Method for manufacturing processed product

By using a short pulse laser and interference processing on a two-layer structure, the method effectively forms a hierarchical structure with excellent water repellency in a single step, addressing the inefficiencies of existing technologies and achieving rapid, cost-effective, and energy-efficient surface treatment.

WO2024225146A1PCT designated stage expired Publication Date: 2024-10-31SHINSHU UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015339
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-17
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods struggle to directly produce a hierarchical structure with excellent surface water repellency in a single step, as short-pulse laser processing with nanosecond pulses is inefficient for forming such structures due to excessive thermal effects.

Method used

Irradiating a two-layer structure consisting of a base material and a thin film with a short pulse laser using an interference processing method to form a predetermined uneven structure and scatter particles, creating a hierarchical structure with enhanced water repellency in one step.

Benefits of technology

This method enables the direct production of a workpiece with excellent surface water repellency in a single step, achieving high water repellency and maintaining transparency, while being energy-efficient and compact, with processing times under one minute and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015339_31102024_PF_FP_ABST
    Figure JP2024015339_31102024_PF_FP_ABST
Patent Text Reader

Abstract

By subjecting a two-layer structure containing a substrate and a thin film formed on the substrate to irradiation with a short pulse laser using interference machining, the method for manufacturing a processed product forms a relief structure having a prescribed period on the surface of the substrate and forms particles that are scattered on the relief structure.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of processed products

[0001] The present invention relates to a method for manufacturing a workpiece.

[0002] Forming a fine concave-convex structure on the surface of a material has been known as a means for imparting water repellency to the surface of the material. Furthermore, as such a fine concave-convex structure, a structure (hierarchical structure) is known in which a concave-convex periodic structure with a relatively long period and a concave-convex periodic structure with a shorter period are formed on the surface of the concave-convex periodic structure in a hierarchical manner (see, for example, Non-Patent Document 1).

[0003] Another example of a fine uneven structure that exhibits high surface water repellency is a reentrant structure in which the convex portions are formed in an inverse tapered shape, i.e., the cross-sectional width of the convex portions increases the further away from the material surface (see, for example, Patent Document 1, Non-Patent Documents 2 and 3, etc.). Patent Document 1 describes the use of a pulsed laser to form a fine uneven structure. Non-Patent Documents 2 and 3 describe that fine spherical particles can be formed by irradiating the surface of a workpiece with a nanosecond pulsed laser that adds thermal processing.

[0004] Japanese Patent Application Laid-Open No. 2022-26796

[0005] B. Bhushan: “Lessons from nature for green science and technology: an overview and bioinspired superliquiphobic / philic surfaces”, Phil Trans A Math Phys Eng Sci. , Vol. 377, No. 2138, p. 20180274 (2019))S. J. Henley, J. D. Carey, S. R. P. Silva: Metal nanoparticle production by pulsed laser nanostructuring of thin metal films. Applied Surface Science 253(19), 8080-8085 (2007). doi:10.1016 / j. apsusc. 2007.02.132Prashant Kumar, Mamidipudi Ghanashyam Krishna, Ashok Bhattacharya: Excimer Laser Induced Nanostructuring of Silicon Surfaces. Journal of Nanoscience and Nanotechnology, 9(5), 3224-3232 (2009). DOI: https: / / doi. org / 10.1166 / jnn. 2009.207

[0006] As exemplified by the lotus effect, which was discovered based on the motif of lotus leaves and produces a superhydrophobic surface, a hierarchical structure is one of the most suitable structures for enhancing water repellency. However, when comparing the thermal effects of short-pulse laser processing with pulse widths, the order of magnitude is nanoseconds > picoseconds > femtoseconds. Prior art (Non-Patent Documents 2, 3, etc.) uses nanosecond pulse lasers, which may be suitable for efficiently forming spherical particles, but the thermal effects are so great that it is difficult to form a hierarchical structure as is.

[0007] Therefore, one aspect of the present invention is to provide a surface processing method that can directly produce a hierarchical structure in one step without complicated steps as a processed product surface with excellent surface water repellency, and the processed product.

[0008] In order to solve the above problems, one aspect of the present invention involves irradiating a two-layer structure including a substrate and a thin film formed on the substrate with a short-pulse laser by an interference processing method, thereby forming a concave-convex structure having a predetermined period on the surface of the substrate and particles scattered on the concave-convex structure.

[0009] According to one aspect of the present invention, it is possible to provide a method for directly producing a processed product having excellent surface water repellency in one step without any complicated steps.

