding strips. Each second notch or tangent line divides the arcuate folding strip into a plurality of folding strip segments, and the upper surface of each folding strip segment is bonded to the lower surface of the arcuate folding piece via an adhesive layer. Providing a plurality of second notches or tangent lines on the upper side of the arcuate folding strip can break the tension of the arcuate folding strip, facilitating bonding of the upper surface of the arcuate folding strip to the lower surface of the arcuate folding piece.

[0042] In a further preferred embodiment, the second notch is a V-shaped notch, a U-shaped notch or a C-shaped notch.

[0043] Compared with the prior art, the present invention has the following advantages:

[0044] This production process for paper containers with flattened opening folded edges makes the opening folded edges of the paper containers smoother after the folded edges of the openings are flattened. Multiple paper containers can be stacked higher and more stably to avoid shaking and tilting of the containers, which can save storage space and provide better logistics efficiency. At the same time, paper containers with smooth opening folded edges are easier to seal, which can improve the sealing and freshness preservation of the paper containers.

[0045] While this paper container contains very little plastic during production, its strength and water resistance are similar to those of traditional plastic containers, meeting the stringent standards limiting plastic use in Europe and the United States. Therefore, this paper container not only reduces production and processing costs but is also more environmentally friendly, promoting the sustainable development of paper packaging materials and contributing positively to addressing current global market trends. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] FIG1 is a schematic structural diagram of a specific embodiment 1 of the present invention;

[0047] FIG2 is a schematic diagram of the folded structure of the paper container in specific embodiment 1 of the present invention;

[0048] FIG3 is a schematic structural diagram of the paper container in FIG2 in an inverted state;

[0049] FIG4 is a schematic structural diagram of a specific embodiment 2 of the present invention;

[0050] FIG5 is a schematic diagram of the folded structure of the paper container in specific embodiment 2 of the present invention;

[0051] FIG6 is a schematic structural diagram of the paper container in FIG5 in an inverted state;

[0052] FIG7 is a schematic diagram of the structure of the folded edge and curled circle in specific embodiment 3 of the present invention. Implementation Method

[0053] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0054] Example 1

[0055] As shown in Figures 1-3, the production process of the open, folded, and flattened paper container in this embodiment adopts the following paper container structure and is formed through the following steps:

[0056] The paper container structure includes a bottom surface 1 and multiple side surfaces 2. The bottom surface 1 is in the shape of a polygon. There is a first notch 3 between two adjacent side surfaces 2. A connecting piece 4 is provided at the first notch 3. The lower side of the connecting piece 4 is provided with a first notch portion 41. Each corner on the bottom surface 1 is provided with a second notch portion 11 connected to the first notch portion 41; the upper side of each side surface 2 is provided with a first strip folding piece 21, the upper side of each first strip folding piece 21 is provided with a second strip folding piece 22, and the upper side of each connecting piece 4 is provided with a There are arc-shaped folding pieces 42, and each arc-shaped folding piece 42 is provided with an arc-shaped folding strip 43 on the upper side. Each first strip folding piece 21 and each arc-shaped folding piece 42 are folded outward and connected in sequence to form an annular plane 5, and the annular plane 5 is parallel to the bottom surface 1; each second strip folding piece 22 and each arc-shaped folding strip 43 are bent downward, and each second strip folding piece 22 is bonded to the lower surface of the corresponding first strip folding piece 21 through an adhesive layer, and each arc-shaped folding strip 43 is bonded to the lower surface of the corresponding arc-shaped folding piece 42 through an adhesive layer;

[0057] The molding steps are as follows:

[0058] (1) Applying a glue layer on both the upper and lower surfaces of the paperboard, and then die-cutting a paper container base sheet on the paperboard according to the unfolded diagram of the paper container and embossing corresponding crease lines 6, so that the corresponding positions on the paper container base sheet form the corresponding contours of the bottom surface 1, each side surface 2, each connecting piece 4, each first strip folding piece 21, each second strip folding piece 22, each arc-shaped folding piece 42, and each arc-shaped folding strip 43;

[0059] (2) folding the bottom surface 1, each side surface 2, and each connecting piece 4 along the corresponding crease line 6 into a semi-finished paper container with an open edge;

[0060] (3) performing a hot pressing treatment between each side surface 2 and the corresponding connecting piece 4 to finalize the shape of the entire paper container semi-finished product;

[0061] (4) Flatten the opening edge of the semi-finished paper container:

