Sulfide solid electrolyte powder and method for manufacturing same, positive electrode layer, and lithium ion secondary battery

The sulfide solid electrolyte powder, with selectively surface-incorporated fluorine, addresses the reactivity issues in all-solid-state batteries by enhancing oxidative stability and conductivity, allowing for the use of high-potential electrodes and improving battery performance.

WO2024225085A1PCT designated stage expired Publication Date: 2024-10-31AGC INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014901
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Sulfide solid electrolytes in all-solid-state lithium-ion batteries exhibit high reactivity with positive electrodes at high voltages, leading to poor electrochemical stability and rapid deterioration.

Method used

A sulfide solid electrolyte powder is developed with a fluorine concentration less than 3% by mass, where fluorine is selectively incorporated into the surface of the particles through a solid-gas reaction with gases containing F elements, forming a Li-F bond to enhance oxidative stability and suppress reaction with positive electrode active materials.

Benefits of technology

The sulfide solid electrolyte powder maintains good lithium ion conductivity and electrochemical stability, enabling the use of high-potential positive electrode materials and improving the output and cycle characteristics of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000032_0000
    Figure 00000032_0000
  • Figure 00000033_0000
    Figure 00000033_0000
Patent Text Reader

Abstract

The present invention relates to a powder that is an aggregate of particles of a sulfide solid electrolyte, wherein the fluoride concentration in the powder is less than 3 mass%, the fluoride concentration on the particle surface measured by using X-ray photoelectron spectroscopy is 0.3 to 20 mass%, and the fluoride concentration in the powder is lower than the fluoride concentration on the particle surface.
Need to check novelty before this filing date? Find Prior Art

Description

Sulfide solid electrolyte powder and its manufacturing method, positive electrode layer and lithium ion secondary battery

[0001] The present invention relates to a sulfide solid electrolyte powder, a method for producing the same, a positive electrode layer, and a lithium ion secondary battery.

[0002] Lithium-ion secondary batteries are widely used in portable electronic devices such as mobile phones and laptop computers. Conventionally, liquid electrolytes have been used in lithium-ion secondary batteries. However, in recent years, all-solid-state lithium-ion secondary batteries, which use solid electrolytes as the electrolyte, have been attracting attention due to their potential for improved safety, high-speed charging and discharging, and compact housings.

[0003] Solid electrolytes are broadly classified into sulfide solid electrolytes and oxide solid electrolytes. Among them, sulfide solid electrolytes exhibit high ionic conductivity because they contain sulfide ions with high polarizability. 10 GeP 2 S 12 LGPS type crystals such as Li 6 P.S. 5 Argyrodite-type crystals such as Cl, Li 7 P 3 S 11 LPS crystallized glass and the like are known.

[0004] Interface Stability in Solid-State Batteries, Chem. Mater. 2016, 28, 266-273

[0005] On the other hand, sulfide solid electrolytes are known to have a narrow theoretical potential window and poor electrochemical stability due to their particularly high reactivity with positive electrodes that operate at high voltages (Non-Patent Document 1). That is, when assembled into a cell for an all-solid-state battery, sulfide solid electrolytes are prone to react with the positive electrode active material, raising concerns about rapid deterioration during battery operation.

[0006] In view of the above circumstances, an object of the present invention is to provide a sulfide solid electrolyte powder that maintains good lithium ion conductivity, is inhibited from reacting with a positive electrode active material, and has excellent oxidation stability. Another object of the present invention is to provide a method for producing the sulfide solid electrolyte powder, and a positive electrode layer and a lithium ion secondary battery that use the sulfide solid electrolyte powder.

[0007] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by pulverizing a sulfide solid electrolyte, followed by a solid-gas reaction with a gas containing element F, thereby incorporating element F into the surface of each particle constituting the powder, and have thus completed the present invention.

[0008] That is, the present invention relates to the following [1] to [9]. [1] A powder which is an aggregate of particles of a sulfide solid electrolyte, wherein the fluorine concentration in the powder is less than 3 mass %, and the fluorine concentration at the particle surfaces measured using X-ray photoelectron spectroscopy is 0.3 to 20 mass %, and the fluorine concentration in the powder is lower than the fluorine concentration at the particle surfaces. [2] The sulfide solid electrolyte powder according to [1], which exhibits an F1s peak in a spectrum measured using X-ray photoelectron spectroscopy, wherein the F1s peak includes a peak derived from Li—F bonds, and the ratio of the area of ​​the peak derived from Li—F bonds to the area of ​​the F1s peak is 0.90 or more. [3] The specific surface area of ​​the powder is 5 m 2 [4] A sulfide solid electrolyte powder according to any one of [1] to [3], wherein the sulfide solid electrolyte powder has a densitometric value of 0.01 / g or more. [5] A positive electrode layer comprising the sulfide solid electrolyte powder according to any one of [1] to [3]. [6] A lithium ion secondary battery comprising the sulfide solid electrolyte powder according to any one of [1] to [3].

[0009] [6] A method for producing a powder consisting of an aggregate of sulfide solid electrolyte particles, the method comprising: preparing a sulfide solid electrolyte; pulverizing the sulfide solid electrolyte to obtain a pulverized sulfide solid electrolyte; and contacting the pulverized sulfide solid electrolyte in a dry state with a gas containing F element while dispersing and fluidizing the pulverized sulfide solid electrolyte in a flowing air stream to cause a solid-gas reaction. [7] The gas containing F element is F 2 Gas, HF gas, NF 3 Gas, SF 6 Gas, CF 4 Gas, and BF 3 [8] The method for producing a sulfide solid electrolyte powder according to [6] above, wherein the solid-gas reaction is carried out at a temperature within a range of −100 to 500° C. [9] The specific surface area of ​​the pulverized sulfide solid electrolyte is 5 m or less. 2 / g or more.

[0010] The present invention provides a sulfide solid electrolyte powder that maintains good lithium ion conductivity, is inhibited from reacting with a positive electrode active material, and has excellent oxidation stability, a method for producing the same, and a positive electrode layer and a lithium ion secondary battery that include the sulfide solid electrolyte powder. As a result, it is possible to realize an all-solid-state lithium ion secondary battery that is excellent in output characteristics and cycle characteristics, and it is also possible to provide a lithium ion secondary battery that is used together with a high-potential positive electrode active material such as a 5 V class or above 5 V class.

[0011] Fig. 1 is a flow diagram showing a method for producing sulfide solid electrolyte powder according to this embodiment. Fig. 2 is a conceptual diagram showing a method for producing sulfide solid electrolyte powder according to this embodiment, in which pulverized sulfide solid electrolyte is brought into contact with a gas containing F element while being dispersed and fluidized in a flowing air current, thereby causing a solid-gas reaction. Fig. 3 is a conceptual diagram showing a method for producing sulfide solid electrolyte powder, in which pulverized sulfide solid electrolyte is left to stand and brought into contact with a gas containing F element, thereby causing a solid-gas reaction.

[0012] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified as desired without departing from the spirit of the present invention. Furthermore, the term "to" indicating a range of values ​​is used to mean that the values ​​before and after it are included as the lower and upper limits.

[0013] <Sulfide Solid Electrolyte Powder> The sulfide solid electrolyte powder according to this embodiment is an aggregate of sulfide solid electrolyte particles. The fluorine concentration in the powder is less than 3 mass %, and the fluorine concentration at the particle surface measured using X-ray photoelectron spectroscopy (XPS) is 0.3 to 20 mass %. The fluorine concentration in the powder is lower than the fluorine concentration at the particle surface.

