Semiconductor device and manufacturing method therefor

By using a combination of multi-layer sacrificial layer structures and different etching processes in MEMS device manufacturing, the problem of interface layer damage is solved, reducing costs and increasing productivity.

WO2024221967A1PCT designated stage expired Publication Date: 2024-10-31RUNXIN SENSING TECHNOLOGY (NANCHANG) CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/138466
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-12-13
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In the manufacturing process of MEMS devices, the interface layer is easily corroded when the sacrificial layer is removed, causing device failure. Existing technologies are difficult to effectively reduce interface layer damage and are costly, affecting production capacity.

Method used

A multi-layer sacrificial layer structure is adopted, and an etching process that is not easy to damage the interface layer is used in the adjacent position. The sacrificial layer is removed in conjunction with conventional etching processes to form a cavity structure, which reduces interface layer damage and maintains cost-effectiveness.

Benefits of technology

It effectively reduces the damage to the interface layer, maintains the structural stability and production efficiency of the device, reduces costs, and improves production capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138466_31102024_PF_FP_ABST
    Figure CN2023138466_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A semiconductor device and a manufacturing method therefor. The method comprises: providing a sensitive material layer; on the sensitive material layer, forming a first sacrificial layer and a first sidewall layer surrounding the first sacrificial layer; on the first sacrificial layer and the first sidewall layer, forming a second sacrificial layer and a second sidewall layer surrounding the second sacrificial layer, wherein the second sidewall layer is connected to the first sidewall layer, and the material of the second sacrificial layer is different from the material of the first sacrificial layer; in the second sidewall layer, forming a release hole connected to the second sacrificial layer; removing the second sacrificial layer by means of the release hole by using a first etching process, so as to expose the first sacrificial layer; and removing the first sacrificial layer by means of the release hole by using a second etching process, so as to form a cavity structure in the first sidewall layer and the second sidewall layer.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and method for manufacturing the same

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to Chinese patent application No. 202310474824.1, filed on April 28, 2023, which is incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for manufacturing the same. Background Art

[0004] A micro-electro-mechanical system (MEMS) is a miniature system that integrates mechanical components, drive elements, optical systems, and electronic control systems. MEMS devices, with their advantages of small size and low power consumption, have found widespread application in smartphones, tablets, game consoles, automobiles, drones, and other fields. Similar to integrated circuits, MEMS devices are also developing towards high performance, miniaturization, low cost, and integration.

[0005] In related technologies, the cavity structure of a MEMS device is formed by removing a sacrificial layer between the MEMS functional layer and the sidewall layer through a release hole using a wet or dry etching process. However, an interface layer typically exists between the MEMS functional layer and the sidewall layer. When removing the sacrificial layer, the etching reaction gas or liquid can corrode the interface layer, causing a reaction and cracking between the MEMS functional layer and the sidewall layer, leading to serious process problems and device failure.

[0006] Summary of the Invention

[0007] The Summary of the Invention introduces a series of simplified concepts that will be further described in the Detailed Description of the Invention. The Summary of the Invention of this disclosure is not intended to limit the key features and essential technical features of the claimed technical solution, nor is it intended to determine the scope of protection of the claimed technical solution.

[0008] One aspect of an embodiment of the present disclosure provides a method for manufacturing a semiconductor device, the method comprising:

[0009] Provide sensitive material layer;

[0010] forming a first sacrificial layer and a first sidewall layer surrounding the first sacrificial layer on the sensitive material layer;

[0011] forming a second sacrificial layer and a second sidewall layer surrounding the second sacrificial layer over the first sacrificial layer and the first sidewall layer, wherein the second sidewall layer is connected to the first sidewall layer, and a material of the second sacrificial layer is different from that of the first sacrificial layer;

[0012] forming a release hole in the second sidewall layer connected to the second sacrificial layer;

[0013] Using a first etching process, removing the second sacrificial layer through the release hole to expose the first sacrificial layer;

[0014] A second etching process is adopted to remove the first sacrificial layer through the release hole to form a cavity structure in the first sidewall layer and the second sidewall layer.

[0015] In some embodiments, an interface layer is formed between the first sidewall layer and the sensitive material layer, and an etching rate of the interface layer by the first etching process is greater than an etching rate of the interface layer by the second etching process.

[0016] In some embodiments, materials of the interface layer and the second sacrificial layer include silicon oxide, and material of the first sacrificial layer includes silicon.

[0017] In some embodiments, a material of the first sidewall layer includes silicon oxide, and a material of the second sidewall layer includes silicon.

