Process for synthesizing porous silica particles using low-pressure gaseous carbon dioxide

Exposing a silicate-polyamine solution to carbon dioxide accelerates silica precipitation, overcoming the limitations of existing methods by achieving rapid, high-yield, and controlled silica production suitable for pharmaceutical applications and scalable manufacturing.

WO2024223751A1PCT designated stage expired Publication Date: 2024-10-31UNIVERSITY OF LIMERICK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/061417
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for synthesizing porous silica face challenges such as requiring harsh reagents, generating waste, using organic solvents, and difficulty in scaling up due to poor control over key properties and separation costs, with prior art methods taking several hours and involving harsh conditions.

Method used

A method involving a solution of silicate and an organic polyamine exposed to carbon dioxide, which significantly accelerates the silica precipitation rate, allowing for higher surface area and yield, and can be performed under standard conditions without strong acids or organic solvents, enabling more controlled and scalable production.

Benefits of technology

The method achieves rapid silica precipitation with increased surface area and yield, is environmentally benign, and allows for precise control of silica properties, making it suitable for pharmaceutical applications and scalable manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024061417_31102024_PF_FP_ABST
    Figure EP2024061417_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing silica, wherein the method comprises the steps of: providing a solution comprising: a silicate, and an organic polyamine or a salt thereof; and exposing the solution to carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] PROCESS FOR SYNTHESIZING POROUS SILICA PARTICLES USING LOW- PRESSURE GASEOUS CARBON DIOXIDE

[0002] Field of the Invention

[0003] The present invention relates to a method for producing silica, to silica obtainable by the method, and to a use of a polyamine and carbon dioxide to increase the rate of precipitation of silica. The present invention can allow for the properties of the silica to be tailored.

[0004] Background of the Invention

[0005] Porous silica has wide-ranging applications, including as sorbents, fillers and additives for food and drug products, for molecular storage, and in drug discovery (e.g. as excipients), catalysis, polymer composites and biosensors.

[0006] Methods for synthesising silica include exposing a solution comprising a silicate (e.g. sodium silicate) to harsh acidic compounds, such as HC1, to neutralise the silicate solution. Neutralisation of the solution causes the reactive precipitation of particles of silica from the reaction mixture. Calcination and / or acidic washing can be used to remove any amine used to “template” the silica.

[0007] In order to control precipitation precisely, the change in pH needs to be controlled precisely. Typically, dilute acids are used to control the pH. However, the use of dilute acids generates a dilute reaction mixture that greatly enhances separation costs and enlarges the environmental footprint.

[0008] WO 2017 / 037460 Al discloses a calcination-free, bio-inspired silica-production process using various amines as templates and various organic and inorganic acids for neutralization. However, controlling the pH of the reaction mixture using these methods is challenging and not always reproducible.

[0009] CN112174147A and CN108046278A disclose the use of CO2 as an acidifying agent in a tubular reactor. The gas-liquid (G-L) slug flow regime gives better mass transfer characteristics; however, the approach is not scalable as increasing the tube diameter will change the flow regime thus affecting the mass transfer performance and hence the particle properties. Scale-out or numbering approach is generally used to retain the transport properties (e.g. mixing, mass transfer, and heat transfer); however, very few examples are available in the literature for manufacturing scale. Moreover, for a multiphase system (G-L), it is further complicated to number-up reactors. The disclosures require the maintenance of a temperature of 0-80°C and 0- 90°C respectively.

[0010] CN 104860319A discloses a batch process with complex reactor geometry that is similar to an annular centrifugal extractor and reports a reaction time of l-5h. The complex geometry is difficult to scale up and has the inherent limitations associated with a batch process, such as controllability, safety, and scalability. This document also requires the addition of 5-15% PEG as a surfactant, which will add to material cost and the subsequent energy-intensive calcination required to remove the PEG.

[0011] CN112174147A and CN104860319A use ethanol as an organic solvent, which will further increase the cost and it can form an azeotrope with water making separation difficult and costly.

[0012] Further, CN108046278A uses metal salts in the process which have higher orders of magnitude concentration compared to the silicon source.

[0013] CN103785349B discloses a method of preparing a solid amine gas adsorbent material. The process involves preparing a silicate-containing solution from fly ash at a temperature of about 90°C and over a reaction time of 90 minutes. An organic amine such as poly(ethyleneimine) (PEI) or tetraethylenepentamine (TEPA) is added to the silicate and an acidic gas, such as CO2, is introduced while stirring. The acidic gas was added until the pH of the solution had decreased to be within the range of from 9 to 11. This formed a precipitate. The precipitate was filtered, aged at 110°C, dried and dehydrated to provide the solid amine gas adsorbent material. The adsorbent material produced by the disclosed method has a specific surface area range of from 8.71 to 15.03m2 / g.

[0014] Cai et al. Chemical Engineering Journal 151 (2009) 380-386 and Quang et al. ACS Sustainable Chem. Eng. 2017, 5, 3170-3178 have reported the use of elevated pressure CO2 to precipitate silica. Cai et al. used 2 bar pressure and 60-80°C temperature with reaction time ranging from 1-3 h, while Quang et al. used up to 3 bar pressure and 110°C temperature and a reaction time of more than 24 h.

[0015] Overall, the prior art can suffer from requiring the use of harsh reagents and / or conditions, producing significant quantities of waste, generating dilute solid-liquid mixtures that are difficult to separate, use of organic solvents, provide poor control of key properties in the resulting silica, and provide difficulties for scaling up. Summary of the Invention

[0016] According to a first aspect, the claimed invention provides a method for producing silica, wherein the method comprises the steps of: providing a solution comprising a silicate and an organic polyamine or a salt thereof; and exposing the solution to carbon dioxide.

[0017] The present inventors have surprisingly recognised that producing silica as required by the first aspect makes the rate of reaction and / or precipitation significantly faster than was previously possible with CO2. While methods of the prior art typically take several hours, the claimed method can be performed within minutes. It is thought that the specific combination of a polyamine, such as pentaethylenehexamine (PEHA), and carbon dioxide leads to these significant benefits. Without being bound to theory, it is thought that the presence of polyamines, such as PEHA, may catalyse the precipitation of silica.

[0018] The inventors have found that exposing the solution to carbon dioxide until the pH of the solution has decreased below 9 (e.g. 8 or lower) can provide significant benefits. In particular, decreasing the pH of the solution below 9 can provide increased yield and increased surface area of the silica. As demonstrated in the Examples, the method of the first aspect enables silica particles with significantly greater surface areas than silica particles of the prior art.

[0019] The present inventors have surprisingly recognised that the method of the first aspect can achieve this high rate of reaction even under standard conditions (i.e. room temperature, atmospheric pressure of carbon dioxide). In addition, the method of the first aspect does not require strong inorganic acids such as HC1 to precipitate the silica.

[0020] The inventors have found that the reaction time of the method of the first aspect affects the quality of the precipitated silica. The reaction time must be long enough to enable effective precipitation of the silica. However, prolonged reaction time may result in unfavourable agglomeration or aggregation of the silica, adversely affecting product quality. Preferably the reaction time (i.e. the time for which the solution is exposed to carbon dioxide, or the time from initial exposure of the solution to carbon dioxide to separation of the silica from the solution) is 60 minutes or less, such as 30 minutes or less, or 15 minutes or less. This allows for effective precipitation whilst reducing the amount of agglomeration and / or aggregation of the silica.

[0021] Furthermore, as well as achieving the high rate of reaction and being able to do so under standard conditions, the method of the first aspect does not impact the performance of the silica produced when compared to those prepared by conventional processes. In particular, the silica has a charged surface, which makes them particularly useful for pharmaceutical applications (e.g. to bind pharmaceutically active molecules and / or in controlled release applications). The silica also have a suitable pore size / porosity and surface area.

