Manufacturing method for contact body used for vibrating actuator, and vibrating actuator

The method of coating and vacuum-impregnating a sintered body with a high viscosity resin increases resin content in the contact body's pores, addressing the issue of reduced holding force due to wear by ensuring a consistent and high resin presence, thus enhancing the vibration type actuator's performance and durability.

WO2024225098A1PCT designated stage expired Publication Date: 2024-10-31CANON KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014987
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing vibration type actuators face challenges in maintaining a high holding force due to limited resin content in the contact body's pores, especially when the contact surface is worn, as the resin content decreases with wear, affecting the actuator's performance.

Method used

A method for manufacturing a contact body with a higher resin content in the pores on the contact surface and deeper positions, involving coating a sintered body with a fluid resin of 8,000 mPa·s viscosity and performing an impregnation process under vacuum conditions, where the sintered body is held at a pressure lower than atmospheric pressure, ensuring the resin penetrates deeper and maintains a higher concentration.

Benefits of technology

This approach results in a contact body with a higher resin content on the contact surface and deeper areas, enhancing the holding force of the vibration type actuator and maintaining it even when the contact surface is worn, thereby improving the actuator's performance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014987_31102024_PF_FP_ABST
    Figure JP2024014987_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A manufacturing method for a contact body according to the present invention is for manufacturing a contact body used in a vibrating actuator, and is characterized by comprising: an application step for applying a fluid resin having a viscosity of 8,000 mPa・s or higher on a portion of the surface of a sintered body having void parts therein; a coating step for coating void parts in a portion, of the surface of the sintered body, different from the aforementioned portion; and an impregnation step for keeping the sintered body coated with the fluid resin under a first atmospheric pressure that is less than ambient atmospheric pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing contact body used in vibration type actuator, and vibration type actuator

[0001] The present invention relates to a method for manufacturing a contact member used in a vibration type actuator, and to a vibration type actuator.

[0002] A vibration-type actuator is known in which a vibrating body and a contact body come into contact with each other, causing a predetermined vibration in the vibrating body, and applying a frictional driving force from the vibrating body to the contact body, thereby causing the contact body to move relatively to the vibrating body (hereinafter also referred to as "relative movement"). In a vibration-type actuator, an electromechanical energy conversion element such as a piezoelectric element is joined to the vibrating body, and vibration is generated in the vibrating body by applying an AC voltage to the electromechanical energy conversion element.

[0003] Such vibration actuators utilize the frictional force generated by contact, and are therefore characterized by their large holding force, which means that the positional relationship between the vibrating body and the contact body can be maintained (the vibrating body and the contact body can be stopped in that position) even when an external force is applied in a non-energized state.

[0004] Patent Document 1 describes a friction material in which a stainless steel sintered body is impregnated with a resin mixed with hard particles as a contact body used in such a vibration actuator. In this friction material, the impregnated resin acts as a sliding material, contributing to improved wear resistance and maintaining a high coefficient of friction. At the same time, the hard particles exert a spike effect, maintaining a high coefficient of friction even after being placed in high-temperature, high-humidity conditions, and good results can be expected.

[0005] Japanese Patent Application Laid-Open No. 2022-30103

[0006] In contact bodies made of sintered stainless steel with resin in the pores, the greater the resin content in the pores on the contact surface where the contact body comes into contact with the vibrating body, the greater the holding force that a vibration actuator using the contact body is expected to exhibit. Therefore, there has been a demand for the development of contact bodies with a greater resin content in the pores on the contact surface. Furthermore, if the resin content is high even in positions deeper than the contact surface, it is expected that the vibration actuator will maintain its holding force even if the contact surface wears.

[0007] The present invention aims to provide a method for manufacturing a contact body used in a vibration actuator, which has a higher resin content in the pores on the contact surface and also has a higher resin content at positions deeper than the contact surface.

[0008] Another object of the present invention is to provide a vibration actuator including a contact body in which the resin content is greater in the pores on the contact surface and the resin content is greater even at positions deeper than the contact surface.

[0009] The method for manufacturing a contact body used in a vibration type actuator according to the present invention is characterized by including a coating step of coating a part of the surface of a sintered body having voids with a fluid resin having a viscosity of 8,000 mPa·s or more, a coating step of covering the voids on the surface of the sintered body different from the part, and an impregnation step of holding the sintered body coated with the fluid resin under a first pressure that is lower than atmospheric pressure.

[0010] The vibration type actuator according to the present invention is a vibration type actuator including a vibrator having an electromechanical energy conversion element and an elastic body, and a contact body that is in contact with the surface of the elastic body at a contact surface, and the vibrator and the contact body move relatively due to vibration of the vibrator, and the contact body includes a sintered body having voids and a resin part in which resin is contained in the voids, and the ratio of the area occupied by the resin part to the contact surface is A 0 (%), and the ratio of the area occupied by the resin portion on the surface when the contact surface is polished 50 μm in the depth direction perpendicular to the contact surface is A 50 (%), A 0 is 8% or more, and the following general formula (1) is satisfied: (A 0 -A 50 ) / A 0 ≦0.25 (1)

[0011] According to the present invention, a method for manufacturing a contact body used in a vibration actuator can be provided, which has a higher resin content in the pores on the contact surface and also has a higher resin content at positions deeper than the contact surface.

[0012] Furthermore, according to the present invention, it is possible to provide a vibration type actuator including a contact body in which the resin content is higher in the pores on the contact surface and the resin content is also higher at positions deeper than the contact surface.

