Modification method for air separation membrane
By constructing a Ni-Co-O nanowire structure on the surface of the PANI separation membrane, the deficiencies in the nitrogen and oxygen separation effect and mechanical properties of the existing PANI air separation membrane are solved, and the separation of high oxygen content and high purity air is achieved, significantly improving It improves the separation effect and the membrane's ability to withstand pressure differences, and reduces production costs.
Patent Information
- Application Number
- PCT/CN2023/119080
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2023-09-15
- Publication Date
- 2024-10-31
AI Technical Summary
The existing PANI air separation membrane has poor nitrogen and oxygen separation effects and limited mechanical properties. It is difficult to separate high oxygen content and high purity air and is easily damaged, resulting in low production costs and efficiency.
By constructing a Ni-Co-O nanowire structure on the surface of the PANI separation membrane, the stable loading and connection of copper ions and PANI molecular fibers is used to form a Cu-Ni-Co-O composite oxide, which enhances the oxygen-phobic and mechanical properties of the membrane. , improve the nitrogen and oxygen separation effect.
The nitrogen and oxygen separation effect is significantly improved, and the oxygen concentration can reach more than 50% VOL, which improves the mechanical properties and pressure difference resistance of the membrane, reduces the need for pressurizing equipment, reduces production costs and improves efficiency.
Smart Images

Figure CN2023119080_31102024_PF_FP_ABST
Abstract
Description
Modification method of air separation membrane Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and in particular relates to a method for modifying an air separation membrane. Background Art
[0002] Air separation technology, also known as air separation technology, is a relatively low-cost method for separating gaseous components in air. It is commonly used to separate nitrogen and oxygen in air. It mainly uses adsorption, separation, and cryogenic methods.
[0003] Generally speaking, membrane separation utilizes membrane permeation technology, utilizing the permeability of oxygen and nitrogen permeation membranes to achieve a rough separation of nitrogen and oxygen components, thereby achieving enrichment to a certain extent. Furthermore, membrane separation is the most universally applicable and relatively low-cost method. However, due to limitations in existing separation membrane technology, the actual maximum oxygen-enriched air that can be obtained is only approximately 28-32% vol oxygen content. It is difficult to achieve air with a higher oxygen content, and it is impossible to produce high-purity products. Furthermore, most existing membrane separation methods utilize PANI self-supporting membranes, which have limited actual strength and are prone to breakage during use. Once damage occurs and cannot be detected in time, it will cause huge losses to the company.
[0004] Modification of air separation membranes is a relatively important research and development direction. For example, the common practice of modifying PANI with PI to prepare a PANI-PI composite separation membrane improves its mechanical strength, but the actual separation effect is still relatively limited and it is difficult to achieve a significant improvement. Technical issues
[0005] In order to solve the problems of limited practical use effect of existing PANI material air separation membranes, poor nitrogen and oxygen separation effect, and need to improve mechanical properties, the present invention provides a modification method for air separation membranes.
[0006] The main objectives of the present invention are:
[0007] 1. It can effectively improve the nitrogen and oxygen separation performance of existing PANI separation membranes;
[0008] 2. It can improve the mechanical properties of existing PANI separation membranes. Technical Solutions
[0009] To achieve the above objectives, the present invention adopts the following technical solutions.
[0010] A method for modifying an air separation membrane,
[0011] The method comprises:
[0012] 1) Dissolving a soluble copper salt in a DMF aqueous solution to prepare a Cu-DMF aqueous solution as a treatment solution;
[0013] 2) Immersing the PANI separation membrane in a treatment solution for constant temperature immersion treatment, adjusting the pH value to neutral or alkaline with ammonia water, and then adding an oxidant to obtain a pretreated carrier;
[0014] 3) The pretreated support is placed in an aqueous solution of nickel salt and cobalt salt for hydrothermal loading, and then placed in an ammonia solution and air atmosphere for low-temperature heat treatment to achieve modification.
[0015] As a preference,
[0016] Step 1) The DMF aqueous solution is prepared by mixing DMF and water in a volume ratio of 1: (3.8-4.2) to dissolve each other.
[0017] As a preference,
[0018] The copper ion concentration in the Cu-DMF aqueous solution is 0.2-0.5 mol / L.
[0019] As a preference,
[0020] Step 2) the constant temperature immersion treatment is carried out at 15-20°C;
[0021] Step 2) The pH value is adjusted to 7.0-9.0 with aqueous ammonia.