[0014] The sulfide solid electrolyte powder according to this embodiment has a fluorine concentration of 0.3 to 20 mass% on the particle surface as measured using XPS. By incorporating elemental fluorine into the surface of each particle constituting the powder, oxidative decomposition at high potentials is suppressed, achieving excellent oxidation stability. This is because the elemental lithium present on the particle surface of the sulfide solid electrolyte bonds with the introduced elemental fluorine to form a Li—F bond with a wide potential window. It is believed that this shifts the properties in a direction that electrochemically suppresses oxidative decomposition, improving electrochemical stability.

[0015] Therefore, when the sulfide solid electrolyte powder according to this embodiment is used as a positive electrode layer or the like in a lithium ion secondary battery or the like, deterioration during battery operation can be suppressed. As a result, it is possible to realize an all-solid-state lithium ion secondary battery with excellent output characteristics and cycle characteristics, and it is also possible to provide a lithium ion secondary battery that uses the powder together with a high-potential positive electrode active material of 5 V class or over 5 V class.

[0016] The fluorine concentration on the particle surface may be 0.3 to 20% by mass, preferably 0.6 to 15% by mass, more preferably 0.6 to 12% by mass, and even more preferably 0.6 to 10% by mass. From the viewpoint of achieving good oxidation stability, the fluorine concentration is 0.3% by mass or more, and preferably 0.6% by mass or more.

[0017] On the other hand, if fluorine element is incorporated not only on the particle surface but also inside the particles, P-S bonds in the crystal structure of the sulfide solid electrolyte are broken and P-F bonds are formed. As a result, there is a concern that the performance of the electrolyte may be reduced due to changes in the arrangement, occupancy, and occupied sites of the elements. From the above viewpoint, the fluorine concentration is 20% by mass or less, preferably 15% by mass or less, more preferably 12% by mass or less, and even more preferably 10% by mass or less.

[0018] The sulfide solid electrolyte powder according to this embodiment, which will be described in detail later, is prepared by bringing a pulverized sulfide solid electrolyte in a dry state into contact with a gas containing element F while dispersing and fluidizing the powder in a flowing air current, thereby causing a solid-gas reaction, thereby incorporating element F into the surface of the powder. The fluorine concentration on the surface of the resulting particles can be adjusted by the concentration of element F in the gas during the solid-gas reaction, the total amount of element F in the gas introduced, the treatment temperature, etc.

[0019] In this specification, the fluorine concentration on the particle surface is a value measured using XPS. Specifically, the XPS spectrum of the particle surface is measured by XPS analysis of a sulfide solid electrolyte powder. Taking into account the influence of surface contamination, the total concentration (atomic number) of all elements detected from the spectrum, excluding carbon element (C) and oxygen element (O), is set to 100 at% (atoms%), and the atomic composition ratio of fluorine element (F) (proportion of the number of atoms, at%) is quantified. The atomic composition ratio (at%) of fluorine element (F) obtained in this way is converted to a mass ratio (mass%), and the fluorine concentration (mass%) on the particle surface is determined. The spectrum measured by XPS analysis is analyzed using analysis software Multipak manufactured by ULVAC PHI. The Shirley method is applied to remove the background of the spectrum, and the relative sensitivity coefficient included in the analysis software is used.

[0020] The fluorine concentration in the sulfide solid electrolyte powder according to this embodiment is less than 3% by mass, and may be 0.01% by mass or more but less than 3% by mass, preferably 0.01 to 1% by mass, more preferably 0.05 to 0.6% by mass, and even more preferably 0.05 to 0.3% by mass. From the viewpoint of suppressing cleavage of P—S bonds within the crystal structure of the sulfide solid electrolyte, the fluorine concentration is less than 3% by mass, preferably 1% by mass or less, more preferably 0.6% by mass or less, and even more preferably 0.3% by mass or less. The lower limit of the fluorine concentration in the powder is not particularly limited, but considering that the fluorine concentration on the particle surface is 0.3% by mass or more, it is typically 0.01% by mass or more, and may be 0.05% by mass or more.

[0021] The fluorine concentration in the powder in this specification is considered to be the same as the fluorine content in the sulfide solid electrolyte powder. A specific method will be described in detail in the Examples below, but the fluorine content obtained by subjecting the sulfide solid electrolyte powder to an alkali dissolution treatment, adjusting the pH, and then quantitatively analyzing the result using a fluoride ion composite electrode is taken as the fluorine concentration in the powder.

[0022] As described above, the sulfide solid electrolyte powder according to this embodiment incorporates elemental fluorine on the surface of the particles that make up the powder, but incorporates very little or no elemental fluorine inside the particles. This suppresses the cleavage of P-S bonds and the formation of P-F bonds within the crystal structure of the sulfide solid electrolyte, thereby suppressing the deterioration of electrolyte properties such as lithium ion conductivity that are associated with changes in the arrangement, occupancy, and site occupation of elements. Furthermore, the incorporation of elemental fluorine on the particle surface can suppress oxidative decomposition at high potentials, thereby achieving good oxidation stability. Therefore, the sulfide solid electrolyte powder according to this embodiment has a lower fluorine concentration in the powder than on the particle surface.

[0023] From the above viewpoints, the ratio of the fluorine concentration at the particle surface to the fluorine concentration in the powder is preferably 5 to 50, more preferably 7 to 48, and even more preferably 8 to 45. Here, the ratio is preferably 5 or more, more preferably 7 or more, and even more preferably 8 or more. There is no particular upper limit to the ratio, and a larger value is preferable. The ratio is generally about 50 or less. The ratio may also be 48 or less, or 45 or less.

[0024] In this embodiment, for example, a pulverized sulfide solid electrolyte obtained by pulverizing a sulfide solid electrolyte is brought into contact with a gas containing elemental F to cause a solid-gas reaction while being dispersed and fluidized in a flowing air current in a dry state. This allows elemental F to be selectively incorporated into the surface of the pulverized sulfide solid electrolyte while suppressing the incorporation of elemental F into the interior of the pulverized sulfide solid electrolyte, thereby obtaining desired particles.

[0025] The sulfide solid electrolyte powder according to this embodiment contains elemental fluorine at least on the particle surface, and exhibits an F1s peak in the spectrum measured by XPS analysis. The sulfide solid electrolyte must be measured in its powder form during the above measurement. This is because pressing the powder against an In foil or molding it into a pellet may result in a change in composition due to deterioration or deformation of the sample.

[0026] The ratio of the area of ​​the peak derived from the Li-F bond to the area of ​​the F1s peak is preferably 0.90 or more, more preferably 0.95 or more, even more preferably 0.98 or more, the larger the ratio the more preferable, and most preferably 1.00. When the area ratio is less than 1, it means that the F element is also bonded to elements other than the Li element. An example of an element other than the Li element is the P element. When the S element of the P-S bond in the crystal structure of the sulfide solid electrolyte is replaced with the F element to form a P-F bond, this can lead to disturbances in the crystal structure, which can affect the performance of the electrolyte. From the viewpoint of suppressing such effects, the area ratio is preferably within the above-mentioned range.

[0027] In this specification, the area of ​​the F1s peak and the area of ​​the peak derived from the Li—F bond are peak areas in the spectrum measured by XPS analysis.