[0018] In some embodiments, the first sidewall layer has a first width, the second sidewall layer has a second width, and the second width is greater than the first width.

[0019] In some embodiments, before forming a release hole in the second sidewall layer connected to the second sacrificial layer, the method further includes:

[0020] forming a covering layer on the second sidewall layer, wherein the covering layer is made of a material different from that of the second sidewall layer, and an etching rate of the covering layer by the second etching process is lower than an etching rate of the second sidewall layer by the second etching process;

[0021] The forming of the release hole connected to the second sacrificial layer in the second sidewall layer includes: etching the cover layer and the second sidewall layer in sequence to form the release hole.

[0022] In some embodiments, the first etching process includes a wet etching process, and the second etching process includes a dry etching process.

[0023] In some embodiments, the first sacrificial layer and the first sidewall layer have a first thickness, the second sacrificial layer and the second sidewall layer have a second thickness, and the second thickness is greater than the first thickness.

[0024] In some embodiments, the sensitive material layer includes a piezoelectric layer, a first electrode is formed on a first surface of the sensitive material layer, and a second electrode is formed on a second surface of the sensitive material layer.

[0025] Another aspect of the embodiments of the present disclosure provides a semiconductor device, which is manufactured using the above method.

[0026] According to the manufacturing method of the semiconductor device and the semiconductor device provided by the embodiment of the present disclosure, multiple sacrificial layers are formed in the vertical direction, and sacrificial layers and etching processes that are not easy to damage the interface layer are used at the position adjacent to the interface layer to achieve the effect of reducing damage to the interface layer; while the release of the remaining sacrificial layers still maintains the conventional etching process, which can not only reduce costs and maintain production capacity, but also reduce damage to the interface layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The following drawings of the present disclosure are incorporated herein as part of the present disclosure for understanding the present disclosure. The drawings show embodiments of the present disclosure and their descriptions are used to explain the principles of the present disclosure.

[0028] FIG1 is a schematic cross-sectional view of a semiconductor device at the first stage obtained by sequentially implementing various steps in a method for manufacturing a semiconductor device according to the related art;

[0029] 2 is a schematic cross-sectional view of a semiconductor device at a second stage obtained by sequentially implementing steps in a method for manufacturing a semiconductor device in the related art;

[0030] 3 shows a schematic cross-sectional view of a semiconductor device at a third stage obtained by sequentially implementing steps in a method for manufacturing a semiconductor device in the related art;

[0031] FIG4 is a schematic flow chart showing a method for manufacturing a semiconductor device according to a specific embodiment of the present disclosure;

[0032] 5 is a schematic cross-sectional view of a semiconductor device at the first stage obtained by sequentially implementing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0033] 6 is a schematic cross-sectional view of a semiconductor device at a second stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0034] 7 is a schematic cross-sectional view of a semiconductor device at a third stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0035] 8 is a schematic cross-sectional view of a semiconductor device at a fourth stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0036] 9 is a schematic cross-sectional view of a semiconductor device at a fifth stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0037] 10 is a schematic cross-sectional view of a semiconductor device at a sixth stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0038] 11 is a schematic cross-sectional view of a semiconductor device at a seventh stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0039] 12 is a schematic cross-sectional view of a semiconductor device at an eighth stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0040] 13 is a schematic cross-sectional view of a semiconductor device at a ninth stage obtained by sequentially performing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure;

[0041] 14 is a schematic cross-sectional view of a semiconductor device at a tenth stage obtained during the process of sequentially implementing steps of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0042] In the following description, a number of specific details are provided to provide a more thorough understanding of the present disclosure. However, it will be apparent to those skilled in the art that the present disclosure may be practiced without one or more of these details. In other examples, some technical features well known in the art are not described to avoid confusion with the present disclosure.

[0043] It should be understood that the present disclosure can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided to make the disclosure thorough and complete and to fully convey the scope of the present disclosure to those skilled in the art. In the accompanying drawings, the dimensions and relative sizes of layers and regions may be exaggerated for clarity. Identical reference numerals throughout represent identical elements.

[0044] It should be understood that when an element or layer is referred to as being "on," "adjacent to," "connected to," or "coupled to" another element or layer, it may be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. Conversely, when an element is referred to as being "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" another element or layer, there may be no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or parts, these elements, components, regions, layers, and / or parts should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or part from another element, component, region, layer, or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer, or part discussed below may be represented as a second element, component, region, layer, or part.