[0022] As a preference,
[0023] The oxidant is added at a ratio of 0.2 to 0.3 mol per liter of the treatment solution.
[0024] As a preference,
[0025] Step 3) The molar ratio of nickel to cobalt in the aqueous solution of nickel salt and cobalt salt is 1:(0.45-0.55), and the total molar amount of nickel and cobalt is 0.12-0.18 mol / L;
[0026] The hydrothermal loading is carried out at 90-105° C. for 6-12 h.
[0027] As a preference,
[0028] The ammonia water is saturated ammonia water, and the low-temperature heat treatment is carried out in ammonia water to control the reaction temperature to be 90-105° C. and the reaction time to be 16-24 h.
[0029] As a preference,
[0030] The low-temperature heat treatment in the air atmosphere is performed at a controlled temperature of 60-80° C. and the heat treatment is performed for at least 6 hours.
[0031] The core solution of this invention lies in constructing a particle load on the surface of the PANI separation membrane. In earlier research, technicians discovered that Ni-Co-O nanowire structures can be effectively interspersed within the paper-based PANI material. These nanowire structures, through their super-oxophobicity, can accelerate the movement of oxygen molecules through the PANI separation membrane, creating a strong rate difference and improving the oxygen transmission rate. This new system can also achieve multi-stage separation and purification, producing effects that conventional PANI separation membranes cannot achieve.
[0032] However, when Ni-Co-O was used to modify the existing PANI separation membrane, it was found that it was difficult to achieve effective loading, its loading rate was low, and the actual effect was poor. Therefore, the present invention conducted targeted research and improvements.
[0033] During the research and improvement process, it was discovered that the loading of Ni-Co-O nanowires depends primarily on structural intercalation. While previous studies have shown that paper-based PANI materials offer a favorable structural environment for Ni-Co-O intercalation, conventional PANI separation membranes lack this. Therefore, the present invention further utilizes a deposition method to prepare the Ni-Co-O composite shell.
[0034] Specifically, the present invention first introduces copper ions using a specific solvent, while simultaneously allowing the PANI surface to exhibit recrystallization equilibrium. During this process, subsequent ammonia and oxidants are added, allowing the copper ions to be wrapped around the PANI molecular fibers and fixed on the surface of the original PANI separation membrane. The action of amino groups and copper ions first creates a stable load and connection between the copper ions and the PANI molecular fibers. Subsequently, in an alkaline environment, under the action of an oxidant, the partially dissolved ANI is added to the PANI molecular chains and copper ion particles, forming a more stable wrapping polymerization. The formation of this copper compound actually produces a doping-strengthening effect, making the PANI self-supporting structure more stable and, to a certain extent, enhancing mechanical properties.
[0035] After the copper ions are fixed and the copper compound is precipitated, step 3 is performed. Through the advantages of its own metal deposition, Ni-Co-O is deposited and coated on the surface of the copper compound to form a stable load. The Ni and Co elements are hydrothermally loaded into a composite oxide, and then undergo hydrothermal reduction with ammonia water and secondary oxidation with air to form a composite form of metal@metal oxide, which is loaded on the surface of the copper compound to form Cu-Ni-Co-O, which is used to further improve the nitrogen and oxygen separation effect. This is mainly because the Ni-Co-O coating layer formed has extremely strong oxygen-repellent properties. Due to the existence of the pressure difference, oxygen and nitrogen can only pass through the separation membrane in one direction. At this time, due to the presence of the Ni-Co-O coating layer with super oxygen repellency, oxygen actually obtains an "accelerated" process, which actually increases its kinetic entropy, thereby making the nitrogen and oxygen separation effect better. Under the same pressure difference conditions, the rate at which oxygen passes through the separation membrane will also be higher than the original separation membrane and the commercially available PANI separation membrane. Based on this feature, another technical effect is actually further produced. In conventional nitrogen-oxygen separation processes, the use of multiple membranes does not effectively raise the oxygen concentration threshold; it merely stabilizes the oxygen content in the resulting oxygen-enriched air. This is because, without external forces, once the actual relative nitrogen and oxygen concentrations reach a certain range, they pass through at nearly equal rates, preventing further oxygen enrichment of the oxygen-enriched air. However, the separation membrane of the present invention, after being doped and strengthened with a Ni-Co-O coating, can significantly increase the oxygen concentration in the oxygen-enriched air after multiple membrane separations. In experiments, the highest oxygen concentration even reached over 50% vol, resulting in a highly effective result. Furthermore, conventional PANI separation membranes also have certain drawbacks when performing multiple membrane separations. Specifically, the gas pressure after the first pass through the membrane is relatively low, making it difficult to generate a sufficient pressure differential for the second pass, typically requiring pressurization equipment. However, the separation membrane of the present invention has been mechanically strengthened to a certain extent, further increasing the initial air pressure and enabling it to pass through the multiple membranes without pressurization, saving the cost of pressurization equipment and improving actual production efficiency. Beneficial effects