[0022] The method of the first aspect is highly controllable, which in turn leads to the ability to tightly control the properties of the silica produced.

[0023] The method of the first aspect is also beneficial because the silica can be more readily separated from the solution than conventional processes that require the use of more dilute solutions to provide precise control of the precipitation. This is due to the addition of a gaseous acidifying agent, i.e. carbon dioxide, which does not introduce more water to the reaction mixture, and which therefore avoids any dilution of the formed silica slurry.

[0024] Furthermore, the method of the first aspect has the benefit that it can be used in either batch or continuous (e.g. flow) manufacturing processes. Therefore, the method is more scalable than conventional processes that are not suitable for continuous manufacturing processes. However, the method also benefits from being able to be performed in conventional batch reaction vessels that are readily available.

[0025] In addition, the sodium carbonate formed in the present invention is thought to help to avoid the solution reaching lower pH values that could adversely affect the yield of silica.

[0026] The method of the first aspect is able to be performed without needing to use strong inorganic acids and / or using relatively benign conditions (e.g. atmospheric temperature / pressure). In addition, the method of the first aspect can be performed without organic solvents (e.g. ethanol), excess surfactants, or stoichiometric amounts of metal salts. This can make the method of the first aspect more environmentally benign than conventional methods.

[0027] Furthermore, conventional carbon dioxide-based precipitation technologies are either performed in batch or tubular reactors with gas-liquid slug flow. Tubular reactors with gas-liquid slug flow will lose their advantage during scale-up as the flow regime will change. The present invention preferably uses stirred and / or bubble column reactors that are amenable to scale-up and have significantly more flexibility for manipulating underlying gas-liquid mass transfer and mixing.

[0028] Preferably the silicate is sodium silicate. It will be understood that the polyamine has two or more amine groups. The polyamine may be referred to as an organic polyamine. The polyamine may be an amine of Formula (I):

[0029] Formula (I), wherein each R1, R2and R3is independently represented by H, or Cl -6 alkyl or Cl -6 alkenyl and is optionally substituted by one or more ether, thioether, ester, amide, sulfone, carbamate or urea groups; wherein n represents an integer from 1 to 10; and wherein the or each m represents an integer from 0 to 6. The amine of Formula (I) may specifically be TETA (triethylentetramine) or PEHA (pentaethylenehexamine). The polyamine may alternatively be a poly(ethyleneimine) (PEI) or a poly(allyl amine) (PAA). The amine may be TETA, PEHA, PEI, tetraethylenepentamine (TEPA) or PAA.

[0030] The combination of carbon dioxide and a polyamine, such as pentaethylenehexamine, for the precipitation of silica from silicate is not known. It is particularly surprising that the present inventors have found this combination to have such beneficial effect, especially with regard to the conditions that can be used, the rate of precipitation that can be achieved, and the controllability of the process to control the properties of the silica produced.

[0031] According to a second aspect, the claimed invention provides silica obtainable (e.g. obtained) by the method of the first aspect. The silica may comprise a polyamine of Formula (I) and / or a salt (e.g. hydrogen carbonate salt) thereof, and / or a carbonate salt (e.g. a metal carbonate salt).

[0032] According to a third aspect, the claimed invention provides a use of a polyamine, for example of Formula (I), to increase the rate of precipitation of silica in a method of precipitating silica, wherein the method is as defined by the first aspect. The increase in rate may be observed relative to a method that does not use the polyamine.

[0033] The present application includes the subject-matter of the following clauses:

[0034] 1. A method for producing silica, wherein the method comprises the steps of: providing a solution comprising: a silicate, and an organic polyamine or a salt thereof; and exposing the solution to carbon dioxide. 2. The method of clause 1, wherein the polyamine is an amine of Formula (I):

[0035] Formula (I), wherein: each R1, R2and R3is independently represented by H, or Cl -6 alkyl or Cl -6 alkenyl and is optionally substituted by one or more ether, thioether, ester, amide, sulfone, carbamate or urea groups; n represents an integer from 1 to 10; and the or each m represents an integer from 0 to 6.

[0036] 3. The method of clause 2, wherein the polyamine is TETA (triethylentetramine) or PEHA (pentaethylenehexamine).

[0037] 4. The method of clause 1, wherein the amine is a poly(ethyleneimine) (PEI) or a poly(allyl amine) (PAA).

[0038] 5. The method of any preceding clause, wherein the temperature of the solution and / or the carbon dioxide when the solution is exposed to the carbon dioxide is from 0°C to 50°C.

[0039] 6. The method of clause 5, wherein the temperature is from 10°C to 35 °C.

[0040] 7. The method of any preceding clause, wherein the partial pressure of the carbon dioxide is 50kPa to IMPa.

[0041] 8. The method of clause 7, wherein the partial pressure of the carbon dioxide is from 90kPa to 500kPa.

[0042] 9. The method of any preceding clause, wherein the exposure of the solution to the carbon dioxide is stopped when the pH of the solution becomes 9 or lower.

[0043] 10. The method of clause 9, wherein the exposure of the solution to the carbon dioxide is stopped when the pH of the solution becomes 7 or lower.

[0044] 11. The method of any preceding clause, wherein the concentration of the polyamine in the solution is from O.OlmM to IM.

[0045] 12. The method of any preceding clause, wherein relative molar amount of the silicate in the solution with respect to the molar amount of amine groups in the polyamine is from 3% to 200%.

[0046] 13. The method of any preceding clause, wherein the silicate salt is a metasilicate, orthosilicate or pyrosilicate salt of a group I or group II metal.

[0047] 14. The method of clause 13, wherein the silicate salt is sodium metasilicate.

[0048] 15. The method of any preceding clause, wherein the concentration of the silicate in the solution is from O. lmM to 3M.

[0049] 16. The method of any preceding clause, wherein the step of exposing the solution to carbon dioxide is performed in a continuous stirred tank reactor (CSTR) or a bubble column reactor.

[0050] 17. The method of any preceding clause, wherein the method comprises isolating the silica after the solution has been exposed to the carbon dioxide. 18. The method of clause 17, wherein the method comprises washing the isolated silica.

[0051] 19. Use of a polyamine to increase the rate of precipitation of silica in a method of precipitating silica, wherein the method is as defined by any preceding clause.

[0052] 20. The use of clause 19, wherein the increase in the rate of precipitation is 200% or more, relative to a method that does not use the polyamine.

[0053] 21. Silica obtainable by the method of any one of clauses 1 to 18.

[0054] 22. The silica of clause 21, wherein the silica comprises: a polyamine of Formula (I) and / or a salt thereof, and / or a carbonate salt.

[0055] 23. The silica of clause 21 or 22, wherein the silica has a BET specific surface area of 200 m2 / g or more.

[0056] 24. The silica of any one of clauses 21 to 23, wherein the silica has: a Dx(10) of from 1pm to 50pm, a Dx(50) of from 2pm to 200pm, and a Dx(90) of from 5pm to 300pm.

[0057] 25. The silica of any one of clauses 21 to 24, wherein the silica has a zeta potential of -20 mV or more.

[0058] Detailed Description of the Invention

[0059] The present invention relates to a method of producing silica (i.e., silica particles, or SiCU).

[0060] Providing the solution may include dissolving the silicate and / or the polyamine in the solvent (e.g. water). The solvent of the solution may be an aqueous solvent (i.e. containing water). It will be appreciated that the solution may contain components that are not in solution, although the silicate and the polyamine should normally be dissolved in the solution.