[0045] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," etc., may be used herein for convenience of description to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that in addition to the orientations shown in the figures, the spatially relative terms are intended to include different orientations of the device in use and operation. For example, if the device in the drawings is flipped, then the elements or features described as "under the other elements" or "under it" or "under it" will be oriented as "on" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be oriented otherwise (rotated 90 degrees or in other orientations) and the spatial descriptors used herein are interpreted accordingly.

[0046] The purpose of the terms used herein is only to describe specific embodiments and is not intended to limit the present disclosure. When used herein, the singular forms "a", "an", and "the" are intended to include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "comprising" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0047] As shown in Figures 1, 2 and 3, in the manufacturing method of MEMS devices in the related art, in order to obtain a cavity structure, it is first necessary to form a sacrificial layer 103 surrounded by a sidewall layer 102 on the sensitive material layer 302, wherein the sidewall layer 102 and the sacrificial layer 103 have a high etching selectivity ratio; then, a wet or dry process is used to remove the sacrificial layer 103 through the release hole 104 formed in the sidewall layer 102, thereby forming a cavity structure 106 surrounded by the sidewall layer 102.

[0048] However, there is usually an interface layer 307 between the sensitive material layer 302 and the sidewall layer 102. This interface layer is generally formed when the surface of the sensitive material layer 302 is oxidized during the formation of the sidewall layer 102 and is relatively difficult to remove. When removing the sacrificial layer 103, the etching reaction gas or liquid will react with the interface layer 307, causing the interface layer 307 to be etched away, thereby causing the sensitive material layer 302 and the sidewall layer 102 connected by the interface layer 307 to crack, resulting in serious process problems and causing device failure.

[0049] The main reason why interface layer 307 is corroded from the sides during the release of sacrificial layer 103 is that the interface layer 307 and sacrificial layer 103 are made of the same or similar materials, and the etchant used to remove sacrificial layer 103 will also react with interface layer 307. If an etchant that is less likely to damage interface layer 307 is used to remove sacrificial layer 103, the release of sacrificial layer 103 will take longer, resulting in higher costs and limiting mass production capacity.

[0050] To address the above problem, as shown in FIG4 , an embodiment of the present disclosure proposes a method 200 for manufacturing a semiconductor device, comprising the following steps S210 to S260 .

[0051] Step S210: providing a sensitive material layer.

[0052] Step S220 , forming a first sacrificial layer and a first sidewall layer surrounding the first sacrificial layer on the sensitive material layer.

[0053] Step S230 , forming a second sacrificial layer and a second sidewall layer surrounding the second sacrificial layer above the first sacrificial layer and the first sidewall layer, wherein the second sidewall layer is connected to the first sidewall layer, and the material of the second sacrificial layer is different from that of the first sacrificial layer.

[0054] Step S240 , forming a release hole in the second sidewall layer connected to the second sacrificial layer.

[0055] Step S250 : Using a first etching process, remove the second sacrificial layer through the release hole to expose the first sacrificial layer.

[0056] Step S260 , using a second etching process different from the first etching process to remove the first sacrificial layer through the release hole to form a cavity structure in the first sidewall layer and the second sidewall layer.

[0057] The manufacturing method 200 of the semiconductor device of the embodiment of the present disclosure forms multiple sacrificial layers in the vertical direction, and uses sacrificial layers and etching processes that are not easy to damage the interface layer at the position adjacent to the interface layer to achieve the effect of reducing damage to the interface layer; while the release of most of the sacrificial layers still maintains the conventional etching process, which can not only reduce costs and maintain production capacity, but also reduce damage to the interface layer.

[0058] In order to fully understand the present disclosure, detailed structures and steps will be presented in the following description to illustrate the technical solutions proposed by the present disclosure. The preferred embodiments of the present disclosure are described in detail below. However, in addition to these detailed descriptions, the present disclosure may also have other implementation methods.

[0059] The implementation process of the method for manufacturing a semiconductor device according to an embodiment of the present disclosure is exemplarily described below with reference to Figures 5 to 14. Figures 5 to 14 show cross-sectional schematic diagrams of a semiconductor device obtained by sequentially implementing each step of the method for manufacturing a semiconductor device according to an embodiment of the present disclosure.

[0060] First, step S210 is performed to provide a semiconductor substrate 300. The semiconductor substrate 300 can be any suitable semiconductor substrate, such as a bulk silicon substrate. It can also be at least one of the following materials: Si, Ge, SiGe, SiC, SiGeC, InAs, GaAs, InP, or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon-on-insulator (SOI), stacked silicon-on-insulator (SSOI), stacked silicon-germanium-on-insulator (S-SiGeOI), silicon-germanium-on-insulator (SiGeOI), and germanium-on-insulator (GeOI). It can also be double-side polished silicon wafers (DSPs), ceramic substrates such as alumina, quartz, or glass substrates.

