Glass plate manufacturing method and manufacturing apparatus

By pre-bending glass plates into a convex curved surface before breaking, the method stabilizes the breaking process, improving end surface quality and addressing the issues of peeling and cracking in existing glass plate manufacturing techniques.

WO2024225064A1PCT designated stage expired Publication Date: 2024-10-31NIPPON ELECTRIC GLASS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014709
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing methods for breaking glass plates along a vertical scribe line often result in defective end surfaces due to unstable contact between the glass plate and the fulcrum member, leading to peeling and minute cracks, primarily caused by the curvature of the glass plate in cross-section.

Method used

The glass plate is pre-bent into a convex curved surface in cross-section parallel to the lateral direction before breaking, stabilizing the contact with the fulcrum member and improving the end surface properties by using a folding mechanism that includes a holding member, a pressing member, and a curving mechanism to adjust the curvature.

Benefits of technology

This method enhances the end surface quality of the glass plate by ensuring a stable breaking process, reducing vibrations and destabilization, and preventing scratches and contamination during the breaking process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014709_31102024_PF_FP_ABST
    Figure JP2024014709_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This method of manufacturing a glass plate is provided with a snap-cleaving step P2 in which a glass plate G, which assumes a vertical posture and has scribe lines S extending in the vertical direction formed on an obverse surface Ga side, is snap-cleaved and partitioned into a first region G1 and second regions G2 that are horizontally neighboring with the scribe lines S as boundaries. The method is further provided with a preparation step P1 of bringing the glass plate G, prior to being snap-cleaved, into a curved state such that the form of the obverse surface Ga is a convex-curved face in cross-section parallel to the horizontal direction. After the preparation step P1, the snap-cleaving step P2 is performed on the glass plate G in the curved state.
Need to check novelty before this filing date? Find Prior Art

Description

Glass plate manufacturing method and manufacturing device

[0001] The present disclosure relates to a technique for breaking a glass sheet in a vertical position along a scribe line extending in the vertical direction.

[0002] As a method for manufacturing a glass sheet, there is a method using a downdraw method, typified by an overflow downdraw method, a slot downdraw method, a redraw method, etc. An example of a manufacturing process of a glass sheet using this method is as follows.

[0003] First, a glass ribbon is continuously formed from molten glass. At this time, portions called "edge portions" that are thicker than the central portion are formed at both ends in the width direction of the glass ribbon. Next, the glass ribbon is cut in the width direction at predetermined lengths, thereby continuously cutting out glass sheets that will become product glass sheets from the glass ribbon. Next, unnecessary portions (portions that will not become products), including the edge portions, are cut out from the cut glass sheets. Thereafter, the glass sheets from which the unnecessary portions have been cut out are subjected to various processes, such as grinding, polishing, and cleaning, to produce product glass sheets.

[0004] When a glass sheet is manufactured using the down-draw method, the formed glass ribbon is in a vertical position. Therefore, from the viewpoint of saving space in the planar direction, a glass sheet cut from the vertically oriented glass ribbon may be transported in the vertical position, and an unnecessary portion may be cut out from the glass sheet on the transport path. Such a form of cutting out an unnecessary portion is disclosed in Patent Document 1.

[0005] In the technique disclosed in Patent Document 1, a glass sheet in a vertical position is first transported laterally into a scribe line formation area on a transport path, and then a scribe line is formed vertically on the front surface of the glass sheet. Then, downstream of the scribe line formation area, a back surface support member is brought into contact with the glass sheet from the back surface side, and the area around the scribe line is bent using the back surface support member as a fulcrum so that the front surface side is convex, and the glass sheet is bent and split along the scribe line to cut out the unnecessary portion.

[0006] International Publication No. 2022 / 219922

[0007] When a glass sheet in a vertical position is bent and broken as in the embodiment disclosed in Patent Document 1, the end surface quality of the bent and broken glass sheet may be poor, with glass peeling and numerous small cracks being observed on the end surface of the bent and broken glass sheet. In view of this situation, the technical problem to be solved is to improve the end surface quality of the bent and broken glass sheet when a glass sheet in a vertical position is bent and broken along scribe lines extending in the vertical direction.

[0008] As a result of extensive research, the inventors discovered that when a glass sheet in a vertical orientation is bent and split along a scribe line extending in the vertical direction, the curvature state of the glass sheet in a cross section parallel to the horizontal direction is a factor that affects the quality of the edge surface of the bent and split glass sheet. Specifically, the inventors discovered that if the glass sheet is bent and split in a state where the surface on which the scribe line is formed is a concavely curved surface in a cross section parallel to the horizontal direction due to warping or the like of the glass sheet, the edge surface quality becomes poor. This is due to unstable contact between the glass sheet and a member that serves as a fulcrum for curving the glass sheet during splitting (a rear surface support member in Patent Document 1). Furthermore, the inventors discovered that if the glass sheet is bent and split in a state where the surface on which the scribe line is formed is a convexly curved surface in a cross section parallel to the horizontal direction, the contact state between the fulcrum and the glass sheet becomes stable, resulting in good edge surface quality.