[0061] The solvent may be water (i.e. an aqueous solution), for example deionised water. The solution may contain water in an amount of 50 wt% or more, or 70 wt% or more, or 80 wt% or more, such as 85 wt% or more, preferably 90 wt% or more, or 92 wt% or more, or 94 wt% or more, such as 95 wt% or more, or 96 wt% or more. The solution may contain water in an amount of 99.99 wt% or less, such as 99.9 wt% or less, preferably 99.8 wt% or less, such as 99.7 wt% or less, or 99.5 wt% or less, such as 99.2 wt% or less, such as 99 wt% or less, or 98 wt% or less. The amount of water in the solution may be from 50 wt% to 99.99 wt%, or from 80 wt% to 99.8 wt%, preferably from 90 wt% to 99.5 wt%.

[0062] The solution may comprise the silicate (e.g. sodium metasilicate) in a concentration of O. lmM or more, such as ImM or more, or 2mM or more, preferably 5mM or more, such as lOmM or more, or 15mM or more, or 20mM or more, for example 25mM or more. The concentration of the silicate may be 3M or less, such as 2M or less, or IM or less, for example 800mM or less, or 600mM or less, preferably 400mM or less, or 300mM or less, for example 200mM or less, for example 170mM or less, or 150mM or less. The concentration of the silicate may be from O. lmM to 3M, such as from 5mM to IM, or from 15mM to 400mM, such as 30mM or 60mM or 120mM.

[0063] The solution may comprise the polyamine (e.g. pentaethylenehexamine) in a concentration of 0.0 ImM or more, such as 0.05mM or more, preferably O. lmM or more, for example 0.5mM or more, or ImM or more, for example 2mM or more, or 3mM or more, or 4mM or more. The concentration of the polyamine in the solution may be IM or less, or 500mM or less, such as 250mM or less, preferably lOOmM or less, or 75mM or less, or 50mM or less, such as 40mM or less, or 30mM or less, for example 25mM or less. The concentration of the polyamine in the solution may be from O.OlmM to IM, for example from O. lmM to lOOmM, or from ImM to 50mM, such as 5mM, lOmM or 20mM.

[0064] The solution may contain silicate in a molar amount, relative to the molar amount of the polyamine, of 50% or more, or 100% or more, preferably 200% or more, or 300% or more, or 400% or more, such as 500% or more, such as 550% or more. The relative molar amount of the silicate may be 10,000% or less, such as 5,000% or less, preferably 2,000% or less, such as 1,000% or less, or 800% or less, such as 700% or less, or 650% or less. The relative molar amount of the silicate may be from 50% to 10,000%, such as from 200% to 2,000%, or from 400% to 800%.

[0065] The solution may contain silicate in an amount by weight, relative to the weight of the polyamine, of 50% or more, or 100% or more, preferably 200% or more, or 300% or more, or 400% or more, such as 450% or more, such as 500% or more. The relative amount of the silicate may be 10,000% or less, such as 5,000% or less, preferably 2,000% or less, such as 1,000% or less, or 800% or less, such as 700% or less, or 650% or less, or 600% or less by weight. The relative amount of the silicate may be from 50% to 10,000%, such as from 200% to 2,000%, or from 400% to 800% by weight. The weight of the silicate may be calculated in relation to the hydrate of the silicate salt.

[0066] The present invention can use a significantly lower amount of the polyamine compared to conventional methods, such as that described by CN103785349B. The solution may contain silicate in a molar amount, relative to the molar amount of amines (i.e. amine groups, or nitrogen atoms) in the polyamine, of 0.1% or more, such as 1% or more, such as 3% or more, or 5% or more, such as 10% or more, or 15% or more, preferably 20% or more, or 25% or more, for example 30% or more, or 32% or more, such as 34% or more. The relative molar amount of the silicate, relative to the molar amount of amines (or nitrogen atoms) in the polyamine, may be 400% or less, such as 200% or less, or 150% or less, preferably 100% or less, such as 80% or less, or 60% or less, or 50% or less, such as 45% or less, or 40% or less, for example 38% or less, or 36% or less. The relative molar amount of the silicate may be from 0.1% to 500%, such as from 3% to 200%, or from 10% to 150%, preferably from 20% to 100%, such as from 25% to 60%. The molar amount of amines in the polyamine may be determined by titration.

[0067] The mildly acidic nature of CO2 allows for efficient and highly controllable neutralisation of the pH of the solution, which is otherwise difficult to achieve with strong acids such as HC1 or H2SO4. The flow rate of CO2 can be easily adjusted using a regulator for better and more rapid control of pH. Any excess CO2 will get disengaged in the reactor and will help maintain desired or neutral pH. The solution may be agitated (e.g. stirred) while the solution is exposed to the carbon dioxide.

[0068] The step of exposing the solution to carbon dioxide may be performed in any suitable reactor system. The reactor system may be, or include, a fluidic device. For example, the reactor may include a continuous stirred tank reactor (CSTR), a bubble column reactor, a tubular reactor, a pinched tube, a fluidic oscillator, a vortex diode, a helical coil, and / or a coiled flow inverter. Preferably the solution is exposed to the carbon dioxide in a CSTR or a bubble column reactor. Such CSTR and bubble column reactors do not suffer from gas-liquid slug flow problems associated with tubular reactors. Therefore, CSTR and bubble column reactors are more amenable to scale-up and have significantly more flexibility for manipulating underlying gasliquid mass transfer and mixing than tubular reactors. A stream of carbon dioxide may be passed through the solution, for example the carbon dioxide may be bubbled through the solution. A pump, such as a dosing pump and / or a peristaltic pump, may be used to pump the solution through a reactor system. The reaction may preferably be performed in a CSTR with a tubular reactor (e.g. helical coil) or a bubble column reactor.

[0069] The carbon dioxide is preferably exposed to the solution using one or more spargers, for example a trickle bed and / or a bubble column. The skilled person will appreciate that the rate of addition of carbon dioxide (i.e. mass transfer rate of carbon dioxide) in the reactor can be controlled, for example, by adjusting stirring speed, the number and / or distribution of sparger(s), and / or the design of sparger(s) (e.g. to adjust the bubble size (e.g. the average bubble size and / or the distribution size distribution)). Controlling the rate of mass transfer of carbon dioxide allows the rate of neutralisation of the solution, and therefore the rate of precipitation of the silica particles, to be controlled.

[0070] Figure 1 of the accompanying drawings shows a process flow diagram of silica synthesis that can be used to implement the claimed invention. The system includes CO2 gas cylinder 1, gas regulator 2, feed tank 3 that contains an aqueous solution of sodium silicate and pentaethylenehexamine, dosing pump 4, reactor 5 that is a CSTR or a bubble column reactor, pH probe 6, temperature probe 7, peristaltic pump 8, tubular reactor 9 and product collection tank 10. In some embodiments, tubular reactor 9 is optional.

[0071] It will be appreciated that the method of the present invention can work with carbon dioxide at around atmospheric pressure. However, the skilled person will appreciate that other pressures of carbon dioxide could be successfully used. The partial pressure of the carbon dioxide may be 50kPa or more, such as 70kPa or more, or 80kPa or more, preferably 90kPa or more, or 95kPa or more, such as lOOkPa or more, or HOkPa or more, or 120kPa or more, for example 150kPa or more, or 200kPa or more. The partial pressure of carbon dioxide may be IMPa or less, such as 800kPa or less, preferably 500kPa or less, such as 300kPa or less, or 200kPa or less, for example 150kPa or less, or 120kPa or less. The partial pressure of carbon dioxide may be from 50kPa to IMPa, such as from 50kPa to 500kPa, or from 90kPa to 500kPa, or from 95kPa to 200kPa.

