Trench-type silicon carbide mosfet device and manufacturing method therefor

By forming a deeper second conductivity type shielding region and well region in the trench SiC MOSFET device, the problem of insufficient reliability and process complexity of the device in extreme environments is solved, and high reliability and simplified production processes are achieved. goal.

WO2024222405A1PCT designated stage expired Publication Date: 2024-10-31NANJING THIRD GENERATION SEMICON TECH INNOVATION CENT CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/085630
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-02
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Trench SiC MOSFET devices have insufficient reliability in extreme environments such as high temperature, high frequency, and radiation resistance, and the process complexity is high, which affects the difficulty of mass production.

Method used

By forming a first trench on a first conductive type substrate and filling it with a second conductive type epitaxial layer as a shielding region and a well region, a superjunction or semi-superjunction structure is formed, and the depth of the shielding region is significantly increased to reduce The electric field intensity inside the small gate trench simplifies the process flow and improves device reliability.

Benefits of technology

It effectively reduces the electric field intensity inside the gate trench in the off state, improves the reliability of the device, simplifies the process flow, and reduces the process complexity. It is suitable for batch production of high-reliability trench silicon carbide MOSFET devices. Production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085630_31102024_PF_FP_ABST
    Figure CN2024085630_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A trench-type silicon carbide MOSFET device and a manufacturing method therefor. The method comprises: forming a first conductivity type epitaxial layer (3) on a first conductivity type substrate (2); etching to remove part of the first conductivity type epitaxial layer (3) to form a first trench (4); growing a second conductivity type epitaxial layer (6), filling a region in the first trench (4) with the second conductivity type epitaxial layer (6) as a second conductivity type shielding region (6-1), and covering a region of the first conductivity type epitaxial layer (3) with the second conductivity type epitaxial layer (6) as a second conductivity type well region (6-2); forming a first conductivity type source region (9) in the second conductivity type well region (6-2); and forming a gate trench (7) in the first conductivity type epitaxial layer (3).
Need to check novelty before this filing date? Find Prior Art

Description

Trench-type silicon carbide MOSFET device and manufacturing method thereof

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 25, 2023, with application number 202310450705.2, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of semiconductor technology, for example, to a trench silicon carbide MOSFET device and a manufacturing method thereof. Background Art

[0003] The development of power electronics systems has placed higher demands on the performance of semiconductor devices, particularly in terms of high temperature, high frequency, radiation resistance, and high voltage. While traditional silicon device manufacturing processes are mature, the inherent properties of the material limit its application in extreme operating environments. Compared to silicon, silicon carbide (SiC) offers a wider bandgap, higher electron saturation drift velocity, stronger radiation resistance, higher breakdown electric field, and higher thermal conductivity. This makes SiC a promising material for applications in power electronics, aerospace systems, high-speed rail traction equipment, and military electronic communications systems.

[0004] Compared with planar-gate SiC metal-oxide-semiconductor field-effect transistor (MOSFET) devices, trench SiC MOSFET devices form channels on the trench sidewalls, which not only improves channel mobility but also eliminates the junction field effect transistor (JFET) effect, significantly reducing the device on-resistance, while also reducing the cell size and increasing the power density.

[0005] However, trench SiC MOSFET devices face several challenges in actual manufacturing. First, in the off state, the gate oxide layer at the trench corners must withstand a high electric field strength, which affects device reliability. Second, the manufacturing process for trench SiC MOSFET devices is relatively complex. The structures currently used to address the former problem (such as the formation of a P-shield layer and superjunction structures) further complicate the process, significantly increasing the difficulty of mass production of trench SiC MOSFET devices.

[0006] Summary of the Invention

[0007] The present application provides a trench-type silicon carbide MOSFET device and a manufacturing method thereof, wherein a gate trench is formed to form a longitudinal conductive channel, and a second conductive type shielding region and a second conductive type well region are formed by etching and epitaxial backfilling. The depth of the second conductive type shielding region is significantly greater than the depth of the gate trench, which can effectively reduce the electric field strength borne by the gate dielectric inside the gate trench in the off state, thereby improving the reliability of the device.