[0009] Based on the above findings, a first method for manufacturing a glass plate for solving the above problems is a method for manufacturing a glass plate that includes a bending and splitting step of bending and splitting a glass plate that is in a vertical position and has a scribe line formed on its surface side extending in the vertical direction, thereby dividing a first region and a second region that are adjacent in the horizontal direction along the scribe line, and is characterized in that the method further includes a preparation step of bending the glass plate before bending and splitting so that the surface has a convex curved shape in a cross section parallel to the horizontal direction, and that after the preparation step, the bending and splitting step is performed on the curved glass plate.

[0010] In the first glass sheet manufacturing method, when a vertically oriented glass sheet is bent and split along a scribe line extending in the vertical direction, a preparation step is performed to curve the glass sheet before bending it so that the surface has a convex curved shape in a cross section parallel to the horizontal direction. Thus, in this manufacturing method, the preparation step is performed to make the surface (surface) along which the scribe line is formed into a convex curved shape in a cross section parallel to the horizontal direction, and then the bending and splitting step is performed to bend and split the glass sheet. This stabilizes the contact state between the glass sheet and a member that serves as a fulcrum for curving the area around the scribe line of the glass sheet during bending and splitting, making it possible to improve the edge quality of the glass sheet after bending and splitting.

[0011] The second method for manufacturing a glass plate is the same as the first method for manufacturing a glass plate as described above, except that in the preparation step, the glass plate is pressed from the back surface side by a pressing member.

[0012] In the second glass plate manufacturing method, the glass plate is pressed from the back side by a pressing member in the preparation process, so that the surface (front surface) on which the scribe line is formed on the glass plate can be smoothly and reliably made into a convex curved surface in a cross section parallel to the horizontal direction.

[0013] The third glass plate manufacturing method is the same as the second glass plate manufacturing method described above, except that the glass plate has second regions on both sides of the first region in the horizontal direction, and in the preparation step, the upper part of the glass plate is held by a holding member to hang the glass plate, and the lower part of the first region is pressed by a pressing member.

[0014] In the third method for manufacturing a glass sheet, in a preparation step before breaking the glass sheet, a lower part of the first region of the glass sheet suspended by the holding member is pressed by a pressing member. By having the pressing member press the lower part of the first region in this manner, it is possible to avoid vibrations originating from the lower part of the glass sheet during breaking, and thus to avoid instability in breaking due to the vibrations.

[0015] The fourth glass plate manufacturing method is the same as the third glass plate manufacturing method described above, except that the first region includes an effective portion that will become a product and an ineffective portion that will not become a product, and in the preparation step, the pressing member is brought into contact with only the ineffective portion of the effective portion and the ineffective portion.

[0016] In the fourth method for manufacturing a glass plate, in the preparation step, of the effective portion and the non-effective portion included in the first region of the glass plate, the pressing member contacts only the non-effective portion that will not become a product. As a result, the pressing member does not contact the effective portion that will become a product, and it is possible to preferably avoid the occurrence of scratches in the effective portion and contamination of the effective portion, and it is possible to protect the effective portion.

[0017] The fifth method for manufacturing a glass plate is the same as the third or fourth method for manufacturing a glass plate, except that in the preparation step, one lateral end portion and the other lateral end portion of the first region are supported by support members from both the front and back sides, respectively, and the lower portion of the first region is pressed by a pressing member between the support member supporting the one lateral end portion and the support member supporting the other lateral end portion, and the operation of having the support members support the first region and the operation of having the pressing member press the first region are synchronized.

[0018] In the fifth method for manufacturing a glass plate, in the preparation step, the operation of having the support member support the first region and the operation of the pressing member pressing the first region are synchronized, so that the timing at which the support member and the pressing member operate is fixed. By fixing the operation timing in this manner, the timing at which the pressing member contacts the first region can be easily adjusted, for example, by simply adjusting the relative positional relationship between the support member and the pressing member.

[0019] The sixth glass plate manufacturing method is any one of the second to fifth glass plate manufacturing methods described above, except that the pressing member has a shape extending in the horizontal direction, and the curvature of the contact portion of the pressing member with the glass plate in a cross section parallel to the horizontal direction is adjustable.

[0020] In the sixth method for manufacturing a glass plate, the curvature of the contact portion of the pressing member can be adjusted, and therefore it is possible to easily change the curvature of the surface of the glass plate that has become a convex curved surface.

[0021] A seventh method for producing a glass plate is any one of the first to sixth methods for producing a glass plate, wherein in the preparation step, the glass plate before being split is curved so that the surface has a convex curved shape in a cross section parallel to the longitudinal direction.