[0010] FIG. 1 is a diagram for explaining an overview of one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of the uneven structure of a base material. FIG. 3 is a diagram for explaining a multi-beam interference processing method. FIG. 4 is a table summarizing interference patterns, pitches, etc. of two- to four-beam interference processing methods. FIG. 5 is a diagram for explaining the angle of incidence of branched beams in a multi-beam interference processing method. FIG. 6 is a diagram showing a processing layout (arrangement of laser spots). FIG. 7 is an FE-SEM photograph of a laser-processed product obtained by an experiment. FIG. 8 is an image diagram relating to the production of a processed product in one process. FIG. 9 is a photograph taken in the water repellency evaluation for Example 1 (pulse frequency 400 kHz, number of shots 1).

[0011] The manufacturing method according to this embodiment includes irradiating a two-layer structure including a substrate and a thin film formed on the substrate with a short-pulse laser by an interference processing method, thereby forming a concave-convex structure having a predetermined period on the surface of the substrate and particles scattered on the concave-convex structure.

[0012] FIG. 1 is a schematic diagram illustrating an outline of the manufacturing method according to this embodiment. As shown in FIG. 1(a), a two-layer structure (two-layer structure) 1a consisting of a substrate 2 and a thin film 3 formed on the substrate 2 is prepared. Then, as shown in FIG. 1(b), this two-layer structure 1a is irradiated with short-pulse laser light LB from the side of the thin film 3, and the laser head is scanned to process the surface of the two-layer structure 1a. During this process, much of the thin film material sublimes, but at or near the irradiation spot, the thermal influence of the short-pulse laser melts and turns into particles due to its own interfacial tension. It is then rapidly cooled and remains as a solid on the surface, resulting in a state in which particles are scattered and attached to the substrate (FIG. 1(c)). Furthermore, since interference processing is performed simultaneously with the formation of the particles 5, a concavo-convex structure corresponding to the interference pattern is also formed on the substrate 2. The diameter of the particles 5 scattered on the substrate 2 is determined by the thickness of the thin film and is set smaller than the pitch of the interference pattern. Therefore, the dispersion state of the particles can be said to be a state in which a fine uneven structure is formed on the substrate, albeit at random, and by irradiating the short pulse laser in this embodiment, a hierarchical structure including an uneven structure having a predetermined period and an even finer uneven structure formed on the uneven structure is formed all at once. In other words, according to this embodiment, a workpiece having a highly water-repellent surface structure can be directly processed in one step without going through a complicated processing step. According to this embodiment, it is possible to directly process a workpiece having a highly water-repellent surface structure in one step at an industrially feasible cost. 2 This enables ultra-high-speed direct processing of over 1 / min. Furthermore, the use of lasers has the advantage of consuming less energy than other general processing devices and allowing for a more compact manufacturing system.

[0013] 1 illustrates a process in which only the thin film 3 is transformed into particles, but depending on the manufacturing conditions (the material constituting the substrate 2, the irradiation conditions such as the focal depth of the laser), part of the material of the substrate 2 may be contained in the particles 5. Furthermore, the laser processing does not necessarily transform the entire thin film 3 into particles 5, and part of the thin film 3 may remain on the substrate 2 in the structure (laser-processed product) after processing.

[0014] Furthermore, in this specification, the property obtained by this embodiment is referred to as water repellency or surface water repellency, but since such a property is expressed due to the physical structure, the structure of the processed product obtained by this embodiment may have the property of repelling and sliding off liquids other than water (including oil, etc.) or fluids, or even substances containing such liquids or fluids, from the surface.

[0015] The short-pulse laser light irradiated in this embodiment is laser light composed of a pulse train including multiple pulses with a constant peak intensity. In this specification, a short-pulse laser refers to a laser with a pulse width on the order of nanoseconds or less. Furthermore, in this embodiment, it is preferable to use an ultrashort-pulse laser. An ultrashort-pulse laser refers to a laser with a pulse width on the order of picoseconds or less. Specifically, the short-pulse laser is a nanosecond laser, a picosecond laser, or a femtosecond laser, with a picosecond laser being preferred. The pulse width of the laser used in this embodiment can be appropriately selected depending on the material of the workpiece (two-layer structure) and the intended use of the workpiece. However, it is preferable to use an ultrashort-pulse laser, particularly a picosecond laser. This facilitates both the effect of directly changing a portion of the workpiece from a solid to a gas (sublimation) and the effect of thermally affecting the workpiece. This facilitates the aforementioned change in the thin film during laser irradiation, i.e., the phenomenon in which the material of the thin film of the workpiece (two-layer structure) melts and remains as particles. Specifically, the pulse width t used in this embodiment may be 1 ps≦t<1 fs.