[0028] In XPS analysis, a pass energy is selected so that the half-width of the Ag3d5 / 2 peak is 0.65 eV or less. The resulting spectrum is subjected to charge correction with reference to literature. Compared to the F1s peak, the peak derived from the Li-F bond is observed at a peak top in the range of 684.8 to 685.8 eV, and the peak derived from the P-F bond is observed 2.6 eV higher in binding energy than the peak derived from the Li-F bond.

[0029] The area of ​​each peak in the spectrum measured by XPS analysis is determined using the analysis software Multipak manufactured by ULVAC PHI, as in the case of determining the fluorine concentration on the particle surface. The Shirley method is also used to remove the background from the spectrum. Then, the peaks derived from the Li—F bond are separated from the F1s peak, and their areas are compared.

[0030] The specific surface area of ​​the sulfide solid electrolyte powder according to this embodiment is 5 m 2 / g or more is preferable, and 5 to 30m 2 / g is more preferable, and 10 to 25m 2 / g is more preferable, and 13 to 20m 2 / g is particularly preferred. Here, the larger the specific surface area, the smaller the particle diameter of the particles constituting the powder, meaning that the powder is a fine powder. Generally, the finer the particles, the more reactive they are, making homogenization difficult. In contrast, the sulfide solid electrolyte powder according to this embodiment is prepared by bringing the pulverized sulfide solid electrolyte into contact with a gas containing element F while dispersing and fluidizing it in a flowing air stream, thereby causing a solid-gas reaction. Therefore, even if the powder is fine, element F can be selectively introduced onto the surface, and desired particles can be obtained.

[0031] In this way, the sulfide solid electrolyte powder according to this embodiment can achieve the effects of the present invention even if the particles forming the aggregates are fine powders. 2 / g or more is preferable, and 10m 2 / g or more is more preferable, and 13m 2 The upper limit is not particularly limited, but from the viewpoint of handling, it is preferably 30 m 2 / g or less is preferable, and 25m 2 / g or less is more preferable, and 20m 2 / g or less is more preferable.

[0032] The specific surface area can be adjusted by appropriately changing the conditions for pulverizing the sulfide solid electrolyte.

[0033] The specific surface area in this specification is called the BET specific surface area, and is a value determined by the nitrogen adsorption BET multipoint method.

[0034] The average particle size of the particles constituting the sulfide solid electrolyte powder according to this embodiment is preferably such that the specific surface area falls within the above range. Although this varies depending on the type of sulfide solid electrolyte, the average particle size is preferably 0.1 to 5 μm, more preferably 0.3 to 3 μm, and even more preferably 0.5 to 2 μm. From the viewpoint of more significantly achieving the effects of the present invention, the average particle size is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 2 μm or less. Furthermore, while there is no particular lower limit for the average particle size, from the viewpoint of ease of handling, it is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more.

[0035] In this specification, the average particle size refers to the median size at which 50% by volume of the particles have a particle size equal to or less than this value when measured with a particle size distribution analyzer using a laser diffraction method.

[0036] The sulfide solid electrolyte before pulverization, which is the base of the sulfide solid electrolyte powder according to this embodiment, can be a conventionally known one. 7 P 3 S 11 Sulfide solid electrolytes having a crystal structure containing Li, P, and S elements, called LPS systems, such as Li 10 GeP 2 S 12The sulfide solid electrolyte may be a sulfide solid electrolyte having a crystal structure containing Li, Ge, P, and S, which is called an LGPS system, such as a sulfide solid electrolyte having an argyrodite-type crystal structure containing Li, P, S, and Ha, a sulfide solid electrolyte made of Li-P-S-Ha-based crystallized glass, or a sulfide solid electrolyte having a thiolisicon-type crystal structure. Alternatively, the sulfide solid electrolyte may be a sulfide solid electrolyte containing a crystalline phase having the above-mentioned crystal structure and an amorphous phase.

[0037] The argyrodite-type crystal structure has the composition formula Ag 8 GeS 6 The sulfide solid electrolyte powder according to this embodiment is not limited to the above crystal structure, and some elements may be substituted with other elements.

[0038] When the sulfide solid electrolyte powder according to this embodiment has an argyrodite-type crystal structure, it is more preferable that the Ha element contains at least one element, and even more preferable that the Ha element contains two or more elements, selected from the group consisting of Cl, Br, and I. Furthermore, it is more preferable that the sulfide solid electrolyte according to this embodiment contains at least one of Cl and Br, and even more preferable that the Ha element contains Cl and Br.

[0039] The argyrodite-type crystal structure preferably has the above structure, but the composition formula is Li α P.S. β Ha γIt is preferable that the element ratios satisfy the relationships of 5≦α≦7, 4≦β≦6, and 1.3≦γ≦2. It is more preferable that the element ratios satisfy the relationships of 5.1<α<6.3, 4<β<5.3, and 1.4≦γ≦1.9, and even more preferable that the element ratios satisfy the relationships of 5.2<α<6.2, 4.1<β<5.2, and 1.5≦γ≦1.8. That is, α is preferably 5 or more, more preferably greater than 5.1, even more preferably greater than 5.2, and preferably 7 or less, more preferably less than 6.3, and even more preferably less than 6.2. β is preferably 4 or more, more preferably greater than 4, even more preferably greater than 4.1, and preferably 6 or less, more preferably less than 5.3, and even more preferably less than 5.2. γ is preferably 1.3 or more, more preferably 1.4 or more, even more preferably 1.5 or more, and preferably 2 or less, more preferably 1.9 or less, and even more preferably 1.8 or less.

[0040] In the argyrodite-type crystal structure, some of the S element is replaced by Ha element, O element, Se element, Te element, BH element, etc. 4 , CN, etc. Also, a portion of the P element may be substituted with Si element, Al element, Sn element, In element, Cu element, Sb element, Ge element, etc.

[0041] The lithium ion conductivity of the sulfide solid electrolyte powder according to this embodiment is set to 1.0×10 from the viewpoint of obtaining good battery characteristics when used in a lithium ion secondary battery. -4 S / cm or more is preferable, and 5.0 × 10 -4 S / cm or more is more preferable, and 1.0 × 10 -3 S / cm or more is more preferable, and 2.5×10 -3 S / cm or more is particularly preferred.

[0042] The lithium ion conductivity in this specification is a value determined by applying a pressure of 380 MPa to a sulfide solid electrolyte powder to form a compact, and measuring the compact using an AC impedance measuring device. The AC impedance measurement conditions are a measurement frequency of 100 Hz to 1 MHz, a measurement voltage of 100 mV, and a measurement temperature of 25°C.

[0043] The oxidation stability of the sulfide solid electrolyte powder according to this embodiment can be evaluated using cyclic voltammetry measurement, and details will be explained in the examples described later.

[0044] The sulfide solid electrolyte powder according to the present embodiment is suitably used in an all-solid-state lithium ion secondary battery by treating it as desired by a conventionally known method, and then applying pressure together with a positive electrode active material or a negative electrode active material to form a positive electrode layer or a negative electrode layer, which is an electrode mixture, or by applying pressure together with an additive such as a binder as needed to form a solid electrolyte layer.

[0045] <Positive Electrode Layer> When used in a lithium-ion secondary battery, the sulfide solid electrolyte powder according to this embodiment can form a positive electrode layer together with a positive electrode active material and, if necessary, other components such as a binder. That is, the positive electrode layer according to this embodiment contains the sulfide solid electrolyte powder described in the above <Sulfide Solid Electrolyte Powder>. Preferred aspects of this sulfide solid electrolyte powder are also the same as the preferred aspects of the above <Sulfide Solid Electrolyte Powder>.