[0008] The present application provides a method for manufacturing a trench silicon carbide MOSFET device, comprising:

[0009] S1, forming a first conductive type epitaxial layer on a first conductive type substrate;

[0010] S2, etching and removing a portion of the first conductive type epitaxial layer to form a first trench;

[0011] S3, growing a second conductive type epitaxial layer, filling the first trench with the second conductive type epitaxial layer as a second conductive type shielding region, and covering the first conductive type epitaxial layer with the second conductive type epitaxial layer as a second conductive type well region;

[0012] S4, forming a first conductivity type source region in the second conductivity type well region;

[0013] S5, forming a gate trench in the first conductivity type epitaxial layer;

[0014] S6, forming a gate dielectric layer inside the gate trench;

[0015] S7, forming a gate electrode on the gate dielectric layer;

[0016] S8, forming an isolation dielectric layer on the gate electrode;

[0017] S9, forming a source ohmic contact layer on the surfaces of the first conductivity type source region and the second conductivity type well region, and forming a source electrode on the surface of the source ohmic contact layer;

[0018] S10, forming a drain ohmic contact layer under the first conductive type substrate, and forming a drain electrode on a surface of the drain ohmic contact layer.

[0019] In one or more embodiments, the first trench formed in step S2 has a depth greater than 1.0 μm, an aspect ratio greater than 2:1, an etching angle no less than 80 degrees, and a spacing between adjacent first trenches no greater than 6.0 μm.

[0020] In one or more embodiments, the ratio of the depth of the second conductive type shielding region to the depth of the first conductive type epitaxial layer in step S3 is greater than 1:4, and the second conductive type shielding region and the first conductive type epitaxial layer form a super junction or semi-super junction structure.

[0021] In one or more embodiments, the thickness of the second conductive type well region formed in step S3 is no more than 2.5 μm, and after step S3 is completed, the first trench is completely filled without voids.

[0022] In one or more embodiments, the second conductive type epitaxial layer in step S3 is grown epitaxially, and the epitaxial growth is constant doping concentration growth or variable doping concentration growth, with an average doping concentration of 1e17 cm -3 ~1e18cm -3 .

[0023] In one or more embodiments, in step S5 , the gate trench is disposed between adjacent first trenches and passes through the second conductive type well region and the first conductive type source region, and the top of the gate trench is flush with the top of the first conductive type source region.

[0024] In one or more embodiments, after step S2 and before step S3 , ion implantation is performed on the bottom of the first trench to form a second conductive type electric field protection area.

[0025] In one or more embodiments, a second conductivity type high concentration doping implantation is added after step S4 and before step S5 to form a second conductivity type heavily doped region in the second conductivity type well region.

[0026] The present application also provides a trench silicon carbide MOSFET device, wherein the trench silicon carbide MOSFET device is manufactured by any of the above-mentioned methods for manufacturing a trench silicon carbide MOSFET device, and the structure includes:

[0027] drain electrode;

[0028] a first conductive type substrate located above the drain electrode;

[0029] an epitaxial layer of the first conductive type located on the substrate of the first conductive type;

[0030] a first trench located in the first conductivity type epitaxial layer;

[0031] a second conductive type epitaxial layer located in the first trench and above the first conductive type epitaxial layer, the second conductive type epitaxial layer filling the first trench as a second conductive type shielding region, and the second conductive type epitaxial layer covering the first conductive type epitaxial layer as a second conductive type well region;

[0032] a first conductivity type source region located in the second conductivity type well region;

[0033] a gate trench located in the first conductivity type epitaxial layer;

[0034] a gate dielectric layer located in the gate trench;

[0035] a gate electrode located on the gate dielectric layer;

[0036] an isolation dielectric layer located above the gate electrode;

[0037] A source electrode is located on the surfaces of the first conductive type source region and the second conductive type well region.