[0072] The temperature of the solution and / or the carbon dioxide when the solution is exposed to the carbon dioxide may be around room temperature. The temperature of the solution, carbon dioxide and / or silica particles during the method may be around room temperature. The temperature may be 0°C or more, such as 5°C or more, preferably 10°C or more, or 15°C or more, such as 20°C or more. The temperature may be 50°C or less, such as 40°C or less, preferably 35°C or less, such as 30°C or less, such as 25°C or less. The temperature may be from 0°C to 50°C, such as from 10°C to 35°C, for example from 20°C to 25°C, for example from 20°C to 25°C.

[0073] The length of time the solution is exposed to carbon dioxide and / or the length of time between the solution being initially exposed to carbon dioxide and the silica being separated from the solution should be long enough to ensure that precipitation occurs and to provide a significant yield of silica, but not so long as to cause agglomeration and / or aggregation. The solution may be exposed to carbon dioxide for a period of time of 60 minutes or less, such as 30 minutes or less, preferably 15 minutes or less, such as 10 minutes or less. The period of time may be 30 seconds or more, such as 1 minute or more, or 2 minutes or more, or 4 minutes or more, such as 5 minutes or more. The period of time may be from 30 seconds to 60 minutes, such as from 2 minutes to 15 minutes.

[0074] The method may comprise monitoring the pH of the solution during the exposure of the solution to the carbon dioxide. The pH of the solution will decrease as it is exposed to the carbon dioxide. The solution may be exposed to carbon dioxide until the pH of the solution becomes substantially constant (e.g. stops decreasing). The solution may be exposed to carbon dioxide until the pH of the solution becomes within a desired range. For example, the flow of carbon dioxide through the solution may be stopped (or the solution may stop being exposed to the carbon dioxide) when the pH of the solution becomes within the desired range. The range may be 9 or lower, especially below 9, such as 8.5 or lower, or 8.2 or lower, or 8 or lower, or 7.5 or lower, such as 7 or lower, for example 6.8 or lower, or 6.6 or lower, for example 6.5 or lower. The range may be from 9 to 2, such as from 9 to 3, or from 9 to 3.6, or from 9 to 4, or from 9 to 5, such as from 9 to 6, or from 9 to 6.2, such as from 9 to 6.4. The range may be from 9 to 4, or from 4 to 8.5 (e.g. from 6 to 8.5), or from 8.2 to 4 (e.g. from 6 to 8.2), such as from 7 to 5, or from 7 to 6. The range may be from 9 to 4.5, such as from 8.5 to 4.5 (e.g. from 8.5 to 6), or from 8.2 to 4.5 (e.g. from 8.2 to 6), such as from 7 to 5, or from 7 to 6. pH values below 9 provide higher yield of silica and higher silica surface area.

[0075] In one embodiment, the temperature of the solution and / or the carbon dioxide when the solution is exposed to the carbon dioxide may be from 0°C to 50°C (e.g. from 10°C to 35°C); the solution may be exposed to carbon dioxide and / or the length of time between the solution being initially exposed to carbon dioxide and the silica being separated from the solution for a period of time of 60 minutes or less (e.g. from 2 minutes to 15 minutes); and the solution is exposed to carbon dioxide until the pH of the solution becomes below 9, such as from pH of the solution during the exposure of the solution to the carbon dioxide may be 9 or lower (e.g. from 8.2 to 4, or from 8.2 to 4.5).

[0076] The increase in rate may be observed relative to a method that does not use the polyamine. The rate of precipitation, relative to a method that does not use the polyamine, may be more than 100%, such as 110% or more, or 120% or more, for example 150% or more, or 200% or more, such as 400% or more, or 600% or more, such as 1000% or more. The rate may be determined by calculating the weight of silica that precipitates over a given timeframe.

[0077] The exposure of the solution to the carbon dioxide causes silica particles to precipitate from the solution, forming a slurry of silica. The silica slurry can be passed through reactors such as a tubular reactor and / or a fluidic oscillator to allow the silica particles to grow further.

[0078] The precipitated silica may be separated from the liquid phase / solution (e.g. isolated). The silica- containing slurry may be subjected to filtration and / or centrifugation to remove the liquid phase and isolate the silica. The silica may be washed, for example to remove salts, for example using water (e.g. deionised water). The silica (e.g. after being washed) may be dried. The slurry and / or the (isolated) silica may be exposed to an acidic agent (e.g. HC1 and / or sulfuric acid) to remove the organic polyamine “template”, prior to optionally being centrifuged, washed and / or dried to obtain purified silica. The polyamine may, alternatively or additionally, be removed by calcination.

[0079] The silica or the slurry thereof may be treated with an acidic agent (e.g. HC1 and / or sulfuric acid) to remove the organic polyamine and / or achieve desired properties, such as zeta potential and / or surface area, for example as described in WO 2017 / 037460 Al.

[0080] Polyamine

[0081] It will be understood that the polyamine has two or more amine groups. The polyamine may be referred to as an organic polyamine. The choice of polyamine may influence the surface area, porosity, and / or zeta potential of the silica. As such the polyamine may be chosen to influence these parameters.

[0082] The polyamine may be an amine of Formula (I). Formula (I) is represented by the following structure :

[0083] Formula (I); wherein: each R1, R2and R3is independently represented by H, or Cl -6 alkyl or Cl -6 alkenyl and is optionally substituted by one or more ether, thioether, ester, amide, sulfone, carbamate or urea groups; n represents an integer from 1 to 10; and the or each m represents an integer from 0 to 6.

[0084] Preferably each R1, R2and R3is not substituted. Thus, preferably each R1, R2and R3is independently represented by H, or Cl-6 alkyl or Cl-6 alkenyl. Each R1, R2and R3may be independently represented by H, or Cl -4 alkyl or Cl -4 alkenyl; for example H, or Cl -3 alkyl or Cl -3 alkenyl; more preferably H, or Cl -2 alkyl or Cl -2 alkenyl; or H or Cl alkyl; most preferably each R1, R2and R3is represented by H. Preferably each R1group is the same. Preferably each R2group is the same. Preferably each R3group is the same. n may represent an integer from 1 to 8, such as from 1 to 7, or from 1 to 6, for example from 1 to 5. n may represent an integer from 2 to 10, or from 3 to 10, such as from 4 to 10, or from 5 to 10. n may represent an integer from 2 to 8, such as from 3 to 7, or from 4 to 6. Most preferably, n is 5.

[0085] The or each m may represent an integer from 0 to 5, such as from 0 to 4, or from 0 to 3, preferably from 0 to 2, such as 0 or 1. The or each m may represent an integer from 1 to 5, such as from 1 to 4, or from 1 to 3, preferably 1 or 2. Most preferably, m is 1.

[0086] The polyamine of Formula (I) may be TETA (triethylentetramine) or PEHA (pentaethylenehexamine). Further examples of suitable polyamines include bis(3- aminopropyl)amine, bis(3-dimethylaminopropyl)amine, spermidine and spermine. Most preferably the polyamine is PEHA.

[0087] The polyamine may alternatively be a poly(ethyleneimine) (PEI) or a poly(allyl amine) (PAA). The amine may be TETA, PEHA, PEI, tetraethylenepentamine (TEPA) or PAA.

[0088] It may be that: each R1, R2and R3is independently represented by H, or Cl -6 alkyl or Cl -6 alkenyl; and n represents an integer from 2 to 8; and m represents an integer from 0 to 4; or that each R1, R2and R3is independently represented by H, or Cl -3 alkyl or Cl -3 alkenyl; and n represents an integer from 3 to 7; and m represents an integer from 0 to 3; or that each R1, R2and R3is independently represented by H, or Cl -3 alkyl or Cl -3 alkenyl; and n represents an integer from 3 to 7; and m represents an integer from 0 to 3; or that each R1, R2and R3is independently represented by H or Cl alkyl (preferably H); and n represents an integer from 4 to 6 (preferably 5); and m represents an integer from 0 to 2 (preferably 1).