[0013] FIG. 1 is a schematic diagram illustrating a contact surface of a contact body according to the first to third embodiments. FIG. 2 is a diagram illustrating the resin ratio of a contact body according to the first to third embodiments. FIG. 3 is a diagram illustrating a vibration type actuator according to the first to third embodiments. FIG. 4 is a diagram illustrating a vibrating body of a vibration type actuator according to the first to third embodiments. FIG. 5 is a diagram illustrating a vibrating body of a vibration type actuator according to the first to third embodiments. FIG. 6 is a perspective view illustrating a method for manufacturing a contact body according to the first embodiment. FIG. 7 is a cross-sectional view illustrating a method for manufacturing a contact body according to the first embodiment. FIG. 8 is a cross-sectional view illustrating a method for manufacturing a contact body according to the first embodiment. FIG. 9 is a cross-sectional view illustrating a method for manufacturing a contact body according to the second embodiment. FIG. 10 is a cross-sectional view illustrating a method for manufacturing a contact body according to the second embodiment. FIG. 11 is a cross-sectional view illustrating a method for manufacturing a contact body according to the third embodiment. FIG. 12 is a cross-sectional view illustrating a method for manufacturing a contact body according to the third embodiment. FIG. 13 is a diagram illustrating a vibration type actuator having a ring-shaped contact body. FIG. 14 is a diagram illustrating the configuration of an imaging device such as a camera equipped with the vibration type actuator of the present invention. FIG. 15 is a diagram illustrating the configuration of an imaging device such as a camera equipped with the vibration type actuator of the present invention. FIG. 16 is a perspective view showing a schematic structure of a robot equipped with a vibration type actuator of the present invention.

[0014] As a contact body used in a vibration actuator, a sintered body containing resin in the pores is known, which is obtained by performing an impregnation process on a sintered body having pores. In order for the contact body to exert a high holding force with the vibrator included in the vibration actuator, it is required that the pores on the surface of the contact body that comes into contact with the vibrator (hereinafter referred to as the contact surface) contain a large amount of resin.

[0015] As a result of extensive research, the present inventors have found that a larger amount of resin can be contained in the pores by performing the impregnation treatment in a vacuum environment. That is, the inventors have found that the process of applying a fluid resin to the surface of a sintered compact and then placing the sintered compact in a vacuum environment, or the process of applying a resin to the surface of a sintered compact placed in a vacuum environment, improves the resin content in the pores compared to impregnation treatment performed only under normal pressure.

[0016] Furthermore, the inventors have found that the efficiency of the impregnation treatment in a vacuum environment can be improved by covering in advance the surface of the sintered body other than the surface to be coated with resin (hereinafter referred to as the coating surface) with a hard-to-adhere jig, container, etc. The mechanism behind this is presumed to be as follows.

[0017] First, as an impregnation treatment, a sintered body is held in a vacuum environment, with the surface to be coated covered with resin and the other surfaces covered with a poorly adhesive jig or container. Resin may also be applied to the surface of the sintered body while held in a vacuum environment. At this time, gases such as air present inside the pores of the sintered body escape to the outside of the sintered body, where the air pressure is lower, due to the difference in air pressure between the inside of the pores and the outside of the sintered body. The sintered body is then held under atmospheric pressure or an atmospheric pressure close to atmospheric pressure. At this time, the air outside the sintered body is drawn into the pores, where the air pressure is lower, and the resin applied to the surface of the sintered body is forced into the pores.

[0018] In this way, by covering the surface other than the coating surface with a container or a hard-to-adhere jig in advance and performing the impregnation treatment in a vacuum environment, it is possible to obtain a contact body with a high resin content at the contact surface.Furthermore, it is possible to obtain a contact body in which the resin content at the contact surface is less likely to decrease even when the contact surface is worn.

[0019] Hereinafter, each embodiment of the present invention will be described in detail with reference to the drawings.

[0020] 2 is a diagram illustrating the schematic configuration of a vibration actuator 1. The vibration actuator 1 has a vibrating body 2 and a contact body 6 that contacts the vibrating body 2. The vibrating body 2 has an elastic body 3 and a piezoelectric element 4 that is an electromechanical energy conversion element bonded to a surface of the elastic body 3 facing in a second direction. The elastic body 3 has a flat plate portion and two protrusions 5 provided in a first direction outside the plane of the plate portion. The vibration actuator can be manufactured by a step of preparing a vibrator that has an electromechanical energy conversion element and an elastic body, and a step of contacting the elastic body with a contact body.

[0021] A "contact body" refers to a member that comes into contact with the vibrating body and moves relative to the vibrating body due to vibrations generated in the vibrating body. The contact between the contact body and the vibrating body is not limited to direct contact where no other member is interposed between them. The contact between the contact body and the vibrating body may also be indirect contact where another member is interposed between the contact body and the vibrating body, as long as the contact body moves relative to the vibrating body due to vibrations generated in the vibrating body. The "other member" is not limited to a member independent of the contact body and the vibrating body (for example, a high-friction material including a sintered body). The "other member" may also be a surface-treated portion of the contact body or the vibrating body formed by plating, nitriding, or the like.

[0022] 3A is a diagram illustrating a first vibration mode (hereinafter referred to as "mode A") of the two bending vibration modes excited in the vibrating body 2. A common electrode (full-surface electrode) (not shown) is formed on the surface of the piezoelectric element 4 facing the elastic body 3, and drive electrodes (not shown) are formed on the surface opposite to the surface facing the elastic body 3, which are divided into two equal parts in the length direction.

[0023] The A-mode is a secondary bending vibration in the longitudinal direction (X direction) of the vibrating body 2, and has three nodal lines that are approximately parallel to the short side direction (Y direction (width direction)) of the vibrating body 2. A-mode vibration can be excited in the vibrating body 2 by applying an alternating voltage with a predetermined frequency and a phase shift of 180° to the drive electrodes of the piezoelectric element 4. The protrusions 5 are arranged near positions that become nodes in the A-mode vibration, and when A-mode vibration is excited in the vibrating body 2, it performs a reciprocating motion in the X direction.

[0024] 3B is a diagram illustrating a second vibration mode (hereinafter referred to as "B mode") of the two bending vibration modes excited in the vibrating body 2. The B mode is a primary bending vibration in the short-side direction (Y direction) of the vibrating body 2, and has two nodal lines that are approximately parallel to the longitudinal direction (X direction). B-mode vibration can be excited in the vibrating body 2 by applying an in-phase alternating voltage at a predetermined frequency to the drive electrodes of the piezoelectric element 4. The protrusion 5 is disposed near a position that becomes an antinode in the B-mode vibration, and when B-mode vibration is excited in the vibrating body 2, the protrusion 5 performs a reciprocating motion in the axial direction (Z direction) of the protrusion 5.