[0038] In one or more embodiments, a second conductive type electric field protection zone is provided at the bottom of the first trench.

[0039] In one or more embodiments, a second conductivity type heavily doped region is formed in the second conductivity type well region. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] FIG1 is a process flow chart of a method for manufacturing a high-reliability trench silicon carbide MOSFET;

[0041] FIG2 is a flow chart of a method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0042] FIG3 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0043] FIG4 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0044] FIG5 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0045] FIG6 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0046] FIG7 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0047] FIG8 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0048] FIG9 is a flow chart of another method for manufacturing a high-reliability trench silicon carbide MOSFET according to the first embodiment;

[0049] FIG10 is a schematic structural diagram of a high-reliability trench silicon carbide MOSFET according to Example 2;

[0050] FIG11 is a schematic structural diagram of a high-reliability trench silicon carbide MOSFET according to Example 3;

[0051] FIG12 is a schematic structural diagram of a high-reliability trench silicon carbide MOSFET according to a fourth embodiment.

[0052] Explanation of the accompanying drawings: 1. drain electrode; 2. first conductive type substrate; 3. first conductive type epitaxial layer; 4. first trench; 5. gate dielectric layer; 6. second conductive type epitaxial layer; 6-1. second conductive type shielding region; 6-2. second conductive type well region; 7. gate trench; 8. gate electrode; 9. first conductive type source region; 10. source electrode; 11. isolation dielectric layer; 12. second conductive type electric field protection region; 13. second conductive type heavily doped region; 14. first conductive type current spreading layer. DETAILED DESCRIPTION

[0053] A high-reliability trench silicon carbide MOSFET device and a manufacturing method thereof of the present application are described and explained below with reference to the accompanying drawings and embodiments.

[0054] Example 1

[0055] A method for manufacturing a high-reliability trench silicon carbide MOSFET device is shown in FIG1 . The method includes the following steps. Each step will be described below in conjunction with FIG2 to FIG9 .

[0056] S1. As shown in FIG2 and FIG3 , a first conductive type epitaxial layer 3 is formed on a first conductive type substrate 2; the first conductive type substrate 2 is a first conductive type silicon carbide substrate, the substrate material is 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC, the substrate thickness ranges from 10 μm to 1000 μm, and the doping concentration is 1e18 cm -3 ~5e19cm -3 The first conductive type epitaxial layer 3 is a first conductive type silicon carbide epitaxial layer, the material is 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC, the thickness range is 8μm to 200μm, and the doping concentration is 1e14cm -3 ~1e16cm -3 In some embodiments of the present application, the first conductivity type epitaxial layer 3 is grown by epitaxial growth.

[0057] S2. As shown in FIG4 , a portion of the first conductive type epitaxial layer 3 is etched away to form a first trench 4. This step includes forming an etch mask layer on the surface of the first conductive type epitaxial layer 3 by chemical vapor deposition, then forming a patterned etch mask layer by photolithography, and performing inductively coupled plasma etching on the first conductive type epitaxial layer 3 using the patterned etch mask layer to remove a portion of the first conductive type epitaxial layer 3 to form a first trench 4. The width of the first trench 4 ranges from 0.5 μm to 3.5 μm.

[0058] In some other embodiments of the present application, step S2 forms the first groove 4 through a deep trench etching process, the etching method adopts reactive ion etching or inductively coupled plasma etching, and the etching gas is one or more combinations of sulfur hexafluoride SF6, hydrogen bromide HBr, chlorine Cl2, oxygen O2, and argon Ar gas.

[0059] The first trenches 4 formed in step S2 have a depth greater than 1.0 μm, an aspect ratio greater than 2:1, an etching angle no less than 80 degrees, for example, an angle range of 80° to 90°, and a spacing between adjacent first trenches 4 no greater than 6.0 μm.