[0089] Silicate

[0090] The solution includes a silicate, preferably a silicate salt. Silicates include metasilicate (SiOr ). orthosilicate (SiO ) and pyrosilicate (Si2C>76') salts. Preferably the silicate is a metasilicate.

[0091] The silicate may be a silicate salt, for example an inorganic silicate salt, i.e. a metal silicate salt. The metal may be of group I or group II, preferably group I, for example the salt may be a group I metasilicate. The metal may be lithium, sodium or potassium. Preferably the metal is sodium. Most preferably the silicate is sodium metasilicate. Other possible silicates include TEOS (tetraethyl orthosilicate), alkoxy silanes (e.g. TMOS - tetramethyl orthosilicate), diol- modified silanes such as tetrakis(2-hydroxyethoxy)silane, and organic complexes of silicon (e.g. hexavalent catechol complex).

[0092] The silicate salt may be a metasilicate, orthosilicate or pyrosilicate salt of a group I or group II metal.

[0093] Silica Particles

[0094] Preferably the silica particles are microporous.

[0095] Samples of the silica of the invention where the polyamine has not been removed tend to have a low BET specific surface area (SSA). The silica particles may have a BET SSA of 5 m2 / g or more, such as 10 m2 / g or more, or 15 m2 / g or more, for example 20 m2 / g or more. The BET SSA may be 100 m2 / g or less, such as 60 m2 / g or less, for example 50 m2 / g or less, or 45 m2 / g or less, such as 40 m2 / g or less. The BET SSA may be from 5 to 100 m2 / g, such as from 10 to 50 m2 / g, or from 20 to 40 m2 / g.

[0096] Samples of the silica of the invention where the polyamine has been removed have a high BET surface area. The silica particles may have a BET SSA of 200 m2 / g or more, such as 300 m2 / g or more, such as 340 m2 / g or more, or 350m2 / g or more, for example 375 m2 / g or more, or 400 m2 / g or more, such as 410 m2 / g or more, or 415 m2 / g or more, for example 420 m2 / g or more, 450 m2 / g or more, or 480 m2 / g or more, such as 500 m2 / g or more. The silica particles may have a BET SSA of 600 m2 / g or less, such as 550 m2 / g or less, or 520 m2 / g or less, or 500 m2 / g or less, for example 475 m2 / g or less, or 450 m2 / g or less, or 430 m2 / g or less. The silica particles may have a BET SSA of from 200 to 600 m2 / g, preferably from 300 to 600 m2 / g, such as from 350 to 500 m2 / g, or from 400 to 450 m2 / g. It is noted that WO 2017 / 037460 Al discloses BET SSA values of below 340 m2 / g. BET SSA may be measured using Micromeritics® TriStar II Plus 3030 nitrogen adsorption equipment.

[0097] The silica particles may be present as primary particles (i.e. crystals) or secondary particles (i.e. aggregates). The formation of aggregates may be facilitated by downstream processes such as acid treatment, washing, centrifugation and drying.

[0098] Even despite any acid treatment and / or washing steps, the silica particles may contain carbonate (e.g. sodium carbonate) and / or the polyamine of Formula (I) or a salt thereof. It would be difficult to remove absolutely every trace of the carbonate produced from the carbon dioxide and / or the remaining polyamine template. These components may each individually be present in a trace amount or more, for example in an amount of O. lppb or more, e.g. Ippb or more, such as lOppb or more, or lOOppb or more, or Ippm or more, and / or lOppm or less, such as lOOppm or less by weight.

[0099] Particle size (e.g. diameter) parameters may be determined using laser diffraction, for example using a Mastersizer 3000 (Malvern Panalytical Ltd). The reported size values may correspond to the size of aggregates. As such, the size of primary particles can be much smaller.

[0100] The Dx(10) of the silica particles may be 1pm or more, such as 2pm or more, or 3 pm of more. The Dx(10) of the silica particles may be 50 pm or less, such as 30 pm or less, or 20 pm or less, such as 15 pm or less, or 12 pm or less, for example 11pm or less, or 10 pm or less. For example, the Dx(10) of the silica may be from 1pm to 50pm, or from 2pm to 15pm, such as from 3pm to 10pm. Where the reactor system includes a CSTR, the Dx(10) may be 8pm or less, such as 6pm or less, for example 5pm or less, or 4pm or less. Where the reactor system includes a CSTR, the Dx(10) may be from 1pm to 8pm, such as from 2pm to 6pm, or from 3pm to 5pm.

[0101] The Dx(50) of the silica particles may be 2pm or more, such as 5pm or more, such as 6pm or more, or 7pm or more, or 8pm or more. The Dx(50) of the silica particles may be 200pm or less, such as 150pm or less, or 120 pm or less, for example 100pm or less, or 80pm or less, for example 70pm or less. The Dx(50) of the silica particles may be from 2pm to 200pm, such as from 5pm to 100pm, or from 7pm to 80pm. Where the reactor system includes a CSTR, the Dx(50) may be 50pm or less, such as 40pm or less, or 30 pm or less, or 20pm or less, for example 15pm or less, or 12pm or less. Where the reactor system includes a CSTR, the Dx(50) may be from 2pm to 50pm, such as from 5pm to 30pm, or from 7pm to 15pm.

[0102] The Dx(90) of the silica particles may be 5 pm or more, such as 10pm or more, or 12 pm or more, or 15pm or more, such as 18pm or more, or 20pm or more. The Dx(90) of the silica particles may be 300pm or less, such as 250pm or less, or 200pm or less, such as 150pm or less. The Dx(90) of the silica particles may be from 5pm to 300pm, such as from 10pm to 200pm, or from 18pm to 150pm. Where the reactor system includes a CSTR, the Dx(90) may be 100pm or less, such as 80pm or less, or 60pm or less, for example 50pm or less, or 40pm or less, such as 35pm or less, or 30pm or less. Where the reactor system includes a CSTR, the Dx(90) may be from 5pm to 100pm, such as from 10pm to 40pm, or from 18pm to 35pm.

[0103] The surface area moment mean (i.e. D[3, 2]) of the silica particles may be 1pm or more, such as 2pm or more, or 3pm or more, for example 4pm or more. The surface area moment mean of the silica particles may be 50pm or less, such as 40pm or less, or 30pm or less, or 20pm or less, for example 15pm or less, or 12pm or less, such as 10pm or less. The surface area moment mean of the silica particles may be from 1pm to 50pm, for example from 2pm to 20pm, or from 3pm to 15pm, such as from 2pm to 12pm.

[0104] The volume moment mean (i.e. D[4, 3]) of the silica particles may be 2pm or more, such as 4pm or more, or 6pm or more, or 8pm or more, for example 9pm or more, or 10 pm or more. The volume moment mean of the silica particles may be 150pm or less, such as 130pm or less, or 110pm or less, or 100pm or less, for example 90pm or less, or 80pm or less. The volume moment mean of the silica particles may be from 2pm to 150pm, or from 4pm to 110pm, such as from 8pm to 90pm. Where the reactor system includes a CSTR, the volume moment mean may be 60pm or less, such as 50pm or less, or 40pm or less, for example 30pm or less, or 25pm or less, or 20pm or less. Where the reactor system includes a CSTR, the volume moment mean may be from 2pm to 60pm, for example from 4pm to 40pm, or from 8pm to 25pm.