[0046] The positive electrode active material and other components contained in the positive electrode layer according to this embodiment may be conventionally known materials, such as a binder, a current collector, and a conductive additive.

[0047] The positive electrode active material is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMnO 2 ), lithium nickel cobalt manganese oxide, Li(Ni x Co y Mn z M a ) O 2 (x+y+z+a=1, 0≦x≦1, 0≦y≦1, 0≦z≦1, 0≦a≦1, and M is at least one selected from Al, Mg, Nb, Ti, Cu, Zn, and Cr), Li a M b (P.O. 4 ) c(wherein 1≦a≦4, 1≦b≦2, and 1≦c≦3, and M is at least one selected from Fe, V, Co, Mn, Ni, and VO), polyacetylene, polyaniline, polypyrrole, polythiophene, and polyacene. The positive electrode active material may be used alone or in combination of two or more types.

[0048] The sulfide solid electrolyte powder is used as a Li(Ni) x Mn y ) O 4 (x+y=2), Li(Mn x Ni y Fe z ) O 4 Spinel-type positive electrode active materials such as (x + y + z = 2), Li, which is known as a 5V or higher class positive electrode 2 CoPO 4 When the positive electrode layer is made using F or other positive electrode active materials, the excellent oxidation stability of the sulfide solid electrolyte is more significantly utilized, which is preferable.

[0049] The content of the positive electrode active material relative to the entire positive electrode layer according to this embodiment is, for example, preferably 50 to 99% by mass, more preferably 60 to 97% by mass, and even more preferably 70 to 95% by mass. From the viewpoint of increasing charge / discharge capacity, the content is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. Furthermore, from the viewpoint of ensuring lithium ion conductivity and electronic conductivity in the positive electrode layer, the content is, for example, preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 95% by mass or less.

[0050] The content of the sulfide solid electrolyte powder relative to the entire positive electrode layer according to this embodiment is, for example, preferably 1 to 30 mass%, more preferably 2 to 25 mass%, and even more preferably 3 to 20 mass%. Here, from the viewpoint of facilitating the movement of lithium ions absorbed and released by the positive electrode active material within the positive electrode layer and between the positive electrode layer and the solid electrolyte layer, the content is preferably 1 mass% or more, more preferably 2 mass% or more, and even more preferably 3 mass% or more. Furthermore, from the viewpoint of maintaining a high charge / discharge capacity due to the positive electrode active material, the content is, for example, preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less.

[0051] The positive electrode layer according to this embodiment can be formed by a conventionally known method, and may be formed by wet molding or dry molding.

[0052] In the case of wet molding, for example, the components constituting the positive electrode layer are dispersed or dissolved in a solvent to form a slurry, which is then coated in a layer (sheet), dried, and optionally pressed. If necessary, heat may be applied to remove the binder. The thickness of the positive electrode layer can be easily adjusted by adjusting the coating amount of the slurry, etc.

[0053] In the case of dry molding, for example, the positive electrode layer may be formed by dry press molding a material containing components constituting the positive electrode layer onto the surface of an object on which the positive electrode layer is to be formed (such as a positive electrode current collector or a solid electrolyte layer). Alternatively, the positive electrode layer may be formed on another substrate, which is then transferred to the surface of the object on which the positive electrode layer is to be formed.

[0054] From the viewpoint of being able to industrially and stably form a strong positive electrode layer on the surface of the object on which the positive electrode layer is to be formed, it is preferable to form the positive electrode layer on the surface of the object by wet molding using a solvent.

[0055] The thickness of the positive electrode layer is not particularly limited and may be appropriately determined depending on the desired battery performance. The thickness of the positive electrode layer is, for example, preferably 10 to 500 μm, more preferably 20 to 500 μm, and even more preferably 30 to 300 μm. From the viewpoint of achieving high capacity, the thickness is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. Furthermore, from the viewpoint of ensuring lithium ion conductivity and electronic conductivity in the thickness direction, the thickness is preferably 500 μm or less, and more preferably 300 μm or less.

[0056] <Sulfide Solid Electrolyte Layer> When used in a lithium ion secondary battery, the sulfide solid electrolyte powder according to this embodiment can form a sulfide solid electrolyte layer together with other components such as a binder, as necessary. In this case, the sulfide solid electrolyte layer contains the sulfide solid electrolyte powder described in the above <Sulfide Solid Electrolyte Powder>. Preferred aspects of this sulfide solid electrolyte powder are also the same as the preferred aspects of the above <Sulfide Solid Electrolyte Powder>.

[0057] As the binder and other components contained in the sulfide solid electrolyte layer, conventionally known binders and other components can be used.

[0058] The content of the sulfide solid electrolyte powder in the entire sulfide solid electrolyte layer is preferably 80 mass % or more, more preferably 90 mass % or more. The upper limit of the content is not particularly limited, but is, for example, 99.9 mass % or less.

[0059] The sulfide solid electrolyte layer can be formed by a conventionally known method, and may be formed by wet molding or dry molding.

[0060] In wet molding, for example, the components constituting the sulfide solid electrolyte layer are dissolved in a solvent or dispersed in a dispersion medium to form a slurry, which is then applied in a layer (sheet), dried, and optionally pressed to form the sulfide solid electrolyte layer. If necessary, a binder removal treatment may be performed by applying heat. The thickness of the sulfide solid electrolyte layer can be easily adjusted by adjusting the amount of the slurry applied, etc.

[0061] In the dry molding, a sulfide solid electrolyte layer can be formed by placing a powder of the sulfide solid electrolyte on the surface of a positive electrode, a negative electrode, etc. and dry press molding the powder. Alternatively, a sulfide solid electrolyte layer may be formed on another substrate and then transferred onto the surface of a positive electrode, a negative electrode, etc.

[0062] The sulfide solid electrolyte powder according to this embodiment may be used in the above-described positive electrode layer or sulfide solid electrolyte layer, or may be mixed with a negative electrode active material to form a negative electrode layer. Conventionally known negative electrode active materials, current collectors, binders, conductive additives, and the like used in the negative electrode layer may be used.

[0063] <Lithium-ion secondary battery> The lithium-ion secondary battery according to this embodiment includes the sulfide solid electrolyte powder described in the above <Sulfide solid electrolyte powder>. Preferred aspects of this sulfide solid electrolyte powder are also the same as the preferred aspects of the above <Sulfide solid electrolyte powder>.

[0064] The lithium ion secondary battery according to this embodiment may contain the sulfide solid electrolyte powder, and may include, for example, the cathode layer described in the above <Cathode Layer>, an electrolyte layer, and an anode layer. In this case, at least one of the electrolyte layer and the anode layer may contain the sulfide solid electrolyte powder. In another aspect, the lithium ion secondary battery may include the sulfide solid electrolyte layer described in the above <Sulfide Solid Electrolyte Layer>, a cathode layer, and an anode layer. In this case, at least one of the cathode layer and the anode layer may contain the sulfide solid electrolyte powder.

[0065] The lithium ion secondary battery may be made of a conventionally known material for its exterior body. The lithium ion secondary battery may also be made of a conventionally known shape, such as a coin shape, a sheet shape (film shape), a folded shape, a wound bottomed cylindrical shape, a button shape, or the like, which may be appropriately selected depending on the application.