[0025] The vibrating body 2 is configured so that the nodal lines in the A mode and the B mode are approximately perpendicular in the XY plane. A flexible substrate (not shown) is attached to the piezoelectric element 4, and by supplying an AC current to the piezoelectric element 4 through the flexible substrate, it is possible to simultaneously excite the vibrating body 2 in the A mode and the B mode. Therefore, by exciting the A mode and the B mode vibrations with a predetermined phase difference, it is possible to generate elliptical motion at the tip of the protrusion 5 in the ZX plane.

[0026] In the vibration actuator 1, the vibrating body 2 is in contact with the contact body 6. Therefore, in a state where the contact body 6 is supported so as to be drivable in the driving direction (longitudinal direction of the contact body 6) shown by the arrow in Figure 2, by simultaneously exciting A-mode and B-mode vibrations in the vibrating body 2, the contact body 6 can be frictionally driven by the protrusions 5 and driven in the driving direction.

[0027] 2 does not show the support member that supports the contact body 6 so that it can be driven, the holding member that holds the vibrating body 2, the pressure means for bringing the vibrating body 2 into contact with the contact body 6, etc. In this embodiment, the vibrating body 2 is fixed and the contact body 6 is drivable, but it is also possible to configure the contact body 6 to be fixed and the vibrating body 2 to be driven together with the holding member. Also, as shown in FIG. 7, the contact body 66 may be ring-shaped, and multiple vibrating bodies 2 may be arranged and driven to rotate.

[0028] 4A to 4D are diagrams illustrating a method for manufacturing the contact body 6 shown in Fig. 2. The contact body 6 of this embodiment includes a sintered body 6a shown in Fig. 4A. The sintered body 6a is preferably a sintered body containing martensitic stainless steel equivalent to SUS420J2, for example.

[0029] The sintered body 6a is produced by molding a raw material powder obtained by mixing SUS410L powder and carbon powder, each having a particle size of 150 μm or less, and then maintaining the resulting molded body at a predetermined temperature below the melting point to bond the powder particles together (sintering step). The sintered density of the sintered body 6a is preferably in the range of 6.1 g / cc to 6.6 g / cc.

[0030] In order to improve the wear resistance of the friction sliding surface, the Vickers hardness of the sintered body 6a is preferably 550 HV0.2 or more, and more preferably 600 HV0.2 or more. The hardness of the sintered body 6a is adjusted by sinter hardening, which is a heat treatment during the sintering process by adjusting the cooling rate in the sintering furnace, or by quenching. The Vickers hardness of the sintered body 6a can be measured using a micro-Vickers test. In order to reduce the effect on the hardness measurement of deformation near the surface of the sintered body 6a due to the presence of voids in the sintered body 6a, it is preferable to measure the hardness using a micro-Vickers test force of 200 g (= 0.2 kg) on ​​the metal surface polished after resin impregnation.

[0031] A two-component curing liquid adhesive can be used as the fluid resin to be applied to the sintered body 6a. Furthermore, to facilitate observation of the resin contained in the pores, the resin may be pre-contained with a fluorescent dye. The resin (adhesive) may be a mixture of a liquid epoxy resin as the main component and an amine compound as the main component of the curing agent. The viscosity after mixing is preferably 8,000 mPa·s or more and 30,000 mPa·s or less. Since a high coefficient of friction is expected after curing, the viscosity of the resin is preferably 8,000 mPa·s. Furthermore, to further improve the holding force when the contact body is used in a vibration actuator, it is desirable to add hard particles to the resin. The hard particles are preferably GC, a high-purity, high-hardness SiC abrasive grains.

[0032] Next, as shown in Fig. 4A, a covering member 90 is prepared to cover the surfaces of the sintered body 6a other than the surface to be coated with resin (hereinafter referred to as the coating surface). The covering member 90 is preferably made of rubber, and more preferably, at least a portion of the surface of the covering member 90 contains a hard-to-adhere material such as Teflon (registered trademark). Because the covering member 90 is made of rubber and is flexible, the sintered body 6a can be easily removed from the covering member 90. Because the covering member 90 contains a hard-to-adhere material on its surface, the sintered body 6a can be easily removed from the covering member 90.

[0033] 4B shows a longitudinal cross-sectional view of the sintered body 6a of Fig. 4A set in a covering member 90. In the covering process, the sintered body 6a is fitted into a covering member 90 having a cavity matching the shape of the sintered body 6a, so that the surfaces other than the surface 6c to be coated with resin are in contact with the covering member 90. As a result, the pores on the surfaces of the sintered body 6a other than the surface 6c are covered.

[0034] 4C, a liquid epoxy resin 6e is applied to the surface 6c (application surface) of the sintered body 6a that will become the friction portion. The application of the resin 6e may be performed, for example, using a dispenser device (not shown). After the application of the resin 6e, it is confirmed that the resin 6e has been applied to at least the entire surface 6c.

[0035] Then, in the impregnation step, the surface of the covering member 90 on the side where the epoxy resin 6e is not applied is brought into contact with the plate surface in the heated vacuum heating device, and a vacuum is then created. The temperature of the plate surface of the vacuum heating device is preferably, for example, about 80°C. The viscosity of the epoxy resin 6e is reduced by the heat conducted to the epoxy resin 6e via the covering member 90 and the sintered body 6a, thereby facilitating the movement of the epoxy resin 6e inside the pores.

[0036] Here, the vacuum heating device is a device capable of heating and maintaining a pressure lower than atmospheric pressure in a closed space. The vacuum state is preferably a state in which the pressure is reduced to, for example, −0.085 MPa.

[0037] The reason why the impregnation efficiency is improved by the process of this embodiment will be explained. According to the principle that air moves from high pressure to low pressure, the air present in the pores of the sintered body 6a in a vacuum state passes through the applied epoxy resin 6e. When the sintered body 6a is then returned to atmospheric pressure, the applied resin is forced into the pores of the sintered body 6a by the atmospheric pressure, allowing the resin to be impregnated at a high content even at deeper positions in the sintered body 6a.

