Red phosphorus flame-retardant polyamide composite material, preparation method therefor and use thereof

By adding metazirconic acid or zirconic anhydride to the red phosphorus flame-retardant PA66 material, the corrosion problem of the material under the action of heat, oxygen, and water is solved, achieving both low corrosion and high toughness, and significantly improving the flame retardant performance. and CTI value, extending the service life of the product.

WO2024221895A1PCT designated stage expired Publication Date: 2024-10-31KINGFA SCI & TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/134340
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-23
Filing Date
2023-11-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Red phosphorus flame-retardant PA66 material easily produces phosphine and oxygen-containing acids under the action of heat, oxygen, and water, leading to corrosion of metals in close contact and affecting the conductive performance and service life of the product. Existing modification methods are difficult to Take into account low corrosion and high toughness.

Method used

By adding metazirconic acid or zirconic anhydride, its strong coordination ability is used to reduce the free amount of phosphate, form a complex to inhibit the oxidation of red phosphorus, reduce the release of phosphine and metal corrosion, while maintaining good toughness of the material.

Benefits of technology

It achieves low corrosion, good toughness and high CTI value of red phosphorus flame retardant polyamide composite materials, significantly improves the flame retardant performance and phosphine release, and extends the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023134340-FTAPPB-I100001
    Figure PCTCN2023134340-FTAPPB-I100001
  • Figure PCTCN2023134340-FTAPPB-I100002
    Figure PCTCN2023134340-FTAPPB-I100002
  • Figure PCTCN2023134340-FTAPPB-I100003
    Figure PCTCN2023134340-FTAPPB-I100003
Patent Text Reader

Abstract

Provided in the present invention are a red phosphorus flame-retardant polyamide composite material, a preparation method therefor and the use thereof. The red phosphorus flame-retardant polyamide composite material comprises the following components in parts by weight: 13.9-70.89 parts of PA66, 4-8.45 parts of red phosphorus, 10-35 parts of a reinforcing material, 6-20 parts of a toughening agent and 0.1-1 part of a zirconium compound, the zirconium compound being at least one of metazirconic acid or zirconic anhydride. The red phosphorus flame-retardant polyamide composite material has the characteristics of low corrosivity, good toughness, red phosphorus being less prone to oxidation and high CTI value.
Need to check novelty before this filing date? Find Prior Art

Description

A red phosphorus flame-retardant polyamide composite material and its preparation method and application Technical Field

[0001] The present invention relates to the field of engineering plastics, and more particularly to a red phosphorus flame-retardant polyamide composite material, a preparation method and an application thereof. Background Art

[0002] Polyamide has very excellent mechanical properties, wear resistance, heat resistance, solvent resistance, etc., and is widely used in machinery manufacturing, power tools, electronic appliances, transportation and other fields.

[0003] PA66 is one of the most common polyamides. Since the flame retardancy of PA66 itself is only V-2, its application in the field of electronic appliances is limited, so flame retardant modification is required. Red phosphorus, as a halogen-free flame retardant, has the advantages of little impact on mechanical properties, better electrical properties and smoke density than halogen flame retardant systems, light density, and high cost performance. Therefore, red phosphorus is often used as a flame retardant in PA66. However, because red phosphorus itself is prone to produce phosphine under the action of heat, oxygen, and water, and then transforms into oxygen-containing acids, it corrodes metals in close contact, affecting the conductivity of the product, causing product quality abnormalities and shortening the product's service life. This is also one of the main reasons why some industries ban red phosphorus materials.