[0016] The laser light source that emits the short pulse laser is not particularly limited and can be appropriately selected depending on the purpose. Specific examples of the laser light source include an excimer laser, an Nd:YAG laser, and an Nd:YVO 4 Examples of such lasers include lasers and semiconductor lasers.

[0017] The particles formed on the substrate by the method of this embodiment can be said to be convex portions with a shape having a constriction at the base, but since the constriction at the base is larger than that of the conventional convex portions having a simple reverse tapered shape, higher water repellency can be exhibited. Therefore, it is preferable that the shape of the particles formed on the substrate is close to a sphere. For example, the roundness of the particles may be preferably 0.5 or more, more preferably 0.75 or more, and even more preferably 0.9 or more. The roundness can be measured, for example, by image analysis.

[0018] The size of the particles is not particularly limited, but is preferably on the order of nanometers. Nanometer-order particle sizes can exhibit high water repellency and also impart good optical properties to the resulting workpiece. In this specification, optical properties refer to properties related to light transmission, scattering, etc. when light is irradiated onto the workpiece, particularly transparency and scattering properties. Nanoparticle particles can suppress, for example, the scattering of visible light. Therefore, for example, if the workpiece is transparent, its transparency (light transmittance) can be maintained or the transparency does not change significantly even after laser processing. Therefore, from the perspective of suppressing the scattering of visible light to maintain transparency or suppress a decrease in transparency, it is preferable that the average particle size (average particle diameter) of the particles be less than the wavelength of visible light. Furthermore, the average particle size of the particles may be more preferably 400 nm or less, even more preferably 380 nm or less. Furthermore, the lower limit of the average particle size of the particles is not particularly limited, but due to manufacturing constraints, it may be preferably 10 nm or more, more preferably 50 nm or more. The average particle size of the particles may be a value determined by image analysis of the workpiece.

[0019] The particles may be dispersed on the substrate in a number of particles, but when viewed from above, the number of particles may be, for example, 0.01 particles / μm 2 or more, preferably 1 to 1000 particles / μm 2 , more preferably 10 to 100 pieces / μm 2 The distribution (density) of such particles can be determined by analyzing a top view image of the workpiece.

[0020] Furthermore, it is preferable that the particles are present in a larger amount on the protruding portions (convex portions) of the uneven structure of the substrate, more preferably on the top surfaces of the convex portions, so that substances that come into contact with the surface of the workpiece tend to come into contact with the particles first, making it easier to repel such substances.

[0021] In this embodiment, simultaneously with the formation of the particles as described above, a concave-convex structure having a predetermined period is also formed on the surface of the substrate. The concave-convex structure formed on this substrate may be a concave-convex structure having a predetermined period, i.e., a structure in which a plurality of convex portions or a plurality of concave portions are repeatedly arranged at a predetermined interval in at least one axial direction along the surface direction of the substrate (e.g., the x direction in the xy plane). The cross-sectional contour shape of the concave-convex structure may be a smooth shape with no or almost no edges (FIG. 1), or may have edges (FIG. 2). However, from the viewpoint of suppressing light scattering, the cross-sectional contour of the concave-convex structure may preferably be a smooth curve, more preferably a sinusoidal curve.

[0022] 2 is a schematic diagram showing a cross section of the uneven structure of the substrate 2, with particles omitted. As shown in FIG. 2, the uneven structure formed on the surface of the substrate 2 has a tooth width f 1 and a groove width f 2 and recesses having a depth h are alternately formed at a pitch (period) τ. In the uneven structure obtained by this embodiment, the pitch (period) τ may be preferably 200 nm to 200 μm, more preferably 200 nm to 380 nm. When the uneven structure formed on the substrate has a predetermined period within the above range, high water repellency can be exhibited and the period also contributes to suppressing the scattering of visible light. Furthermore, from the viewpoint of further suppressing the scattering of visible light, the period is more preferably less than the wavelength of visible light. Note that the period of the uneven structure of the substrate is preferably larger than the average particle size of the particles formed on the substrate. The desired period of the uneven structure can be adjusted by appropriately setting the conditions for short-pulse laser irradiation (described below).

