Low-cost bridge steel and manufacturing method thereof
Through Nb-Ti-B composite alloy and magnesium metallurgical technology, combined with deoxidation alloying, vacuum treatment and electromagnetic stirring and other processes, high-performance bridge steel is formed, which solves the problem of insufficient low-temperature impact performance and welding performance of bridge steel and achieves low-temperature Cost, high strength and high toughness enhance market competitiveness.
Patent Information
- Application Number
- PCT/CN2023/100372
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-06-15
- Publication Date
- 2024-10-31
AI Technical Summary
While ensuring the strength of existing bridge steel, it is difficult to achieve low-temperature impact properties of more than 120J under low-temperature conditions. At the same time, the processing performance and welding performance of the steel plate must be taken into consideration. As a result, the cost is relatively high under the requirements of high strength, high toughness and low yield-strength ratio. High, and the welding performance is insufficient.
Using Nb-Ti-B composite alloy technology and magnesium metallurgy technology, through deoxidation alloying, vacuum treatment, electromagnetic stirring and two-stage rolling process, a metallographic structure of granular bainite + ferrite + pearlite is formed, reducing precious metals. The use of elements improves strength and welding performance, and improves internal stress and performance through high redness treatment.
It has achieved the improvement of high strength, toughness and welding performance of bridge steel at low cost, reduced alloy design costs, improved market competitiveness, and achieved an impact absorption energy of more than 120J under low temperature conditions of -40°C, and 180 degrees There are no obvious cracks on the curved outer surface.
Smart Images

Figure CN2023100372_31102024_PF_FP_ABST
Abstract
Description
Low-cost bridge steel and manufacturing method thereof Technical Field
[0001] The present invention relates to the technical field of steel production, in particular to low-cost bridge steel and a manufacturing method thereof. Background Art
[0002] With the rapid development of my country's economy, infrastructure construction has also been vigorously developed. Among them, the bridge industry is developing rapidly. With the continuous improvement of bridge quality, heavy load, high speed and large span have become the main development directions. The new generation of high-performance bridge steel that integrates high strength, high toughness, low yield ratio, easy welding and other properties is the preferred material for key components of large-span and heavy-load railway steel bridges. The demand is clear and urgent.
[0003] The continuous improvement of bridge quality requires a qualitative change in steel quality, especially for extra-thick bridge steel. It is extremely difficult to achieve a low-temperature impact strength of -40°C exceeding 120J while maintaining strength. At the same time, the processing and welding properties of the steel plate must also be taken into consideration. Therefore, the development of efficient and easy-to-weld bridge products is crucial to the company's future development.
[0004] Summary of the Invention
[0005] The present invention aims to solve the above-mentioned technical problems, overcomes the shortcomings of the prior art, and provides a low-cost bridge steel, whose chemical composition and mass percentage are as follows: C: 0.10% to 0.16%, Si: 0.15% to 0.35%, Mn: 1.20% to 1.60%, P≤0.018%, S≤0.005%, Nb: 0.020% to 0.040%, V: 0.020% to 0.050%, Ti: 0.008% to 0.030%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0005% to 0.0020%, Mg: 0.0008% to 0.0015%, Al: 0.015% to 0.030%, and the balance is Fe and unavoidable impurities.
[0006] The technical solution further defined in the present invention is:
[0007] The chemical composition and mass percentage of the low-cost bridge steel mentioned above are as follows: C: 0.12%~0.13%, Si: 0.25%~0.35%, Mn: 1.40%~1.60%, P≤0.015%, S≤0.003%, Nb: 0.030%~0.040%, V: 0.020%~0.030%, Ti: 0.010%~0.020%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0008%~0.0012%, Mg: 0.0010%~0.0013%, Al: 0.020%~0.025%, and the balance is Fe and unavoidable impurities.
[0008] The chemical composition and mass percentage of the low-cost bridge steel mentioned above are as follows: C: 0.12%~0.15%, Si: 0.20%~0.25%, Mn: 1.30%~1.50%, P≤0.015%, S≤0.002%, Nb: 0.025%~0.035%, V: 0.030%~0.040%, Ti: 0.015%~0.030%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0018%~0.0020%, Mg: 0.0009%~0.0013%, Al: 0.018%~0.028%, and the balance is Fe and unavoidable impurities.
