Sliding member
The sliding member's DLC layer with alternating high and low concentration zones addresses the challenges of DLC layer brittleness by enhancing conformability and seizure resistance, improving sliding performance through precise additive element distribution and intermediate layer integration.
Patent Information
- Application Number
- PCT/JP2024/014551
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional sliding members with DLC layers face challenges in achieving fine separation and improved shape conformability and seizure resistance due to the brittleness and hardness of the DLC layer, leading to increased friction and reduced oil clearance.
A sliding member with a DLC layer containing a preset additive element, featuring high and low concentration portions alternately formed in the direction perpendicular to the thickness, promoting fine separation and improved conformability and seizure resistance by varying the additive element concentration.
The alternating concentration structure enhances shape conformability and seizure resistance by facilitating the DLC layer's deformation and reducing friction, while the intermediate layer improves adhesive force and fixability, leading to improved sliding performance.
Smart Images

Figure JP2024014551_31102024_PF_FP_ABST
Abstract
Description
Sliding member CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application is based on Japanese Application No. 2023-073393 filed on April 27, 2023, the contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a slide member.
[0003] Conventionally, sliding members used in bearings have been known to have a diamond-like carbon (DLC) layer formed on the outermost surface that slides against a mating material (see Patent Document 1). A sliding member with a DLC layer formed thereon has a reduced coefficient of friction with the mating material. Therefore, a sliding member with a DLC layer formed thereon has the characteristic of having a reduced frequency of seizure. On the other hand, because the DLC layer is very hard, it is resistant to wear and deformation. Therefore, there is a problem in that it is difficult to ensure oil clearance between a sliding member with a DLC layer and a mating material due to conformity. Furthermore, peeling due to the brittleness of the DLC layer leads to a local increase in the coefficient of friction and a decrease in seizure resistance.
[0004] In the case of Patent Document 1, a DLC layer has a cause portion that is the cause of intentional separation. Separation of the DLC layer originates from this cause portion, causing the DLC layer to deform and conform to the base material, improving conformability. However, performance requirements for sliding members are increasing, and the sliding conditions between the sliding member and the mating member are becoming even stricter. Therefore, even finer separation of the DLC layer is required.
[0005] Japanese Patent Application Laid-Open No. 2019-143802
[0006] Therefore, an object of the present invention is to provide a sliding member in which the DLC layer is separated into finer layers, thereby further improving conformability and, as a result, further improving seizure resistance.
[0007] A sliding member according to one embodiment includes a bearing alloy layer and a first DLC layer provided on the sliding side of the bearing alloy layer with respect to a mating material, the first DLC layer being formed of DLC containing a predetermined additive element, and having high-concentration portions having a high concentration of the additive element and low-concentration portions having a lower concentration of the additive element than the high-concentration portions alternately formed in a direction perpendicular to the thickness direction.
[0008] As described above, in the slide member according to one embodiment, the first DLC layer has high-concentration and low-concentration portions formed in a direction perpendicular to the thickness direction due to the concentration gradient of the additive element. That is, in the first DLC layer of the slide member according to one embodiment, high-concentration and low-concentration portions are formed alternately at the atomic level. Therefore, separation of the first DLC layer is promoted starting from the portions of the strength change caused by the concentration gradient of the additive element. Therefore, the first DLC layer is separated more finely, which can further improve the conformity of the shape and the seizure resistance.