[0023] The tooth width f of the convex portion in the concave-convex structure 1 The groove width f of the recessed portion is preferably 25 nm to 5 μm, and more preferably 50 nm to 500 nm.2 The depth of the recess (groove depth) h is preferably 25 nm to 5 μm, and more preferably 50 nm to 500 nm. 2 It may be about the same.

[0024] In this embodiment, the laser irradiation processing is preferably performed by, for example, an interference processing method. Examples of interference processing methods include surface wave interference processing and multi-beam interference processing. In this embodiment, however, since a uniform pitch is intentionally desired, multi-beam interference processing is preferred. By using the interference processing method, a fine interference pattern on the order of micrometers or nanometers can be arbitrarily formed within the laser spot diameter, and thus a periodic uneven structure of tens to hundreds of projections and recesses can be formed with a period (pitch) smaller than the laser spot diameter by a single laser sweep.

[0025] FIG. 3 shows an example of an optical unit used in the multi-beam interference processing method. As shown in FIG. 3, in the multi-beam interference processing method, light is split into multiple beams, and some or all of the split beams are combined to output an interference beam. In the example shown in FIG. 3, the optical unit 20 is composed of a laser oscillator 21, a diffractive optical element (DOE) 22 that splits the laser, a collimator lens 23 that collimates the multiple split beams, a beam expander 24 that expands the inter-beam distance, a mask 25 that removes all but the primary beam of the split laser light, and a condenser lens 26. The number of beams can be two or more, and there is no upper limit. However, in the manufacturing method of this embodiment, a two- to six-beam interference processing method is preferably used. By using two or more beams, a periodic structure in which multiple grooves are arranged at a predetermined pitch in a uniaxial direction within the surface of the substrate can be obtained. For details of the multi-beam interference processing method, see, for example, "A. A. Maznev, T. F. Crimmins, and K. A.: How to make femtosecond pulses overlap, Optics LEetters, Vol. 23, No. 17, 1378-1380, (1998)".

[0026] For reference, Fig. 4 shows the azimuth angle of the laser beam, the interference pattern, and the theoretical pitch (pitch of the interference fringes) τ when the number of beams is 2 to 4, as an example. i As can be seen from FIG. 4, when the number of beams is 2, a stripe-shaped interference pattern is formed, and when the number of beams is 3 or 4, a dot-shaped interference pattern is formed. Regardless of the number of beams and the interference pattern, the period (pitch) τ of the interference fringes in the interference processing method i By appropriately setting the period (pitch) τ of the uneven structure (Fig. 2), it is possible to obtain the desired period (pitch) τ of the interference fringes. i In order to further suppress the scattering of visible light, the pitch τ of the interference fringes is preferably 200 nm to 200 μm, and more preferably 200 nm to 380 nm. i It is more preferable that the pitch τ of the interference fringes is smaller than the wavelength of visible light, and can be set to, for example, less than 380 nm. i can be adjusted by adjusting the angle of incidence θ (FIG. 5) of the branched beam Ls with respect to the normal direction of the surface of the workpiece (two-layer structure) 1a. When attempting to obtain a preferable pitch τ (i.e., a pitch less than the wavelength of visible light) from the viewpoint of suppressing scattering of visible light in the uneven structure of the substrate, for example, when using a laser oscillator with a wavelength of 515 nm, the angle of incidence θ of the branched beam can be set to 42.8° or more in the two-beam interference processing method, 51.5° or more in the three-beam interference processing method, and 73.5° or more in the four-beam interference processing method.

[0027] Furthermore, in this embodiment, the number of shots during laser irradiation, i.e., the number of times each processing point is irradiated, may be one or multiple times. That is, the irradiation method may be a method in which irradiation of one processing point is completed and then the next processing point is moved to, or a method in which irradiation of one processing point is performed intermittently and continuously multiple times and then the next processing point is moved to. A large number of shots is preferable from the viewpoint of increasing the groove width and / or groove depth (FIG. 2) of the uneven structure formed on the substrate and enhancing the contribution of the uneven structure of the substrate to improving water repellency. However, from the viewpoint of manufacturing efficiency, the number of shots is preferably 10 or less, more preferably 8 or less. Furthermore, a small number of shots is preferable from the viewpoint of increasing the number of particles formed by sublimation and / or solidification of the thin film and / or increasing the particle diameter. A single shot is particularly preferable from the viewpoint of increasing the number of particles.