[0105] Two or more of the Dx(10), the Dx(50), the Dx(90), the surface area moment mean and the volume moment mean may be used to define the particles. For example, the particles may have: a Dx(10) of from 1pm to 50pm (e.g. from 2pm to 15pm), a Dx(50) of from 2pm to 200pm (e.g. from 5pm to 100pm), and a Dx(90) of from 5pm to 300pm (e.g. from 10pm to 200pm); or a Dx(10) of from 3pm to 10pm, a Dx(50) of from 7pm to 80pm, and a Dx(90) of from 18pm to 150pm; or a surface area moment mean of from 1pm to 50pm (e.g. from 3pm to 15pm) and a volume moment mean of from 2pm to 150pm (e.g. from 4pm to 110pm); or a surface area moment mean of from 2pm to 12pm and a volume moment mean of from 8pm to 90pm; or a Dx(10) of from 1pm to 50pm (e.g. from 2pm to 15pm), a Dx(50) of from 2pm to 200pm (e.g. from 5pm to 100pm), a Dx(90) of from 5pm to 300pm (e.g. from 10pm to 200pm), a surface area moment mean of from 1pm to 50pm (e.g. from 3pm to 15pm), and a volume moment mean of from 2pm to 150pm (e.g. from 4pm to 110pm); or a Dx(10) of from 3pm to 10pm, a Dx(50) of from 7pm to 80pm, a Dx(90) of from 18pm to 150pm, a surface area moment mean of from 2pm to 12pm, and a volume moment mean of from 8pm to 90pm.

[0106] Samples of the silica of the invention where the polyamine has not been removed tend to have a relatively high zeta potential. The zeta potential of the silica particles may be -20 mV or more, such as -15mV or more, or -12mV or more, or -lOmV or more, such as -9mV or more. The zeta potential of the silica particles may be 2mV or less, such as ImV or less, preferably OmV or less, such as -0.5mV or less, or -l .OmV or less, such as -1.5mV or less, or -2.0mV or less. The zeta potential of the silica particles may be from -20mV to 2mV, such as from -12mV to OmV, or from -lOmV to -0.5mV, for example from -lOmV to -1.5mV. The zeta potential range may increase further by using other amine templates, as discussed in WO 2017 / 037460 Al .

[0107] Samples of the silica of the invention where the polyamine has been removed (e.g. by acid wash) tend to have a relatively low zeta potential. The zeta potential of silica particles from which the polyamine has been removed may be -40mV or more, such as -35mV or more, or -30mV or more, such as -28mV or more. The zeta potential of silica particles from which the polyamine has been removed may be 2mV or less, such as OmV or less, -2mV or less, -lOmV or less, or -15mV or less, for example -18mV or less. The zeta potential of silica particles from which the polyamine has been removed may be from -40 to OmV, such as from -35 to -2mV.

[0108] Examples

[0109] Dried samples of silica were analyzed in Quantachrome AUTOSORB AS-1 or Micromeritics® TriStar II Plus 3030 nitrogen adsorption equipment for surface area measurements. Microporous analysis was selected and Rouquerol criteria were used for selecting the appropriate pressure range for the BET data analysis.

[0110] Example 1 : Comparative Example using HC1 (Batch Mode)

[0111] Synthesis: 2.132 mb of sodium metasilicate pentahydrate solution (0.703 M) and 2.052 mb of pentaethylenehexamine (0.122 M) solution were added to a plastic jar (Corning® Gosselin™ Straight Container, 180 mL), and 42 mb of water was added. Maintain stirring at 500 RPM and insert a pre-calibrated pH probe and start pH meter and data acquisition using EasyDirect pH software. One-shot (3.68 mL) of 1.0 M hydrochloric acid was added using a 5 mL micropipette. The change in pH over time was recorded. The pH stabilized at 7 ± 0.05 after 5 min.

[0112] Work-up: 1.0 M hydrochloric acid (~1.2 mL) was added to lower the pH to 2.0, to extract the amine. This was stirred for 15-20 min before being centrifuged at 4400 RPM for 4-5 min. Silica cake was washed at least 3-4 times with 50 mL DI water each time. A spatula was used to break the silica cake and a vortex mixer was used to resuspend the slurry. The conductivity of the supernatant was below 5 pS / cm after the final wash. The cake was resuspended in 15 mL DI water using vortex mixer and / or ultrasound bath. 5 mL of the resultant slurry was withdrawn for mastersizer / zetasizer analysis. The remaining slurry was spread on the petri dish and the water was allowed to evaporate at ambient conditions. The sample on the petri dish was dried in an oven at 70°C. Example 2: Use of CO2 as acidifying agent (Semi-Batch Mode)

[0113] Synthesis: 2.132 mL of sodium metasilicate pentahydrate solution (0.703 M) and 2.052 mL of pentaethylenehexamine (0.122 M) solution were added to a plastic jar (Corning® Gosselin™ Straight Container, 180 mL), and 42 mL of water was added. The solution was stirred at 500 RPM. A pre-calibrated pH probe was inserted; data acquisition was performed using EasyDirect pH software. Dry ice was stored in a squeeze bottle and the outlet nozzle was connected with the silicon tube dipped in the reaction mixture. The gas bubbled through the reaction mixture for 300 s and the pH of the reaction mixture decreased with time. The rate of CO2 addition was adjusted to control the rate of change of the pH. The pH attained a constant value and did not decrease further even after purging more CO2.

[0114] Work-up: 5 mL reaction mass sample was taken before the centrifuge / washing step for mastersizer analysis. The silica cake was washed with DI water at least 4 times with ~50 mL DI water each washing cycle. The cake was broken with a spatula and the slurry was mixed using a vortex mixer before centrifuging. The centrifuge conditions were 4 min, 4400 RPM and 5-15°C. The conductivity of the supernatant was below 5 pS / cm after final wash. After final washing, 15 mL of DI water was added to the cake and the lump was broken with spatula and subjected to sonication bath for ~3 min. 5 mL of the slurry was taken for the Mastersizer / zetasizer analysis and remaining slurry was spread on a Petri dish for drying. The water was evaporated overnight, and the petri dish was kept in oven at 70°C for more than 1-2 days.

[0115] Figure 2 of the accompanying drawings shows the change in pH over the course of experiments using the protocols described in Examples 1 and 2.

[0116] Figure 2A specifically compares the pH profile of HC1 vs. CO2 as the acidic agent. It can be seen that CO2 experiment reaches the reaction endpoint at pH 7.0 in almost half the time compared to the HC1 experiment. This can significantly affect the production time for a fixed capacity in batch mode or reactor volume for a fixed capacity in continuous mode. In addition, there is an initial steep decrease in the pH of the experiment using HC1, whereas the decrease was more controlled when CO2 was used. This shows that the use of CO2 can more carefully control the decrease of pH of the solution.

[0117] Figure 2B specifically compares the effect of the rate of CO2 addition on the pH of the solution. Increasing the CO2 addition rate increases the rate at which the pH of the solution decreases. This can be used to tailor characteristics of the silica, for example the particle size distribution and possibly total surface area. Analysis of Silica Samples from Examples 1-2

[0118] The particle size (diameter) distribution was measured using Mastersizer 3000 (Malvern Panalytical Ltd). The silica slurry was suspended using vortex mixer and ultrasound bath (2-3 min) before injecting the sample. 1 m of the sample was injected for analysis and measurements were taken at least 4 times per sample.

[0119] Figure 3 of the accompanying drawings shows particle size distributions (PSDs) of the silica of Examples 1 and 2.

[0120] The PSDs suggests a bimodal distribution that can be attributed to aggregated particles or secondary nucleation. Figure 3A shows the comparison of different acids (HC1 and CO2). Figure 3B shows comparison of PSD with fast and slow addition rate of CO2.

[0121] Figure 4 of the accompanying drawings shows the diameter parameters corresponding to Figure 3. Figure 4A shows the comparison of different acids (HC1 and CO2). Figure 4B shows comparison of PSD with fast and slow addition rate of CO2.

[0122] It can be seen that the PSD for carbon dioxide at the high rate of addition is similar to the PSD for the comparative experiment using HC1.