[0009] Schematic diagram showing a cross section taken along line II in FIG. 2 Schematic diagram of the sliding member according to one embodiment as viewed from an end in the axial direction Schematic diagram showing a cross section of another embodiment of the sliding member according to one embodiment Schematic diagram showing a main part of the sliding member according to one embodiment Schematic diagram of the formation interface in the sliding member according to one embodiment as viewed from the direction of arrow V in FIG. 4 Schematic diagram for explaining the structure of the first DLC layer of the sliding member according to one embodiment Schematic diagram showing a cross section of another embodiment of the sliding member according to one embodiment Schematic diagram showing the conditions of a seizure test Schematic diagram showing contact between the first DLC layer and a mating material in the sliding member according to one embodiment Schematic diagram showing conformance due to contact between the first DLC layer and a mating material in the sliding member according to one embodiment
[0010] An embodiment of a slide member will be described below with reference to the drawings. As shown in FIGS. 1 and 2 , a slide member 10 includes a first DLC layer 11 and a bearing alloy layer 12. The first DLC layer 11 is provided on the side of the bearing alloy layer 12 that slides against a counter material. The first DLC layer 11 is laminated on the bearing alloy layer 12 and adheres to the bearing alloy layer 12. The bearing alloy layer 12 is formed of, for example, a Cu-based or Al-based alloy. The slide member 10 may also include a backing metal layer 13 formed of Fe, steel, or the like. The first DLC layer 11 forms a sliding surface 14 that slides against the counter material on the side opposite the bearing alloy layer 12. The first DLC layer 11 has a Vickers hardness (HV) of 250 HV to 1500 HV. This reduces the aggressiveness of the first DLC layer 11 to the counter material.
[0011] The first DLC layer 11 contains a predetermined additive element. The additive element is one or more elements selected from carbide-forming elements such as W, Co, Zr, Ta, Nb, V, Ti, Cr, Si, Ni, and Mo. The first DLC layer 11 contains 1 vol% to 60 vol% of the additive element as a whole. This facilitates conformability of the first DLC layer 11. Furthermore, as shown in FIG. 3 , the slide member 10 may include an intermediate layer 15 in addition to the first DLC layer 11 and the bearing alloy layer 12. The intermediate layer 15 is provided between the first DLC layer 11 and the bearing alloy layer 12. The intermediate layer 15 is formed of one or more elements selected from W, Co, Zr, Ta, Nb, V, Ti, Cr, Si, Ni, and Mo, similar to the additive element. As shown in FIG. 1 , the end of the first DLC layer 11 on the bearing alloy layer 12 side is a formation interface 16. 3 , in the case of slide member 10 having intermediate layer 15, the end of first DLC layer 11 on the intermediate layer 15 side is formation interface 16. Hereinafter, when referred to as formation interface 16 in this specification, it refers to the end face of first DLC layer 11 on the bearing alloy layer 12 side and the end face of first DLC layer 11 on the intermediate layer 15 side.
[0012] 4 and 5, the first DLC layer 11 includes a high-concentration portion 21, a low-concentration portion 22, and a core portion 23. The high-concentration portion 21 and the low-concentration portion 22 differ in the concentration of the additive element contained in the first DLC layer 11. The high-concentration portion 21 and the low-concentration portion 22 are alternately formed in a direction perpendicular to the thickness direction, that is, in the planar direction of the formation interface 16, in other words, in the direction along the sliding surface 14.
[0013] The high-concentration portion 21 has an additive element concentration of 1 vol% to 60 vol%, while the low-concentration portion 22 has an additive element concentration of 0.5 vol% to 59 vol%. This reduces the impact on sliding performance of the first DLC layer 11 while facilitating conformal shape. The high-concentration portion 21 is a region where the additive element concentration is relatively higher than that of the low-concentration portion 22. The additive element concentration does not change clearly at the boundary between the high-concentration portion 21 and the low-concentration portion 22. In other words, as schematically shown in FIG. 4 , the additive element concentration changes continuously at the boundary between the high-concentration portion 21 and the low-concentration portion 22. In FIG. 4 , for ease of understanding, the high-concentration portion 21, which has a high additive element concentration, is schematically shown in a dark color, and the low-concentration portion 22 is shown in a light color. Furthermore, the high-concentration portion 21 does not necessarily have to be formed as a distinct columnar shape in the thickness direction of the first DLC layer 11. That is, the high-concentration portions 21 may be formed in a three-dimensional hemispherical range centered on the core portion 23. Even when the high-concentration portions 21 are formed three-dimensionally, low-concentration portions 22 exist between adjacent high-concentration portions 21. In the first DLC layer 11, the difference in concentration between the region with the highest concentration of the additive element in the high-concentration portions 21 and the region with the lowest concentration of the additive element in the low-concentration portions 22 is preferably 1 vol % or more. By forming such a concentration difference, separation of the first DLC layer 11 is promoted, and shape conformity is more likely to occur.