[0038] Furthermore, if surfaces other than the resin-coated surface 6c are in contact with the atmosphere, air will enter from these surfaces when the pressure is returned to atmospheric pressure, preventing the resin from penetrating into the pores. Therefore, in this embodiment, by covering the surfaces of the sintered body other than the coated surface with a covering member 90, the resin can be effectively contained in the pores.

[0039] In this embodiment, an example in which both heating and evacuation are performed has been described, but heating may be omitted. Furthermore, instead of a rubber container, silicone tape may be used as a covering member, and the surface of the sintered body other than the application surface may be covered with the silicone tape. Furthermore, instead of sealing the pores of the sintered body with a covering member, a highly viscous resin that does not contain a fluorescent dye may be applied in advance to the surfaces of the sintered body 6a other than the surface to be coated with the resin, and then cured.

[0040] Furthermore, the order of the steps included in the manufacturing process is not limited to the order described above. For example, the manufacturing process may include a step of applying a resin to the coated surface of the sintered body after applying a pressure below atmospheric pressure (second pressure), and then holding the sintered body under a pressure below atmospheric pressure (first pressure). In this case, the first pressure and the second pressure may be the same. By holding the sintered body under the same pressure as in the impregnation step in advance, water molecules adhering to the inside of the pores of the sintered body and gas within the pores can be removed. Furthermore, the first pressure may be lower than the second pressure. By performing the coating step under a second pressure higher than the first pressure, the resin can be applied while vacuuming, thereby shortening the time required for the manufacturing process.

[0041] After the impregnation process, the inside of the vacuum heating device is returned from the vacuum state to atmospheric pressure (1 atmosphere). It is also possible to return the pressure to atmospheric pressure higher than the atmospheric pressure at which the impregnation process was carried out, rather than returning it all at once. Furthermore, to harden the epoxy resin 6e, the sintered body is left in an environment at a constant temperature for a certain period of time. To quickly harden the resin, it is preferable to leave the sintered body in an environment at approximately 80°C for about 30 minutes. Since the epoxy resin used hardens at room temperature, leaving it at a high temperature is not essential. Once the resin has hardened, the sintered body 6a is removed from the covering member 90.

[0042] In this series of resin impregnation processes, a larger amount of resin is applied than the amount that will actually penetrate into the holes, so after hardening, the resin remains on the surface corresponding to the contact surface. In order to remove this resin and to adjust the flatness of the contact surface and back surface and the thickness of the contact body 6 to the specified values, grinding is performed after the resin hardens, and further polishing is performed to adjust the surface roughness, etc., to obtain the contact body 6 as a finished product.

[0043] The structure of the contact surface of the contact body 6 is explained using the schematic diagram in FIG. 1A. FIG. 1A shows an image of the contact surface, which was photographed using an optical microscope in fluorescence observation mode and then binarized so that the resin portion is white and the rest of the surface is black, combined with an image of the pores (shown as a grid-like shape) that do not contain resin. The image of the pores can be obtained by photographing the same position using the optical microscope in reflected light observation mode. The photograph can be taken, for example, using a Carl Zeiss Axio Imager. A1m, which can obtain an observation image with a magnification of 200x and a photographing range of approximately 363 μm × 272 μm. Based on these observation images, the proportion of the area occupied by the resin portion on the contact surface of the contact body (hereinafter referred to as the "resin ratio") can be measured for each polishing depth.

[0044] Alternatively, the resin percentage may be calculated by other methods, such as by using images obtained using a laser microscope and depth data. If the resin contained in the pores does not contain a fluorescent dye, the resin content of the resin previously contained can be calculated by further impregnating the pores on the surface with a resin containing a fluorescent dye.

[0045] In measuring the resin content, it is desirable to measure multiple locations on the contact body surface that are spaced apart from each other and calculate the average value. In evaluating a ring-shaped contact body, it is particularly desirable to measure at 90° intervals or 30° intervals in the circumferential direction and calculate the average value.

[0046] Thus, the contact surface of the contact body is composed of a metal portion, a resin portion in which resin is contained in the pores, and pores that do not contain resin. In other words, the total proportion of the "metal portion," "resin portion," and "pores that do not contain resin" in the contact surface of the contact body 6 is 100%. The total proportion of the "pores" and "metal portion" in the sintered body is 100%, and the total proportion of the "resin portion" and "pores that do not contain resin" is the proportion of the "pores" in the sintered body. When SUS410L powder with a particle size of 150 μm or less is used as the raw material for the sintered body, the pores in the sintered body 6a have a maximum length of several μm to approximately 100 μm.

[0047] The ratio of the area occupied by the resin part to the contact surface is A. 0 (%), and the ratio of the area occupied by the resin portion to the surface when the contact surface is polished by 50 μm in the depth direction perpendicular to the contact surface is A. 50 (%), A 0 is 8% or more, and it is desirable that the following general formula (1) is satisfied: (A 0 -A 50 ) / A 0 ≦0.25 (1)

[0048] In this way, a higher proportion of the resin portion (resin rate) on the contact body surface allows the vibration actuator to exhibit a high holding force. Furthermore, a small rate of decrease in the resin rate within a certain polishing depth range of the contact body allows the vibration actuator to exhibit a high holding force even when the contact body surface is worn. Furthermore, because the resin content is less likely to decrease even at positions deeper than the surface of the sintered body, the resin content on the surface of the resulting contact body is likely to be at or above a certain level even when there is variation in the amount of polishing of the sintered body surface during the manufacturing process.

[0049] Example 1 An example of manufacturing the contact body 6 according to the first embodiment will be specifically described below. Instead of fitting the sintered body 6a into the covering member 90, the surfaces other than the coated surface are covered with a highly viscous resin, which is then cured. After that, epoxy resin is applied to the coated surface, and the sintered body 6a and the covering member 90 are left in a vacuum environment to be impregnated with the resin. In this example, a ring-shaped contact body as shown in FIG. 7 was manufactured.

[0050] In this example, martensitic stainless steel equivalent to JIS standard SUS420J2 was used as the sintered body 6a. The sintered body 6a was manufactured by molding a raw material powder made by mixing SUS410L powder with a particle size of 150 μm or less and carbon powder, and then maintaining the resulting molded body at a predetermined temperature below the melting point of the stainless steel to bond the powder together (sintering process).