[0009] Another object of the present invention is to provide a low-cost bridge steel manufacturing method, comprising the following steps:
[0010] S1. Smelting is carried out in a smelting furnace with a tapping temperature of 1620-1680 degrees. Deoxidation and alloying are performed during the tapping process, and ferroboron is added for boron alloying.
[0011] S2. After the molten steel arrives at the LF furnace, it is alloyed as required. After deoxidation and alloying, it is sent to the RH for vacuum treatment. The vacuum time is 15 to 18 minutes. After vacuum treatment, it is simmered in 200 to 230 meters of magnesium-aluminum wire. After magnesium treatment, it is statically stirred for 12 to 15 minutes.
[0012] S3, after the molten steel reaches the continuous casting, it is cast, with an overheat of 30 to 40 degrees, using electromagnetic stirring technology, using weak cooling mode for cooling, and moving the dynamic light pressure as far back as possible;
[0013] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1200±50 degrees and a heating time of 10-15 min / cm;
[0014] S5, adopts two-stage rolling process, the second rolling temperature is 880-950 degrees, the final rolling temperature is 790-870 degrees, the cooling temperature is 750-830 degrees, and the red-returning temperature is 550-650 degrees;
[0015] S7. The rolled piece is directly pile-cooled on the cooling bed for 10 to 20 hours. After the pile-cooling is completed, it is straightened, sheared, marked, inspected for flaws, and put into storage.
[0016] In the aforementioned low-cost bridge steel manufacturing method, the finished steel plate has a thickness of 5 to 80 mm.
[0017] In the aforementioned low-cost bridge steel manufacturing method, the metallographic structure of the steel plate is mainly granular bainite + ferrite + pearlite.
[0018] The aforementioned low-cost bridge steel manufacturing method has a steel grade of Q235~Q370MPa, and the steel plate has the following properties: yield strength 225~370MPa, tensile strength 400~510MPa, elongation after fracture >20%, -40 degree impact absorption energy >47J, and no cracks visible to the naked eye on the outer surface when bent at 180 degrees.
[0019] The beneficial effects of the present invention are:
[0020] (1) The present invention adopts Nb-Ti-B composite alloy technology to form niobium carbonitride compounds. At the same time, a trace amount of boron solid-solution pins the grain boundaries and precipitates a small amount of BN, which promotes the formation of ferrite, improves the strength and toughness of the product, reduces the use of precious elements such as Cr, Ni, Mo, and Cu, reduces the alloy design cost, and improves market competitiveness;
[0021] (2) The present invention adopts magnesium metallurgy technology to enhance the use effect of element B. The application of magnesium reduces the harm of sulfides, improves the utilization rate of boron, stabilizes the mechanical properties of the product, and also improves the welding performance of the product, thereby improving the use effect of bridge steel.
[0022] (3) The present invention adopts high superheat combined with electromagnetic stirring technology and uses a weak cooling mode, which can even out the grain size of the ingot cooling, ensure that the boron element is dissolved in the ferrite grains to a greater extent, and precipitates between the grains after rolling, thereby improving the strength and hardenability of the product;
[0023] (4) The use of the Nb-Ti-B composite alloy in the present invention can ensure that more M / A components are formed around the bulk ferrite, thereby improving the welding performance of the product;
[0024] (5) The steel plate with high reddening in the present invention is directly stacked and cooled off the production line, which can play the role of self-tempering, improve the internal stress of the steel plate, uniformize the structure and performance, and also reduce the manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the metallographic structure of the steel plate. DETAILED DESCRIPTION
[0026] Example 1
[0027] The present embodiment provides a low-cost bridge steel with a thickness of 9 mm, and its chemical composition and mass percentage are as follows: C: 0.13%, Si: 0.23%, Mn: 1.31%, P: 0.009%, S: 0.002%, Nb: 0.031%, V: 0.043%, Ti: 0.018%, Cr: 0.02%, Ni: 0.02%, Mo: 0.05%, Cu: 0.02%, B: 0.0009%, Mg: 0.0011%, Al: 0.021%, and the balance is Fe and unavoidable impurities.
[0028] The manufacturing method comprises the following steps:
[0029] S1. Smelting is carried out in a smelting furnace with a tapping temperature of 1651 degrees. Deoxidation and alloying are performed during the tapping process, and ferroboron is added for boron alloying.