[0014] The core 23 is provided on the bearing alloy layer 12 side of the first DLC layer 11. When the first DLC layer 11 and the bearing alloy layer 12 are directly laminated, the core 23 is provided at the formation interface 16, which is the end of the first DLC layer 11 on the bearing alloy layer 12 side. Furthermore, when an intermediate layer 15 is provided, the core 23 is provided at the formation interface 16, which is the end of the first DLC layer 11 on the intermediate layer 15 side. The core 23 is provided corresponding to the high concentration portion 21 of the first DLC layer 11. That is, the core 23 is located at the end of each high concentration portion 21 of the first DLC layer 11 on the bearing alloy layer 12 side. The core 23 is a region of the first DLC layer 11 where the concentration of the additive element is high. In this case, the concentration of the additive element in the core 23 is preferably 60% or more. The region of the first DLC layer 11 other than the additive element is composed of a-C:H. 4, for ease of understanding, the core portion 23 is shown in white. The concentration of the additional element also changes continuously between the high concentration portion 21 and the core portion 23.
[0015] As shown in Fig. 6, the outer diameter a of the cores 23 is set to 1 nm ≤ a ≤ 125 nm. Using the outer diameter a of the cores 23 as a reference, the shortest distance Da between the cores 23 is 2 a ≤ Da ≤ 8 a. The distance Da between the cores 23 corresponds to the shortest distance to the centers of adjacent cores 23 in the cross section of the first DLC layer 11 in the thickness direction, as shown in Figs. 1, 4, and 6. Therefore, the shortest distance Da between the cores 23 is set to several nanometers to several hundred nanometers, which is sufficiently smaller than conventional structures. The structure of the first DLC layer 11 shown in Fig. 4 is also formed in the cross section in the direction of arrow X in Fig. 1.
[0016] 5, nuclei 23 are arranged generally evenly at formation interface 16, which is the end of first DLC layer 11 on the bearing alloy layer 12 side. These nuclei 23 are formed at formation interface 16 by the additive elements when only the additive elements are sputtered prior to forming first DLC layer 11 by sputtering. At this time, the additive elements forming nuclei 23 are arranged generally regularly while maintaining a spacing Da that correlates with the outer diameter a of nuclei 23, based on their own interactions and the sputtering conditions.
[0017] As shown in FIG. 6 , the distance Db between adjacent high-concentration portions 21 is preferably about Db = 2a, based on the outer diameter a of core portion 23. In this case, the distance Db may be in the range of about 2a ≦ Db ≦ 8a. Similarly, the distance Dc between adjacent low-concentration portions 22 is preferably about Dc = 2a, based on the outer diameter a of core portion 23. In this case, the distance Dc may also be in the range of about 2a ≦ Dc ≦ 8a. The high-concentration portions 21 grow from formation interface 16 in the thickness direction of first DLC layer 11 corresponding to core portion 23 by sputtering carbon (C) forming first DLC layer 11 together with the additive element. That is, high-concentration portions 21 are formed extending from core portion 23 toward the opposite side from bearing alloy layer 12. Furthermore, low-concentration portions 22 having a lower concentration of the additive element than high-concentration portions 21 are formed between high-concentration portions 21 formed corresponding to core portions 23.
[0018] As shown in Figure 4, the concentration of the additive element changes continuously at the boundary between the high-concentration portion 21 and the low-concentration portion 22, and the concentration of the additive element does not change clearly at the boundary between the high-concentration portion 21 and the low-concentration portion 22. Therefore, the distances Db and Dc are defined and calculated as follows: First, the center point of the nucleus 23 at the formation interface 16 is extracted. From this center point, a circular region is defined along the formation interface 16 with a radius equal to 1 / 4 of the distance Da. The width of this region, i.e., the length of the portion corresponding to the diameter of the circular region centered on the center point, is defined as the distance Dc. Then, the region sandwiched between the defined distances Dc is defined as the distance Db.