[0051] A two-component curing adhesive was used as the resin to be impregnated into the pores of the sintered body 6a. Furthermore, a fluorescent dye was mixed into the resin (adhesive) in advance to observe the resin contained in the pores. In this example, the resin (adhesive) used consisted of a base agent whose main component was a liquid epoxy resin and a curing agent whose main component was an amine compound. The viscosity of the two resin components after mixing was 8,000 mPa·s or more and 30,000 mPa·s or less. Furthermore, to further improve the holding force when the contact body is used in a vibration actuator, GC, a hard particle made of SiC abrasive grains with extremely high purity and hardness, was dispersed in the resin.

[0052] Next, a highly viscous resin that does not contain fluorescent dye was applied to the surfaces of the sintered body 6a other than the surface to be coated with the resin and then cured to cover the surfaces other than the coated surface. In the coating process, a two-liquid resin mixture was applied to the entire surface to be coated (surface 6c) of the sintered body 6a using a dispenser.

[0053] Furthermore, in the impregnation process, the surface of the covering member 90 on the side where the epoxy resin 6e was not applied was brought into contact with a plate surface in a vacuum heating device heated to about 80°C, and a vacuum was created. In this example, the air pressure was reduced to -0.085 MPa as the step of creating a vacuum.

[0054] After the interior of the vacuum heating device was returned to normal pressure (1 atmosphere), the sintered body 6a was left in an environment of about 80°C for about 30 minutes. After confirming that the resin had hardened, the sintered body 6a was removed from the covering member 90. The obtained composite of the sintered body and resin was polished using a copper surface plate and free diamond abrasive grains (3 µm) to smooth the contact surface, thereby obtaining a contact body.

[0055] Next, the manufactured contact bodies were evaluated. Fluorescence and reflected light observations of the surfaces of the contact bodies were performed using an optical microscope, and the resin content of the surfaces of the contact bodies was calculated. Both images were taken at 200x magnification using a Carl Zeiss Axio Imager A1m, with a photographed area of ​​approximately 363 μm × 272 μm.

[0056] The results of measuring the resin ratio for each polishing depth are shown in Figure 1B. Note that instead of filling the pores of the sintered body with the covering member of this example, a highly viscous resin that does not contain fluorescent dye was applied to the surfaces of the sintered body 6a other than the coated surface and then cured.

[0057] In FIG. 1B, the results of the conventional manufacturing method disclosed in Patent Document 1 are shown by a dotted line, and the results of this example are shown by a solid line.

[0058] The density of a sintered body sintered in the same lot as the measured sintered body was measured by the Archimedes method and was found to be 6.3 g / cc. Since the density of ingot SUS420J2 is 7.75 g / cc, the proportion of voids in the sintered body is approximately 19%.

[0059] The proportion of voids on the polished surface at each polishing depth was measured using images taken at 200x magnification using a Carl Zeiss Axio Imager A1m in reflected light observation mode. The measurement range was approximately 363 μm × 272 μm. Polishing scratches of a few microns or less in depth caused by the abrasive grains used during polishing were not counted as voids.

[0060] The resin percentage was measured using images of the same field of view captured using a Carl Zeiss Axio Imager A1m in fluorescence observation mode. Because the resin contains a fluorescent dye, only the resin portion emits light when observed under a fluorescence microscope, allowing the percentage of the impregnated resin portion to be measured.

[0061] As shown in Figure 1B, the resin content decreased with increasing distance from the coating surface. The rate of change was particularly large up to a polishing depth of approximately 0.05 mm. This is thought to be because there are few necks where sintered powder particles bond together at a depth of approximately 0 to 0.05 mm, which is the outermost layer of the sintered body 6a.

[0062] In this example, the decrease in resin content was smaller at a polishing depth of about 0.05 mm or more than that of the conventional manufacturing method. Also, the resin content on the polished surface at the same polishing depth was higher than that of the conventional manufacturing method.

[0063] [Second embodiment] A second embodiment of the present invention will be described with reference to Figures 5A to 5C. Figures 5A to 5C are diagrams illustrating a method for manufacturing the contact body 6 of Figure 2. The method for manufacturing the sintered body 6a is the same as in the first embodiment. Furthermore, the resin contained in the pores may be the same, so a description thereof will be omitted.

[0064] As shown in Figure 5A, difficult-to-adhere jigs 91a and 91b are prepared to prevent the pores of the sintered body 6a from coming into contact with the atmosphere during resin impregnation. The difficult-to-adhere jig 91 obtained by combining the difficult-to-adhere jigs 91a and 91b has cavities larger than those of the sintered body. The difficult-to-adhere jigs 91a and 91b are preferably made of difficult-to-adhere plastics or rubbers such as EPDM rubber, polypropylene resin, or Teflon resin. A release agent may be applied to the difficult-to-adhere jigs.

[0065] 5B shows a longitudinal cross-sectional view of the sintered body 6a of FIG. 5A set between the difficult-to-adhere jigs 91a and 91b and coated with resin. The epoxy resin 6e is not only applied to the surface to be coated using a dispenser (not shown), but also to the surfaces of the sintered body 6a other than the surface in contact with the difficult-to-adhere jig 91, i.e., the gap between the difficult-to-adhere jig 91a and the sintered body 6a, which are filled with epoxy resin 6e. To protect the contact surface, it is desirable for the gap between the difficult-to-adhere jig 91a and the sintered body 6a to be 5 μm or larger. This process prevents the pores in the sintered body 6a from contacting the atmosphere.

[0066] Thereafter, the surface of the hard-to-adhere jig 91 on the side not coated with the epoxy resin 6e is brought into contact with the plate surface in the heated vacuum heating device, and a vacuum is then created. The temperature of the plate surface of the vacuum heating device is preferably, for example, about 80°C. When the pressure is then returned to atmospheric pressure, the coated resin is forced into the pores of the sintered body 6a by the atmospheric pressure, thereby accelerating impregnation.