[0066] <Method for Producing Sulfide Solid Electrolyte Powder> The method for producing sulfide solid electrolyte powder according to this embodiment includes the following steps in order, as shown in Fig. 1 : Step 1: A step of preparing a sulfide solid electrolyte; Step 2: As step S1, a step of pulverizing the sulfide solid electrolyte to obtain pulverized sulfide solid electrolyte; Step 3: As step S2, a step of contacting the pulverized sulfide solid electrolyte in a dry state with a gas containing F element while dispersing and flowing it in a flowing air stream to cause a solid-gas reaction.

[0067] Each step will be explained below in order.

[0068] Step 1: Step 1 is a step of preparing a sulfide solid electrolyte. The sulfide solid electrolyte may be synthesized or a commercially available one may be used. When synthesizing the sulfide solid electrolyte, a conventionally known method may be used.

[0069] When synthesizing a sulfide solid electrolyte, it is preferable to include, for example, a step of obtaining a raw material mixture, a step of reacting the raw material mixture, and a step of crystallizing or amorphizing the raw material mixture.

[0070] The reaction in the step of reacting the raw material mixture may be a thermal reaction or a mechanochemical reaction. The raw material mixture may be heated to crystallize or amorphize the mixture to obtain a sulfide solid electrolyte. In this case, a separate crystallization or amorphization step may not be included. In addition to the step of obtaining a crystalline phase or an amorphous phase, the method may also include a step of increasing the crystallinity or a step of rearranging the crystals.

[0071] The raw materials vary depending on the composition of the desired crystalline or amorphous phase, but may contain, for example, Li, P, and S. When an argyrodite-type crystalline phase containing Ha or an LPSHA-type crystallized glass containing Ha is desired, a raw material containing Ha in addition to Li, P, and S may be used.

[0072] Specifically, for example, when argyrodite-type crystals or Li-P-S-Ha-based crystallized glass is obtained, raw materials containing Li, P, S, and Ha are used. 7 P 3 S 11When obtaining LPS crystals or LPS crystallized glass such as those mentioned above, raw materials containing Li, P, and S are used. 10 GeP 2 S 12 When obtaining LGPS-based crystals such as those described above, raw materials containing Li, Ge, and S are used. When obtaining thiolisicon-type crystals, raw materials containing Li, S, Ge, and P are used. Conventionally known raw materials can be used for each of the above raw materials.

[0073] Step 2 Step 2 is a step of pulverizing the sulfide solid electrolyte prepared in Step 1 to obtain a pulverized sulfide solid electrolyte (Step S1). A conventionally known method can be used for the pulverization. Examples of the pulverization method include mixed pulverization by mechanical milling. When using a mechanical mill using a ball mill, examples include a rotary ball mill that imparts rotational motion to a container, a vibration ball mill that imparts vibrational motion, a planetary ball mill that imparts revolution and rotational motion, a bead mill, and Attritor (registered trademark). Among these, a planetary ball mill or a bead mill, which have a higher pulverization power, are preferred. Alternatively, a disk mill, a turbo mill, a vibration mill, or the like may be used.

[0074] The pulverization may be dry pulverization or wet pulverization using a dispersion medium. In the wet pulverization method, additives such as a dispersant may be further added in addition to the sulfide solid electrolyte and the dispersion medium.

[0075] The dispersion medium is not particularly limited, but since the sulfide solid electrolyte has a property of easily reacting with water and deteriorating, a non-aqueous solvent is preferred.

[0076] The type of non-aqueous solvent is not particularly limited, and examples thereof include hydrocarbon solvents, organic solvents containing a hydroxy group, organic solvents containing an ether group, organic solvents containing a carbonyl group, organic solvents containing an ester group, organic solvents containing an amino group, organic solvents containing a formyl group, organic solvents containing a carboxy group, organic solvents containing an amide group, organic solvents containing a benzene ring, organic solvents containing a mercapto group, organic solvents containing a thioether group, organic solvents containing a thioester group, organic solvents containing a disulfide group, and alkyl halides.

[0077] Examples of hydrocarbon solvents include cyclohexane, heptane, octane, and toluene, and cyclohexane, heptane, and octane are preferred from the viewpoint of low saturated water concentration. Also, from the viewpoint of adjusting the water concentration, it is preferred to mix these hydrocarbon solvents with toluene, dibutyl ether, or the like to form mixed solvents.

[0078] In order to prevent a decrease in lithium ion conductivity due to a reaction between the sulfide solid electrolyte and water during pulverization of the sulfide solid electrolyte, the water concentration in the dispersion medium is preferably low. The water concentration of the dispersion medium may be, for example, 170 ppm by mass or less, 150 ppm by mass or less, 120 ppm by mass or less, or 100 ppm by mass or less.

[0079] When a dispersant is used as the additive, examples thereof include an ether compound, an ester compound, and a nitrile compound.

[0080] The crushing is carried out so that the specific surface area of ​​the crushed sulfide solid electrolyte is 5m 2 The specific surface area of ​​the pulverized sulfide solid electrolyte is preferably 5 to 30 m / g or more. 2 / g is more preferable, and 10 to 25m 2 / g is more preferable, and 13 to 20m 2 / g is particularly preferred. The solid-gas reaction in step 3 can be carried out homogeneously even if the pulverized sulfide solid electrolyte is a very fine powder, and desired particles can be obtained. In order to obtain such a fine powder, the specific surface area should be 5 m 2 / g or more is preferable, and 10m 2 / g or more is more preferable, and 13m 2 The upper limit is not particularly limited, but from the viewpoint of handling, it is preferably 30 m 2 / g or less is preferable, and 25m 2 / g or less is more preferable, and 20m 2 / g or less is more preferable.

[0081] The pulverized sulfide solid electrolyte obtained in step 2 may be subjected to a drying step before being subjected to the subsequent step 3. By drying, even if a dispersion medium or additives remain in the sulfide solid electrolyte, they can be removed. As the drying method, a conventionally known method can be used, and for example, drying can be performed using a hot plate, a drying furnace, an electric furnace, or the like.

[0082] The temperature in the drying step is not particularly limited, but may be, for example, 100 to 200° C. The time for the drying step is also not particularly limited, but may be, for example, 10 minutes to 24 hours. The drying step may also be carried out under reduced pressure, for example, at an absolute pressure of 50 kPa or less.

[0083] Step 3: Step 3 is a step in which the pulverized sulfide solid electrolyte obtained in Step 2 or the subsequent drying step is dispersed and fluidized in a flowing air stream, and is brought into contact with a gas containing F element to cause a solid-gas reaction (Step S2). At this time, the pulverized sulfide solid electrolyte is in a dry state. This results in a powder that is an aggregate of particles of the sulfide solid electrolyte according to this embodiment.

[0084] The pulverized sulfide solid electrolyte is said to be in a dry state when the amount of the solvent used for pulverization, i.e., the pulverization solvent, remaining in the pulverized sulfide solid electrolyte is 5 mass% or less. The amount of remaining pulverization solvent can be determined, for example, by thermal gravimetric measurement. Furthermore, when the pulverization of the sulfide solid electrolyte is performed by dry pulverization, the obtained pulverized sulfide solid electrolyte can be said to be in a dry state.