[0062] (4-1) Folding each of the first strip-shaped folding pieces 21 and each of the arc-shaped folding pieces 42 outward to form folded edges;

[0063] (4-2) Connecting the folded edges in sequence to form an annular plane 5, and applying a coating on the upper surface of the annular plane 5;

[0064] (4-3) Bend each second strip-shaped folding piece 22 and each arc-shaped folding strip 43 downward;

[0065] (4-4) Flatten each first strip fold 21 and the corresponding second strip fold 22 so that the upper surface of each second strip fold 22 is bonded to the lower surface of the corresponding first strip fold 21 through the adhesive layer; flatten each arc-shaped fold 42 and the corresponding arc-shaped fold 43 so that the upper surface of each arc-shaped fold 43 is bonded to the lower surface of the corresponding arc-shaped fold 42 through the adhesive layer, thereby obtaining the paper container.

[0066] In the above-mentioned paper container structure, the arc-shaped folded pieces 42 on each connecting piece 4 are folded outwardly and connected to the first strip folded pieces 21 on each side surface 2, which can increase the stiffness of each corner of the paper container opening; the above-mentioned annular plane 5 parallel to the bottom surface 1 constitutes a flat opening folded edge of the paper container, improves the strength and flatness of the opening folded edge, and facilitates sealing. If the opening of the paper container is to be sealed with a film, the contact area between the edge of the film and the annular plane 5 is increased, ensuring that the edge of the film can be firmly sealed on the edge of the opening of the paper container.

[0067] In the above step (3), the folded side surfaces 2 are connected to the corresponding connecting pieces 4 by heat pressing, which can improve the strength of the entire paper container and prevent leakage even if liquid is placed in the paper container.

[0068] In the above step (4-2), the annular plane 5 is formed by each first strip folding piece 21, each second strip folding piece 22, each arcuate folding piece 42, and each arcuate folding strip 43. Applying a coating on the upper surface of the annular plane 5 can enhance the toughness and strength of the annular plane 5 and make the processing more stable.

[0069] In step (4-4), the upper surface of each second strip-shaped folded piece 22 is flattened to fit against the lower surface of the corresponding first strip-shaped folded piece 21, and the upper surface of each arcuate folded piece 43 is flattened to fit against the lower surface of the corresponding arcuate folded piece 42. This increases the thickness of the annular plane 5, making it flatter and supporting the bottom of the annular plane 5. This improves the strength and flatness of the opening edge of the paper container, making it easier to process. The above-mentioned paper container can be made into a lunch box, a tray, etc.

[0070] The water-based coating in step (4-2) is an acrylate polymer coating.

[0071] In step (1), before die-cutting, the upper and lower surfaces of the paperboard are laminated or coated with a glue layer. When the paper container is folded into a semi-finished product with an open edge, the upper surface of the paperboard becomes the inner surface of the paper container, and the lower surface of the paperboard becomes the outer surface of the paper container. Laminating or coating the inner and outer surfaces of the paper container on both sides can make both the inner and outer surfaces of the paper container waterproof and facilitate hot pressing and bonding the inner and outer surfaces of the paper container. When the inner surface of each side surface 2 and the inner surface of the corresponding connecting piece 4 are hot pressed in step (3), the side surface 2 of the paper container and the connecting piece 4 are bonded more tightly.

[0072] The connecting piece 4 is divided into a first fan-shaped folded piece 44, a central trapezoidal folded piece 45 and a second fan-shaped folded piece 46 by two crease lines 6. The lower side of the central trapezoidal folded piece 45 is provided with the first corner notch 41. The lower side of the arc-shaped folded piece 42 is connected to the upper side of the central trapezoidal folded piece 45 through the corresponding crease line 6. In the step (2), the outer surface of the first fan-shaped folded piece 44 is bonded to the outer surface of the central trapezoidal folded piece 45 through the adhesive layer along the corresponding crease line 6, and the inner surface of the first fan-shaped folded piece 44 is bonded to the outer surface of the central trapezoidal folded piece 45. The adhesive layer is bonded to the inner surface of the adjacent side surface 2, the outer surface of the second fan-shaped folded piece 46 is bonded to the outer surface of the central trapezoidal folded piece 45, and the inner surface of the second fan-shaped folded piece 46 is bonded to the inner surface of the adjacent side surface 2. In step (4-4), the upper surface of the end of the first strip-shaped folded piece 21 is bonded to the lower surface of the end of the adjacent arc-shaped folded piece 42, and the upper surface of the end of the second strip-shaped folded piece 22 is bonded to the lower surface of the end of the adjacent arc-shaped folded strip 43. Arranging the connecting piece 4 as an integrally connected first fan-shaped folded piece 44, central trapezoidal folded piece 45, and second fan-shaped folded piece 46 can increase the crease when the paper container is folded. The lower side of the above-mentioned arc-shaped folding piece 42 is only connected to the upper side of the central trapezoidal folding piece 45 through the corresponding crease line 6, and is not connected to the first fan-shaped folding piece 44 or the upper side of the first fan-shaped folding piece 44, so that the two ends of the arc-shaped folding piece 42 have a larger area to cross-fit with the end of the first strip folding piece 21, which can strengthen the connection between the end of the arc-shaped folding piece 42 and the end of the first strip folding piece 21, and improve the strength of the annular plane 5.