[0036] Based on the above, the present invention actually produces the following beneficial effects:
[0037] The present invention introduces copper compounds through the recrystallization process of PANI, and uses the PANI self-supporting structure as a carrier and the copper compounds as crystallization nucleation points to achieve effective loading of Ni-Co-O components. The PANI separation membrane is modified with the Ni-Co-O component, thereby significantly improving its nitrogen and oxygen separation ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] FIG1 is a SEM characterization image of the modified MeO-PANI separation membrane in Example 1 of the present invention. Modes for Carrying Out the Invention
[0039] The present invention is further described in detail below with reference to specific embodiments and the accompanying drawings. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0040] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0041] Unless otherwise specified, the PANI separation membranes used in the present invention are all commercially available high-density PANI air separation membranes with an average membrane thickness of 60 μm, and are also used as comparative example 1 for performance comparison.
[0042] Example 1: A method for modifying an air separation membrane, characterized in that:
[0043] The method comprises:
[0044] 1) DMF and deionized water were mixed in a volume ratio of 1:4 to prepare a DMF aqueous solution, to which copper chloride was added at a concentration of 0.3 mol / L to prepare a Cu-DMF aqueous solution as a treatment solution;
[0045] 2) The PANI separation membrane was immersed in the treatment solution for 10 min at a constant temperature of 20°C. The pH value was adjusted to 9.0 with saturated ammonia water. Ammonium persulfate was added at a ratio of 0.25 mol per liter of the treatment solution for 2 h to obtain a pretreated support.
[0046] 3) The pretreated support was placed in an aqueous solution of 0.1 mol / L nickel nitrate and 0.05 mol / L cobalt nitrate for hydrothermal treatment at 95 °C for 9 h, then placed in saturated ammonia water for hydrothermal treatment at 95 °C for 20 h, and finally treated in an air atmosphere at 70 °C for 6 h to complete the modification of the PANI separation membrane.
[0047] Characterization of the separation membrane sample obtained in step 3) revealed a thickness of approximately 56-57 μm, which is slightly lower than that of the original PANI separation membrane. This is likely due to the introduction of the doped particles causing some shrinkage of the PANI molecular chains, which in turn improves the mechanical properties. Furthermore, the SEM characterization results of the membrane sample obtained in step 3) are shown in Figure 1. As can be clearly seen from Figure 1, the modified MeO-PANI separation membrane of the present invention utilizes the self-supporting PANI molecular structure as a carrier, immobilizing the Cu-Ni-Co-O particles through molecular chain intertwining and coating.
[0048] The prepared membrane material was subjected to air separation test. The test was conducted using the pressure permeation method. A simple clamping mechanism was used to clamp the membrane sample between the two chambers. The measurement area of each chamber was 0.1 m 2 One of the two chambers is used as a plenum chamber to introduce air. A pressure relief port is provided on the edge of the membrane sample inside the plenum chamber to release gas from the surface of the plenum chamber to ensure stable pressure in the plenum chamber. A conventional constant-pressure relief valve is installed in the pressure relief port, and the pressure relief parameter is set to 0.105-0.405 MPa (corresponding to a pressure slightly higher than the input end of the plenum chamber). The other chamber is used as an extraction chamber to extract the treated gas passing through the membrane sample and characterize the treated gas. Before air is introduced into the plenum chamber, the extraction chamber is evacuated to a pressure of ≤100 Pa. Air is then introduced into the plenum chamber and the air pressure at the input end is controlled. At this time, the pressure difference is approximately ≥0.1 MPa. The treated gas is promptly extracted to maintain the pressure of the extraction chamber ≤1000 Pa. At the same time, the flow rate of the extracted treated gas is characterized. When a stable flow rate is achieved, the characterization measurement is continued. After measuring more than 20 measurement points, the average value is recorded.