[0085] In step 3, the dried, pulverized sulfide solid electrolyte is contacted with a gas containing element F while being dispersed and fluidized in a flowing air stream, thereby causing a solid-gas reaction between the pulverized sulfide solid electrolyte (solid) and the gas containing element F, resulting in the incorporation of element F into the surface of the pulverized sulfide solid electrolyte, thereby obtaining desired particles.

[0086] The flowing airflow means, for example, flowing a gas containing F element from the bottom to the top of the container, as shown by the arrows, through the pulverized sulfide solid electrolyte 1 in the container, as shown in FIG. 2 . The gas containing F element introduced from the bottom of the container is discharged from the top of the container, and in the process, the pulverized sulfide solid electrolyte 1 is stirred up, resulting in a dispersed flow of the pulverized sulfide solid electrolyte 1. Note that the pulverized sulfide solid electrolyte 1 tends to fall to the bottom of the container due to gravity, but the continuous inflow of the gas containing F element causes it to be stirred up again and dispersed in the flow. Also, reference numeral 2 in FIG. 2 denotes a filter, which prevents the pulverized sulfide solid electrolyte 1 from escaping the container.

[0087] Furthermore, the manner in which the pulverized sulfide solid electrolyte is dispersed and flowed by the flowing airflow is not limited to that shown in FIG. 2 . That is, it is sufficient that the gas containing the element F is passed through so that the pulverized sulfide solid electrolyte is suspended, and the pulverized sulfide solid electrolyte is dispersed and flowed. For example, the flow path through which the gas containing the element F flows is not particularly limited, and the gas may be passed from the top to the bottom of the container, or may be introduced through a side wall of the container, or may be discharged through a side wall of the container. Furthermore, the shape of the container is not particularly limited as long as the pulverized sulfide solid electrolyte is dispersed and flowed, and any shape is possible, such as a vertically elongated container as shown in FIG. 2 . Furthermore, a pipe may be used as the container, and the pulverized sulfide solid electrolyte may be transported by the flowing airflow while being dispersed and flowed.

[0088] In addition, in a conventional gas treatment of pulverized sulfide solid electrolyte, a gas is passed through the pulverized sulfide solid electrolyte 1 while the pulverized sulfide solid electrolyte 1 is left stationary, as shown in Fig. 3. In this case, the pulverized sulfide solid electrolyte 1 is not dispersed and fluidized, and therefore, the reaction of particles that are close to the gas among the particles that make up the pulverized sulfide solid electrolyte proceeds locally. As a result, the obtained powder contains a mixture of particles in which the reaction has progressed not only on the surface but also inside, and particles in which no reaction has occurred, making it difficult to obtain a sulfide solid electrolyte powder having the properties of the present embodiment.

[0089] In contrast, in the production method according to the present embodiment, the pulverized sulfide solid electrolyte is dispersed and fluidized, so that a solid-gas reaction between each particle constituting the powder and a gas containing elemental F occurs uniformly, and elemental F is uniformly incorporated into the surface of the particles without changing the internal crystal structure of the particles, thereby obtaining the desired sulfide solid electrolyte powder according to the present embodiment.

[0090] The gas containing the F element is not particularly limited, but for example, F 2 Gas, HF gas, NF 3 Gas, SF 6 Gas, CF 4 Gas, and BF 3 It is preferable that the gas contains at least one gas selected from the group consisting of F 2 It is more preferable that the gas contains at least one of a nitrogen gas and a HF gas.

[0091] The gas containing the F element is further mixed with nitrogen gas (N 2 It may also be a mixed gas with other gases.

[0092] The amount of fluorine treatment in step 3, i.e., the total inflow amount of F contained in the F-containing gas, is preferably 0.01 to 3 mass%, more preferably 0.03 to 1 mass%, and even more preferably 0.05 to 0.5 mass%, relative to the total amount of pulverized sulfide solid electrolyte. From the viewpoint of favorably progressing the solid-gas reaction, the total inflow amount is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and even more preferably 0.05 mass% or more. Furthermore, from the viewpoint of suppressing the incorporation of F into the interior of the sulfide solid electrolyte particles, the total inflow amount is preferably 3 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less.

[0093] The temperature of the solid-gas reaction in step 3 is preferably −100 to 500° C., more preferably −50 to 200° C. Here, from the viewpoint of favorably progressing the solid-gas reaction, the temperature is preferably −100° C. or higher, more preferably −50° C. or higher. Furthermore, from the viewpoint of suppressing the incorporation of elemental F into the interior of the sulfide solid electrolyte particles, the temperature is preferably 500° C. or lower, more preferably 200° C. or lower.

[0094] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. Examples 2 to 22 are working examples, and Examples 1 and 23 to 29 are comparative examples.

[0095] Example 1: Li under a dry nitrogen atmosphere 5.4 P.S. 4.4 Cl 0.8 Br 0.8 Lithium sulfide powder (manufactured by Sigma, purity 99.98%), diphosphorus pentasulfide powder (manufactured by Sigma, purity 99%), lithium chloride powder (manufactured by Sigma, purity 99.99%), and lithium bromide powder (manufactured by Sigma, purity 99.995%) were weighed and placed in a quartz test tube and vacuum sealed. After dissolving at 750 ° C. for 1 hour, the mixture was cooled to obtain a sulfide solid electrolyte. The obtained sulfide solid electrolyte was crushed in a mortar, then placed in a mixed solvent of heptane and dibutyl ether, and a 1 mm diameter alumina ball was added. The mixture was wet-pulverized for 120 minutes in a planetary ball mill. Thereafter, the mixture was dried at 180 ° C. for 3 hours to obtain a pulverized sulfide solid electrolyte in a dry state as shown in Table 1. The pulverized sulfide solid electrolyte obtained above was crushed by passing through a mesh before use.

[0096] <Examples 2 to 6, 8, 9, 14 to 19, 23, and 25> The pulverized sulfide solid electrolytes obtained in the same manner as in Example 1, except that the wet-pulverization conditions were changed to vary the specific surface area, were dried and crushed to prepare them in a dry state for use in a solid-gas reaction. Thereafter, the sulfide solid electrolytes were subjected to F treatment at the F treatment temperatures shown in Table 1 to obtain the F treatment amounts shown in Table 1. 2 Gas N 2 A gas containing elemental fluorine, appropriately diluted with a gas, was passed through the system, and the pulverized sulfide solid electrolyte was dispersed and fluidized while the pulverized sulfide solid electrolyte was brought into contact with the gas containing elemental fluorine, causing a solid-gas reaction. The F treatment amount refers to the amount of treatment with elemental fluorine, i.e., the total amount of elemental fluorine contained in the gas containing elemental fluorine relative to the total amount of pulverized sulfide solid electrolyte. This resulted in a powder that was an aggregate of sulfide solid electrolyte particles.

[0097] <Examples 7, 10 to 13, 20 to 22, 24, and 26> Pulverized sulfide solid electrolytes were obtained in the same manner as in Example 1, except that the specific surface area was varied by changing the wet-pulverization conditions. These were dried and crushed to prepare them in a dry state for use in a solid-gas reaction. HF gas was then added to the solid electrolytes at the F treatment temperatures shown in Table 1, with N 2 2 A gas containing F element appropriately diluted with a gas was passed through the furnace, and the pulverized sulfide solid electrolyte was dispersed and fluidized while the pulverized sulfide solid electrolyte was brought into contact with the gas containing F element to cause a solid-gas reaction, thereby obtaining a powder that was an aggregate of sulfide solid electrolyte particles.