[0073] In step (4-4), multiple second notches 431 are provided on the upper side of each of the curved folding strips 43. Each second notch 431 divides the curved folding strip 43 into multiple folding strip segments. The upper surface of each folding strip segment is bonded to the lower surface of the curved folding piece 42 via an adhesive layer. Providing multiple second notches 431 on the upper side of the curved folding strip 43 breaks the tension of the curved folding strip 43, facilitating bonding the upper surface of the curved folding strip 43 to the lower surface of the curved folding piece 42. These second notches 431 are V-shaped.

[0074] Example 2

[0075] As shown in Figures 4-6, the production process of the paper container with an open, folded edge and flattened in this embodiment differs from that in Example 1 in that:

[0076] The first fan-shaped folded sheet 44 and the second fan-shaped folded sheet 46 are each separated into two third fan-shaped folded sheets 47 by a crease line 6. In step (2), the inner surfaces of the two third fan-shaped folded sheets 47 are bonded together along the corresponding crease line 6 by means of an adhesive layer, and then the outer surface of the third fan-shaped folded sheet 47 adjacent to the central trapezoidal folded sheet 45 is bonded together with the outer surface of the central trapezoidal folded sheet 45 by means of an adhesive layer. The thickness of the combined third fan-shaped folded sheet 47 is thicker than that of the original first fan-shaped folded sheet 44 and the second fan-shaped folded sheet 46, and can better improve the strength of the corners of the side wall of the paper container.

[0077] A reinforcing connecting piece 8 is provided on the upper side of the third fan-shaped folded piece 47 adjacent to the corresponding side surface 2 and integrally connected to the third fan-shaped folded piece 47. In step (4-4), the reinforcing connecting piece 8 is bent outward, and the upper surface of the reinforcing connecting piece 8 is bonded to the lower surface of the corresponding arc-shaped folded piece 42 via an adhesive layer. This bonding of the reinforcing connecting piece 8 to the lower surface of the arc-shaped folded piece 42 can further enhance the strength of the annular plane 5.

[0078] Example 3

[0079] As shown in FIG7 , the production process of the paper container with an open, folded edge and flattened surface in this embodiment differs from that in Example 1 in that:

[0080] After folding in step (4-1) and before flattening in step (4-4), the folded edge in step (4-1) can be rolled up, and then the coating in step (4-2) is applied to the surface of the rolled folded edge. After the coating is applied, the rolled folded edge is flattened.

[0081] The above-mentioned curling specifically comprises the following steps:

[0082] (4-1-1) Humidifying the folded edges of semi-finished paper containers;

[0083] (4-1-2) Apply a layer of lubricating oil on the edge of the folded edge of the semi-finished paper container;

[0084] (4-1-3) Roll the folded edge after applying lubricating oil.

[0085] In the above step (4-1-1), the folded edge of the semi-finished paper container is subjected to a humidification pretreatment, which can increase the moisture content of the opening edge of the semi-finished paper container, thereby increasing its toughness and reducing the risk of cracking.

[0086] In the above step (4-1-2), a layer of lubricating oil is applied to the edge of the folded edge of the semi-finished paper container in order to reduce the friction of the paperboard during the subsequent rolling process.

[0087] The humidification treatment in step (4-1-1) specifically includes the following steps:

[0088] (4-1-1-1) Control the air humidity in the steaming room to 80% RH, and then place the semi-finished paper container in the steaming room for 2 hours;

[0089] (4-1-1-2) In the steam room, spray or brush the folded edges with water every 20 minutes, and spray or brush with water twice.