[0123] However, the addition rate of CO2 was found to affect the pH profile, allowing for the particle diameter to be tailored. In particular, a slower rate of addition of CO2 provided larger particle sizes.

[0124] Example 3: Semi-Batch Experiment using CO2 gas

[0125] 5.0 g of sodium metasilicate pentahydrate (0.024 mol) and 0.913 g of pentaethylenehexamine (0.004 mol) were dissolved in 783 mb of deionized water to obtain a solution of 30 mM and 5 mM respectively. The resulting solution was stirred in a 1000 mb beaker using a magnetic stirrer. CO2 gas was purged in this solution and pH was measured continuously. Purging with CO2 was stopped when pH reached a constant value (slightly below 7). Half of the reaction mixture was immediately centrifuged, washed, and dried to obtain silica particles. The other half was treated with hydrochloric acid (pH ~ 2) to remove the amine template. The resulting silica slurry was centrifuged, washed, and dried to obtain silica particles.

[0126] Figure 5 of the accompanying drawings shows the pH profile of the reaction under semi-batch conditions. It can be seen that the pH reaches the desired level after around 220 seconds. Example 4: Continuous Experiment using Fluidic Oscillator and Helical Coil in series

[0127] 6.0 g of sodium metasilicate pentahydrate (0.028 mol) and 1.096 g of pentaethylenehexamine (0.005 mol) were dissolved in 939 mL of deionized water to obtain a solution of 30 mM and 5 mM respectively. The solution was prepared in a 1000 mL bottle which was also used as feed storage. The solution was pumped at a flow rate of 10 mL / min using a dosing pump. The solution was mixed with CO2 in a cross-mixer and passed through a fluidic oscillator (~ 40mL) under recirculation using a peristaltic pump operated at 115 RPM. The reaction mixture then passed through a 60 mL helical coiled reactor. An annular flow regime was obtained at a higher gas flowrate. The product was collected in a stirred beaker. The residence time of the liquid was a few seconds, and the outlet pH was below 7. The product was collected for ~ 45 min and was subjected to hydrochloric acid treatment (pH ~ 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles.

[0128] Example 5: Continuous Experiment using CSTR at Low Concentration

[0129] 10.0 g of sodium metasilicate pentahydrate (0.047 mol) and 1.826 g of pentaethylenehexamine (0.008 mol) were dissolved in 1565 mL of deionized water to obtain a solution of 30 mM and 5 mM respectively. The solution was prepared in a 1000 mL bottle(s) which was also used as feed storage. The solution was pumped at a flow rate of 10 mL / min using a dosing pump into a 100 mL CSTR. CO2 gas was sparged in the CSTR and the two steady-state product samples were collected for 50 min each. The first sample was directly centrifuged, washed, and dried to obtain silica particles. The second sample was subjected to hydrochloric acid treatment (pH < 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles.

[0130] Figure 6 of the accompanying drawings shows the pH profile of the reaction in a CSTR. It can be seen that the pH reaches the desired level after around 1800 seconds.

[0131] Example 6: Continuous Experiment using CSTR at High Concentration

[0132] 25.0 g of sodium metasilicate pentahydrate (0.118 mol) and 4.565 g of pentaethylenehexamine (0.02 mol) were dissolved in 968 mL of deionized water to obtain a solution of 120 mM and 20 mM respectively. The solution was prepared in a 1000 mL bottle(s) which was also used as feed storage. The solution was pumped at a 20 mL / min flow rate using a dosing pump into a 100 mL CSTR resulting in a residence time of 5 min. CO2 gas was sparged in the CSTR and the two steady-state product samples were collected for 50 min each. The first sample was directly centrifuged, washed, and dried to obtain silica particles. The second sample was subjected to hydrochloric acid treatment (pH < 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles. Figure 7 of the accompanying drawings shows the pH profile of the reaction in a CSTR at higher concentration. It can be seen that the pH reaches the desired level after around 900 seconds.

[0133] Example 7: Continuous Experiment using CSTR and tubular reactor in series at Medium Concentration

[0134] This Example was performed in the apparatus illustrated in Figure 1.

[0135] 20.0 g of sodium metasilicate pentahydrate (0.094 mol) and 3.652 g of pentaethylenehexamine (0.02 mol) were dissolved in 1560 mb of deionized water to obtain a solution of 60 mM and 10 mM respectively. The solution was pumped at a 16 mL / min flow rate using a dosing pump into a CSTR and helical coiled reactor in series (total volume = 160 mb) resulting in a residence time of 10 min. CO2 gas was sparged in the CSTR and the slurry passed through the helical coil and the two steady-state product samples were collected for 50 min each. The first sample was directly centrifuged, washed, and dried to obtain silica particles. The second sample was subjected to hydrochloric acid treatment (pH < 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles.

[0136] Figure 8 of the accompanying drawings shows the pH profile for CSTR and helical coil in series at medium concentration. It can be seen that the pH reaches the desired level after around 1800 seconds.

[0137] Analysis of Silica Samples from Examples 3-7

[0138] Figure 9 of the accompanying drawings shows the adsorption and desorption isotherm of the silica sample obtained in the acid-treated sample of Example 5. The isotherm suggests that the particles have micropores.

[0139] Figures 10 and 11 of the accompanying drawings show the BET plot and Rouquerol plot respectively. The BET surface area of the sample was 424 m2 / g, which is higher than the values reported in WO 2017 / 037460 Al.

[0140] Figure 12 of the accompanying drawings shows SEM images of the acid-treated silica particles produced in Example 1. It can be seen from the images that particles are present as aggregates. Aggregates are formed likely due to the downstream process of acid treatment, washing, centrifugation, and drying. Figure 13 of the accompanying drawings shows the particle size distribution of the silica prepared by Examples 1-5.

[0141] Figure 14 of the accompanying drawings compares the average particle diameter of certain percentile ranges and the surface area and volume moment means for silica of Examples 1-5. Table 1 shows the zeta potential values of the non-HCl treated particles.

[0142] Table 1 : Zeta potential for silica (without HC1 treatment)

[0143] Example 8: Continuous Experiment using bubble column reactor at medium concentration with a CO2 flowrate of 0.5 L / min

[0144] Stock solutions of sodium metasilicate pentahydrate (1.0 M) and pentaethylenehexamine (0.166 M) were prepared in deionized water. These stock solutions were used to prepare feed solution by mixing 120 mb each of sodium silicate and pentaethylenehexamine and diluting it with deionized water to obtain 2 L of final volume. This resulted in the final concentration of 60 mM and 10 mM of sodium silicate and pentaethylenehexamine respectively. The feed solution was pumped at a flowrate of 20 mL / min using a dosing pump into a bubble column reactor (diameter = 67 mm, active volume = 200 mL) resulting in a residence time of 10 min. CO2 gas was sparged into the reactor using an air stone sparger. The gas flowrate was controlled at 0.5 L / min using a digital gas flow meter (SMC PFM725S-C6-A-W). Two steady-state samples were collected for 30 min each. The first sample was directly centrifuged, washed, and dried to obtain silica particles. The second sample was subjected to hydrochloric acid treatment (pH ~ 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles.

[0145] Example 9: Continuous Experiment using bubble column reactor at medium concentration with a CO2 flowrate of 1.0 L / min

[0146] Stock solutions of sodium metasilicate pentahydrate (1.0 M) and pentaethylenehexamine (0.166 M) were prepared in deionized water. These stock solutions were used to prepare feed solution by mixing 120 mL each of sodium silicate and pentaethylenehexamine and diluting it with deionized water to obtain 2 L of final volume. This resulted in the final concentration of 60 mM and 10 mM of sodium silicate and pentaethylenehexamine respectively. The feed solution was pumped at a flowrate of 20 mL / min using a dosing pump into a bubble column reactor (diameter = 67 mm, active volume = 200 mL) resulting in a residence time of 10 min. CO2 gas was sparged into the reactor using an air stone sparger. The gas flowrate was controlled at 1.0 L / min using a digital gas flow meter (SMC PFM725S-C6-A-W). Two steady-state samples were collected for 15 min each. The first sample was directly centrifuged, washed, and dried to obtain silica particles. The second sample was subjected to hydrochloric acid treatment (pH ~ 2) to remove the amine template. The silica slurry was further centrifuged, washed, and dried to obtain silica particles.