[0019] By providing intermediate layer 15 between first DLC layer 11 and bearing alloy layer 12, the additional element growing from formation interface 16 is more firmly fixed to intermediate layer 15. That is, intermediate layer 15 is preferably formed of an element that is the same as the additional element or that has a high material commonality with the additional element. By selecting elements in this way to form intermediate layer 15, core portion 23 is more easily formed in intermediate layer 15, and the fixation to intermediate layer 15 is also improved. Intermediate layer 15 is preferably formed to a thickness of approximately 0.1 μm to 1 μm. This ensures a strong adhesive force between first DLC layer 11 and bearing alloy layer 12.
[0020] As shown in FIG. 7 , the slide member 10 may further include a second DLC layer 30. The second DLC layer 30 is laminated on the sliding side of the first DLC layer 11, i.e., on the surface of the first DLC layer 11 opposite the bearing alloy layer 12. The second DLC layer 30 is formed of DLC, similar to the first DLC layer 11. The second DLC layer 30 has a lower concentration of additive elements than the entire first DLC layer 11. That is, the second DLC layer 30 has a lower concentration of additive elements than the first DLC layer 11 on which it is laminated, and the concentration of additive elements is set to 0 to 20 vol%. By setting the concentration of additive elements in the second DLC layer 30 in this manner, the second DLC layer 30 can reduce aggressiveness toward a mating material and easily adjust the difference in hardness between the second DLC layer 30 and the first DLC layer 11. Furthermore, when the thickness of the first DLC layer 11 is T1 and the thickness of the second DLC layer 30 is T2, T1 > T2. As described above, the second DLC layer 30 is formed thinner than the first DLC layer 11. The hardness of the second DLC layer 30 is preferably set to 250 HV to 1500 HV. In this case, the difference in hardness between the first DLC layer 11 and the second DLC layer 30 is more preferably 100 HV or less. This reduces the aggressiveness of the second DLC layer 30 to the mating material. The concentrations of the additive elements in the first DLC layer 11, the high-concentration portion 21, the low-concentration portion 22, and the second DLC layer 30 were measured from a cross section of the slide member 10 using an electron probe microanalyzer (EPMA). The concentration of the additive element throughout the first DLC layer 11 was calculated by averaging the concentrations of the additive elements in the high-concentration portion 21 and the low-concentration portion 22.
[0021] Next, an example of a method for manufacturing slide member 10 will be described. First DLC layer 11 is formed using a sputtering apparatus as described above. The material on which bearing alloy layer 12 is formed is contained in a chamber. The chamber containing the material has an internal volume of, for example, 1.0×10 -3The pressure is reduced to below 1 Pa. After the pressure reduction, the material is pretreated using, for example, an inert gas. Upon completion of the pretreatment, nuclei 23 are formed on the surface of bearing alloy layer 12, which will become formation interface 16. Prior to the formation of nuclei 23, an intermediate layer 15 may be formed on the surface of bearing alloy layer 12. Intermediate layer 15 is formed by sputtering an additive element alone onto the surface of bearing alloy layer 12. Nuclei 23 are formed at formation interface 16 by performing sputtering for a short period of time, such as several minutes. At this time, nuclei 23 are formed at formation interface 16 approximately uniformly at intervals Da corresponding to the outer diameters a of nuclei 23 due to the interaction of the additive elements, as shown in FIG. 6 . The outer diameters a and intervals Da of nuclei 23 are controlled, for example, by the sputtering time required, bias voltage, the target used, and the pressure in the chamber. The outer diameters a and intervals Da are controlled, in particular, by the pressure in the chamber.