[0004] In order to solve the corrosion problem of red phosphorus flame retardant PA66, the following three solutions are commonly proposed: (1) reducing the generation of phosphine and oxygen-containing acids, such as the patented red phosphorus flame retardant reinforced thermoplastic polyamide composition and the patented method for preparing microencapsulated ultrafine red phosphorus, which use microencapsulated red phosphorus for modification. By encapsulating the red phosphorus, the contact between the red phosphorus and water and oxygen is reduced. However, in the actual production process, it undergoes twin-screw shearing, heating and single-screw injection molding, etc., which makes it difficult to solve the generation of phosphine and oxygen-containing acids from the source, and thus corrosion is inevitable; (2) by weakening the screw shearing or introducing nitrogen during the production process for protection, such as the patented acid-free, high electrical insulation red phosphorus flame retardant reinforced nylon and its preparation method, which avoids contact with oxygen by introducing nitrogen, thereby reducing corrosion to metals, but the production process is too complicated and expensive; (3) using adsorbents, fillers, and metal oxides for absorption and inhibition, such as the patented Reduction of phosphine release in plastic articles comprising red phosphorus flame retardant reinforced nylon and its preparation method, which avoids contact with oxygen by introducing nitrogen, thereby reducing corrosion to metals, but the production process is too complicated and expensive; (3) using adsorbents, fillers, and metal oxides for absorption and inhibition, such as the patented Reduction of phosphine release in plastic articles comprising red phosphorus flame retardant reinforced nylon and its preparation method, which avoids contact with oxygen by introducing nitrogen, thereby reducing corrosion to metals, but the production process is too complicated and expensive; Phosphorus uses activated carbon and zeolite to adsorb phosphine, reducing the generation of oxygen-containing acids and lowering corrosion, but these adsorbents significantly damage the toughness of the material; a patented low-odor red phosphorus flame-retardant reinforced polyamide material adsorbs phosphine by adding diatomaceous earth; a patented use of iron oxides in eliminating the pungent odor in red phosphorus flame-retardant nylon reduces the generation of phosphine by adding iron oxides; a patented low-corrosion, low-odor glass fiber reinforced red phosphorus flame-retardant nylon 66 composite material and preparation method thereof reduces the generation of phosphine by adding hydroxides, talc, magnesium oxide, calcium oxide, etc., but these fillers, adsorbents, metal oxides, and hydroxides have a significant negative impact on the mechanical properties of the material, especially the toughness, affecting its application in high-toughness products.

[0005] Therefore, it is necessary to solve the problem that the current red phosphorus flame retardant PA66 is difficult to achieve both low corrosion and high toughness.

[0006] Summary of the Invention

[0007] The primary purpose of the present invention is to overcome the aforementioned problem of the difficulty in achieving both low corrosion and high toughness in current red phosphorus flame-retardant PA66, and to provide a red phosphorus flame-retardant polyamide composite material. The red phosphorus flame-retardant polyamide composite material has the characteristics of low corrosion, good toughness, resistance to red phosphorus oxidation, and a high CTI value.

[0008] A further object of the present invention is to provide a method for preparing the above-mentioned red phosphorus flame retardant polyamide composite material.

[0009] A further object of the present invention is to provide an application of the red phosphorus flame-retardant polyamide composite material in the preparation of electronic and electrical components.

[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0011] A red phosphorus flame-retardant polyamide composite material comprises the following components in parts by weight:

[0012] The zirconium compound is at least one of metazirconic acid and zirconic anhydride.

[0013] The mass percentage of PA66 in the red phosphorus flame-retardant polyamide composite material of the present invention is generally above 15%.

[0014] Through multiple studies, the inventors of the present invention discovered that metazirconic acid has a strong coordination ability for phosphate. When metazirconic acid is added to a red phosphorus flame-retardant polyamide composite, when red phosphorus reacts with heat, oxygen, and water to form phosphine and further converts to phosphate, the metazirconic acid coordinates the phosphate, reducing the free phosphate content, thereby reducing the material's metal corrosion and the amount of phosphine released. Metazirconic acid also has no significant negative impact on the toughness of the red phosphorus flame-retardant polyamide composite, allowing the composite to maintain good toughness and meet the requirements of application scenarios. Furthermore, metazirconic acid forms a complex after coordination with phosphate. On the one hand, this complex can inhibit the oxidation of red phosphorus, thereby maintaining the good flame retardant properties of the red phosphorus flame-retardant polyamide composite. Specifically, the color change of the red phosphorus flame-retardant polyamide composite under the double 85 test is significantly improved, indicating that the oxidation of red phosphorus is effectively suppressed. On the other hand, the complex formed after coordination can maintain a high CTI value for the red phosphorus flame-retardant polyamide composite. Zirconic anhydride forms metazirconic acid after hydrolysis. Adding zirconic anhydride to red phosphorus flame-retardant polyamide composite materials can achieve similar effects as metazirconic acid.