[0030] S2. After the molten steel arrives at the LF furnace, it is alloyed as required. After deoxidation and alloying, it is sent to the RH for vacuum treatment. The vacuum time is 17 minutes. After vacuum treatment, 210 meters of magnesium-aluminum wire is added. After magnesium treatment, static stirring is carried out for 13 minutes.
[0031] S3, after the molten steel reaches the continuous casting, it is casted with a superheat of 33 degrees. Electromagnetic stirring technology is used, and weak cooling mode is used for cooling. Dynamic light pressure is moved as far back as possible;
[0032] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1231 degrees and a heating time of 13 min / cm;
[0033] S5, adopts two-stage rolling process, second rolling temperature is 896 degrees, final rolling temperature is 830 degrees, cooling temperature is 790 degrees, and returning to red temperature is 590 degrees;
[0034] S7. The rolled piece is directly pile-cooled on the cooling bed for 16 hours. After the pile-cooling is completed, it is straightened, sheared, marked, inspected for flaws, and put into storage.
[0035] Example 2
[0036] The present embodiment provides a low-cost bridge steel with a thickness of 55 mm, and its chemical composition and mass percentage are as follows: C: 0.12%, Si: 0.17%, Mn: 1.55%, P: 0.011%, S: 0.001%, Nb: 0.026%, V: 0.043%, Ti: 0.023%, Cr: 0.02%, Ni: 0.03%, Mo: 0.0:2%, Cu: 0.02%, B: 0.0007%, Mg: 0.0011%, Al: 0.019%, and the balance is Fe and unavoidable impurities.
[0037] The manufacturing method comprises the following steps:
[0038] S1. Smelting is carried out in a smelting furnace with a tapping temperature of 1669 degrees. Deoxidation and alloying are performed during the tapping process, and ferroboron is added for boron alloying.
[0039] S2. After the molten steel arrives at the LF furnace, it is alloyed as required. After deoxidation and alloying, it is sent to the RH for vacuum treatment. The vacuum time is 16 minutes. After vacuum treatment, 220 meters of magnesium-aluminum wire is added. After magnesium treatment, static stirring is carried out for 15 minutes.
[0040] S3, after the molten steel reaches the continuous casting, it is casted with a superheat of 36 degrees. Electromagnetic stirring technology is used, and weak cooling mode is used for cooling. Dynamic light pressure is moved as far back as possible;
[0041] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1206 degrees and a heating time of 115 min / cm;
[0042] S5, adopts two-stage rolling process, second rolling temperature is 886 degrees, final rolling temperature is 798 degrees, cooling temperature is 770 degrees, and red-return temperature is 560 degrees;
[0043] S7. The rolled piece is directly pile-cooled on the cooling bed for 12 hours. After the pile-cooling is completed, it is straightened, sheared, marked, inspected for flaws, and put into storage.
[0044] Example 3
[0045] The present embodiment provides a low-cost bridge steel with a thickness of 68 mm, and its chemical composition and mass percentage are as follows: C: 0.15%, Si: 0.33%, Mn: 1.53%, P: 0.015%, S: 0.002%, Nb: 0.031%, V: 0.041%, Ti: 0.009%, Cr: 0.01%, Ni: 0.02%, Mo: 0.03%, Cu: 0.02%, B: 0.0013%, Mg: 0.0010%, Al: 0.022%, and the balance is Fe and unavoidable impurities.
[0046] The manufacturing method comprises the following steps:
[0047] S1. Smelting is carried out in a smelting furnace with a tapping temperature of 1636 degrees. Deoxidation and alloying are performed during the tapping process, and ferroboron is added for boron alloying.
[0048] S2. After the molten steel arrives at the LF furnace, it is alloyed as required. After deoxidation and alloying, it is sent to the RH for vacuum treatment. The vacuum time is 16 minutes. After vacuum treatment, 210 meters of magnesium-aluminum wire is added. After magnesium treatment, static stirring is carried out for 13 minutes.
[0049] S3, after the molten steel reaches the continuous casting, it is casted with a superheat of 37 degrees. Electromagnetic stirring technology is used, and weak cooling mode is used for cooling. Dynamic light pressure is moved as far back as possible;
[0050] S4, after the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1209 degrees and a heating time of 13 min / cm;
[0051] S5, adopts two-stage rolling process, second opening temperature is 883 degrees, final rolling temperature is 797 degrees, opening cooling temperature is 759 degrees, and returning to red temperature is 5553 degrees;
[0052] S7. The rolled piece is directly pile-cooled on the cooling bed for 18 hours. After the pile-cooling is completed, it is straightened, sheared, marked, inspected for flaws, and put into storage.