[0022] In the seventh method for manufacturing a glass plate, the surface on which the scribe line is formed becomes a convex curved surface in a cross section parallel to the longitudinal direction as a result of the preparation step, which allows the starting point of the cleavage in the cleaving step to be stabilized near the center of the glass plate in the longitudinal direction.

[0023] Based on the above findings, an eighth method for manufacturing a glass plate for solving the above problems is a method for manufacturing a glass plate comprising a bending and splitting step of bending and splitting a glass plate that is in a vertical position and has a scribe line formed on its front surface that extends vertically, thereby dividing a first region and a second region that are adjacent in the horizontal direction along the scribe line, the method further comprising a preparation step of bringing the glass plate into a state for bending and splitting, the glass plate having the second region on both sides with the first region sandwiched in between, after the preparation step, carrying out the bending and splitting step on the glass plate in a curved state, the preparation step being characterized in that an upper part of the glass plate is held by a holding member to suspend the glass plate, and a pressing member is used to press the lower part of the first region from the back surface side.

[0024] In an eighth glass sheet manufacturing method, when a vertically oriented glass sheet is bent and broken along a scribe line extending in the vertical direction, a preparatory step is performed before the glass sheet is bent and broken, in which a lower portion of a first region of the glass sheet suspended by a holding member is pressed from the backside. By pressing the lower portion of the first region, located between the second regions on both sides in the horizontal direction, from the backside in this manner, the surface (front surface) on which the scribe line is formed can be made a convexly curved surface in a cross section parallel to the horizontal direction, and the glass sheet can then be bent and broken by the bend and break step. This stabilizes the contact state between the glass sheet and a member that serves as a fulcrum for curving the area around the scribe line during bend and break, thereby improving the quality of the edge surface of the glass sheet after bend and break. Furthermore, in this manufacturing method, the lower portion of the first region of the glass sheet is pressed by a pressing member during the preparatory step before the glass sheet is bent and broken. By having the pressing member press the lower portion of the first region in this manner, it is possible to avoid vibrations originating from the lower portion of the glass sheet during bend and thus avoid instability of the bend due to the vibrations.

[0025] Based on the above findings, a first glass plate manufacturing apparatus for solving the above problems is a glass plate manufacturing apparatus equipped with a bending and splitting mechanism that bends and splits a glass plate in a vertical position, with a scribe line extending vertically formed on the surface side, to separate a first region and a second region that are adjacent in the horizontal direction, with the scribe line as a boundary, and is characterized in that the bending and splitting mechanism is equipped with a curvature imparting mechanism that curves the glass plate before bending and splitting so that the surface shape becomes a convex curved surface in a cross section parallel to the horizontal direction.

[0026] The first glass sheet manufacturing apparatus can provide the same functions and effects as the first glass sheet manufacturing method described above.

[0027] Based on the above findings, a second glass plate manufacturing apparatus for solving the above problem is a glass plate manufacturing apparatus equipped with a bending and splitting mechanism that bends and splits a glass plate in a vertical position with a scribe line extending vertically formed on the front surface side, thereby dividing a first region and a second region that are adjacent in the horizontal direction at the scribe line as a boundary, wherein the glass plate has the second region on both sides of the first region in the horizontal direction, and the bending and splitting mechanism is characterized by having a holding member that holds the upper part of the glass plate and suspends it, and a pressing member that presses the lower part of the first region from the back surface side.

[0028] The second glass plate manufacturing apparatus can achieve the same functions and effects as the above-described eighth glass plate manufacturing method.

[0029] According to the glass plate manufacturing method and manufacturing apparatus of the present disclosure, when a glass plate in a vertical position is bent and split along a scribe line extending in the vertical direction, it is possible to improve the quality of the end surface of the glass plate after bending and splitting.

[0030] Fig. 2 is a front view showing a glass sheet manufacturing apparatus. Fig. 3 is a cross-sectional view showing the A-A cross section in Fig. 1. Fig. 4 is a cross-sectional view showing the B-B cross section in Fig. 1, showing a time point before the preparation step is performed. Fig. 5 is a cross-sectional view showing a time point during the preparation step. Fig. 6 is a plan view showing a curvature imparting mechanism. Fig. 7 is a cross-sectional view showing a bending step.

[0031] Hereinafter, a method and an apparatus for manufacturing a glass sheet according to an embodiment will be described with reference to the accompanying drawings. Note that the X direction, Y direction, and Z direction shown in each drawing referred to in the description of the embodiment are directions perpendicular to one another. The Y direction coincides with the up-down direction.

[0032] FIG. 1 shows a glass sheet manufacturing apparatus 1 (hereinafter simply referred to as manufacturing apparatus 1). In a glass sheet manufacturing method using this manufacturing apparatus 1, a bending / breaking step P2 (see FIG. 6) is performed to bend and break a glass sheet G in a vertical position, with a scribe line S extending in the vertical direction (Y direction) formed on the surface Ga side. This manufacturing method includes the bending / breaking step P2 and a preparation step P1 (see FIG. 4) to prepare the glass sheet G for bending / breaking. After the preparation step P1, the bending / breaking step P2 is performed to bend and break the glass sheet G. In the preparation step P1, the glass sheet G is curved before bending so that the surface Ga has a convex curved shape in a cross section parallel to the horizontal direction (X direction).