[0015] That is, the red phosphorus flame-retardant polyamide composite material of the present invention has the characteristics of low corrosivity, good toughness, red phosphorus not being easily oxidized, and high CTI value.

[0016] Preferably, the red phosphorus flame retardant polyamide composite material comprises the following components in parts by weight:

[0017] Preferably, the zirconium compound is metazirconic acid.

[0018] Optionally, the relative viscosity of the PA66 is 2.36-2.7, and the terminal amino group concentration is 36.6-82 mmol / Kg.

[0019] Preferably, the relative viscosity of the PA66 is 2.65-2.7, and the terminal amino group concentration is 39.5-82 mmol / Kg.

[0020] By selecting PA66 within this relative viscosity and amino end concentration range, the resulting red phosphorus flame-retardant polyamide composite material releases less phosphine and has lower corrosion to metals.

[0021] The amino group concentration of the PA66 of the present invention can be measured by potentiometric titration.

[0022] Red phosphorus can be added in the form of red phosphorus masterbatch or red phosphorus powder. When added in the form of red phosphorus masterbatch, the weight percentage of red phosphorus in the red phosphorus flame-retardant polyamide composite material is obtained by multiplying the weight percentage of the red phosphorus masterbatch by the percentage of red phosphorus in the red phosphorus masterbatch.

[0023] Preferably, the red phosphorus is added in the form of red phosphorus masterbatch.

[0024] More preferably, the red phosphorus content of the red phosphorus masterbatch is 40-65 wt%.

[0025] Optionally, the reinforcing material is at least one of glass fiber, carbon fiber, aramid fiber or ceramic fiber.

[0026] More preferably, the reinforcing material is glass fiber.

[0027] Further preferably, the cross section of the glass fiber is elliptical, and the ratio of the maximum diameter to the minimum diameter of the ellipse is (2.5-4):1.

[0028] When the cross section of the glass fiber is elliptical, the obtained red phosphorus flame retardant polyamide composite material releases less phosphine and has higher notched impact strength.

[0029] Optionally, the toughening agent is at least one of a copolymer of ethylene and acrylic acid or a polyolefin elastomer grafted with maleic anhydride.

[0030] Preferably, the toughening agent is a copolymer of ethylene and acrylic acid.

[0031] In order to obtain more excellent or new properties, the red phosphorus flame retardant polyamide composite material of the present invention may further include other conventional processing aids in the art. The type and amount of each processing aid may be selected and adjusted according to actual needs.

[0032] Preferably, the red phosphorus flame retardant polyamide composite material further comprises 0.2 to 2 parts of a processing aid.

[0033] More preferably, the processing aid is at least one of an antioxidant or a lubricant.

[0034] Optionally, the antioxidant is at least one of antioxidant 1098, antioxidant 245, antioxidant 1790 or antioxidant 445.

[0035] Optionally, the lubricant is at least one of a fatty acid ester lubricant, a metal soap lubricant, a fatty alcohol lubricant or a fatty acid lubricant.

[0036] The preparation method of the red phosphorus flame retardant polyamide composite material comprises the following steps:

[0037] The components except red phosphorus and the reinforcing material are mixed and melted, and then the red phosphorus and the reinforcing material are added from a side feed port, and the mixture is extruded and granulated to obtain the red phosphorus flame retardant polyamide composite material.

[0038] Red phosphorus can be added in the form of either masterbatch or powder. The main difference between the two is that when adding masterbatch, a nitrogen atmosphere is not required at the side feed port. However, when adding powder, a nitrogen atmosphere is required to prevent direct contact between the powder and air, which could cause fire or explosion hazards. Adjusting the process (whether to create a nitrogen atmosphere) based on the different forms of red phosphorus addition is standard practice in the field.

[0039] The application of the above-mentioned red phosphorus flame-retardant polyamide composite material in the preparation of electronic and electrical components also falls within the protection scope of the present invention.