[0053] The properties of the steel plates of Examples 1, 2, and 3 are as follows:
[0054] In addition to the above embodiments, the present invention may also have other implementations. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A low-cost bridge steel, characterized by: Its chemical composition and mass percentage are as follows: C: 0.10%~0.16%, Si: 0.15%~0.35%, Mn: 1.20%~1.60%, P≤0.018%, S≤0.005%, Nb: 0.020%~0.040%, V: 0.020%~0.050%, Ti: 0.008%~0.030%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0005%~0.0020%, Mg: 0.0008%~0.0015%, Al: 0.015%~0.030%, and the balance is Fe and unavoidable impurities.
2. The low-cost bridge steel according to claim 1, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.12%~0.13%, Si: 0.25%~0.35%, Mn: 1.40%~1.60%, P≤0.015%, S≤0.003%, Nb: 0.030%~0.040%, V: 0.020%~0.030%, Ti: 0.010%~0.020%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0008%~0.0012%, Mg: 0.0010%~0.0013%, Al: 0.020%~0.025%, and the balance is Fe and unavoidable impurities.
3. The low-cost bridge steel according to claim 1, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.12% ~ 0.15%, Si: 0.20% ~ 0.25%, Mn: 1.30% ~ 1.50%, P≤0.015%, S≤0.002%, Nb: 0.025% ~ 0.035%, V: 0.030% ~ 0.040%, Ti: 0.015% ~ 0.030%, Cr≤0.05%, Ni≤0.05%, Mo≤0.05%, Cu≤0.05%, B: 0.0018% ~ 0.0020%, Mg: 0.0009% ~ 0.0013%, Al: 0.018% ~ 0.028%, and the balance is Fe and unavoidable impurities.
4. A low-cost bridge steel manufacturing method, characterized in that: Applicable to any one of claims 1 to 3, comprising the following steps: S1. Smelting is carried out in a smelting furnace with a tapping temperature of 1620-1680 degrees. Deoxidation and alloying are performed during the tapping process, and ferroboron is added for boron alloying; S2. After the molten steel reaches the LF furnace, alloying operation is carried out as required. After deoxidation and alloying, it is sent to the RH for vacuum treatment. The vacuum time is 15 to 18 minutes. After vacuum treatment, 200 to 230 meters of magnesium-aluminum wire is put into it. After magnesium treatment, static stirring is carried out for 12 to 15 minutes. S3, after the molten steel reaches the continuous casting, it is casted, the superheat is 30-40 degrees, electromagnetic stirring technology is used, weak cooling mode is used for cooling, and dynamic light pressure is moved back as much as possible; S4. After the billet is cooled, it is sent to the heating furnace for heating at a temperature of 1200±50 degrees for a heating time of 10~ 15min / cm; S5, adopt two-stage rolling process, the second rolling temperature is 880-950 degrees, the final rolling temperature is 790-870 degrees, the cooling temperature is 750-830 degrees, and the red-returning temperature is 550-650 degrees; S7. The rolled piece is directly cooled on the cooling bed for 10 to 20 hours. After cooling, it is straightened, sheared, marked, inspected and put into storage.
5. A low-cost bridge steel manufacturing method according to claim 4, characterized in that: The thickness of the finished steel plate is 5 to 80 mm.
6. A low-cost bridge steel manufacturing method according to claim 4, characterized in that: The metallographic structure of the steel plate is mainly granular bainite + ferrite + pearlite.
7. A low-cost bridge steel manufacturing method according to claim 4, characterized in that: The steel grade is Q235~Q370MPa, and the properties of the steel plate are: yield strength 225~370MPa, tensile strength 400~510MPa, elongation after fracture>20%, -40 degree impact absorption energy>47J, and no cracks visible to the naked eye on the outer surface of 180 degree bending.
Citation Information
Patent Citations
Low-cost high-performance Q500 bridge steel and production method thereof
CN112210719A
345MPa-grade weather-resistant bridge steel and manufacturing method thereof
CN113046627A
Efficient welding bridge steel and manufacturing method thereof
CN113234999A
Thin-gauge alloy steel and production method thereof
CN114517272A
Thin-gauge bridge steel and production method thereof
CN114525453A