[0033] The glass sheet G to be broken is a glass sheet G continuously cut from a glass ribbon formed by a downdraw method (e.g., an overflow downdraw method) by cutting the glass ribbon at predetermined lengths. The plurality of glass sheets G cut from the glass ribbon are sequentially carried into the manufacturing apparatus 1 and broken.

[0034] The glass sheet G has a rectangular shape. The horizontal dimension of the glass sheet G is, for example, 1500 mm or more and 3500 mm or less, and the vertical dimension is, for example, 1500 mm or more and 3500 mm or less. At both horizontal end portions of the glass sheet G, there are respectively ear portions Gx formed during the formation of the glass ribbon. The ear portions Gx are thicker than other portions of the glass sheet G. The glass sheet G is flexible, and, as an example, the thickness of the glass sheet G (the thickness of the portions excluding the ear portions Gx) is 150 μm to 2000 μm.

[0035] The scribe lines S are formed on one side and the other side of the glass sheet G in the lateral direction. The scribe line S forms a boundary between a first region G1 and a second region G2 included in the glass sheet G, and the first region G1 and the second region G2 are adjacent to each other in the lateral direction with the scribe line S sandwiched therebetween. In this embodiment, the glass sheet G has second regions G2 on both sides of the first region G1 in the lateral direction. The first region G1 and the second region G2 are separated in the bending and cutting process P2, and the second region G2 is discarded as an unnecessary portion. The lateral dimension of the second region G2 is, for example, 20 mm or more and 700 mm or less.

[0036] The first region G1 of the glass sheet G includes a useful portion G1a, which will later become a product glass sheet, and a non-useful portion G1b, which will not become a product glass sheet and will be removed. In FIG. 1 , the boundary between the useful portion G1a and the non-useful portion G1b is indicated by a two-dot chain line. The useful portion G1a is located in the center of the first region G1, and the non-useful portion G1b is located so as to surround the useful portion G1a. The non-useful portion G1b is a portion that will be cut and removed in a subsequent process. The width of the non-useful portion G1b is, for example, 200 mm or less. Meanwhile, the glass sheet made of the useful portion G1a cut out in a subsequent process is divided into multiple glass sheets by cutting as needed. Furthermore, the glass sheet made of the useful portion G1a is subjected to edge processing using a grindstone, cleaning, inspection, etc., to become a product glass sheet. Such a product glass sheet is used, for example, as a glass substrate for a display.

[0037] The manufacturing apparatus 1 includes a cutting mechanism 2 for performing a preparation step P1 and a cutting step P2.

[0038] The main components of the bending and splitting mechanism 2 include a holding member 3 that holds the upper part (upper edge) of the glass plate G and suspends the glass plate G, a support member 4 that supports one lateral end and the other lateral end of the first region G1 from both the front and back sides, a curving mechanism 5 for executing the preparation process P1, and a pushing member 6 that pushes the second region G2 from the surface Ga side during the bending and splitting process P2 after the preparation process P1, to curve the periphery of the scribe line S so that the surface Ga side is convex.

[0039] A plurality of holding members 3 (three in this embodiment) are arranged along the upper portion of the first region G1 of the glass sheet G. In this embodiment, the holding members 3 are chucks that clamp the upper portion of the first region G1 from both the front and back sides. The chucks grip the non-effective portion G1b of the first region G1. Note that the holding members 3 may be suction pads that suction-hold the front surface Ga or back surface Gb of the upper portion of the first region G1. In this case, the non-effective portion G1b of the first region G1 is suction-held by the suction pad.

[0040] Each of the plurality of holding members 3 is connected to a running body 7. The running body 7 is capable of running along a rail (not shown) extending in the X direction. As the running body 7 runs along the rail, the glass sheet G before the preparation process P1 is carried into the manufacturing apparatus 1, and the first region G1 (the glass sheet G from which the second region G2 has been cut off) after the bending and cutting process P2 is carried out from the manufacturing apparatus 1.

[0041] The support member 4 extends in the vertical direction and is capable of supporting the entire vertical length of the first region G1. As shown in Fig. 2, the support member 4 includes a fulcrum member 8 disposed on the rear surface Gb side of the glass sheet G, and a pressing member 9 disposed on the front surface Ga side of the glass sheet G so as to face the fulcrum member 8 across the glass sheet G.