[0028] In this embodiment, a structure (two-layer structure) consisting of a substrate and a thin film formed thereon is used as the workpiece to be irradiated with a short-pulse laser. By irradiating such a two-layer structure with a short-pulse laser from the side where the thin film is formed, a periodic structure having irregularities with a predetermined period is formed on the substrate, and at the same time, particles are formed in the thin film that constitutes the surface layer. In this way, a structure having a periodic structure having irregularities with a predetermined period on the surface of the substrate and particles scattered on the periodic structure can be obtained in a short time.

[0029] In this specification, the term "two-layer structure" refers to a configuration consisting of a substrate and a thin film that is thinner than the substrate, and the substrate itself may be a single layer or two or more layers. When the substrate is two or more layers, the layers may be made of the same material or different materials. Furthermore, the thin film itself may be a single layer or two or more layers. When the thin film is two or more layers, the layers may be made of the same material or different materials.

[0030] The thin film in the two-layer structure may cover the entire surface of the substrate, or may only cover a part of the surface of the substrate, but from the viewpoint of scattering particles over the entire surface of the workpiece, it is preferable that the thin film cover the entire surface of the substrate.

[0031] The two-layer structure serving as the workpiece is not particularly limited in its configuration (shape, size, material, etc.) as long as it has a two-layer structure consisting of a substrate and a thin film, and can be appropriately selected depending on the application of the final laser-processed product. The shape of the two-layer structure is roughly the same as the shape of the substrate, and may be flat, prismatic, cylindrical, cylindrical, spherical, oval spherical, or amorphous, but a flat plate is preferred because it can be used in many applications. The surface of the two-layer structure or the substrate is not limited to a flat surface, but may also be a curved surface, or a combination of a flat surface and a curved surface. The thin film may be formed with a uniform thickness on such a substrate. In this specification, the term "uniform thickness" not only refers to a completely uniform thickness, but also includes a thickness that is preferably within a range of ±10%, more preferably ±5%, of the predetermined thickness.

[0032] The thickness of the thin film in the two-layer structure is preferably less than the wavelength of visible light. Furthermore, it can be preferably 1 nm to 1 μm, more preferably 30 to 380 nm, and even more preferably 50 to 400 nm. The inventors have discovered that the thickness of the thin film on the workpiece is related to the particle diameter of the resulting laser-processed product, and that the particle diameter of the resulting laser-processed product can be controlled by the thickness of the thin film. Based on this discovery, the thickness of the thin film can be determined depending on the particle diameter desired in the laser-processed product to be obtained.

[0033] The materials of the two-layer structure are not particularly limited, either for the substrate or the thin film. In this embodiment, water repellency is imparted to the structure by forming a microstructure on the surface of the structure using a laser. Therefore, it is not necessary to consider the compatibility of the water repellent with the material of the structure, as is the case when applying a water repellent to the surface. Materials constituting the two-layer structure may be inorganic materials such as metals, alloys, and metal oxides (including materials known as glass and ceramics), natural or synthetic organic materials such as resins, elastomers, and rubber, or combinations thereof. Examples of metals or alloys include stainless steel, copper, aluminum, gold, platinum, silver, iron, lead, zinc, tin, titanium, vanadium, chromium, nickel, tungsten, magnesium, solder, brass, steel, carbon steel, stainless steel, and duralumin. Examples of resins include acrylic (PMMA), polyethylene terephthalate (PET), polycarbonate (PC), polyvinyl chloride (PVC), and polyethylene (PE). The above materials may be used alone or in combination for the substrate and the thin film.

[0034] The substrate and the thin film included in the two-layer structure are preferably in close contact with each other. That is, the substrate and the thin film are preferably bonded without the use of another material such as an adhesive. For example, the thin film may be deposited on the substrate by a known film formation method such as vapor deposition, sputtering, chemical vapor deposition, spin coating, or spraying.

[0035] Furthermore, although the substrate and thin film included in the two-layer structure are made of different materials, it is preferable that they are made of similar materials, since this increases their mutual adhesion or integration and improves operability during processing. For example, similar materials may mean that the substrate and thin film are both made of inorganic materials, or both made of organic materials. Furthermore, the substrate and thin film may both be metal oxides, both be metals, or both be resins.