[0040] Preferably, the electronic and electrical components are connectors, circuit breakers or contactors.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The red phosphorus flame-retardant polyamide composite material has the characteristics of low corrosion, good toughness, red phosphorus not being easily oxidized and high CTI value. DETAILED DESCRIPTION

[0043] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0044] Some of the reagents selected in the embodiments and comparative examples of the present invention are described as follows:

[0045] PA66-1#: viscosity 2.7, amino group content 47mmol / kG, PA66 EP-158, Zhejiang Huafeng Group; viscosity is calibrated according to GB / T 12006.1-2009 Plastics Polyamides Part 1, and the following PA66 is calibrated in the same way.

[0046] PA66-2#: viscosity 2.65, amino group content 82 mmol / kG, PA66 EP158NH, Zhejiang Huafeng Group;

[0047] PA66-3#: viscosity 2.7, amino group content 39.5 mmol / kG, PA66 50BWFS, ASCEND Group;

[0048] PA66-4#: viscosity 2.38, amino group content 49.2 mmol / kG, PA66 21ZLV, ASCEND Group;

[0049] PA66-5#: viscosity 2.57, amino group content 36.6 mmol / kG, PA66 88X, ASCEND Group;

[0050] PA66-6#: viscosity 2.62, amino group content 40.3 mmol / kG, PA66 EPR27, Shenma Group;

[0051] PA66-7#: viscosity 2.36, amino group content 40.2 mmol / kG, PA66 EPR24, Shenma Group;

[0052] Red phosphorus masterbatch 1#: HDFRMB40, red phosphorus content 40%, Yunnan Haoding New Materials Co., Ltd.

[0053] Red phosphorus masterbatch 2#: HDFRMB65BK, red phosphorus content 65%, Yunnan Haoding New Materials Co., Ltd.

[0054] Red phosphorus powder 3#: encapsulated, red phosphorus content over 85%, FSE-M1001, Shaoyang Fusen Flame Retardant Material Co., Ltd.

[0055] Reinforcement material 1#: Glass fiber: Glass fiber ECS301CL-3, the cross section of the glass fiber is circular, Chongqing International Composite Materials Co., Ltd.

[0056] Reinforcement material 2#: Glass fiber: Glass fiber ECS301HP-3-M2.5, the cross section of the glass fiber is elliptical, and the ratio of the maximum diameter to the minimum diameter of the cross section is 2.5:1, Chongqing International Composite Materials Co., Ltd.

[0057] Reinforcement material 3#: Glass fiber: Glass fiber ECS301HP-3-M4, the glass fiber has an elliptical cross-section, and the ratio of the maximum diameter to the minimum diameter of the cross-section is 4:1; Chongqing International Composite Materials Co., Ltd.

[0058] Toughening agent 1#: PC-28, maleic anhydride grafted POE, Foshan Nanhai Bochen Polymer New Materials Co., Ltd.

[0059] Toughener 2#: Nucrel 3990, ethylene and acrylic acid copolymer, Dow Chemical;

[0060] Zirconium compound 1#: metazirconic acid, Aladdin Reagent Co., Ltd.

[0061] Zirconium compound 2#: zirconic anhydride, Yixing Xinxing Zirconium Industry Co., Ltd.;

[0062] Processing aid 1#: antioxidant 1098, commercially available;

[0063] Processing aid 2#: lubricant, cetyl palmitate, commercially available;

[0064] Carbon black: BLACK PEARLS M717, Cabot, USA.

[0065] Unless otherwise specified, the components (such as processing aids) used in the parallel examples and comparative examples are all the same commercially available products.

[0066] The properties of the red phosphorus flame retardant polyamide composite materials provided in the embodiments and comparative examples of the present invention were measured according to the following test methods:

[0067] (1) Izod notched impact strength: tested in accordance with ISO 180:2019;

[0068] (2) Flame retardant performance: tested according to UL 94, specimen size 125×13×1.6mm;

[0069] (3) Phosphine release: ① Equipment: drying dish (caliber 300 mm), Dräger phosphine tester, stopwatch; ② Continuously inject at 285°C, 280°C, 275°C, and 270°C, sampling at 40-second intervals, continuously inject 20 molds, take the sample from the 21st mold, place it in a drying dish, seal it, press the stopwatch, and take the reading at 5 minutes; ③ Phosphine release = reading of the detector / mass of the sample (ppm / kg).