[0098] Examples 27 to 29: The pulverized sulfide solid electrolyte obtained in the same manner as in Example 1, except that the wet pulverization conditions were changed to vary the specific surface area, was dried and crushed to prepare a dry state for use in a solid-gas reaction. The pulverized sulfide solid electrolyte was then placed at the bottom of a container and treated with F to achieve the F treatment amount shown in Table 1. 2 Gas N 2 A gas containing F element appropriately diluted with a gas was passed through the furnace, and the pulverized sulfide solid electrolyte was brought into contact with the gas containing F element to cause a solid-gas reaction. The F treatment temperature was room temperature (25°C). As a result, a powder that was an aggregate of sulfide solid electrolyte particles was obtained.

[0099] <Evaluation> Fluorine concentration on particle surface A sulfide solid electrolyte powder was subjected to wide scan XPS analysis using an X-ray photoelectron spectrometer (PHI5000 VersaProbeIII, manufactured by ULVAC PHI) equipped with a slow evacuation and slow leak mechanism under the following conditions: (Conditions) Wide scan analysis measurement conditions Analysis area: 100 μm diameter Detection angle: 45° relative to the sample surface X-ray source: Monochrome Al Kα radiation X-ray conditions: 100 μmφ, 25 W, 15 kV Pass energy: 224.0 eV Step energy: 0.4 eV / step Step time: 20 mS / step The powder was fixed to a sample holder using a powder sample holder (manufactured by ULVAC PHI).

[0100] The ratio of the number of fluorine atoms to the total number of atoms of all elements detected from the spectrum obtained above, excluding C and O to take into account the influence of surface contamination, was calculated and converted to a mass ratio, which was used as the fluorine concentration on the particle surface. For spectral analysis measured by XPS analysis, analysis software Multipak manufactured by ULVAC PHI was used. The Shirley method was applied to remove the spectral background, and the relative sensitivity coefficient included in the analysis software was used. The results are shown in Table 1 under "F concentration (surface) (mass %)." Note that blanks in each evaluation in Table 1 indicate that the measurement was not performed.

[0101] Fluorine concentration in powder The sulfide solid electrolyte powder was subjected to an alkaline dissolution treatment to adjust the pH to neutral. Thereafter, the fluorine content in the powder was quantitatively analyzed using a fluoride ion composite electrode (F-2021, manufactured by DKK-TOA Corporation). The value obtained here was calculated as the fluorine concentration in the powder. The results are shown in "F concentration (total) (mass%)" in Table 1.

[0102] F Concentration Ratio The ratio of the fluorine concentration on the particle surface to the fluorine concentration in the powder obtained above was calculated as the F concentration ratio. The results are shown in Table 1.

[0103] Li—F Bond Ratio XPS analysis by narrow scan analysis was performed on the sulfide solid electrolyte powder using an X-ray photoelectron spectrometer (PHI5000 VersaProbeIII, manufactured by ULVAC PHI) equipped with a slow evacuation and slow leak mechanism under the following conditions: (Conditions) Narrow scan analysis measurement conditions Analysis area: diameter 100 μm Detection angle: 45° to the sample surface X-ray source: Monochrome Al Kα radiation X-ray conditions: 100 μmφ, 25 W, 15 kV Pass energy: 27.0 eV Step energy: 0.025 eV / step Step time: 20 mS / step The powder was fixed to a sample holder using a powder sample holder (manufactured by ULVAC PHI).

[0104] The XPS spectrum obtained above was subjected to charge correction so that the Cl2p peak top was 198.8 eV, with reference to the following reference. Of the obtained peaks, the ratio of the area of ​​the peak derived from Li-F bonds, which has a peak top in the range of 684.8 to 685.8 eV, to the area of ​​the F1s peak was determined. This ratio means the ratio of F forming Li-F bonds to the total amount of F, and the total amount of F includes P-F bonds in addition to Li-F bonds. Furthermore, in addition to P-S bonds being broken to form P-F bonds, if a covalent bond in the crystal structure of the sulfide solid electrolyte unexpectedly breaks and recombines with an F element, the recombined F is also included in the total amount of F. Therefore, the proportion of Li-F bonds can be evaluated based on the above area ratio, and it can be evaluated whether fluorine elements are selectively incorporated on the surface of the particles or whether fluorine elements are incorporated into the interior of the particles. The results of the Li-F bond proportion are shown in Table 1. The peak derived from the Li-F bond was separated from the F1s peak using the analysis software Multipak manufactured by ULVAC PHI, and the Shirley method was applied to remove the spectral background. (Reference: Redox activity of argyrodite Li 6 P.S. 5 Cl electrolyte in all-solid-state Li-ion battery: An XPS study, J. Auvergniot et al. , Solid State Ionics, Vol. 300, pp. 78-85 (2017))

[0105] Specific surface area The specific surface area of ​​the sulfide solid electrolyte powder was measured using a specific surface area measuring device (Microtrac-Bell, Belsorp max II adsorption measuring device). 2 Measurement was carried out by the adsorption BET multipoint method to determine the specific surface area. The determined specific surface area can be considered to be the same as the specific surface area of ​​the pulverized sulfide solid electrolyte before the solid-gas reaction, that is, when the sulfide solid electrolyte is pulverized and dried. The measurements, including sampling and measurement, were carried out without contact with the atmosphere. Specifically, as a pretreatment, the sample was decompressed at room temperature for 12 hours or more. The sample weight was 0.5 g, and the relative pressure (P / P0 ) was measured at five or more points in the range of 0.05 to 0.3, and a BET plot was created. The specific surface area was calculated from the obtained BET plot. The results are shown in Table 1. Note that in Examples 27 to 29, the specific surface area is the specific surface area of ​​the pulverized sulfide solid electrolyte before the solid-gas reaction, and is therefore shown in parentheses.

[0106] Lithium ion conductivity: The sulfide solid electrolyte powder was pressed under a pressure of 380 MPa and used as a measurement sample. Measurements were performed using an AC impedance measuring device (VSP potentiostat / galvanostat, manufactured by Bio-Logic Sciences Instruments) under the following conditions: Measurement frequency: 100 Hz to 1 MHz, Measurement voltage: 100 mV, Measurement temperature: 25°C. The lithium ion conductivity at 25°C was determined from the obtained Nyquist plot.

[0107] The evaluation results are shown in Table 1. The lithium ion conductivity was 1.0 × 10 -3 If the resistance is 1.0 x 10 S / cm or more, it is considered to be good and is marked with "○". -4 S / cm or more 1×10 -3 If it is less than 1.0 x 10 S / cm, it is considered to be somewhat good and is marked with "△". -4 If it was less than S / cm, it was deemed to be poor and was marked "X".

[0108] Oxidation Stability The oxidation stability of the sulfide solid electrolyte powder was evaluated by cyclic voltammetry. First, 60 mg of the sulfide solid electrolyte powder was filled into a PEEK housing and manually compressed with a stainless steel stamp to obtain a solid electrolyte pellet.

[0109] Next, a working electrode composite was prepared to provide electronic conductivity as a working electrode. Specifically, a carbon nanotube having a specific surface area of ​​62 m2 measured by the BET method was used as the electronic conductive component of the working electrode composite. 2 / g of commercially available carbon black (Super C65, manufactured by TIMCAL) was dried in a Buchi oven at 300°C for 24 hours, and then heated at 800°C for 12 hours in a H 2 / Ar reduction flow (H in Ar 2The sulfide solid electrolyte powder and the carbon black were mixed in a mass ratio of 9:1 and pulverized and mixed in an agate mortar for 15 minutes. Then, 12 mg of the powder obtained by pulverization and mixing was placed on the solid electrolyte pellet obtained above and uniaxially pressed at 35 kN (440 MPa) for 3 minutes to prepare a working electrode.