[0061] Exemplarily, an isolation layer 301 and a first electrode 303 may also be formed on the semiconductor substrate 300, and the first electrode 303 may be embedded in the isolation layer 301, or the first electrode 303 may also be embedded in the sensitive material layer 302. In one example, after forming the isolation layer, a first electrode material layer covering the isolation layer may be deposited, and then a patterned mask layer may be formed on the first electrode material layer, wherein the mask layer defines a pattern of the first electrode, and then the first electrode material layer is etched using the patterned mask layer as a mask to form the first electrode, and finally, the patterned mask layer is removed. In another example, a lift-off process may also be used to form the first electrode, that is, a patterned mask layer is first formed on the surface of the isolation layer 301, and then a first electrode material layer covering the patterned mask layer is formed, and finally the patterned mask layer is lifted off, and the first electrode material layer above it is removed to obtain the first electrode.

[0062] The first electrode may be made of a conductive material or a semiconductor material. The conductive material may be a metal material having conductive properties. The metal material may be aluminum (Al), copper (Cu), gold (Au), platinum (Pt), or alloys of other metals and copper. The semiconductor material may be Si, Ge, SiGe, SiC, SiGeC, or the like.

[0063] Next, as shown in FIG5 , a sensitive material layer 302 is formed on the semiconductor substrate. The semiconductor device of the disclosed embodiment is a MEMS device, and the sensitive material layer 302 is used to implement the microelectromechanical functions of the MEMS device. A sensitive material refers to a material that can sense small changes in physical, chemical, or biological quantities and exhibit distinct characteristic changes based on the changes. Specifically, these materials include heat-sensitive materials, force-sensitive materials, light-sensitive materials, and voltage-sensitive materials. In some embodiments, the sensitive material layer can be a piezoelectric layer. A piezoelectric layer generates voltage when subjected to external pressure. Conversely, if voltage exists on both sides of the piezoelectric layer, the piezoelectric layer will slightly deform. Based on these characteristics of the piezoelectric layer, conversion between acoustic waves and electrical signals can be achieved.

[0064] For example, a piezoelectric material can be deposited using a deposition method such as chemical vapor deposition, physical vapor deposition, or atomic layer deposition, and a metal element can be doped into the piezoelectric material to form a piezoelectric layer. The doped metal element includes one or more of scandium, zirconium, calcium, titanium, magnesium, and the like. For example, the material of the piezoelectric layer can specifically include aluminum nitride, lead zirconate titanate, zinc oxide, and the like, but this is not limited in the presently disclosed embodiments.

[0065] 5 , after forming the sensitive material layer 302, a second electrode 304 may be formed on the sensitive material layer 302. When the sensitive material layer 302 is a piezoelectric layer, the first electrode, the piezoelectric layer, and the second electrode constitute a composite thin film. The composite thin film may also include other film layers in addition to the aforementioned film layers. These layers may be appropriately configured based on the actual device and are not specifically limited herein.

[0066] In one example, the method for forming the second electrode 304 includes: depositing a second electrode material layer covering the sensitive material layer 302. The second electrode material layer can be a metal material layer or a semiconductor material layer. Then, forming a patterned mask layer on the second electrode material layer, wherein the mask layer defines a pattern of the second electrode. Then, using the patterned mask layer as a mask, etching the second electrode material layer to form the second electrode 304. Finally, removing the patterned mask layer.

[0067] In another example, a lift-off process can also be used to form the second electrode 304, that is, first a patterned mask layer is formed on the surface of the sensitive material layer 302, then a second electrode material layer covering the patterned mask layer is formed, and finally the patterned mask layer is lifted off and the second electrode material layer above it is removed to obtain the second electrode.

[0068] Next, step S220 is performed to form a first sacrificial layer 305 and a first sidewall layer 306 surrounding the first sacrificial layer 305 on the sensitive material layer 302. The first sidewall layer 306 has a first width. The first sidewall layer 306 surrounds the first sacrificial layer 305, that is, the first sidewall layer 306 does not need to cover the first sacrificial layer 305.