[0049] The above characterization test results clearly demonstrate that step 2) of the present invention can significantly enhance the mechanical properties of the separation membrane, enabling it to withstand pressure differentials up to 0.3 MPa without damage. Further loading with Ni—Co—O weakened the membrane's ability to withstand these differential pressures, but the oxygen concentration of the treated oxygen-enriched air (process gas) increased significantly, reaching over 40% vol. This demonstrates a significant improvement in the membrane's performance. The modification process of the present invention significantly enhances the nitrogen-oxygen separation efficiency of existing PANI membranes.
[0050] Example 2: A method for modifying an air separation membrane, characterized in that:
[0051] The method comprises:
[0052] 1) DMF and deionized water were mixed in a volume ratio of 1:4 to prepare a DMF aqueous solution, to which copper chloride was added at a concentration of 0.2 mol / L to prepare a Cu-DMF aqueous solution as a treatment solution;
[0053] 2) The PANI separation membrane was immersed in the treatment solution for 10 min at a constant temperature of 15°C. The pH value was adjusted to 8.5 with saturated ammonia water. Ammonium persulfate was added at a ratio of 0.2 mol per liter of the treatment solution for 2 h to obtain a pretreated support.
[0054] 3) The pretreated support was placed in an aqueous solution of 0.1 mol / L nickel nitrate and 0.05 mol / L cobalt nitrate and hydrothermaled at 90 °C for 12 h, then placed in saturated ammonia water and hydrothermaled at 90 °C for 24 h, and finally treated in an air atmosphere at 60 °C for 6 h to complete the modification of the PANI separation membrane.
[0055] The prepared membrane material was subjected to air separation test. The test was conducted using the pressure permeation method. A simple clamping mechanism was used to clamp the membrane sample between the two chambers. The measurement area of each chamber was 0.1 m 2 One of the two chambers is used as a plenum chamber to introduce air. A pressure relief port is provided on the edge of the membrane sample inside the plenum chamber to release gas from the surface of the plenum chamber to ensure stable pressure in the plenum chamber. A conventional constant-pressure relief valve is installed in the pressure relief port, and the pressure relief parameter is set to 0.105-0.405 MPa (corresponding to a pressure slightly higher than the input end of the plenum chamber). The other chamber is used as an extraction chamber to extract the treated gas passing through the membrane sample and characterize the treated gas. Before air is introduced into the plenum chamber, the extraction chamber is evacuated to a pressure of ≤100 Pa. Air is then introduced into the plenum chamber and the air pressure at the input end is controlled. At this time, the pressure difference is approximately ≥0.1 MPa. The treated gas is promptly extracted to maintain the pressure of the extraction chamber ≤1000 Pa. At the same time, the flow rate of the extracted treated gas is characterized. When a stable flow rate is achieved, the characterization measurement is continued. After measuring more than 20 measurement points, the average value is recorded.
[0056] The characterization results above demonstrate that the modified PANI membrane significantly enhances its nitrogen and oxygen separation capacity. Furthermore, it can withstand greater pressure differentials. This increased pressure differential increases air flow rates, effectively increasing nitrogen and oxygen separation efficiency and making the membrane less susceptible to damage during use.
[0057] Example 3: A method for modifying an air separation membrane, characterized in that:
[0058] The method comprises:
[0059] 1) DMF and deionized water were mixed in a volume ratio of 1:4 to prepare a DMF aqueous solution, to which copper chloride was added at a concentration of 0.5 mol / L to prepare a Cu-DMF aqueous solution as a treatment solution;
[0060] 2) The PANI separation membrane was immersed in the treatment solution for 10 min at a constant temperature of 20°C. The pH value was adjusted to 9.0 with saturated ammonia water. Ammonium persulfate was added at a ratio of 0.3 mol per liter of the treatment solution for 2 h to obtain a pretreated support.
[0061] 3) The pretreated support was placed in an aqueous solution of 0.1 mol / L nickel nitrate and 0.05 mol / L cobalt nitrate and hydrothermaled at 105 °C for 6 h, then placed in saturated ammonia water and hydrothermaled at 105 °C for 16 h, and finally treated at 80 °C in an air atmosphere for 6 h to complete the modification of the PANI separation membrane.