[0036] From the viewpoint of more reliably forming a structure consisting of a concave-convex structure and particles according to this embodiment, it is preferable that the temperature characteristics or thermal behavior of the material constituting the thin film and the material constituting the substrate are different from each other. For example, the thin film may have sublimation characteristics (the property of being sublimable) at least under the conditions of laser irradiation, and the substrate may have lower sublimation characteristics than the thin film under the same conditions. That is, the thin film may be sublimable within a temperature range in which the substrate is difficult to sublimate. In other words, under the same conditions of laser irradiation, the sublimation temperature (sublimation point or sublimation temperature range) of the thin film is preferably lower than the boiling temperature (boiling point or boiling temperature range) or sublimation temperature of the substrate, and preferably overlaps with or is close to the melting temperature (melting point or melting temperature range) of the substrate. Furthermore, the thin film may be composed of a material having a sublimation temperature at normal pressure, for example, a sublimation temperature of 600 to 1400°C, preferably 800 to 1200°C. The sublimation temperature of the thin film at atmospheric pressure is preferably lower than the boiling or sublimation temperature of the substrate, and may coincide with or be close to the melting temperature of the substrate. In this specification, "close to a predetermined temperature" means that the temperature may deviate from the predetermined temperature (°C) by preferably ±20% or less, more preferably ±10% or less.

[0037] In addition, a transparent two-layer structure, specifically a two-layer structure composed of a transparent substrate and a transparent thin film, can also be used. As described above, in the method of this embodiment, the original optical properties of the workpiece are maintained or not significantly changed even by laser irradiation. Therefore, when a transparent two-layer structure is used as the workpiece, its transparency can be maintained or not significantly impaired even after the laser irradiation process. Therefore, according to this embodiment, a laser-processed product that is highly water-repellent and transparent can be obtained.

[0038] In this specification, "transparent" refers to a material having a visible light transmittance of 70% or more, preferably 80% or more, and more preferably 90% or more. Transparent materials include both colorless materials and colored materials.

[0039] The transparent two-layer structure may be made of a transparent inorganic material or a transparent organic material. For example, the substrate may be made of glass such as soda lime silicate glass, aluminosilicate glass, borate glass, lithium aluminosilicate glass, or borosilicate glass, and the thin film may be made of transparent oxides such as indium tin oxide (ITO), fluorine-doped tin oxide (FTO), gallium-doped zinc oxide (GZO), silicon oxide, titanium oxide, zinc oxide, or alumina.

[0040] The laser processed product obtained by the method of this embodiment may be further combined with a chemical means for improving water repellency, such as a water repellent, to obtain high water or liquid repellency according to the purpose or application.

[0041] As described above, the water-repellent structure of the workpiece obtained by this embodiment has the property of repelling and sliding off liquids or fluids, or substances containing such liquids or fluids, from the surface, thereby imparting high stain resistance to the workpiece. Therefore, the workpiece obtained by this embodiment is suitable for application to components requiring stain resistance. Furthermore, the water-repellent structure imparted by the method of this embodiment has higher durability than, for example, conventional methods such as applying a water-repellent agent. For example, water-repellent agents tend to peel off after long-term use, but the water-repellent surface structure formed by irradiation with a short-pulse laser as in this embodiment is highly durable because there is no risk of peeling after formation. Therefore, the workpiece obtained by this embodiment is suitable for use under conditions requiring long-term water-repellency, liquid-repellency, or stain resistance, or under harsh conditions such as outdoors or in environments where water droplets are likely to splash. Furthermore, according to this embodiment, in addition to having high water-repellency or liquid-repellency as described above, a workpiece with high transparency can also be obtained by appropriately selecting the material of the workpiece.

[0042] The technology according to this embodiment is widely applicable to applications requiring liquid repellency or stain resistance, and specific applications include, for example, building materials, bathroom interior materials, bathroom equipment, furniture, interior decorations, vehicles, conveying equipment, transport equipment, medical supplies, health products, nursing products, care products, food containers, containers for sanitary products, optical equipment, office supplies, clothing, decorative items, etc. Further applications of processed products include lenses for cameras, sensors, etc., particularly transparent materials for on-board equipment such as on-board cameras and on-board sensors, vehicle or architectural windows, display components for image display devices, solar cell components, showcases, partitions, objects, containers for daily sanitary products, eyeglasses, face shields, food containers, etc.

[0043] In addition, one embodiment of the present invention may be a laser-processed product including a substrate containing a first material having a surface with a concave-convex structure having a predetermined periodicity formed thereon, and particles containing a second material different from the first material scattered on the concave-convex structure. In a preferred example, both the first material and the second material can be transparent, for example, the first material can be glass and the second material can be a transparent metal oxide such as ITO.