[0069] For example, as shown in FIG5 , a first sacrificial layer 305 is formed on the sensitive material layer 302. A first trench is formed in the first sacrificial layer 305, extending through the first sacrificial layer 305. The first trench is used to define the bottom boundary of the cavity structure. The sensitive material layer 302 includes a first surface in contact with the semiconductor substrate and a second surface opposite the first surface. The bottom of the first trench in the first sacrificial layer 305 exposes the first surface of the sensitive material layer 302.

[0070] For example, as shown in FIG5 , a first sacrificial layer 305 is first deposited on the sensitive material layer 302 using a deposition process such as chemical vapor deposition (CVD) or physical vapor deposition (PVD). Next, as shown in FIG6 , the first sacrificial layer 305 is etched to form a groove exposing the first surface of the sensitive material layer 302. Specifically, a patterned photoresist layer is formed on the first sacrificial layer 305, the photoresist layer having a window defining the position of the first groove. Thereafter, the first sacrificial layer 305 is dry-etched using the photoresist layer as a mask to form a groove penetrating the first sacrificial layer 305. The etching of the first sacrificial layer 305 stops at the surface of the sensitive material layer 302. After the etching of the first sacrificial layer 305 is completed, the photoresist layer can be removed using a process such as photoresist ashing.

[0071] Next, with continued reference to FIG. 6 , a first sidewall layer 306 is formed to fill the first trench in the first sacrificial layer 305 and cover the surface of the first sacrificial layer. Specifically, the first sidewall layer 306 includes a portion formed in the first trench and a portion covering the surface of the first sacrificial layer 305. The first sidewall layer 306 can be deposited using a deposition method such as chemical vapor deposition, physical vapor deposition, or atomic layer deposition. A high etching selectivity is achieved between the first sidewall layer 306 and the first sacrificial layer 305, so that the first sidewall layer 306 is not affected during removal of the first sacrificial layer 305.

[0072] During the formation of the first sidewall layer 306 , the first surface of the sensitive material layer 302 exposed at the bottom of the trench in the first sacrificial layer 305 is oxidized, thereby forming an interface layer 307 between the sensitive material layer 302 and the first sidewall layer 306 . That is, the interface layer 307 is usually an oxide layer.

[0073] Next, the first sidewall layer 306 above the first sacrificial layer 305 is removed to obtain the first sidewall layer 306 surrounding the first sacrificial layer 305. Specifically, a chemical mechanical polishing process can be used to polish away the first sidewall layer 306 above the first sacrificial layer 305 so that the tops of the first sacrificial layer 305 and the first sidewall layer 306 are flush.

[0074] In some embodiments, a first sidewall layer covering the sensitive material layer 302 may be formed first, a trench may be etched in the first sidewall layer, and then a first sacrificial layer may be formed to fill the trench. In this example, before forming the first sidewall layer, the area of ​​the sensitive material layer 302 corresponding to the first sidewall layer may be etched to form a recessed portion.

[0075] Next, step S230 is performed to form a second sacrificial layer 308 and a second sidewall layer 309 surrounding the second sacrificial layer 308 over the first sacrificial layer 305 and the first sidewall layer 306. The second sidewall layer 309 is connected to the first sidewall layer 306. The material of the second sacrificial layer 308 is different from that of the first sacrificial layer 305. For example, the material of the first sacrificial layer 305 includes silicon, and the material of the second sacrificial layer 308 includes silicon oxide. To match the first sacrificial layer 305 and the second sacrificial layer 308, the materials of the first sidewall layer 306 and the second sidewall layer 309 are also different. For example, the material of the first sidewall layer 306 includes silicon oxide, and the material of the second sidewall layer 309 includes polysilicon.

[0076] In some embodiments, first, as shown in FIG7 , a second sacrificial layer 308 is formed covering the first sacrificial layer 305 and the first sidewall layer 306 . Then, as shown in FIG8 , a second trench connecting the first sidewall layer 306 is formed in the second sacrificial layer 308 , with the bottom of the second trench exposing the top of the first sidewall layer 306 . Next, as shown in FIG9 , a second sidewall layer 309 is formed filling the second trench and covering the second sacrificial layer 308 . Alternatively, a portion of the second sidewall layer 309 may be formed first, and a trench for forming the second sacrificial layer 308 may be formed in the second sidewall layer 309 ; the second sacrificial layer may be filled in the trench, and the second sacrificial layer outside the trench may be removed by a grinding process; and finally, another portion of the second sidewall layer may be formed covering the second sacrificial layer. The specific method for forming the second sacrificial layer 308 and the second sidewall layer 309 may refer to the first sacrificial layer 305 and the first sidewall layer 306 , and will not be described in detail here.