[0062] The prepared membrane material was subjected to air separation test. The test was conducted using the pressure permeation method. A simple clamping mechanism was used to clamp the membrane sample between the two chambers. The measurement area of each chamber was 0.1 m 2 One of the two chambers is used as a plenum chamber to introduce air. A pressure relief port is provided on the edge of the membrane sample inside the plenum chamber to release gas from the surface of the plenum chamber to ensure stable pressure in the plenum chamber. A conventional constant-pressure relief valve is installed in the pressure relief port, and the pressure relief parameter is set to 0.105-0.405 MPa (corresponding to a pressure slightly higher than the input end of the plenum chamber). The other chamber is used as an extraction chamber to extract the treated gas passing through the membrane sample and characterize the treated gas. Before air is introduced into the plenum chamber, the extraction chamber is evacuated to a pressure of ≤100 Pa. Air is then introduced into the plenum chamber and the air pressure at the input end is controlled. At this time, the pressure difference is approximately ≥0.1 MPa. The treated gas is promptly extracted to maintain the pressure of the extraction chamber ≤1000 Pa. At the same time, the flow rate of the extracted treated gas is characterized. When a stable flow rate is achieved, the characterization measurement is continued. After measuring more than 20 measurement points, the average value is recorded.
[0063] The characterization results above demonstrate that the modified PANI membrane significantly enhances its nitrogen and oxygen separation capacity. Furthermore, it can withstand greater pressure differentials. This increased pressure differential increases air flow rates, effectively increasing nitrogen and oxygen separation efficiency and making the membrane less susceptible to damage during use.
[0064] Comparative Example 1: Commercially available high-density PANI air separation membrane with an average membrane thickness of 60 μm.
[0065] The prepared membrane material was subjected to air separation test. The test was conducted using the pressure permeation method. A simple clamping mechanism was used to clamp the membrane sample between the two chambers. The measurement area of each chamber was 0.1 m 2 One of the two chambers is used as a plenum chamber to introduce air. A pressure relief port is provided on the edge of the membrane sample inside the plenum chamber to release gas from the surface of the plenum chamber to ensure stable pressure in the plenum chamber. A conventional constant pressure relief valve is installed in the pressure relief port, and the pressure relief parameter is set to 0.105-0.405 MPa (corresponding to the pressure at the input end of the plenum chamber). The other chamber is used as an extraction chamber to extract the treated gas passing through the membrane sample and characterize the treated gas. Before air is introduced into the plenum chamber, the extraction chamber is evacuated to a pressure of ≤100 Pa. Air is then introduced into the plenum chamber and the air pressure at the input end is controlled. At this time, the pressure difference is approximately ≥0.1 MPa. The treated gas is extracted in a timely manner to maintain the pressure of the extraction chamber ≤1000 Pa. At the same time, the flow rate of the extracted treated gas is characterized. When a stable flow rate is achieved, the characterization measurement is continued. After measuring more than 20 measurement points, the average value is recorded.
[0066] The above test results clearly show that commercially available high-density PANI air separation membranes, even those with higher density and stronger mechanical properties, can only withstand pressure differentials less than 0.2 MPa under relatively low pressure conditions. At a pressure differential of 0.2 MPa, the membrane material breaks, rendering further testing impossible. A comparison with Examples 1-4 of the present invention clearly shows that the separation membranes produced by the present invention exhibit significantly superior mechanical properties and achieve superior air separation performance.
[0067] Furthermore, a three-layer membrane separation test was conducted using the membrane sample produced after the modification treatment in step 3) of Example 1 and the membrane sample of Comparative Example 1. Four compartments were set up during the experiment, with adjacent compartments separated by membrane samples. The remaining procedures were identical to those described above. The test results are shown in the table below.
[0068] When the input pressure was 0.1 MPa, an internal pressurizing device was used to compress the space after each membrane separation to increase the pressure for the next membrane separation. When the input pressure was 0.2 MPa, the pressure was increased to 0.1 MPa only before the third membrane separation. The above test results also demonstrate that the separation membrane of the present invention, after secondary enhancement with Ni-Co-O nanowires, actually further produces the effect of multiple membrane separation and enrichment enhancement.
[0069] Comparative Example 2: A method for modifying an air separation membrane, characterized in that:
[0070] The method comprises:
[0071] The PANI separation membrane was placed in an aqueous solution of 0.1 mol / L nickel nitrate and 0.05 mol / L cobalt nitrate for hydrothermal treatment at 95 °C for 9 h, then placed in saturated ammonia water for hydrothermal treatment at 95 °C for 20 h, and finally treated in an air atmosphere at 70 °C for 6 h to complete the modification treatment of the PANI separation membrane.