[0060] S3. As shown in FIG5 , a second conductive type epitaxial layer 6 is grown, and the second conductive type epitaxial layer 6 is filled in the first trench 4 as a second conductive type shielding region 6-1, that is, the top of the first trench 4 is flush with the top of the second conductive type shielding region 6-1, and the second conductive type epitaxial layer 6 is covered in the area of ​​the first conductive type epitaxial layer 3 as a second conductive type well region 6-2; the second conductive type epitaxial layer 6 is a second conductive type silicon carbide epitaxial layer. Step S3 includes: removing the etching mask layer, forming the second conductive type shielding region 6-1 and the second conductive type well region 6-2 by an epitaxial backfill process, and the second conductive type epitaxial layer 6 is grown epitaxially, and the epitaxial growth is constant doping concentration growth or variable doping concentration growth, and the average doping concentration is 1e17cm -3 ~1e18cm -3 The depth of the second conductive type shielding region 6-1 is the same as that of the first trench 4; the depth of the second conductive type shielding region 6-1 ranges from 1.5 μm to 7 μm, and the width ranges from 0.5 μm to 3.5 μm. The depth of the second conductive type well region 6-2 ranges from 0.5 μm to 1.5 μm.

[0061] In some other embodiments of the present application, the thickness of the second conductive type well region 6-2 formed in step S3 is no more than 2.5 μm, and after step S3 is completed, the first trench 4 is completely filled without voids. When the ratio of the depth of the second conductive type shielding region 6-1 to the depth of the first conductive type epitaxial layer 3 is greater than 1:4, the second conductive type shielding region 6-1 and the first conductive type epitaxial layer 3 form a super junction or semi-super junction structure. At this time, according to the width of the second conductive type shielding region 6-1 and the first conductive type epitaxial layer 3, the doping concentration of the second conductive type shielding region 6-1 and the first conductive type epitaxial layer 3 should meet a certain proportional relationship to achieve charge balance in the super junction structure or semi-super junction structure.

[0062] The growth mode of the second conductive type epitaxial layer 6 in step S3 is epitaxial growth, which adopts constant doping concentration growth or variable doping concentration growth, and the average doping concentration is 1e17cm -3 ~5e18cm -3 The present application forms the second conductive type shielding region 6-1 and the second conductive type well region 6-2 in a single-step process through an epitaxial backfill process, thereby simplifying the process flow. At the same time, the second conductive type shielding region 6-1 can effectively protect the gate dielectric layer 5, avoiding the introduction of a process with a high process difficulty to form an electric field shielding region at the bottom of the gate trench, significantly reducing the process complexity, and the manufacturing method is relatively simple, which can be used to achieve high-performance trench-gate silicon carbide MOSFET device mass production.

[0063] After the first epitaxial growth of the second conductivity type shielding region 6-1 in step S3, a chemical-mechanical planarization (CMP) process is added. At this point, the top of the first trench 4 is flush with the top of the second conductivity type shielding region 6-1. The CMP process flattens the device surface, i.e., the SiC surface, at this point. Subsequently, a second epitaxial growth is performed to form the second conductivity type well region 6-2. With the addition of the CMP process, the second conductivity type epitaxial layer 6 is formed in two steps. While this increases process complexity, the CMP process can improve the flatness of the SiC surface, thereby enhancing the quality of subsequent processes.

[0064] S4. As shown in FIG6 , a first conductivity type source region 9 is formed in the second conductivity type well region 6 - 2. This step includes forming an ion implantation mask layer on the surface of the first conductivity type epitaxial layer 3 by chemical vapor deposition, then forming a patterned etching mask layer by photolithography, and performing ion implantation into the first conductivity type epitaxial layer 3 using the patterned ion implantation mask layer to form the first conductivity type source region 9. After removing the mask, annealing is performed at a temperature of 1400° C. to 2200° C. for 2 to 30 minutes.

[0065] In step S4, a first conductive type source region 9 is formed in the second conductive type well region 6-2 by an ion implantation process. The ion implantation process includes: preparing a patterned mask layer on the surface of the first conductive type epitaxial layer 3, then implanting first conductive type impurities, removing the mask, and annealing at a temperature of 1400°C to 2200°C for 2 minutes to 30 minutes.