[0090] During the humidification process, the semi-finished paper container is completely placed in a steam room. The folded edge is wetted by spraying or brushing water, moistening the surface of the folded edge. This changes the moisture distribution on the surface of the folded edge, causing the surface structure of the folded edge to change. The folded edge of the semi-finished paper container can better maintain its toughness and strength, reducing damage during subsequent processing. Finally, the folded edge of the semi-finished paper container is rounded, achieving a better forming effect. The semi-finished paper container is placed in a steam room with constant temperature and humidity, which can prevent the moisture from drying out too quickly after humidification in an environment with unstable humidity. If a steam room is not available, the folded edge can be covered with a wet towel after wetting to prevent the moisture from drying out too quickly after humidification.

[0091] The lubricant in step (4-1-2) is Dow Corning's food-grade lubricant. Using food-grade lubricant ensures the safety of the entire paper container production process.

[0092] Example 4

[0093] The production process of the paper container with an open, folded edge and flattened in this embodiment differs from that in Example 1 in that:

[0094] In the above-mentioned forming step (1), the glue layer is only applied to the lower surface of the paperboard. When the paper container is folded into a semi-finished product with an open edge, the lower surface of the paperboard becomes the outer surface of the paper container. In step (1), before the paperboard is die-cut, the lower surface of the paperboard is coated with a film or a glue layer, that is, the outer surface of the paper container is coated with a single-sided film or a single-sided coating, so that the outer surface of the paper container is composited with a film layer or a glue layer, which can make the outer surface of the paper container waterproof and facilitate the hot pressing bonding of the outer surface of the paper container.

[0095] In addition, it should be noted that the names of the various parts of the specific embodiments described in this specification may be different. Any equivalent or simple changes made based on the structure, features, and principles described in the patent concept of the present invention are included in the scope of protection of the patent of this invention. Those skilled in the art of the technical field to which the present invention relates may make various modifications, supplements, or replace the specific embodiments described in the description with similar methods. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall fall within the scope of protection of the present invention.

Claims

1. A production process for an open, folded, and flattened paper container, characterized in that The following paper container structure is used and formed through the following steps: The paper container structure includes a bottom surface and multiple side surfaces. The bottom surface is in a polygonal shape. There is a first notch between two adjacent side surfaces. A connecting piece is provided at the first notch. A first notch portion is provided at the lower side of the connecting piece. A second notch portion connected to the first notch portion is provided at each corner of the bottom surface. A first strip folding piece is provided at the upper side edge of each side surface. A second strip folding piece is provided at the upper side edge of each first strip folding piece. An arc-shaped folding piece is provided at the upper side edge of each connecting piece. An arc-shaped folding strip is provided at the upper side edge of each arc-shaped folding piece. Each first strip folding piece and each arc-shaped folding piece are folded outward and connected in sequence to form an annular plane. The annular plane is parallel to the bottom surface. Each second strip folding piece and each arc-shaped folding strip are bent downward, and each second strip folding piece is bonded to the lower surface of the corresponding first strip folding piece through an adhesive layer, and each arc-shaped folding strip is bonded to the lower surface of the corresponding arc-shaped folding piece through an adhesive layer. The molding steps are as follows: (1) Laminating or coating the lower surface of the paperboard with a glue layer, and then die-cutting a paper container base sheet on the paperboard according to the unfolded view of the paper container and embossing corresponding crease lines, so that the corresponding positions on the paper container base sheet form the corresponding contours of the bottom surface, each side surface, each connecting piece, each first strip folding piece, each second strip folding piece, each arc-shaped folding piece, and each arc-shaped folding strip; (2) folding the bottom surface, each side surface, and each connecting piece along the corresponding crease lines into a semi-finished paper container with an opening edge; (3) performing heat pressing treatment on each side surface and the corresponding connecting piece to finalize the shape of the entire paper container semi-finished product; (4) Flatten the opening edge of the semi-finished paper container: (4-1) Folding each first strip folding piece and each arc-shaped folding piece outward to form a folded edge; (4-2) connecting the folded edges in sequence to form a circular plane, and applying a coating on the upper surface of the circular plane; (4-3) Bend each second strip folding piece and each arc-shaped folding strip downward; (4-4) Flatten each first strip folding piece and the corresponding second strip folding piece so that the upper surface of each second strip folding piece fits with the lower surface of the corresponding first strip folding piece; flatten each arc-shaped folding piece and the corresponding arc-shaped folding strip so that the upper surface of each arc-shaped folding strip fits with the lower surface of the corresponding arc-shaped folding piece, thereby obtaining the paper container.