[0110] A 9 mm diameter, 100 μm thick indium foil (ChemPur, purity 99.999%) was placed on the opposite side of the solid electrolyte pellet as a counter electrode. The resulting cell was fixed to an aluminum frame with a torque of 10 Nm, generating a pressure of approximately 60 MPa. Cyclic voltammetry measurements were performed using a three-electrode system, with indium metal used as the counter and reference electrodes.

[0111] When about 1 atom% of Li is incorporated into indium, the voltage drops to 0.62 V vs. Li + A stable open circuit voltage (OCV) of 1000kJ / Li was established. The cell was assembled and allowed to equilibrate for approximately 1 hour.

[0112] Using the equilibrated cell obtained above, cyclic voltammetry measurements were performed using a potentiostat (VMP300, manufactured by Biologic). The measurement temperature was 298 K, and the sweep was started from the OCV toward the higher potential side at a sweep rate of 0.1 mV / sec, and the sweep was performed in the range of 1.9 to 4.0 V vs. In / InLi. From the obtained cyclic voltammogram, the area (mA × V vs. In / InLi) in the range of 2.3 to 4.0 V vs. In / InLi was calculated.

[0113] The evaluation results are shown in Table 1. When the area obtained above was 0.8 or less, where the area of ​​Example 1 in which the solid-gas reaction with the gas containing F element was not carried out was taken as 1, the oxidation stability was deemed to be good and was marked with "◯". When the area was more than 0.8 but not more than 0.99, the oxidation stability was deemed to be somewhat good and was marked with "Δ". When the area was more than 0.99, the oxidation stability was deemed to be poor and was marked with "X".

[0114] In the evaluation results of the lithium ion conductivity and oxidation stability, a powder was determined to be good if it had at least one "○ (good)" and no "× (bad)" in the lithium ion conductivity and oxidation stability, i.e., if both the lithium ion conductivity and the oxidation stability were "○ (good)" or one was "○ (good)" and the other was "△ (fairly good)."

[0115]

[0116] From the above results, it was found that the sulfide solid electrolyte powder according to the present embodiment maintains good lithium ion conductivity while also exhibiting excellent oxidation stability. On the other hand, Examples 23 to 26 showed poor lithium ion conductivity. This is thought to be because the high F treatment amount led to fluorination not only on the surface of the particles constituting the powder but also to the interior, resulting in cleavage of P-S bonds and the formation of P-F bonds, etc. In addition, since the oxidation stability of Examples 23 and 24 was "Fair (fairly good)," attempts were made to improve the oxidation stability by increasing the F treatment amount. However, as shown in Examples 25 and 26, even with an increased F treatment amount, the oxidation stability actually worsened. This is thought to be because fluorine element was incorporated into the interior of the particles, cleaving P-S bonds in the crystalline structure of the sulfide solid electrolyte and the formation of P-F bonds, etc. In Examples 27 to 29, the sulfide solid electrolyte powder was contacted with a gas containing F element without being dispersed and fluidized. As a result, the lithium ion conductivity decreased and no improvement in oxidation stability was observed. This is also believed to be because fluorine element was incorporated into the interior of the particles, and P-S bonds in the crystal structure of the sulfide solid electrolyte were broken to form P-F bonds. Although the exact fluorine concentration on the particle surface of Example 28 was not measured, it was confirmed that the value was between the fluorine concentrations on the particle surface of Examples 27 and 28, and was more than 20 mass%.

[0117] From the results of the examples, it was confirmed that the effects of the present invention can be obtained over a wide range of F treatment amounts and F treatment temperatures. In addition, the effects of the present invention can be obtained even with fine powders having a large specific surface area and a small particle size. Furthermore, the type of gas used in the F treatment can be varied depending on the type of gas. 2The present invention is not limited to gases, and any gas containing F, such as HF gas, can provide good oxidation stability while maintaining lithium ion conductivity. Note that the above examples are based on results obtained when the F treatment temperature was between room temperature and 200°C, but it has been confirmed that even at a low temperature of, for example, -50°C, both the lithium ion conductivity and oxidation stability are excellent.

[0118] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-075082) filed on April 28, 2023, the contents of which are incorporated herein by reference.

[0119] 1. Pulverized sulfide solid electrolyte 2. Filter

Claims

1. A powder of a sulfide solid electrolyte which is an aggregate of particles of the sulfide solid electrolyte, wherein the fluorine concentration in the powder is less than 3 mass%, and the fluorine concentration on the particle surfaces measured using X-ray photoelectron spectroscopy is 0.3 to 20 mass%, and the fluorine concentration in the powder is lower than the fluorine concentration on the particle surfaces.

2. A sulfide solid electrolyte powder according to claim 1, which exhibits an F1s peak in a spectrum measured using X-ray photoelectron spectroscopy, the F1s peak includes a peak derived from a Li-F bond, and the ratio of the area of ​​the peak derived from the Li-F bond to the area of ​​the F1s peak is 0.90 or more.

3. The specific surface area of ​​the powder is 5 m 2 The sulfide solid electrolyte powder according to claim 1, wherein the sulfide solid electrolyte powder has a molecular weight of 1000 or more.

4. A positive electrode layer comprising the sulfide solid electrolyte powder according to any one of claims 1 to 3.

5. A lithium ion secondary battery comprising the sulfide solid electrolyte powder according to any one of claims 1 to 3.

6. A method for producing a powder consisting of an aggregate of sulfide solid electrolyte particles, comprising: preparing a sulfide solid electrolyte; pulverizing the sulfide solid electrolyte to obtain a pulverized sulfide solid electrolyte; and contacting the pulverized sulfide solid electrolyte in a dry state with a gas containing F element while dispersing and flowing the pulverized sulfide solid electrolyte in a flowing air current to cause a solid-gas reaction.

7. The gas containing the F element is F 2 Gas, HF gas, NF 3 Gas, SF 6 Gas, CF 4 Gas, and BF 3 The method for producing a sulfide solid electrolyte powder according to claim 6, further comprising the step of:

8. The method for producing a sulfide solid electrolyte powder according to claim 6 or 7, wherein the solid-gas reaction is carried out within a temperature range of -100 to 500°C.

9. The specific surface area of ​​the pulverized sulfide solid electrolyte is 5 m 2The method for producing a sulfide solid electrolyte powder according to claim 6 or 7, wherein the sulfide solid electrolyte powder has a molecular weight of 1000 or more.

Citation Information

Patent Citations

  • Sulfide solid electrolyte material, cathode body, and lithium solid-state battery

    JP2012048971A

  • Sulfide-based solid electrolyte, method for producing the sulfide-based solid electrolyte, and method for producing all solid-state battery

    JP2019199394A

  • Sulfide-based solid electrolyte powder to be used for lithium ion secondary battery, production method thereof, solid electrolyte layer, and lithium ion secondary battery

    JP2021086796A

  • Positive electrode layer used for lithium ion secondary battery, and lithium ion secondary battery

    JP2021136198A

  • Method of preparing sulfide-based solid electrolyte having excellent air stability

    US20180053966A1