[0066] S5. As shown in FIG7 , a gate trench 7 is formed in the first conductive type epitaxial layer 3; the gate trench 7 is arranged between adjacent first trenches 4 and passes through the second conductive type well region 6-2 and the first conductive type source region 9, and the top of the gate trench 7 is flush with the top of the first conductive type source region 9; step S5 includes: forming a patterned etching mask layer on the surface of the first conductive type epitaxial layer 3, and performing inductively coupled plasma etching using the patterned etching mask layer to form the gate trench 7.

[0067] In some other embodiments of the present application, in step S5, a gate trench 7 is formed in the first conductivity type epitaxial layer 3 by an etching process. The etching process adopts reactive ion etching or inductively coupled plasma etching, and the etching gas is one or more combinations of SF6, HBr, Cl2, O2, and Ar gases. After the gate trench 7 is formed, a high-temperature annealing process is performed to passivate the gate trench 7. The gas used in the passivation process is one or more combinations of monosilane SiH4, hydrogen H2, and Ar gas, and the annealing temperature is 1400° C. to 1800° C.

[0068] The depth of the gate trench 7 formed in step S5 is smaller than the depth of the first trench 4 , and the difference between the depth of the gate trench 7 and the depth of the second conductive type shielding region 6 - 1 is not less than 0.5 μm.

[0069] The distance between the gate trench 7 formed in step S5 and the second conductive type shielding region 6 - 1 is no greater than 2 μm.

[0070] S6. As shown in FIG8 , a gate dielectric layer 5 is formed within the gate trench 7. This step includes forming the gate dielectric layer 5 in the gate trench 7 through an oxidation process and a chemical vapor deposition process. The material of the gate dielectric layer 5 is silicon dioxide (SiO2), silicon nitride (Si3N4), or aluminum oxide (Al2O3). The quality of the gate dielectric layer 5 is then improved through a high-temperature annealing process. The annealing gas is one or more of nitric oxide (NO), nitrous oxide (N2O), H2, and ammonia (NH3). The annealing temperature is 900°C to 1300°C.

[0071] S7. As shown in FIG8 , a gate electrode 8 is formed on the gate dielectric layer 5. The gate dielectric layer 5 wraps around the gate electrode 8, and the top of the gate dielectric layer 5 and the top of the gate electrode 8 are both flush with the top of the first conductivity type source region 9. The gate electrode 8 is formed by atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition, or sputtering. The material of the formed gate electrode 8 is polycrystalline silicon, amorphous silicon, or amorphous silicon, and the doping impurities are aluminum Al, nitrogen N, phosphorus P, or boron B impurities. When polycrystalline silicon material is used, polysilicon is implanted and the polycrystalline silicon surface is flattened by a CMP process.

[0072] S8, forming an isolation dielectric layer 11 on the gate electrode 8. This step includes:

[0073] On the first conductivity type epitaxial layer 3, illustratively, a patterned isolation dielectric layer 11 is formed on the gate electrode 8 by chemical vapor deposition and photolithography. The bottom surface of the isolation dielectric layer 11 contacts the top surface of the gate electrode 8, the gate dielectric layer 5, the gate trench 7, and a portion of the first conductivity type source region 9. In some other embodiments of the present application, the isolation dielectric layer 11 is made of silicon nitride with a thickness of 0.5 μm to 10 μm to form a source window. Exemplarily, the material of the isolation dielectric layer 11 is silicon dioxide, nitride, or a composite of silicon dioxide and nitride.

[0074] S9. Form a source ohmic contact layer on the surfaces of the first conductivity type source region 9 and the second conductivity type well region 6-2, and form a source electrode 10 on the surface of the source ohmic contact layer. This step includes evaporating metal through a source window formed by the isolation dielectric layer 11 on the surfaces of the first conductivity type source region 9 and the second conductivity type well region 6-2.