[0077] For example, after forming the second sidewall layer 309, a cover layer 310 is formed on the second sidewall layer 309. The material of the cover layer 310 is different from that of the second sidewall layer 309. The main function of the cover layer 310 is to maintain the width of the release hole to facilitate subsequent sealing of the release hole. For details, please refer to the following.

[0078] 10 , step S240 is performed to form a release hole in the second sidewall layer 309 that is connected to the second sacrificial layer 308. The release hole is formed above the second sacrificial layer 308, thereby exposing the top of the second sacrificial layer 308. The etchant can remove the second sacrificial layer 308 through the release hole, thereby forming a second cavity structure surrounded by the second sidewall layer 309.

[0079] Specifically, a patterned photoresist layer 311 is first formed on the cover layer 310. The windows of the photoresist layer 311 are used to define the positions of the release holes. Then, the cover layer 310 and the second sidewall layer 309 are sequentially etched using the photoresist layer 311 as a mask to form the release holes.

[0080] Next, as shown in FIG11 , step S250 is performed to perform a first etching process to remove the second sacrificial layer 308 through the release hole to form a second cavity in the second sidewall layer 309. The bottom of the second cavity exposes the first sacrificial layer 305. Exemplarily, the first etching process is a wet etching process using hydrofluoric acid (HF) as the etchant. The first etching process can quickly remove the second sacrificial layer 308, saving etching time. Furthermore, since the first sacrificial layer 305 is formed above the interface layer 307, the first wet etching process cannot damage the interface layer 307, thereby maintaining structural stability.

[0081] As shown in FIG12 , step S260 is performed to continue with a second etching process to remove the first sacrificial layer 305, thereby forming a second cavity in the first sidewall layer 306. The second cavity and the first cavity are connected as a whole, together forming the cavity structure of the MEMS device. The etching rate of the interface layer 307 in the second etching process is lower than the etching rate of the interface layer 307 in the first etching process, thereby reducing damage to the interface layer 307.

[0082] For example, the second etching process can be a dry etching process to reduce the etching rate of the interface layer 307, but is not limited thereto. As long as the etching rate of the interface layer 307 in the second etching process is lower than that in the first etching process, damage to the interface layer can be reduced. In some embodiments, the second etching process can also be a wet etching process that matches the properties of the first sacrificial layer 305. The difference between the first etching process and the second etching process can be due to different process types, i.e., a dry etching process and a wet etching process, respectively; or the difference between the first etching process and the second etching process can also be due to different etchants used.

[0083] In a specific example, the material of the interface layer 307 includes silicon oxide; the material of the first sacrificial layer 305 includes silicon, and the material of the first sidewall layer 306 includes silicon oxide; the material of the second sacrificial layer 308 includes silicon oxide, and the material of the second sidewall layer 309 includes silicon. First, the etchant of the first etching process has a higher etching rate for silicon oxide, so as to remove the second sacrificial layer 308 without damaging the second sidewall layer 309. Although the first etching process also has a higher etching rate for the interface layer 307, the interface layer 307 is not damaged due to the blocking effect of the first sacrificial layer 305. The second etching process subsequently used has a higher etching rate for silicon, so as to remove the first sacrificial layer 305. Since the second etching process has a lower etching rate for silicon oxide, it can reduce damage to the interface layer 307.

[0084] In some embodiments, the first sidewall layer 306 has a first width, and the second sidewall layer 309 has a second width, where the second width is greater than the first width. That is, the width of the second sidewall layer 309 is greater than the width of the first sidewall layer 306, so that the bottom of the second sidewall layer 309 covers a portion of the first sacrificial layer 305. Referring to FIG12 , when the second sidewall layer 309 and the first sacrificial layer 305 are both made of silicon, the second etching process used to remove the first sacrificial layer 305 also has a high etching rate for the second sidewall layer 309. However, since the second sidewall layer 309 has a larger width, it is ensured that after a portion of the second sidewall layer 309 is damaged by the second etching process, the remaining width of the second sidewall layer 309 still meets the design requirements.

[0085] In addition, the second etching process removes a portion of the second sidewall layer 309, thereby increasing the width of the release hole formed in the second sidewall layer 309, which is not conducive to the subsequent sealing process; for this reason, the embodiment of the present disclosure forms a covering layer 310 on the second sidewall layer 309. The material of the covering layer 310 is different from that of the second sidewall layer 309, so it will not be damaged in the second etching process, so that the width of the release hole formed in the covering layer 310 remains unchanged, making it easier to seal the release hole.