[0070] (4) Characterization of phosphorus corrosion: ① Equipment: thermal aging oven, wide-mouth bottle, test tube with a diameter of 12 mm and a length of 100 mm, analytical balance, inductively coupled atomic emission spectrometer (ICP), tweezers; ② Place 50 g of particles in a 500 ml wide-mouth bottle, then take a copper sheet with a specification of 80 mm*10 mm*1.0 mm and insert it into the particles, with the exposed part being 40 mm long. Fill the test tube with 8 ml of deionized water, place the test tube in the wide-mouth bottle, seal it, and then place the wide-mouth bottle at 85°C for 3 days. Remove the copper sheet, visually inspect the corrosion effect, and record the corrosion level.

[0071] Copper sheet corrosion level 1: There is basically no corrosion or rust on the copper sheet;

[0072] Copper corrosion level 2: 1 / 3 of the copper sheet is corroded and rusted;

[0073] Copper corrosion level 3: 2 / 3 of the copper sheet is corroded and rusted;

[0074] Copper corrosion level 4: More than 2 / 3 of the copper sheet is corroded and rusted.

[0075] (5) Double 85 color change test: The red phosphorus flame retardant polyamide composite material is made into a color plate, and its initial LAB value is tested using a colorimeter. The color plate is then placed under 85°C and 85% humidity conditions for 1000 hours, and its LAB value is measured again to calculate △E.

[0076] (6) CTI test: According to the IEC-60112 standard: Determination of the tracking index and comparative tracking index of solid insulating materials, the CTI test is performed on the sample.

[0077] The preparation process of the red phosphorus flame retardant polyamide composite material provided in each embodiment of the present invention (except Example 17) and each comparative example is as follows: the dried PA66, toughening agent, zirconium compound, and processing aid (if any) are weighed in proportion by weight, and mixed evenly in a high-speed mixer to obtain a mixture; a twin-screw extruder with double side feeding is selected, and the feeding port includes a main feeding port, a first side feeding port (i.e., a side feeding port away from the die), and a second side feeding port (i.e., a side feeding port close to the die); the mixture is fed from the main feeding port, the red phosphorus masterbatch is fed from the first side feeding port, and the reinforcing material is fed from the second side feeding port (the aspect ratio of the twin-screw extruder is 48:1, the temperature is set at 270-290°C, and the speed is set at 600RPM); after melt blending, the mixture is cooled, air-dried, and granulated to obtain a red phosphorus flame retardant polyamide composite material.

[0078] Example 17 uses red phosphorus powder instead of red phosphorus masterbatch. The preparation process of its red phosphorus flame-retardant polyamide composite material is basically the same as that of Example 1. The difference is that: based on the preparation process of Example 1, nitrogen is introduced into the first side feeding port so that the red phosphorus powder is fed under a nitrogen atmosphere to avoid hidden dangers such as fire and explosion.

[0079] Examples 1 to 22

[0080] Examples 1 to 22 provide a series of red phosphorus flame-retardant polyamide composite materials, the formulations of which are shown in Table 1, Table 2, and Table 3.

[0081] Table 1: Formulas of Examples 1 to 9 (parts by weight)

[0082] Table 2: Formulas of Examples 10 to 17 (parts by weight)

[0083] Table 3 Formula of Examples 18 to 22 (parts by weight)

[0084] Comparative Example 1

[0085] This comparative example provides a red phosphorus flame-retardant polyamide composite material, the formula of which is different from that of Example 1 in that zirconium compound 1# is not added.

[0086] Comparative Example 2

[0087] This comparative example provides a red phosphorus flame-retardant polyamide composite material, the formula of which is different from that of Example 1 in that the amount of zirconium compound 1# added is 0.05 parts by weight.

[0088] Comparative Example 3

[0089] This comparative example provides a red phosphorus flame-retardant polyamide composite material, the formula of which is different from that of Example 1 in that zirconium compound 1# is replaced by carbon black.

[0090] The properties of the red phosphorus flame retardant polyamide composite materials of the embodiments and comparative examples were tested according to the above-mentioned test methods. The test results are shown in Table 4.