[0075] S10 , forming a drain ohmic contact layer under the first conductive type substrate 2 , and forming a drain electrode 1 on a surface of the drain ohmic contact layer.

[0076] In some other embodiments of the present application, the source ohmic contact and the drain ohmic contact are formed in steps S9 and S10, and a metal layer is formed by evaporation, sputtering or electroplating, and then annealed at 300°C to 1100°C. The metal layer material is one or more combinations of Al, titanium Ti, silver Ag, nickel Ni, platinum Pt, and copper Cu materials.

[0077] The first conductivity type is N-type or P-type, and the second conductivity type is P-type or N-type.

[0078] The present application forms a longitudinal conductive channel by forming a gate trench 7, and forms a second conductive type shielding region 6-1 and a second conductive type well region 6-2 by etching and epitaxial backfilling. The depth of the second conductive type shielding region 6-1 is significantly greater than the depth of the gate trench 7, which can effectively reduce the electric field strength borne by the gate dielectric inside the gate trench 7 in the off state, thereby improving the reliability of the device.

[0079] After forming the first trench 4, the present application forms a second conductivity type well region 6-2 and a second conductivity type shield region 6-1 in a single step through an epitaxial backfill process. The depth of the second conductivity type shield region 6-1 is significantly greater than the depth of the gate trench 7, which can effectively reduce the electric field strength borne by the gate dielectric inside the gate trench 7 in the off state, thereby improving device reliability. The present application significantly reduces the process complexity of trench-gate silicon carbide MOSFET devices, and the manufacturing method is relatively simple, which can be used to achieve high-reliability trench-gate silicon carbide MOSFET devices in mass production.

[0080] A high-reliability trench silicon carbide MOSFET device based on the above-mentioned manufacturing method comprises:

[0081] drain electrode 1;

[0082] a first conductive type substrate 2 located on the drain electrode 1;

[0083] a first conductive type epitaxial layer 3 located on the first conductive type substrate 2;

[0084] a first trench 4 located in the first conductivity type epitaxial layer 3;

[0085] a second conductive type epitaxial layer 6 located in the first trench 4 and above the first conductive type epitaxial layer 3, wherein the second conductive type epitaxial layer 6 fills the first trench 4 as a second conductive type shielding region 6-1, and the second conductive type epitaxial layer 6 covers the first conductive type epitaxial layer 3 as a second conductive type well region 6-2;

[0086] a first conductivity type source region 9 located in the second conductivity type well region 6 - 2 ;

[0087] a gate trench 7 located in the first conductivity type epitaxial layer 3;

[0088] a gate dielectric layer 5 located in the gate trench 7;

[0089] a gate electrode 8 located on the gate dielectric layer 5;

[0090] an isolation dielectric layer 11 located on the first conductive type epitaxial layer 3; wherein the isolation dielectric layer 11 may be located on the gate electrode 8;

[0091] A source electrode 10 is located on the surfaces of the first conductive type source region 9 and the second conductive type well region 6 - 2 .

[0092] Example 2

[0093] A method for manufacturing a high-reliability trench-type silicon carbide MOSFET is provided, which differs from the first embodiment in that, after forming the first trench 4 by an etching process in step S2, a patterned ion implantation mask layer is formed on the surface of the first conductive type epitaxial layer 3, and then ion implantation is performed on the bottom of the first trench 4, that is, the second conductive type dopant is implanted into the bottom of the first trench 4 with the aid of the etching mask layer to form a second conductive type electric field protection zone 12. The depth of the second conductive type electric field protection zone 12 is 0.1 μm to 1 μm, and the doping concentration is a variable doping distribution with an average doping concentration of 5e17 cm -3 ~1e19cm -3 , and the doping concentration of the second conductive type electric field protection zone 12 is significantly higher than that of the second conductive type shielding zone 6-1 and the second conductive type well zone 6-2. After the second conductive type electric field protection zone 12 is formed, the second conductive type shielding zone 6-1 and the second conductive type well zone 6-2 are formed by an epitaxial backfill process, and the remaining steps are exactly the same as in Example 1. The second conductive type electric field protection zone 12 can more effectively protect the gate dielectric layer 5 and improve the reliability of the device. The cross-sectional view of the high-reliability trench silicon carbide MOSFET formed in this embodiment is shown in Figure 10. In this embodiment, a second conductive type electric field protection zone 12 is provided at the bottom of the first trench 4 of the formed high-reliability trench silicon carbide MOSFET.