[0042] Each of the fulcrum member 8 and the presser member 9 is capable of moving along the Z direction (thickness direction of the glass sheet G) as shown by the arrows in Figure 2. Before the preparation step P1, the fulcrum member 8 and the presser member 9 are in a state where they are retracted from the glass sheet G (the state shown in Figure 2). When the preparation step P1 is started, the fulcrum member 8 and the presser member 9 move forward toward the glass sheet G and sandwich and support the first region G1 from both the front and back sides. The state in which the fulcrum member 8 and the presser member 9 support the first region G1 continues until the completion of the bending and cutting step P2. After the bending and cutting step P2, the fulcrum member 8 and the presser member 9 move back from the glass sheet G and release support for the first region G1.

[0043] The fulcrum member 8 is a member that comes into contact with the first region G1 from the back surface Gb side and serves as a fulcrum when the pressing member 6 curves the periphery of the scribe line S so that the front surface Ga side is convex. The pressing member 9 is a member that comes into contact with the first region G1 from the front surface Ga side and presses the first region G1 to prevent it from lifting off the fulcrum member 8 when the pressing member 6 curves the periphery of the scribe line S. The separation distance along the X direction between the fulcrum member 8 and the pressing member 9 and the scribe line S is, for example, 10 to 60 mm.

[0044] The fulcrum member 8 has an intermediate protrusion 8a in the center of the portion facing the glass sheet G. The intermediate protrusion 8a is smoothly curved so that its protruding length gradually decreases from the center toward both ends in the vertical direction. The length of the intermediate protrusion 8a along the vertical direction is 1 / 4 to 3 / 4 of the length of the glass sheet G along the vertical direction. The intermediate protrusion 8a is located below the holding member 3 that holds the upper portion of the glass sheet G. The portion of the fulcrum member 8 that comes into contact with the glass sheet G, including the intermediate protrusion 8a, is elastically deformable and is formed of a porous resin such as sponge or low-resilience sponge, or a foamed resin. The lower limit of the protruding length of the intermediate protrusion 8a is preferably 10 mm or more. The upper limit of the protruding length of the intermediate protrusion 8a is preferably 300 mm or less, more preferably 100 mm or less.

[0045] The holding member 9 has an upper convex portion 9a at the top of the portion facing the glass sheet G and a lower convex portion 9b at the bottom. The protruding lengths of the upper convex portion 9a and the lower convex portion 9b gradually increase from the center toward both ends in the vertical direction. The upper convex portion 9a and the lower convex portion 9b are both positioned so as not to overlap the intermediate convex portion 8a of the fulcrum member 8 in the vertical direction. Furthermore, the upper convex portion 9a is positioned so as to overlap the holding member 3 that holds the upper portion of the glass sheet G in the vertical direction. The portions of the holding member 9 that come into contact with the glass sheet G, including the upper convex portion 9a and the lower convex portion 9b, are elastically deformable and are formed of a porous resin such as sponge or low-resilience sponge, or a foamed resin. The lower limit of the protruding lengths of the upper convex portion 9a and the lower convex portion 9b is preferably 10 mm or more. The upper limit of the protruding length of the upper convex portion 9a and the lower convex portion 9b is preferably 300 mm or less, and more preferably 100 mm or less.

[0046] Due to the above-mentioned configuration of the fulcrum member 8 and the pressure member 9, the portion of the first region G1 sandwiched between the fulcrum member 8 and the pressure member 9 on both the front and back sides (one end and the other end of the first region G1 in the horizontal direction) is curved so that the surface Ga becomes a convex curved surface in a cross section parallel to the vertical direction.

[0047] As shown in FIG. 1 , the curvature imparting mechanism 5 includes a pressing member 10 that presses a lower portion (lower edge portion) of a first region G1 of the glass sheet G from the rear surface Gb side. The pressing member 10 presses the lower portion of the first region G1 between the support member 4 on one side in the lateral direction and the support member 4 on the other side. The pressing member 10 has an elongated shape extending in the lateral direction. Of the effective portion G1a and the non-effective portion G1b in the first region G1, the pressing member 10 contacts only the non-effective portion G1b.

[0048] FIG. 3 shows a time point before the preparation step P1 is performed, and FIG. 4 shows a time point during the preparation step P1. As can be seen from both figures, the pressing member 10 is capable of moving along the Z direction. Before the preparation step P1, the pressing member 10 is retracted from the glass sheet G. When the preparation step P1 is started, the pressing member 10 advances toward the glass sheet G and presses the lower part of the first region G1, curving the glass sheet G before bending so that the surface Ga becomes a convex curved surface in a cross section parallel to the lateral direction. After the bending step P2, the pressing member 10 retracts from the glass sheet G and releases the pressure on the lower part of the first region G1.

[0049] The pressing member 10 is curved so as to gradually protrude toward the glass sheet G as it moves toward the center in the horizontal direction. The pressing member 10 is a vertically oriented plate that is elastically deformable and is made of, for example, a resin plate. The pressing member 10 has higher rigidity than the glass sheet G, and the glass sheet G is deformed when the pressing member 10 comes into contact with the glass sheet G.