[0072] Characterization of the prepared membrane revealed a thickness of approximately 60-61 μm, comparable to that of the original PANI membrane. SEM characterization of the membrane is shown in Figure 2. It is clear from this that the membrane does not effectively immobilize the Ni-Co-O particles.
[0073] The prepared membrane material was subjected to air separation test. The test was conducted using the pressure permeation method. A simple clamping mechanism was used to clamp the membrane sample between the two chambers. The measurement area of each chamber was 0.1 m 2 One of the two chambers is used as a plenum chamber to introduce air. A pressure relief port is provided on the edge of the membrane sample inside the plenum chamber to release gas from the surface of the plenum chamber to ensure stable pressure in the plenum chamber. A conventional constant-pressure relief valve is installed in the pressure relief port, and the pressure relief parameter is set to 0.105-0.405 MPa (corresponding to a pressure slightly higher than the input end of the plenum chamber). The other chamber is used as an extraction chamber to extract the treated gas passing through the membrane sample and characterize the treated gas. Before air is introduced into the plenum chamber, the extraction chamber is evacuated to a pressure of ≤100 Pa. Air is then introduced into the plenum chamber and the air pressure at the input end is controlled. At this time, the pressure difference is approximately ≥0.1 MPa. The treated gas is promptly extracted to maintain the pressure of the extraction chamber ≤1000 Pa. At the same time, the flow rate of the extracted treated gas is characterized. When a stable flow rate is achieved, the characterization measurement is continued. After measuring more than 20 measurement points, the average value is recorded.
[0074] From the characterization results, it can also be seen that its performance has not produced an optimization effect. It can be seen that it is difficult to directly carry out load modification with Ni-Co-O, and it has no effect on improving the performance.
Claims
1. A method for modifying an air separation membrane, It is characterized in that The method comprises: 1) Dissolving a soluble copper salt in a DMF aqueous solution to prepare a Cu-DMF aqueous solution as a treatment solution; 2) The PANI separation membrane is immersed in a treatment solution for constant temperature immersion treatment, the pH value is adjusted to neutral or alkaline with ammonia water, and then an oxidant is added to obtain a pretreated carrier; 3) The pretreated carrier is placed in an aqueous solution of nickel salt and cobalt salt for hydrothermal loading, and after the hydrothermal loading, it is placed in an ammonia solution and an air atmosphere for low-temperature heat treatment in turn to achieve modification.
2. The method for modifying an air separation membrane according to claim 1, It is characterized in that Step 1) The DMF aqueous solution is prepared by mixing DMF and water in a volume ratio of 1: (3.8-4.2) to dissolve each other.
3. A method for modifying an air separation membrane according to claim 1 or 2, It is characterized in that The copper ion concentration in the Cu-DMF aqueous solution is 0.2-0.5 mol / L.
4. The method for modifying an air separation membrane according to claim 1, It is characterized in that Step 2) the constant temperature immersion treatment is carried out at 15-20°C; Step 2) The pH value is adjusted to 7.0-9.0 with aqueous ammonia.
5. A method for modifying an air separation membrane according to claim 1 or 4, It is characterized in that The oxidant is added at a ratio of 0.2 to 0.3 mol per liter of the treatment solution.
6. The method for modifying an air separation membrane according to claim 1, It is characterized in that Step 3) The molar ratio of nickel to cobalt in the aqueous solution of the nickel salt and the cobalt salt is 1:(0.45-0.55), and the total molar amount of nickel and cobalt is 0.12-0.18 mol / L; The hydrothermal loading is carried out at 90-105° C. for 6-12 h.
7. The method for modifying an air separation membrane according to claim 1, It is characterized in that The ammonia water is saturated ammonia water, and the low-temperature heat treatment is carried out in ammonia water to control the reaction temperature to be 90-105°C, and the reaction time is 16-24 hours.
8. The method for modifying an air separation membrane according to claim 1, It is characterized in that The low-temperature heat treatment in the air atmosphere is performed at a temperature of 60-80° C. and the heat treatment is performed for at least 6 hours.
Citation Information
Patent Citations
Separation membrane for air separation technology
CN116272429A
Modification method of air separation membrane
CN116550156A
Hollow Fiber Membrane for Separating Oxygen and Method for Manufacturing thereof
KR1020170034018A
Carbon dioxide reaction apparatus
US20210292925A1
Method and apparatus for producing oxygen and nitrogen and membrane therefor
US4542010A