[0091] Table 4 Performance test results of red phosphorus flame retardant polyamide composite materials of various embodiments and comparative examples

[0092] From Table 4 we can see that:

[0093] The phosphine release of the red phosphorus flame-retardant polyamide composite materials of Examples 1 to 22 is less than 98ppm / kg, the copper sheet corrosion level is 1 to 3, and the change in the LAB value of the double 85 color change test is less than 0.81, indicating that the red phosphorus flame-retardant polyamide composite material of the present invention has low corrosion and red phosphorus is not easily oxidized; the Izod notched impact strength of the red phosphorus flame-retardant polyamide composite materials of Examples 1 to 22 is greater than 15.2kJ / m2, and the flame retardant level reaches V-1 or above, indicating that the red phosphorus flame-retardant polyamide composite material of the present invention maintains good toughness and flame retardant properties and can meet the use requirements of various scenarios. In addition, the CTI values ​​of the red phosphorus flame-retardant polyamide composite materials of Examples 1 to 22 are all above 550V, indicating that the red phosphorus flame-retardant polyamide composite material of the present invention has a high CTI value.

[0094] Comparative Example 1, in which no zirconium compound was added, resulted in a high phosphine release rate of the resulting red phosphorus flame-retardant polyamide composite material, a copper sheet corrosion rating of 4, and a change in the LAB value of the double 85 color change test of 2.3, indicating that the red phosphorus was easily oxidized and highly corrosive, and its CTI value was also low. Comparative Example 2, in which too little zirconium compound was added, resulted in a high phosphine release rate of the resulting red phosphorus flame-retardant polyamide composite material, a copper sheet corrosion rating of 4, indicating that the red phosphorus was easily oxidized and highly corrosive. Comparative Example 3, in which carbon black was added instead of a zirconium compound, resulted in a high change in the LAB value of the double 85 color change test of 1.73, indicating that the red phosphorus was also easily oxidized. The toughness and CTI values ​​were also inferior to those of Example 1.

[0095] Obviously, the above embodiments of the present invention are merely examples for the purpose of clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the claims of the present invention.

Claims

1. A red phosphorus flame retardant polyamide composite material, characterized in that: The composition comprises the following components in parts by weight: The zirconium compound is at least one of metazirconic acid and zirconic anhydride.

2. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The zirconium compound is metazirconic acid.

3. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The relative viscosity of the PA66 is 2.65-2.7, and the terminal amino group concentration is 39.5-82 mmol / Kg.

4. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The red phosphorus is added in the form of red phosphorus masterbatch.

5. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The reinforcing material is at least one of glass fiber, carbon fiber, aramid fiber or ceramic fiber.

6. The red phosphorus flame retardant polyamide composite material according to claim 5, characterized in that: The cross section of the glass fiber is oval.

7. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The toughening agent is a copolymer of ethylene and acrylic acid.

8. The red phosphorus flame retardant polyamide composite material according to claim 1, characterized in that: The red phosphorus flame retardant polyamide composite material also includes 0.2 to 2 parts of processing aid.

9. The method for preparing the red phosphorus flame retardant polyamide composite material according to any one of claims 1 to 8, characterized in that: The steps include: The components except red phosphorus and the reinforcing material are mixed and melted, and then the red phosphorus and the reinforcing material are added from a side feed port, extruded and granulated to obtain the red phosphorus flame-retardant polyamide composite material.

10. Use of the red phosphorus flame retardant polyamide composite material according to any one of claims 1 to 8 in the preparation of electronic and electrical components.

Citation Information

Patent Citations

  • Low-acid-separation red phosphorus inflaming retarding reinforced polyamide material as well as preparation method and application thereof

    CN102382460A

  • Cuo / zno compounds as stabilisers for flame retardant polyamides

    CN104125979A

  • Insulating and high / low-temperature-resistant polyamide heat-conducting and heat-dissipating material and preparation method and application

    CN105694441A

  • Low-odor red phosphorus flame-retardant reinforced polyamide material

    CN107793749A

  • Red phosphorus flame-retardant polyamide composition as well as preparation method and application thereof

    CN112608595A