[0050] The pressing member 10 is held by two arms 11. Each arm 11 is equipped with a holder 12 for holding the pressing member 10. The holder 12 can be rotated around point 13 shown in Figures 3 and 4 to adjust its inclination θ relative to the X direction. Point 13 is equipped with, for example, a screw. The inclination θ is preferably 30° or less. By adjusting the inclination θ, it is possible to adjust the curvature of the contact portion of the pressing member 10 with the first region G1 (the surface of the resin plate) in a cross section parallel to the horizontal direction. Here, "curvature" refers to the curvature of the portion of the pressing member 10 located between one holder 12 and the other holder 12. Adjusting this curvature can change the curvature of the surface Ga of the glass plate G, which has a convex curved surface. Note that by setting the inclination θ to 0°, the pressing member 10 can be extended straight without being curved (see Figure 5).

[0051] The ratio of the lateral dimension L2 of the pressing member 10 to the lateral dimension L1 of the first region G1 (L1 and L2 are shown in FIG. 1 ) is preferably 60% or more from the viewpoint of suitably preventing vibrations from occurring at the lower part of the glass sheet G during bending and breaking, and from the viewpoint of making the curvature of the glass sheet G in a cross section parallel to the lateral direction during bending as uniform as possible when bending and breaking a plurality of glass sheets G continuously using the manufacturing apparatus 1.

[0052] The two arms 11 are each connected to a drive unit 14. The drive unit 14 connected to one of the two arms 11 and the drive unit 14 connected to the other are configured to operate in synchronization. Each of the drive units 14, 14 has a built-in linear motion mechanism, for example, a combination of a cylinder or a ball screw and a linear motion guide, and this mechanism is used to move a plate 15 provided on the arm 11 in the Z direction. As the plate 15 moves in the Z direction, the pressing member 10 moves in the Z direction.

[0053] A fulcrum member 8 is attached to the plate 15 via a dust collector 16. The forward movement of the fulcrum member 8 toward the glass sheet G and the backward movement of the fulcrum member 8 away from the glass sheet G are accompanied by movement of the plate 15 along the Z direction. Furthermore, since the fulcrum member 8 and the pressing member 10 are connected to the common plate 15, the fulcrum member 8 and the pressing member 10 move synchronously along the Z direction. In other words, the fulcrum member 8 and the pressing member 10 move integrally along the Z direction. Note that the positions of the fulcrum member 8 and the pressing member 10 in the Z direction do not necessarily have to coincide. By changing the positions of the fulcrum member 8 and the pressing member 10 in the Z direction, the timing at which the fulcrum member 8 and the pressing member 10 contact the glass sheet G can be adjusted.

[0054] Two drive units 17, each having a structure similar to the drive unit 14, are arranged on the front surface Ga side of the glass sheet G. The two drive units 17, 17 are configured to operate in a synchronized manner. Each of the drive units 17, 17 is capable of moving a plate 18 along the Z direction. A pressing member 9 is attached to the plate 18 via a dust collector 19. The forward movement of the pressing member 9 toward the glass sheet G and the backward movement of the pressing member 9 away from the glass sheet G are accompanied by the movement of the plate 18 along the Z direction. The drive units 17 operate in synchronization with the drive units 14, and the pressing member 9 moves along the Z direction in synchronization with the fulcrum member 8 and the pressing member 10. In other words, the operation of the support member 4 (fulcrum member 8 and pressing member 9) to support the first region G1 and the operation of the pressing member 10 to press the first region G1 are synchronized.

[0055] The dust collectors 16, 19 are each equipped with a flexible cover member 20, 21. The cover members 20, 21 are capable of deforming to conform to the front surface Ga or back surface Gb upon contact with the glass sheet G. As a result, the cover members 20, 21 function to close the space around the scribe line S on the glass sheet G in cooperation with the dust collectors 16, 19, the fulcrum member 8, and the pressing member 9. The dust collectors 16, 19 are capable of sucking in glass powder generated when the glass sheet G is broken and recovering it from the closed space.

[0056] For example, the pressing member 6 is formed in a plate shape extending in the vertical direction. The pressing member 6 is movable along the Z direction. As the pressing member 6 moves along the Z direction, the second region G2 is pressed from the front surface Ga side toward the back surface Gb side when the glass sheet G is broken.

[0057] An adsorption member 22 is disposed at a position facing the pushing member 6 with the glass sheet G (second region G2) sandwiched therebetween. The adsorption member 22 is, for example, composed of a plurality of adsorption pads arranged in the vertical direction. The adsorption member 22 has a function of holding the second region G2 after cutting by adsorbing the back surface Gb of the second region G2 before and after bending.

[0058] The flow of the preparation process P1 and the folding process P2 performed using the manufacturing apparatus 1 will be described below.