[0022] The material on which the core portion 23 is formed is used to form the first DLC layer 11. The first DLC layer 11 is formed by sputtering for a time that is sufficiently longer than that required for forming the core portion 23. When forming the first DLC layer 11, the thickness of the film formed per unit time is set to be larger than that required for forming the core portion 23. After the first DLC layer 11 is formed, the second DLC layer 30 is formed as needed. When forming the second DLC layer 30, the thickness of the film formed per unit time is set to be smaller than that required for the first DLC layer 11. The slide member 10 is formed by the above procedure. Note that the above disclosure is an example of a manufacturing method, and the manufacturing method for forming the high-concentration portion 21 and the low-concentration portion 22 in the first DLC layer 11 is not limited to that disclosed above.
[0023] The operation of the slide member 10 of this embodiment will be described below based on verification of examples and comparative examples. The examples and comparative examples were evaluated based on a seizure test. The seizure test was performed under the conditions shown in FIG. 8. The slide members 10 of the examples and comparative examples, which were molded into a half shape, were used in the seizure test. In the seizure test, the maximum surface pressure at which seizure did not occur was measured when the slide member 10 was caused to slide improperly against a shaft-shaped mating member 40 made of S55C under the conditions shown in FIG. 8, as shown in FIGS. 9 and 10.
[0024] As shown in FIG. 9 , when slide member 10 and mating member 40 slide against each other in an improper contact state, bearing alloy layer 12 of slide member 10 is deformed as shown in FIG. 10 by the force applied from mating member 40. At this time, separation of first DLC layer 11 of slide member 10 according to this embodiment is promoted starting from the portions where the strength varies due to the concentration of the additive element. That is, first DLC layer 11 is formed with alternating high-concentration portions 21 and low-concentration portions 22 having different concentrations of the additive element, resulting in minute differences in strength. This promotes minute separation of first DLC layer 11 starting from the portions where the strength differs. Therefore, as in slide member 10 according to this embodiment, first DLC layer 11 that is finely fractured deforms in accordance with the deformation of bearing alloy layer 12, as shown in FIGS. 10 and 11 . As a result, even when sliding member 10 comes into improper contact with mating member 40, it can easily follow the deformation of bearing alloy layer 12, thereby improving seizure resistance.
[0025] 12 , Examples 1 to 15 are examples in which first DLC layer 11 is laminated directly on bearing alloy layer 12, and no intermediate layer 15 is provided. Examples 16 to 24 are examples in which intermediate layer 15 is provided between first DLC layer 11 and bearing alloy layer 12. Examples 18 to 24 are examples in which second DLC layer 30 is provided in addition to first DLC layer 11.
[0026] On the other hand, Comparative Examples 1 and 2 are examples in which first DLC layer 11 containing an additive element is provided in bearing alloy layer 12, but no concentration distribution of the additive element is formed in first DLC layer 11. In other words, in Comparative Examples 1 and 2, high concentration portions 21 and low concentration portions 22 are not formed in first DLC layer 11. Comparative Examples 3 and 4 are examples in which intermediate layer 15 is provided between first DLC layer 11 and bearing alloy layer 12. First DLC layer 11 in Comparative Examples 3 and 4 does not contain an additive element.
[0027] It can be seen that Examples 1 to 24 have improved seizure resistance compared to Comparative Examples 1 to 4. That is, in first DLC layer 11 in which high-concentration portions 21 and low-concentration portions 22 are alternately formed as in Examples 1 to 24, when stress due to improper contact is applied, destruction is promoted in low-concentration portions 22 having a low concentration of additional elements. Therefore, first DLC layer 11 has improved ability to follow the deformation of bearing alloy layer 12. As a result, the seizure resistance of slide member 10 is improved. Furthermore, Examples 1 to 13 show that the type and combination of additional elements contained in first DLC layer 11 do not affect seizure resistance.
[0028] Examples 12 to 24 show that the smaller the spacing Da between core portions 23, the more improved the seizure resistance. Naturally, as spacing Da between core portions 23 decreases, spacing Db between high-concentration portions 21 and spacing Dc between low-concentration portions 22 also decrease. Therefore, as spacing Da between core portions 23 decreases, finer fractures are promoted in first DLC layer 11. Therefore, first DLC layer 11 is more able to follow the deformation of bearing alloy layer 12. As a result, the seizure resistance of slide member 10 is improved.