[0067] If surfaces other than the resin-coated surface 6c are in contact with the atmosphere when the pressure is returned to atmospheric pressure, air may enter from these surfaces when the pressure is returned to atmospheric pressure, which may prevent the resin from being impregnated. In this embodiment, surfaces other than the resin-coated surface 6c are also in close contact with the resin or the hard-to-adhere jig 91a, so they can be effectively impregnated when the pressure is returned to atmospheric pressure. In this embodiment, both heating and evacuation were performed, but heating may be omitted.

[0068] Thereafter, the epoxy resin 6e is left to harden at approximately 80°C for about 30 minutes. Note that the epoxy resin used hardens at room temperature, so leaving it at a high temperature is not necessary. Once the resin has hardened, the sintered body 6a is released from the difficult-to-adhere jigs 91a and 91b. Because the difficult-to-adhere jigs 91a and 91b are made of a difficult-to-adhere material, the resin coated around the sintered body can be easily released from the difficult-to-adhere jigs 91a and 91b.

[0069] In this series of resin impregnation processes, the amount of resin applied is greater than the amount actually required for impregnation (penetration), so the hardened resin remains on the surface of the sliding portion. To remove this resin and to adjust the flatness of the contact portion and back surface and the thickness of the contact body 6 to the specified values, grinding is performed after the resin has hardened, and further polishing is performed to adjust the surface roughness, etc., to obtain the contact body 6 as a finished product. As a result, the surfaces of the contact body other than the contact surface are coated with resin with a film thickness of 5 μm or more, which is also expected to improve the corrosion resistance of the contact body.

[0070] [Third Embodiment] A third embodiment of the present invention will be described with reference to Figures 6A to 6C. Figures 6A to 6C are diagrams illustrating a method for manufacturing the contact body 6 in Figure 2. The method for manufacturing the sintered body 6a is the same as in the first embodiment. The resin used may also be the same, so its description will be omitted.

[0071] As shown in Figure 6A, a highly workable container 92 is prepared to prevent the pores of the sintered body 6a from coming into contact with the atmosphere during resin impregnation. A general-purpose material with high workability can be used as the material for the highly workable container 92, and AES resin is more preferred. The dimensions of the highly workable container 92 and the dimensions of the sintered body 6a are designed based on the desired dimensions of the contact body 6.

[0072] 6B shows a longitudinal cross-sectional view of the sintered body 6a of FIG. 6A placed in a highly workable container 92 and coated with resin. Liquid epoxy resin 6e is applied to the surface 6ac of the sintered body 6a that will become the friction part using a dispenser (not shown), and the outer surface of the sintered body 6a, i.e., the gap between the highly workable container 92 and the sintered body 6a, is also filled with epoxy resin 6e. This prevents the pores of the sintered body 6a from coming into contact with the atmosphere.

[0073] Thereafter, the surface of the highly workable container 92 on the side not coated with the epoxy resin 6e is brought into contact with the plate surface in the heated vacuum heating device, and a vacuum is then created. The temperature of the plate surface of the vacuum heating device is preferably, for example, about 80°C. When the pressure is then returned to atmospheric pressure, the coated resin is forced into the pores of the sintered body 6a by the atmospheric pressure, thereby accelerating impregnation.

[0074] If surfaces other than the resin-coated surface 6c are in contact with the atmosphere when the pressure is returned to atmospheric pressure, air will enter from these surfaces when the pressure is returned to atmospheric pressure, preventing the resin from being impregnated. In this embodiment, surfaces other than the resin-coated surface 6ac are also covered with resin or a highly workable container 92, so that the resin can be effectively impregnated when the pressure is returned to atmospheric pressure. In this embodiment, both heating and evacuation are performed, but heating may be omitted.

[0075] The epoxy resin 6e is then left to harden at approximately 80°C for approximately 30 minutes. Since the epoxy resin used hardens at room temperature, leaving it at a high temperature is not necessary. During this series of resin impregnation processes, the amount of resin applied is greater than the amount actually impregnated (penetrated), resulting in residual hardened resin on the surface of the sliding portion. To remove this resin and to adjust the flatness of the contact portion and back surface and the thickness of the contact body 6 to the desired values, grinding is performed after the resin hardens, and further polishing is performed to adjust the surface roughness, etc., to obtain the finished contact body 6 shown in Figure 6C. The side surfaces may be cut or polished. In this case, cutting and polishing may be performed together with the highly workable container 92 without removing the sintered body from the highly workable container 92. In other words, the contact body may be obtained by polishing the surface of the composite of the highly workable container, sintered body, and resin. By processing the highly workable container 92 together to obtain the contact body, the surface of the contact body can be protected by the highly workable container.

[0076] <Application Examples of Vibration Actuator> Next, an imaging device and an industrial robot will be described as examples of optical and electronic equipment to which the vibration actuator 1 using the contact body 6 described above is applied.

[0077] 8A is a top view showing a schematic configuration of an imaging device 700 (device), which is an example of optical equipment. The imaging device 700 includes a camera body 730 equipped with an image sensor 710 and a power button 720. The imaging device 700 also includes a lens group (not shown) and a lens barrel 740 equipped with a vibration actuator. The lens group is driven by the vibration actuator. The lens barrel 740 is replaceable as an interchangeable lens, and a lens barrel 740 appropriate for the subject being photographed can be attached to the camera body 730. The vibration actuator described with reference to FIG. 2 can be used as the vibration actuator.

[0078] Driving a lens using a vibration actuator is considered to be suitable for driving an autofocus lens, but is not limited to this, and it is considered possible to drive a zoom lens with a similar configuration. Furthermore, a vibration actuator can also be used to drive an image sensor, or to drive a lens or image sensor during image stabilization.

[0079] 8B is a cross-sectional view showing a simplified example of a configuration in which the vibration actuator 1 is mounted on a lens barrel 740, and is shown as a cross section including the optical axis L. The contact body 6 is arranged so that its contact surface comes into contact with the protrusion 5 (reference numeral omitted in FIG. 8B ) of the vibrating body 2. On the surface of the contact body 6 opposite the contact surface, an output transmission member 9 is installed with a rotor rubber (vibration-proof rubber) 8 sandwiched therebetween.