[0086] In some embodiments, the first sacrificial layer 305 and the first sidewall layer 306 have a first thickness, and the second sacrificial layer 308 and the second sidewall layer 309 have a second thickness, where the first thickness is less than the second thickness. In other words, the first sidewall layer 306 is thinner near the sensitive material layer, while the second sidewall layer 309, with its narrower top, is thicker. This allows the sacrificial layer to be released near the interface layer using a second etching process that is less likely to damage the interface layer 307, thereby reducing release damage. The majority of the sacrificial layer can be released using a conventional first etching process, thus reducing costs, maintaining productivity, and minimizing damage to the interface layer 307.

[0087] 13, the photoresist layer 311 is removed, and a sealing layer 312 is formed on the cover layer 310. The sealing layer 312 seals the release hole in the cover layer 310, so that the cavity is sealed.

[0088] In some embodiments, subsequent steps may be performed based on this. For example, as shown in FIG14 , the semiconductor substrate 300 may be removed, and a second substrate 313 may be formed on the sealing layer 312. The isolation layer 301 between the semiconductor substrate 300 and the sensitive material layer 302 may be adjusted according to the performance of the semiconductor device and may be completely removed, partially, or fully retained.

[0089] At this point, the process steps of the manufacturing method of the semiconductor device according to an embodiment of the present disclosure have been completed. It can be understood that the manufacturing method of the semiconductor device of the embodiment of the present disclosure not only includes the above steps, but may also include other necessary steps before, during or after the above steps, which are all included in the scope of the manufacturing method of the embodiment of the present disclosure.

[0090] According to the manufacturing method of the semiconductor device provided by the present disclosure, multiple sacrificial layers are formed in the vertical direction, and sacrificial layers that are not easily damaged by the interface layer and etching processes are used at positions adjacent to the interface layer to achieve the effect of reducing damage to the interface layer; while the release of most of the sacrificial layers still maintains the conventional etching process, which can not only reduce costs and maintain production capacity, but also reduce damage to the interface layer.

[0091] As shown in FIG14 , an embodiment of the present disclosure further provides a semiconductor device, which can be manufactured using the semiconductor device manufacturing method described above. Specifically, the semiconductor device of the embodiment of the present disclosure includes: a sensitive material layer 302; a first sidewall layer 306 formed on the sensitive material layer 302; and a second sidewall layer 309 formed above the first sidewall layer. The first sidewall layer 306 and the second sidewall layer 309 are made of different materials, and an interface layer 307 is formed between the sensitive material layer 302 and the first sidewall layer 306. Exemplarily, a cover layer 310 is formed above the second sidewall layer 309. A release hole penetrates the cover layer 310 and the second sidewall layer 309, and the width of the portion of the release hole located in the cover layer 310 is smaller than the width of the portion of the release hole located in the second sidewall layer 309. A sealing layer 312 is formed on the cover layer 310 to seal the release hole formed in the cover layer 310. Exemplarily, a second substrate 313 is formed above the sealing layer 312.

[0092] In some embodiments, the sensitive material layer 302 may be a piezoelectric layer; the semiconductor device further includes a first electrode 303 formed on a first surface of the sensitive material layer, and a second electrode 304 formed on a second surface of the sensitive material layer. The first electrode 303, the piezoelectric layer, and the second electrode 304 constitute a composite thin film, which may also include other film layers in addition to the aforementioned ones. These layers can be appropriately configured based on the actual device and are not specifically limited herein.

[0093] The semiconductor device of the embodiment of the present disclosure is manufactured using the above-mentioned manufacturing method, so the interface layer will not be damaged during the manufacturing process and the structure is more stable.

[0094] The present disclosure has been described through the above-described embodiments, but it should be understood that the above-described embodiments are for illustrative and illustrative purposes only and are not intended to limit the present disclosure to the described embodiments. In addition, it will be understood by those skilled in the art that the present disclosure is not limited to the above-described embodiments, and that various variations and modifications may be made based on the teachings of the present disclosure, all of which fall within the scope of protection claimed by the present disclosure. The scope of protection of the present disclosure is defined by the appended claims and their equivalents.