[0044] Another embodiment of the present invention may be a laser-processed product obtained by a method for manufacturing a processed product, which includes preparing a structure including a substrate and a thin film formed on the substrate, and irradiating the structure with a short-pulse laser to form a concave-convex structure having a predetermined period on the surface of the substrate and particles scattered on the concave-convex structure.

[0045] An experimental example will be described below.

[0046] <Preparation of Laser-Processed Product> Glass with an ITO film (ITO film thickness 300±20 nm, average spectral transmittance 80% or more, resistance 5±1 Ω / sq) was used as the workpiece (base material) in this example. A short-pulse laser was irradiated from the side of the workpiece where the ITO film was provided. The laser irradiation was performed using a laser processing device equipped with a laser oscillator (Trumph GmbH, TruMicro 5250, wavelength 515 nm, pulse width 10 ps, ​​repetition frequency 400 kHz).

[0047] The processing in this experiment was performed using a multi-beam interference processing method, specifically, a two-beam interference processing method. The optical unit used for this was a unit having the same configuration as that described with reference to FIG. 3, and included a glass diffractive optical element (DOE) (DS-239-515-Y-A, manufactured by Holo / Or Co. Ltd.) 22, a collimator lens (focal length f 1 = 200 mm) 23, beam expander (focal length f 2 = 60 mm, f 3 = 300 mm) 24, condenser lens (f 4 The mask 25 was made of aluminum tape. The fluence was set to 1.83 to 5.76 mJ / mm 2 The spot diameter was 100 μm (beam expander magnification 1), and the pitch of the interference fringes was 660 nm. The processing layout was a staggered arrangement with a laser spot pitch of 30 μm to minimize gaps (FIG. 6).

[0048] Under the above basic conditions, processing was carried out by varying the pulse frequency (repetition frequency) f between 40 Hz and 400 kHz, the pulse interval tp between 2.5 μs and 2.5 ms, and further varying the number of shots (number of irradiations) per processing point between 1 and 6. In order to change the effective laser frequency (pulse frequency), pulses were thinned out using the pulse picker function of the laser oscillator.

[0049] Table 1 summarizes the conditions of this experiment.

[0050]

[0051] <Evaluation> (Observation of Surface Structure) The obtained laser-processed product was photographed with a field emission scanning electron microscope (FE-SEM). Figure 7 shows 80,000x top-view images of the processed product under the conditions of Example 1 (f = 400 kHz, tp = 2.5 μs), Example 2 (f = 40 kHz, tp = 25 μs), Example 3 (f = 4 kHz, tp = 250 μs), and Example 4 (f = 400 Hz, tp = 2.5 ms), with the number of shots varied from 1 to 6. In all examples and with all shot numbers, a periodic structure of grooves with a pitch of approximately 600 nm repeated along one axial direction of the surface of the processed product, and particles scattered on the periodic structure, were confirmed. From this observation, it was found that by irradiating a predetermined structure according to this embodiment with a predetermined short-pulse laser, a periodic structure (concave-convex structure) due to interference processing and particles scattered on the periodic structure were simultaneously formed in one process (Figure 8).

[0052] (Particle Measurement) The number of particles in a 13 μm × 9.7 μm surface image taken at 10,000x magnification was counted using the counting function of ImageJ. Specifically, the FE-SEM image was converted into a binary image, and dots with 20 to 300 pixels (diameter 40 to 100 nm) and a circularity of 0.5 to 1 were counted from the dot data present in the binary image. The number of particles in the 13 μm × 9.7 μm image was 6 to 901 (approximately 0.047 to 7.15 particles / μm 2 ) It was found that the number of particles was greatest when the number of shots was 1. For example, in the laser processed product produced under the condition of 1 shot number in Example 1 (pulse frequency 400 kHz, pulse interval 2.5 μs), the number of particles in the 13 μm × 9.7 μm image was 901 (approximately 7.15 particles / μm 2 ) was.

[0053] (Wettability Evaluation) For the laser-processed product prepared under the conditions of Example 1 (pulse frequency 400 kHz, pulse interval 2.5 μs) with one shot, the apparent contact angle θ' was measured using distilled water as the sample solution, and θ' was 110.2 ± 2.7°. Meanwhile, the contact angle on the surface of the workpiece (unprocessed surface) before laser irradiation was 37.4 ± 0.1° (mean ± standard deviation), indicating that the apparent contact angle θ' was improved by the above-mentioned laser irradiation. The above measurement of the apparent contact angle θ' of the laser-processed product was performed after storage for three months after laser processing to stabilize the surface condition. Figure 9 shows photographs taken to measure the contact angle before and after laser processing. Figure 9(a) is a photograph before laser processing, and Figure 9(b) is a photograph after laser processing.