[0029] According to Examples 15 and 16, it can be seen that Example 16, which includes intermediate layer 15, exhibits improved seizure resistance. Intermediate layer 15 contributes to improving the fixation of nuclei 23, which serve as starting points for the growth of high-concentration portions 21. That is, intermediate layer 15 is formed of elements with properties identical to or similar to those of the additive elements added to first DLC layer 11, and has a high affinity with nuclei 23. Therefore, the formation of intermediate layer 15 increases the adhesive strength between first DLC layer 11 and bearing alloy layer 12. As a result, detachment of first DLC layer 11 from bearing alloy layer 12 is reduced, and the seizure resistance of slide member 10 is further improved.
[0030] It can be seen that Examples 17 to 24, in which the second DLC layer 30 is provided, have further improved seizure resistance. The second DLC layer 30 contributes to reducing the contact resistance between the slide member 10 and the mating member 40, particularly in the early stages of sliding with the mating member 40. Therefore, by providing the second DLC layer 30, damage during sliding between the slide member 10 and the mating member 40 is reduced, further improving the seizure resistance of the slide member 10. In this case, it can be seen that Examples 21 to 24, in which T1 > T2, have further improved seizure resistance. In this way, by making T1 > T2, separation of the first DLC layer 11, which follows the deformation of the bearing alloy layer 12, is further promoted. As a result, seizure resistance can be further improved. In addition, it can be seen that Example 24, in which the difference in hardness between the first DLC layer 11 and the second DLC layer 30 is 100 HV or less, has further improved seizure resistance. In this way, by reducing the difference in hardness between the first DLC layer 11 and the second DLC layer 30, the adhesive strength between the first DLC layer 11 and the second DLC layer 30 is improved, thereby further improving the seizure resistance.
[0031] The present invention described above is not limited to the above-described embodiment, and can be applied to various embodiments without departing from the gist of the invention.
Claims
1. A sliding member comprising a bearing alloy layer and a first DLC layer provided on the sliding side of the bearing alloy layer with a mating material, wherein the first DLC layer is formed of DLC containing a predetermined additive element, and high concentration portions having a high concentration of the additive element and low concentration portions having a lower concentration of the additive element than the high concentration portions are alternately formed in a direction perpendicular to the thickness direction.
2. The sliding member according to claim 1, further comprising a core portion provided on the bearing alloy layer side of said first DLC layer in correspondence with said high concentration portion, said core portion having a higher concentration of said additional element than said high concentration portion.
3. A sliding member according to claim 2, wherein an outer diameter a of the core portion is 1 nm≦a≦125 nm, and a distance Da between adjacent core portions in a cross section perpendicular to the thickness direction of the first DLC layer is 2a≦Da≦8a.
4. The slide member according to any one of claims 1 to 3, wherein the additional element is one or more elements that form carbides.
5. The sliding member according to claim 4, wherein the additional element is one or more elements selected from the group consisting of W, Co, Zr, Ta, Nb, V, Ti, Cr, Si, Ni and Mo.
6. The sliding member according to claim 1, further comprising an intermediate layer provided between said bearing alloy layer and said first DLC layer, said intermediate layer being formed of one or more elements selected from the group consisting of W, Co, Zr, Ta, Nb, V, Ti, Cr, Si, Ni and Mo.
7. The sliding member according to claim 6, further comprising a second DLC layer provided on the sliding side of the first DLC layer and made of DLC having a lower concentration of the additive element than the concentration of the additive element contained in the entire first DLC layer.
8. The slide member according to claim 7, wherein the thickness T1 of the first DLC layer and the thickness T2 of the second DLC layer satisfy the relationship T1>T2.
9. The sliding member according to claim 7, wherein the difference in hardness between the first DLC layer and the second DLC layer is 100 HV or less.
Citation Information
Patent Citations
Hydrogen storage material and its manufacturing method
JP2004261632A
Hard carbon film
JP2007291429A
Slide member
JP2019143802A
Carbonaceous thin film, process for producing the same and member utilizing the thin film