Claims

1. A method for manufacturing a semiconductor device, comprising: Providing a sensitive material layer; forming a first sacrificial layer and a first sidewall layer surrounding the first sacrificial layer on the sensitive material layer; forming a second sacrificial layer and a second sidewall layer surrounding the second sacrificial layer above the first sacrificial layer and the first sidewall layer, wherein the second sidewall layer is connected to the first sidewall layer, and a material of the second sacrificial layer is different from that of the first sacrificial layer; forming a release hole in the second sidewall layer connected to the second sacrificial layer; Using a first etching process, removing the second sacrificial layer through the release hole to expose the first sacrificial layer; A second etching process different from the first etching process is adopted to remove the first sacrificial layer through the release hole to form a cavity structure in the first sidewall layer and the second sidewall layer.

2. The manufacturing method according to claim 1, characterized in that An interface layer is formed between the first sidewall layer and the sensitive material layer, and an etching rate of the material of the interface layer by the first etching process is greater than an etching rate of the material of the interface layer by the second etching process.

3. The manufacturing method according to claim 2, characterized in that: The materials of the interface layer and the second sacrificial layer include silicon oxide, and the material of the first sacrificial layer includes silicon.

4. The manufacturing method according to claim 3, characterized in that: The material of the first sidewall layer includes silicon oxide, and the material of the second sidewall layer includes silicon.

5. The manufacturing method according to claim 1, characterized in that: The first sidewall layer has a first width, the second sidewall layer has a second width, and the second width is greater than the first width.

6. The manufacturing method according to claim 1, characterized in that: Before forming a release hole connected to the second sacrificial layer in the second sidewall layer, the method further includes: forming a covering layer on the second sidewall layer, wherein the covering layer is made of a material different from that of the second sidewall layer, and an etching rate of the covering layer by the second etching process is lower than an etching rate of the second sidewall layer by the second etching process; The forming of a release hole in the second sidewall layer connected to the second sacrificial layer comprises: etching the cover layer and the second sidewall layer in sequence to form the release hole.

7. The manufacturing method according to claim 1, characterized in that: The first etching process includes a wet etching process, and the second etching process includes a dry etching process.

8. The manufacturing method according to claim 1, characterized in that: The first sacrificial layer and the first sidewall layer have a first thickness, the second sacrificial layer and the second sidewall layer have a second thickness, and the second thickness is greater than the first thickness.

9. The manufacturing method according to any one of claims 1 to 8, characterized in that: The sensitive material layer includes a piezoelectric layer. A first electrode is formed on a first surface of the sensitive material layer, and a second electrode is formed on a second surface of the sensitive material layer.

10. A semiconductor device manufactured by the method according to any one of claims 1 to 9, wherein: The semiconductor device comprises: Sensitive material layer; A first sidewall layer, which is disposed on the sensitive material layer; A second sidewall layer, which is disposed above the first sidewall layer, wherein the first sidewall layer and the second sidewall layer are made of different materials; A cavity structure is disposed between the sensitive material layer and the first sidewall layer and the second sidewall layer.

11. The semiconductor device according to claim 10, wherein: An interface layer is arranged between the first sidewall layer and the sensitive material layer.

12. The semiconductor device according to claim 10, wherein: The material of the first sidewall layer includes silicon oxide, and the material of the second sidewall layer includes silicon.

13. The semiconductor device according to claim 10, wherein: The first sidewall layer has a first width, the second sidewall layer has a second width, and the second width is greater than the first width.

14. The semiconductor device according to claim 10, wherein: The first sidewall layer has a first thickness, the second sacrificial layer and the second sidewall layer have a second thickness, and the second thickness is greater than the first thickness.

15. The semiconductor device according to claim 10, wherein: A covering layer is arranged above the second sidewall layer, and a release hole penetrating the covering layer and the second sidewall layer is formed in the covering layer and the second sidewall layer, and the width of the release hole in the covering layer is smaller than the width of the release hole in the second sidewall layer.

16. The semiconductor device according to claim 15, wherein: A sealing layer is disposed on the cover layer, and the sealing layer seals the release hole formed in the cover layer.

17. The semiconductor device according to claim 16, wherein: A second substrate is disposed above the sealing layer.

18. The semiconductor device according to claim 10, wherein: The sensitive material layer comprises a piezoelectric layer. A first electrode is disposed on a first surface of the sensitive material layer, and a second electrode is disposed on a second surface of the sensitive material layer.

Citation Information

Patent Citations

  • MEMS (Micro-electromechanical System) device, preparation method and electronic device

    CN107973266A

  • MEMS device and manufacturing method thereof

    CN108600928A

  • Film piezoelectric acoustic wave filter and manufacturing method thereof

    CN112039485A

  • Capacitive MEMS microphone structure and manufacturing method thereof

    CN113727265A

  • Manufacturing method of fine structure

    CN114477072A