[0080] Meanwhile, on the holding base 43 that holds the vibrating body 2 so as not to inhibit vibration, a leaf spring 10 is provided on the side opposite the contact body 6 as pressure means for pressing the vibrating body 2 against the contact body 6 with a predetermined force. Also, in order to compress the leaf spring 10 and generate a pressure force, a pressure ring 18 that regulates the amount of deflection of the leaf spring 10 is disposed, and the leaf spring 10 is sandwiched between the pressure ring 18 and the holding base 43. In this way, an appropriate pressure force is applied between the vibrating body 2 and the contact body 6.

[0081] A flange 16a is formed on the barrel unit main body 16, protruding perpendicularly to the optical axis direction (extension direction of the optical axis L), and a manual ring 15 for manual focusing is manually rotatably mounted on one surface of the flange 16a. In addition, a roller ring 19, which can be rotated by rotating the manual ring 15 or by transmitting the output of the vibration actuator 1, is mounted between the manual ring 15 and the vibration actuator 1. When the roller ring 19 is rotated, a cam ring and the like are rotated via an output key 17 provided on the roller ring 19.

[0082] The roller ring 19 has roller shafts 13 formed at multiple locations extending radially, and rollers 14 are attached to the roller shafts 13 so as to be rotatable around them. The output transmission member 9 and manual ring 15 are stacked in the optical axis direction, sandwiching the rollers 14 between them. The inner periphery of the pressure ring 18 engages with the barrel unit main body 16 via a screw or bayonet structure. The compression amount of the leaf spring 10 can be adjusted by rotating the pressure ring 18 and moving it in the optical axis direction. In this way, each part from the holding base 43 through the manual ring 15 to the flange 16a is clamped and pressurized.

[0083] When the vibration actuator 1 is driven, the contact body 6 rotates around the optical axis L, which causes the contact body 6, rotor rubber 8, and output transmission member 9 to rotate integrally around the optical axis L. Then, the roller 14 in contact with the output transmission member 9 rotates around the optical axis L together with the roller ring 19 while rolling on the surface of the manual ring 15, and the output key 17 attached to the roller ring 19 rotates a cam ring (not shown), thereby performing autofocus operations and the like.

[0084] FIG. 9 is a perspective view showing a schematic configuration of a robot 100 (device) equipped with a vibration actuator 1, which is an example of an electronic device. Here, a horizontal articulated robot, which is a type of industrial robot, is shown as an example.

[0085] The robot 100 has an arm joint 111 and a hand 112. The arm joint 111 connects two arms 120 so that the angle at which the two arms intersect can be changed. The hand 112 has an arm 120, a gripper 121 attached to one end of the arm 120, and a hand joint 122 connecting the arm 120 and the gripper 121. Vibration actuators are built into the arm joint 111 and the gripper 121, and perform angle adjustment and rotational movement of the arm 120 and the hand joint.

[0086] For bending the arm joint 111 and gripping the hand 112, a vibration actuator having a TN characteristic (drooping characteristic showing the relationship between load torque and rotation speed) of high torque at low rotation speed is preferably used.

[0087] While the present invention has been described in detail above based on preferred embodiments thereof, the present invention is not limited to these specific embodiments, and various modifications within the scope of the present invention are also included. For example, an XY stage can be cited as an example of a device that can drive a flat contact body in any direction within its plane.

[0088] The disclosure of this embodiment includes the following methods and configurations.

[0089] (Method 1) A method for manufacturing a contact body used in a vibration type actuator, comprising: a coating step of applying a fluid resin having a viscosity of 8,000 mPa·s or more to a portion of the surface of a sintered body having voids; a coating step of covering the voids on the surface of the sintered body different from the portion; and an impregnation step of holding the sintered body coated with the fluid resin under a first pressure that is lower than atmospheric pressure.

[0090] (Method 2) The method for producing a contact body according to Method 1, wherein the impregnation step is carried out after the application step and the coating step.

[0091] (Method 3) The method for producing a contact body according to Method 1, wherein the applying step is carried out under a second pressure that is lower than atmospheric pressure, and then the impregnating step is carried out.

[0092] (Method 4) The method for producing a contact body according to Method 3, wherein the first and second atmospheric pressures are the same.

[0093] (Method 5) The method for producing a contact body according to Method 3, wherein the first atmospheric pressure is lower than the second atmospheric pressure.

[0094] (Method 6) The method for producing a contact body according to Method 1, wherein the coating step is carried out by fitting the sintered body into a coating member and bringing a surface of the coating member into contact with a surface of the sintered body different from the part of the sintered body, and the coating member has a cavity that matches the shape of the sintered body.

[0095] (Method 7) The method for producing a contact body according to Method 6, further comprising the step of removing the sintered body from the covering member after the impregnation step.

[0096] (Method 8) A method for manufacturing a contact body according to Method 1, characterized in that the covering step includes a step of placing the sintered body in a poorly adhesive jig having a cavity larger than the sintered body, and the applying step includes a step of covering with the resin a surface of the sintered body other than a surface of the sintered body that is in contact with the poorly adhesive jig.

[0097] (Method 9) The method for manufacturing a contact body according to Method 8, characterized in that the method includes a demolding step of demolding a sintered body having at least a portion of its surface covered with the resin from the poor-adhesion jig, and the poor-adhesion jig includes a poor-adhesion material on at least a portion of its surface.

[0098] (Method 10) The method for producing a contact body according to Method 1, wherein the covering step includes a step of placing the sintered body in a highly workable container, and the applying step includes a step of covering an outer surface of the sintered body with the resin.

[0099] (Method 11) The method for producing a contact body according to Method 10, characterized in that the method for producing a contact body includes, after the impregnation step, a step of polishing a surface of a composite of the highly workable container, the sintered body, and the resin to obtain the contact body.

[0100] (Method 12) A method for manufacturing a vibration type actuator, comprising the steps of: obtaining a contact body by performing each step described in any one of Methods 1 to 11; preparing a vibrator having an electromechanical energy conversion element and an elastic body; and bringing the elastic body into contact with the contact body, thereby obtaining a vibration type actuator.