[0094] Example 3

[0095] A method for manufacturing a high-reliability trench silicon carbide MOSFET is provided. The method differs from the first embodiment in that, after forming the first conductive type source region 9 in step S4, a patterned ion implantation mask layer is formed on the surface of the first conductive type epitaxial layer 3, and an ion implantation process is used to form a second conductive type heavily doped region 13. The depth of the second conductive type heavily doped region 13 is 0.1 μm to 0.5 μm, and the doping concentration is a variable doping distribution with an average doping concentration of 5e18 cm -3 ~5e19cm -3, and the subsequent steps are exactly the same as those in Example 1. The second conductivity type heavily doped region 13 can effectively improve the third quadrant characteristics of the device. In this embodiment, after step S4 and before step S5, a second conductivity type high concentration doping injection is added to form a second conductivity type heavily doped region 13 in the second conductivity type well region 6-2. A cross-sectional view of the high reliability trench silicon carbide MOSFET formed in this embodiment is shown in Figure 11. In this embodiment, a second conductivity type heavily doped region 13 is formed in the second conductivity type well region 6-2 of the formed high reliability trench silicon carbide MOSFET.

[0096] Example 4

[0097] A method for manufacturing a high-reliability trench silicon carbide MOSFET is provided. The method differs from the first embodiment in that, after forming the second conductive type well region 6-2 in step S3, a patterned ion implantation mask layer is formed on the surface of the first conductive type epitaxial layer 3, and an ion implantation process is used to form a first conductive type current spreading layer 14. The first conductive type current spreading layer 14 has a depth of 0.2 μm to 1.5 μm, a variable doping concentration, and an average doping concentration of 1e16 cm -3 ~1e17cm -3 , and the subsequent steps are exactly the same as in Example 1. The first conductive type current spreading layer 14 can effectively reduce the on-resistance of the device and increase the current density of the device. A cross-sectional view of the high-reliability trench silicon carbide MOSFET formed in this embodiment is shown in Figure 12.

Claims

1. A method for manufacturing a trench silicon carbide MOSFET device, comprising: Forming a first conductivity type epitaxial layer (3) on a first conductivity type substrate (2); Etching and removing a portion of the first conductivity type epitaxial layer (3) to form a first trench (4); Growing a second conductive type epitaxial layer (6), filling the second conductive type epitaxial layer (6) in the first trench (4) as a second conductive type shielding region (6-1), and covering the second conductive type epitaxial layer (6) in a region of the first conductive type epitaxial layer (3) as a second conductive type well region (6-2); forming a first conductivity type source region (9) in the second conductivity type well region (6-2); forming a gate trench (7) in the first conductivity type epitaxial layer (3); forming a gate dielectric layer (5) inside the gate trench (7); forming a gate electrode (8) on the gate dielectric layer (5); forming an isolation dielectric layer (11) on the gate electrode (8); Forming a source ohmic contact layer on the surface of the first conductive type source region (9) and the second conductive type well region (6-2), and forming a source electrode (10) on the surface of the source ohmic contact layer; A drain ohmic contact layer is formed under the first conductive type substrate (2), and a drain electrode (1) is formed on the surface of the drain ohmic contact layer.

2. A method for manufacturing a trench silicon carbide MOSFET device according to claim 1, wherein: The first conductive type epitaxial layer (3) is partially removed by etching to form a first groove (4). The depth of the first groove (4) formed is greater than 1.0 μm, the aspect ratio is greater than 2:1, the etching angle is not less than 80 degrees, and the spacing between adjacent first grooves (4) is not greater than 6.0 μm.