[0059] First, as the traveling body 7 travels, the glass sheet G suspended in a vertical position by the holding members 3 is carried into the manufacturing apparatus 1. When the glass sheet G has been carried into the manufacturing apparatus 1, the state shown in Figures 1 and 3 is reached, and the preparation step P1 is started from this state.

[0060] In the example shown in Fig. 3, the glass sheet G is formed flat along the lateral direction. However, depending on the thermal history of the glass sheet G, the glass sheet G may have a warp in which the front surface Ga is a convexly curved surface in a cross section parallel to the lateral direction, or the glass sheet G may have a warp in which the back surface Gb is a convexly curved surface in a cross section parallel to the lateral direction. The "warp" referred to here does not mean a warp caused by applying an external force to the glass sheet G, but means a warp that the glass sheet G originally has.

[0061] In the preparation step P1, the driving units 14, 14 and the driving units 17, 17 are operated to advance the fulcrum member 8, the holding member 9, and the pressing member 10 toward the glass sheet G. This causes the fulcrum member 8 and the holding member 9 to sandwich and support the first region G1 of the glass sheet G from both the front and back sides. At the same time, the pressing member 10 presses the lower portion of the first region G1 from the back surface Gb side, curving the glass sheet G before bending so that the front surface Ga becomes a convex curved surface in a cross section parallel to the horizontal direction. This stabilizes the contact state between the fulcrum member 8 and the glass sheet G. Furthermore, the space around the scribe line S is closed by cover members 20, 21, etc. Additionally, the pressing member 6 is brought into contact with the front surface Ga of the second region G2 of the glass sheet G, and the suction member 22 is used to suction the back surface Gb of the second region G2. Completion of the preparation step P1 results in the state shown in FIG. 4 .

[0062] Here, as described above, when the glass sheet G has a warp such that the back surface Gb is a convexly curved surface in a cross section parallel to the horizontal direction, the front surface Ga of the glass sheet G is a concavely curved surface in a cross section parallel to the horizontal direction before the preparation step P1 is performed. Therefore, the concave and convex surfaces of the front and back surfaces of the glass sheet G in a cross section parallel to the horizontal direction are reversed before and after the preparation step P1. On the other hand, when the glass sheet G has a warp such that the front surface Ga is a convexly curved surface in a cross section parallel to the horizontal direction, the concave and convex surfaces of the front and back surfaces of the glass sheet G in a cross section parallel to the horizontal direction are not reversed before and after the preparation step P1. In other words, once the preparation step P1 is performed, regardless of whether the glass sheet G has a warp such that the front surface Ga or the back surface Gb is a convexly curved surface in a cross section parallel to the horizontal direction, the curvature state of the glass sheet G in a cross section parallel to the horizontal direction is uniform after the preparation step P1 is performed.

[0063] Once the preparation step P1 is completed, the bending and splitting step P2 is initiated, in which the glass sheet G, which has been formed into a convex curved surface in the preparation step P1, is bent and split along the scribe line S. Specifically, with the back surface Gb of the second region G2 held by the suction member 22, the pressing member 6 presses the second region G2 from the front surface Ga side. This causes the area around the scribe line S to curve so that the front surface Ga becomes convex, with the fulcrum member 8 serving as a fulcrum, and the glass sheet G is bent and split by bending stress. After cutting, the second region G2 is held by the suction member 22 and discarded in a predetermined disposal position. Glass powder generated during the bending and splitting is collected by dust collectors 16 and 19. This completes the bending and splitting step P2, and the glass sheet G is separated into the first region G1 and the second region G2, as shown in FIG. 6 .

[0064] Here, the following modifications can also be applied to the above embodiment.

[0065] In the above embodiment, the pressing member 10 presses the lower portion (lower edge portion) of the first region G1 of the glass sheet G, but this is not limited to this. The pressing member 10 may press a portion above the lower portion of the first region G1. However, even in this case, it is preferable to press the non-effective portion G1b with the pressing member 10 from the viewpoint of avoiding scratches or contamination of the effective portion G1a.

[0066] In the above embodiment, the lower end of the pressing member 10 is located below the lower end (lower side) of the glass sheet G, but this is not limitative. The lower end of the pressing member 10 may be located above the lower end of the glass sheet G.

[0067] In the above embodiment, the portions of the first region G1 (one lateral end and the other lateral end of the first region G1) sandwiched from both the front and back sides by the support members 4 (the fulcrum members 8 and the pressing members 9) are curved so that the surface Ga is a convex curved surface in a cross section parallel to the vertical direction, but this is not limited to this. The portion of the support member 4 facing the glass sheet G may be configured to be approximately parallel to the vertical direction, and the portions of the first region G1 sandwiched from both the front and back sides by the support members 4 may not be curved in a cross section parallel to the vertical direction.