[0101] (Configuration 1) A vibration type actuator comprising: a vibrator having an electromechanical energy conversion element and an elastic body; and a contact body that is in contact with the surface of the elastic body at a contact surface, wherein the vibrator and the contact body move relatively due to vibration of the vibrator; the contact body includes a sintered body having voids and a resin part in which a resin is contained in the voids; and the proportion of the area occupied by the resin part in the contact surface is defined as A. 0 (%), and the ratio of the area occupied by the resin portion to the surface when the contact surface is polished by 50 μm in the depth direction perpendicular to the contact surface is A. 50 (%), A 0 is 8% or more, and the following general formula (1) is satisfied: (A 0 -A 50 ) / A 0 ≦0.25 (1)

[0102] (Configuration 2) The vibration type actuator according to configuration 1, wherein the resin includes an epoxy resin.

[0103] (Configuration 3) The vibration type actuator according to configuration 1, wherein a surface of the contact body different from the contact surface is coated with a resin having a film thickness of 5 μm or more.

[0104] (Configuration 4) The vibration actuator according to Configuration 1, wherein the sintered body is a stainless steel sintered body having a primary particle size of 150 μm or less and a sintered density of 6.1 g / cc to 6.6 g / cc, and hard particles are added to the resin.

[0105] (Configuration 5) An optical device including: the vibration actuator according to any one of configurations 1 to 4; and at least one of an optical element and an imaging element driven by the vibration actuator.

[0106] (Configuration 6) An electronic device comprising: a member; and the vibration type actuator according to any one of configurations 1 to 5, which drives the member.

[0107] The present invention is not limited to the above-described embodiments, and various modifications and variations can be made without departing from the spirit and scope of the present invention. Therefore, the following claims are appended to apprise the public of the scope of the present invention.

[0108] This application claims priority based on Japanese Patent Application No. 2023-071681, filed April 25, 2023, the entire contents of which are incorporated herein by reference.

[0109] REFERENCE SIGNS LIST 1 vibration type actuator 2 vibrating body 6 contact body 6a sintered body 6e resin

Claims

1. A method for manufacturing a contact body used in a vibration type actuator, comprising: a coating step of applying a fluid resin having a viscosity of 8,000 mPa·s or more to a portion of the surface of a sintered body having voids; a coating step of covering the voids on the surface of the sintered body different from the portion; and an impregnation step of holding the sintered body to which the fluid resin has been applied under a first pressure that is lower than atmospheric pressure.

2. The method for producing a contact body according to claim 1, wherein the impregnation step is carried out after the application step and the covering step.

3. The method for producing a contact body according to claim 1, wherein the coating step is carried out under a second pressure lower than atmospheric pressure, and then the impregnation step is carried out.

4. The method for producing a contact body according to claim 3, wherein the first atmospheric pressure and the second atmospheric pressure are the same.

5. A method for producing a contact body according to claim 3, wherein the first atmospheric pressure is lower than the second atmospheric pressure.

6. The method for manufacturing a contact body described in claim 1, characterized in that the coating process is performed by fitting the sintered body into a coating member and contacting a surface of the coating member with a surface of the sintered body that is different from the portion of the sintered body, and the coating member has a cavity that matches the shape of the sintered body.

7. The method for producing a contact body according to claim 6, further comprising the step of removing the sintered body from the covering member after the impregnation step.

8. A method for manufacturing a contact body as described in claim 1, characterized in that the covering step includes a step of placing the sintered body in a poorly adhesive jig having a cavity larger than the sintered body, and the application step includes a step of covering with the resin a surface of the sintered body other than the surface of the sintered body that is in contact with the poorly adhesive jig.

9. The method for manufacturing the contact body described in claim 8, characterized in that the method includes a demolding step of demolding a sintered body having at least a portion of its surface covered with the resin from the poor-adhesion jig, and the poor-adhesion jig includes a poor-adhesion material on at least a portion of its surface.

10. The method for manufacturing a contact body according to claim 1, characterized in that the coating step includes a step of placing the sintered body in a highly workable container, and the coating step includes a step of covering the outer surface of the sintered body with the resin.

11. The method for producing a contact body according to claim 10, characterized in that the method includes, after the impregnation step, a step of obtaining the contact body by polishing the surface of the composite of the highly workable container, the sintered body, and the resin.

12. A method for manufacturing a vibration type actuator, comprising: a step of obtaining a contact body by carrying out each step according to any one of claims 1 to 11; a step of preparing a vibrator having an electromechanical energy conversion element and an elastic body; and a step of bringing the elastic body into contact with the contact body, thereby obtaining a vibration type actuator.

13. A vibration actuator comprising: a vibrator having an electromechanical energy conversion element and an elastic body; and a contact body that is in contact with the surface of the elastic body at a contact surface, wherein the vibrator and the contact body move relatively due to vibration of the vibrator, the contact body including a sintered body having a void portion and a resin portion having a resin contained in the void portion, and a ratio of an area of ​​the resin portion to the contact surface is A. 0 (%), and the ratio of the area occupied by the resin portion to the surface when the contact surface is polished by 50 μm in the depth direction perpendicular to the contact surface is A 50 If (%), A 0 is 8% or more, and the following general formula (1) is satisfied: 0 -A 50 ) / A 0 ≦0.25 (1) 14. The vibration type actuator according to claim 13, wherein the resin includes an epoxy resin.

15. The vibration actuator according to claim 13, characterized in that a surface of said contact body different from said contact surface is coated with a resin having a film thickness of 5 μm or more.

16. The vibration actuator according to claim 13, characterized in that the sintered body is a stainless steel sintered body having a primary particle size of 150 μm or less and a sintered density of 6.1 g / cc to 6.6 g / cc, and hard particles are added to the resin.

17. An optical device comprising: a vibration actuator according to any one of claims 13 to 16; and at least one of an optical element and an imaging element driven by the vibration actuator.

18. An electronic device comprising: a member; and a vibration actuator according to any one of claims 13 to 16 for driving the member.

Citation Information

Patent Citations

  • Vibration actuator, lens unit, and imaging device

    JP2017055554A

  • Friction material, method for producing friction material, vibration type actuator and electronic equipment

    JP2017225333A

  • Vibration type actuator and contact body for use in the same

    JP2022030103A

  • Vibration type actuator, apparatus, contact body, and manufacturing method thereof

    JP2022152714A

  • Friction material and method for producing the same

    JP2022155688A