2. The production process of the paper container with open folded edges and flattened as claimed in claim 1, characterized in that: After folding in step (4-1) and before flattening in step (4-4), the folded edge in step (4-1) can be rolled up, and after rolling up, the coating in step (4-2) is applied to the surface of the rolled folded edge, and after applying the coating, the rolled folded edge is flattened.

3. The production process of the paper container with open folded edges and flattened as claimed in claim 2, characterized in that: The curling specifically comprises the following steps: (4-1-1) Humidifying the folded edge of the semi-finished paper container; (4-1-2) Apply a layer of lubricating oil on the edge of the folded edge of the semi-finished paper container; (4-1-3) Roll the folded edge that has been lubricated.

4. The process for producing an open, folded, and flattened paper container according to claim 3, characterized in that: The humidification treatment in step (4-1-1) specifically includes the following steps: (4-1-1-1) Control the air humidity in the steam room between 70%RH-90%RH, and then place the semi-finished paper container in the steam room for 1 hour to 4 hours; (4-1-1-2) In the steam room, spray or brush the folded edges with water every 15 to 30 minutes. The number of spraying or brushing with water is 2 to 4 times.

5. The production process of the paper container with open folded edges and flattened as claimed in claim 1, characterized in that: The coating in step (4-2) is a water-based coating.

6. The production process of the paper container with open folded edges and flattened as claimed in claim 1, characterized in that: In the step (1), before the cardboard is die-cut, a film or a glue layer is applied on the upper surface of the cardboard.

7. The process for producing an open, folded, and flattened paper container according to claim 6, characterized in that: The connecting sheet is divided into a first fan-shaped folding sheet, a central trapezoidal folding sheet and a second fan-shaped folding sheet by two crease lines, the lower side of the central trapezoidal folding sheet is provided with the first notched corner portion, and the lower side edge of the arc-shaped folding sheet is connected to the upper side edge of the central trapezoidal folding sheet through the corresponding crease line; in the step (2), the outer surface of the first fan-shaped folding sheet is bonded to the outer surface of the central trapezoidal folding sheet through the adhesive layer along the corresponding crease line, the inner surface of the first fan-shaped folding sheet is bonded to the inner surface of the adjacent side surface through the adhesive layer, the outer surface of the second fan-shaped folding sheet is bonded to the outer surface of the central trapezoidal folding sheet through the adhesive layer, and the inner surface of the second fan-shaped folding sheet is bonded to the inner surface of the adjacent side surface through the adhesive layer; in the step (4-4), the upper surface of the end of the first strip folding sheet is bonded to the lower surface of the end of the adjacent arc-shaped folding sheet through the adhesive layer, and the upper surface of the end of the second strip folding sheet is bonded to the lower surface of the end of the adjacent arc-shaped folding strip through the adhesive layer.

8. The production process of the paper container with open folded edges and flattened as claimed in claim 7, characterized in that: The first fan-shaped folded sheet and the second fan-shaped folded sheet are each divided into two third fan-shaped folded sheets by a crease line; in the step (2), the inner surfaces of the two third fan-shaped folded sheets are bonded together along the corresponding crease line through an adhesive layer, and then the outer surface of the third fan-shaped folded sheet adjacent to the central trapezoidal folded sheet is bonded to the outer surface of the central trapezoidal folded sheet through an adhesive layer.

9. The process for producing an open, folded, and flattened paper container according to claim 8, characterized in that: A reinforcing connecting sheet integrally connected to the third fan-shaped folding sheet is provided on the upper side edge of the third fan-shaped folding sheet adjacent to the corresponding side surface; in the step (4-4), the reinforcing connecting sheet is bent outward, and the upper surface of the reinforcing connecting sheet is bonded to the lower surface of the corresponding arc-shaped folding sheet through an adhesive layer.

10. The process for producing an open, folded, and flattened paper container according to claim 1, characterized in that: In the step (4-4), a plurality of second notches or a plurality of tangents are provided on the upper side edge of each of the arc-shaped folding strips, and each of the second notches or tangents divides the arc-shaped folding strip into a plurality of folding strip segments, and the upper surface of each folding strip segment is bonded to the lower surface of the arc-shaped folding piece through an adhesive layer.

Citation Information

Patent Citations

  • Folding type rolled edge square bottom oval wall paper container

    CN216581524U

  • Paper box forming machine

    CN2250234Y

  • According to the build-up of food or the like for forming paper plate with vessel and dividing

    JP1992128215U

  • Heat-insulating container made of paper

    JP1999348966A

  • Blank for paper container with flange, paper container with flange, and paper container

    JP2013052900A