3. A method for manufacturing a trench silicon carbide MOSFET device according to claim 1, wherein: The thickness of the second conductive type well region (6-2) formed in the area where the second conductive type epitaxial layer (6) covers the first conductive type epitaxial layer (3) as the second conductive type well region (6-2) is not greater than 2.5 μm, and after the area where the second conductive type epitaxial layer (6) covers the first conductive type epitaxial layer (3) as the second conductive type well region (6-2) is completed, the first trench (4) is completely filled without voids.

4. A method for manufacturing a trench silicon carbide MOSFET device according to claim 1, wherein: In the growing of the second conductive type epitaxial layer (6), the second conductive type epitaxial layer (6) is grown by epitaxial growth, the epitaxial growth is constant doping concentration growth or variable doping concentration growth, and the average doping concentration is 1e17cm -3 ~1e18cm -3 .

5. A method for manufacturing a trench-type silicon carbide MOSFET device according to claim 1, wherein, in the gate trench (7) formed in the first conductive type epitaxial layer (3), the gate trench (7) is arranged between adjacent first trenches (4) and passes through the second conductive type well region (6-2) and the first conductive type source region (9), and the top of the gate trench (7) is flush with the top of the first conductive type source region (9).

6. A method for manufacturing a trench silicon carbide MOSFET device according to claim 1, wherein: After the etching removes part of the first conductive type epitaxial layer (3) to form a first trench (4) and before the growing of the second conductive type epitaxial layer (6), ion implantation is performed on the bottom of the first trench (4) to form a second conductive type electric field protection area (12).

7. A method for manufacturing a trench silicon carbide MOSFET device according to claim 1, wherein: After forming the first conductive type source region (9) in the second conductive type well region (6-2) and before forming the gate trench (7) in the first conductive type epitaxial layer (3), a second conductive type high concentration doping injection is added to form a second conductive type heavily doped region (13) in the second conductive type well region (6-2).

8. A trench silicon carbide MOSFET device, wherein: The trench silicon carbide MOSFET device is completed by a trench silicon carbide MOSFET device manufacturing method according to any one of claims 1 to 7, comprising: Drain electrode (1); A first conductive type substrate (2) located on the drain electrode (1); A first conductivity type epitaxial layer (3) located on the first conductivity type substrate (2); A first trench (4) located in the first conductivity type epitaxial layer (3); a second conductive type epitaxial layer (6) located in the first trench (4) and above the first conductive type epitaxial layer (3), the second conductive type epitaxial layer (6) filling the first trench (4) as a second conductive type shielding region (6-1), and the second conductive type epitaxial layer (6) covering the region of the first conductive type epitaxial layer (3) as a second conductive type well region (6-2); A first conductivity type source region (9) located in the second conductivity type well region (6-2); A gate trench (7) located in the first conductivity type epitaxial layer (3); A gate dielectric layer (5) located in the gate trench (7); A gate electrode (8) located on the gate dielectric layer (5); an isolation dielectric layer (11) located on the gate electrode (8); A source electrode (10) is located on the surface of the first conductive type source region (9) and the second conductive type well region (6-2).

9. A trench silicon carbide MOSFET device according to claim 8, wherein: A second conductive type electric field protection area (12) is provided at the bottom of the first trench (4).

10. A trench silicon carbide MOSFET device according to claim 8, wherein: A second conductivity type heavily doped region (13) is formed in the second conductivity type well region (6-2).

Citation Information

Patent Citations

  • High-reliability groove type silicon carbide MOSFET device and manufacturing method thereof

    CN116469923A

  • Semiconductor device, and method for manufacturing the same

    CN101981701A

  • Method for preparing silicon carbide UMOSFET device with N-type heavy doping drift layer table board formed by ion implantation

    CN103928345A

  • Semiconductor device and method of manufacturing semiconductor device

    JP2001267570A

  • Silicon carbide semiconductor device, and method of manufacturing the same

    JP2010258386A