[0147] Figure 15 of the accompanying drawings shows the yield of synthesized silica obtained in Examples 4, 5, 7-9. Examples 4 and 5 achieved a yield of approximately 55%, Example 9 achieved a yield of approximately 62%, and Examples 7 and 8 achieved a yield of approximately 70%. This shows that the invention works well with a tubular reactor (using a helical coiled reactor) or a CSTR, that the invention works even better with a bubble tank reactor or the combination of a CSTR with a tubular reactor. Therefore, different apparatuses can be used to perform the present invention.

[0148] Analysis of Silica Samples from Examples 3-9

[0149] The BET surface area was determined for the silica samples obtained from Examples 3-9.

[0150] Figure 16A of the accompanying drawings shows the BET surface area of silica samples (pH = 7) from Examples 5-9 without acid treatment. For the pH 7 samples, Examples 5 and 7 each had a BET surface area of about 20-25 m2 / g; Examples 8 and 9 had a BET surface area of about 30- 35 m2 / g; and Example 6 had a BET surface area of about 35-40 m2 / g.

[0151] This shows that the samples had a relatively low surface area before acidification to remove the template.

[0152] Figure 16B of the accompanying drawings shows the BET surface area of silica samples (pH = 2) from Examples 3-9 following acid treatment to remove the amine template. For the pH 2 samples, Example 4 had a BET surface area of about 380 m2 / g; the BET surface area of Examples 3 and 6 was slightly higher at about 400-450 m2 / g; the BET surface area of Examples 7 and 9 was higher again at about 450-500 m2 / g; and the BET surface area of Examples 5 and 8 was highest at about 500-550 m2 / g. This shows that the samples of the invention that have been acidified during workup, to remove the template, have a surprisingly high surface area. A higher concentration of the silica precursor decreased the surface area slightly (comparing Examples 5 and 6).

[0153] The zeta potential was determined for the silica samples obtained from Examples 3-9.

[0154] Zeta potential along with surface area are important critical quality attributes for porous silica application in drug delivery systems. Zeta potential is an important material property for understanding colloidal stability and drug delivery systems. Furthermore, zeta potential can influence cellular uptake, and drug release kinetics and is useful for targeted drug delivery. Zeta potential can be tailored by using different amine templates and / or partial removal of templates from the silica pores post-synthesis by pH adjustment.

[0155] Figure 17 of the accompanying drawings shows the zeta potential of synthesized silica samples from Examples 3-9. The zeta potential of the pH 7 samples ranged from about -10 (Example 3) to about -2 (Example 8). The zeta potential of the acidified (pH 2) samples ranged from about -28 mV (Examples 8 and 9) to about -18mV (Examples 6 and 7). Therefore, the zeta potential of the particles decreased (i.e. became more negative) after the particles were acidified in the workup.

[0156] Figure 18 of the accompanying drawings shows the SEM images of synthesized silica from Example 8. Figure 18 shows that the silica formed agglomerated particles.

[0157] The shape of the primary particle in Figure 18 is spherical and the size is a few nanometres. However, the primary particles aggregate into larger secondary particles and further agglomerate into ternary particles of a few microns in size. The agglomeration depends on the solution pH and the surface charge or zeta potential.

[0158] RECTIFIED SHEET (RULE 91) ISA / EP

Claims

CLAIMS1. A method for producing silica, wherein the method comprises the steps of: providing a solution comprising: o a silicate, and o an organic polyamine or a salt thereof; and exposing the solution to carbon dioxide.

2. The method of claim 1, wherein the solution is exposed to carbon dioxide until the pH of the solution is below 9.

3. The method of claim 2, wherein the solution is exposed to carbon dioxide until the pH of the solution is from 6 to 8.5.

4. The method of any preceding claim, wherein the polyamine is an amine of Formula (I):Formula (I), wherein: each R1, R2and R3is independently represented by H, or C l -6 alkyl or C l- 6 alkenyl and is optionally substituted by one or more ether, thioether, ester, amide, sulfone, carbamate or urea groups; n represents an integer from 1 to 10; and the or each m represents an integer from 0 to 6.

5. The method of any preceding claim, wherein the organic polyamine is selected from the list consisting of triethylentetramine, pentaethylenehexamine (PEHA), poly(ethyleneimine), tetraethylenepentamine (TEPA) and poly(allyl amine).

6. The method of claim 5, wherein the organic polyamine is PEHA.

7. The method of any preceding claim, wherein the molar amount of the silicate relative to the molar amount of amine groups is from 20% to 100%.

8. The method of any preceding claim, wherein the solution is exposed to the carbon dioxide for 30 minutes or less.

9. The method of any preceding claim, wherein the temperature of the solution and / or the carbon dioxide when the solution is exposed to the carbon dioxide is from 10°C to 35°C.

10. The method of any preceding claim, wherein the partial pressure of the carbon dioxide is from: a) 50kPa to 500kPa; or b) 90kPa to 500kPa.1 1. The method of any preceding claim, wherein the silicate salt is a metasilicate, orthosilicate or pyrosilicate salt of a group I or group II metal.

12. The method of claim 1 1, wherein the silicate salt is sodium metasilicate.

13. The method of any preceding claim, wherein the step of exposing the solution to carbon dioxide is performed in a continuous stirred tank reactor (CSTR) or a bubble column reactor.

14. The method of any preceding claim, wherein the method comprises, after the solution has been exposed to the carbon dioxide, separating the silica from the solution.

15. The method of any preceding claim, wherein the method comprises exposing the silica to an acidic agent to remove the organic polyamine.

16. The method of claim 15, wherein the method comprises washing the silica.

17. The method of any preceding claim, wherein: the solution is exposed to carbon dioxide until the pH of the solution is from 6 to 8.5;the organic polyamine is PEHA; the solution is exposed to the carbon dioxide for 15 minutes or less; the temperature of the solution and / or the carbon dioxide when the solution is exposed to the carbon dioxide is from 10°C to 35°C; the silicate salt is sodium metasilicate; and the method further comprises exposing the silica to an acidic agent to remove the organic polyamine.

18. Use of a polyamine to increase the rate of precipitation of silica in a method of precipitating silica, wherein the method is as defined by any preceding claim.

19. The use of claim 18, wherein the increase in the rate of precipitation is 200% or more, relative to a method that does not use the polyamine.

20. Silica obtainable by the method of any one of claims 1 to 17.

21. The silica of claim 20, wherein the silica comprises:- a polyamine of Formula (I) and / or a salt thereof, and / or- a carbonate salt.

22. The silica of claim 20 or 21, wherein the silica has a BET specific surface area of 200 m2 / g or more.

23. The silica of claim 22, wherein the BET specific surface area is from 300 to 600 m2 / g.

24. The silica of any one of claims 20 to 23, wherein the silica has a zeta potential of from -35mV to -2mV.

Citation Information

Patent Citations

  • Controllable silica micro-powder preparation method

    CN104860319A

  • Method for preparing silicon dioxide with high specific surface area by using tubular continuous flow method

    CN108046278A

  • Method for preparing spherical nano silicon dioxide by tubular continuous flow method

    CN112174147A

  • Silica synthesis

    WO2017037460A1

  • Preparation method of solid amine gas adsorption material

    CN103785349A