[0068] In the above embodiment, the operation of the support member 4 (fulcrum member 8 and pressing member 9) supporting the first region G1 and the operation of the pressing member 10 pressing the first region G1 are synchronized, but this is not limited to this. The pressing member 10 may press the first region G1 after the support member 4 supports the first region G1, or the pressing member 10 may press the first region G1 after the support member 4 supports the first region G1.

[0069] In the above embodiment, a plate (resin plate) is used as the pressing member 10, but the present invention is not limited to this. The pressing member 10 may be made of a material other than a plate, as long as the contact portion of the pressing member 10 with the glass sheet G is curved so as to gradually protrude toward the glass sheet G as it moves toward the center in the lateral direction. However, it is preferable that the curvature of the curve be adjustable.

[0070] REFERENCE SIGNS LIST 1 Glass plate manufacturing apparatus 2 Bending mechanism 3 Holding member 4 Support member 5 Curving mechanism 10 Pressing member G Glass plate G1 First region G1a Effective portion G1b Non-effective portion G2 Second region Ga Front surface Gb Back surface P1 Preparation step P2 Bending step S Scribe line

Claims

1. A method for manufacturing a glass plate, comprising a bending and splitting step of bending and splitting a glass plate in a vertical position and having a scribe line formed on its front surface extending in the vertical direction, to divide a first region and a second region adjacent in the horizontal direction at the scribe line as a boundary, further comprising a preparation step of bending the glass plate before bending and splitting so that the shape of the surface becomes a convex curved surface in a cross section parallel to the horizontal direction, and the bending and splitting step is performed on the glass plate in the curved state after the preparation step.

2. The method for manufacturing a glass plate according to claim 1, characterized in that in the preparation step, the glass plate is pressed from its back surface by a pressing member.

3. The method for manufacturing a glass plate as described in claim 2, characterized in that the glass plate has the second region on both sides of the first region in the horizontal direction, and in the preparation step, an upper part of the glass plate is held by a holding member to suspend the glass plate, and a lower part of the first region is pressed by the pressing member.

4. The method for manufacturing a glass plate according to claim 3, characterized in that the first region includes an effective portion which will become a product and a non-effective portion which will not become a product, and in the preparation step, of the effective portion and the non-effective portion, the pressing member is brought into contact with only the non-effective portion.

5. A method for manufacturing a glass plate as described in claim 3 or 4, characterized in that in the preparation step, one lateral end and the other lateral end of the first region are supported by supporting members from both the front and back sides, and the lower part of the first region is pressed against the pressing member between the supporting member supporting the one lateral end and the supporting member supporting the other lateral end, the operation of having the supporting member support the first region and the operation of having the pressing member press the first region are synchronized.

6. A method for manufacturing a glass plate as described in claim 3 or 4, characterized in that the pressing member is shaped to extend in the horizontal direction, and the curvature of the contact portion of the pressing member with the glass plate in a cross section parallel to the horizontal direction is adjustable.

7. A method for manufacturing a glass plate as described in any one of claims 1 to 4, characterized in that in the preparation step, the glass plate before bending is curved so that the surface shape in a cross section parallel to the longitudinal direction is a convex curved surface.

8. A method for manufacturing a glass plate, comprising a bending and breaking step of bending and breaking a glass plate in a vertical position and having a scribe line formed on its front surface side extending in the vertical direction, thereby dividing a first region and a second region adjacent in the horizontal direction at the scribe line as a boundary, wherein the glass plate has the second region on both sides of the first region in the horizontal direction, and the method further comprises a preparation step of preparing the glass plate in a state for bending and breaking, wherein after the preparation step, the bending and breaking step is performed on the glass plate in a curved state, and in the preparation step, an upper part of the glass plate is held by a holding member to suspend the glass plate, and a lower part of the first region is pressed from the back surface side by a pressing member.

9. A glass plate manufacturing apparatus equipped with a bending and breaking mechanism that bends and breaks a glass plate in a vertical position, the glass plate having a scribe line extending in the vertical direction formed on the surface side, to divide a first region and a second region adjacent in the horizontal direction at the scribe line as a boundary, wherein the bending and breaking mechanism is equipped with a curvature imparting mechanism that curves the glass plate before bending and breaking so that the surface has a convex curved shape in a cross section parallel to the horizontal direction.

10. A glass plate manufacturing apparatus equipped with a bending and breaking mechanism that bends and breaks a glass plate in a vertical position, having a scribe line extending in the vertical direction formed on the front surface side, to separate a first region and a second region adjacent in the horizontal direction at the scribe line, wherein the glass plate has the second region on both sides of the first region in the horizontal direction, and the bending and breaking mechanism comprises a holding member that holds an upper portion of the glass plate to suspend it, and a pressing member that presses a lower portion of the first region from the back surface side.

Citation Information

Patent Citations

  • Method of manufacturing flat glass and apparatus for manufacturing same

    WO2021070583A1

  • Plate glass production method, production device therefor, and plate glass

    WO2022097324A1

  • Method for producing plate glass and apparatus for producing same

    WO2022097352A1