[0054] The above evaluation revealed that by irradiating a structure (two-layer structure) including a substrate and a thin film formed on the substrate with a short-pulse laser, a periodic structure having a predetermined period of irregularities and particles scattered on the periodic structure are simultaneously formed in a short time regardless of the pulse frequency, and that a laser-processed product including such a periodic structure and particles exhibits high water repellency, etc. Furthermore, it was confirmed that the transparency of the laser-processed product obtained by processing a two-layer structure including glass and ITO in this experimental example was visually unchanged from before processing.

[0055] <Considerations on particle formation> The formation of particles when multiple shots of laser irradiation are performed was also considered as follows. The inventors of the present invention have investigated the thermal diffusivity α [m 2 / s], a constant temperature heating surface (temperature T w [K]) is defined as the position in the thickness direction from the surface of the thin film (x = 0 and T = T w ), it was found that the temperature T at any position x from the surface of the thin film and at any time t within the thin film can be calculated based on theoretical formula (1).

[0056] Assuming that the ITO film used in the above experiment was heated to its boiling point (2000°C) by laser irradiation, the time required for the temperature at an arbitrary position x in the thickness direction from the surface of the ITO film to cool to room temperature of 20°C (293K) was calculated based on theoretical formula (1). The thermal diffusivity α [m 2 / s], thermal conductivity k = 10 [W / (mK)], density ρ = 7100 [g / m 3 ], and c = 400 [J / (kg·K)], which were values ​​based on the physical properties of ITO. According to the above calculation, for example, at a point where the position x from the surface is 100 nm, the time t was 100 ns (0.1 μs). Therefore, even with the shortest pulse interval of 2.5 μs (pulse frequency 400 kHz) in the above experimental example, the particles would have cooled by the time of the next laser irradiation (shot). Therefore, from such theoretical considerations, it was found that spherical particles could be produced from an ITO thin film even when multiple shots were repeatedly irradiated with a picosecond laser.

[0057] Although the present invention has been described above based on specific embodiments and examples, the present invention is not limited to these embodiments, etc. Furthermore, the above-described embodiments can be variously changed, modified, substituted, added, deleted, and combined within the scope of the claims, and these also fall within the technical scope of the present invention.

[0058] This application claims priority based on Japanese Patent Application No. 2023-071563, filed on April 25, 2023, the entire contents of which are incorporated herein by reference.

[0059] REFERENCE SIGNS LIST 1 Laser processed object 1a Workpiece (two-layer structure) 2 Base material 3 Thin film 5 Particle 20 Optical unit 21 Laser oscillator 22 Diffractive optical element (DOE) 23 Collimating lens 24 Beam expander 25 Mask 26 Condenser lens

Claims

1. A method for manufacturing a processed product, in which a two-layer structure including a substrate and a thin film formed on the substrate is irradiated with a short-pulse laser by an interference processing method to form a concave-convex structure having a predetermined period on the surface of the substrate and particles scattered on the concave-convex structure.

2. The manufacturing method according to claim 1, wherein the substrate and the thin film are different from each other but are both made of inorganic materials or both made of organic materials.

3. The manufacturing method according to claim 1 or 2, wherein the short pulse laser is a picosecond pulse laser.

4. The manufacturing method according to claim 1 or 2, wherein the thickness of the thin film is less than the wavelength of visible light.

5. The particles have a density of 1 to 1000 particles / μm in plan view. 2 The method according to claim 1 or 2, wherein 6. The manufacturing method according to claim 1 or 2, wherein the cross-sectional contour of the uneven structure having the predetermined period is sinusoidal.

Citation Information

Patent Citations

  • Laser curved surface machining system and super-hydrophobic, anti-icing and wind resistance reducing manufacturing method

    CN112162467A

  • Laser removal method for waterproof material on electronic component surface

    CN112355482A

  • Method for manufacturing bored dielectric layer, and method for manufacturing device including bored dielectric layer

    JP2015088604A

  • Kitchin member and method for manufacturing the same

    JP2020054860A

  • Adhesion prevention structure manufacturing method, adhesion prevention structure manufacturing apparatus, and adhesion prevention structure

    JP2023006980A