Hydrophilic film and optical member

The hydrophilic film, featuring a titanium particle layer and silica coating on a light-transmitting member, addresses the loss of hydrophilicity and scratch issues by restoring and maintaining hydrophilicity and visibility, even in low-light conditions, through photocatalytic properties and enhanced durability.

WO2024225162A1PCT designated stage expired Publication Date: 2024-10-31NIDEC CORP(JP) +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015437
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Hydrophilic window surfaces tend to lose their hydrophilicity over time, especially in environments with limited ultraviolet light exposure, leading to reduced visibility due to dirt adhesion and water droplet accumulation, and are prone to scratches.

Method used

A hydrophilic film with a thickness of 20 nm to 200 nm, containing titanium particles for photocatalytic properties and a silica coating layer, applied to a light-transmitting member, which maintains hydrophilicity and suppresses scratches, allowing for recovery when exposed to ultraviolet light and extended maintenance in low-light environments.

Benefits of technology

The hydrophilic film effectively maintains visibility by restoring hydrophilicity when exposed to UV light and extends the duration of hydrophilicity maintenance even in environments with insufficient UV light, while also enhancing scratch resistance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015437_31102024_PF_FP_ABST
    Figure JP2024015437_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A hydrophilic film 70 contains a plurality of titanium particles and a plurality of silica particles. The hydrophilic film 70 has a surface roughness of 2.0-7.5 nm. It is preferable that a first layer 20 and a second layer 60 disposed on the first layer 20 are provided, and that the first layer 20 contains a plurality of titanium particles, and the second layer 60 contains a plurality of silica particles. The average particle diameter of the titanium particles is preferably 15-100 nm, and the average particle diameter of the silica particles is preferably 5-20 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Hydrophilic film and optical component

[0001] The present disclosure relates to a hydrophilic film and an optical member.

[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor wind and rain. One solution to this problem is to make the surface of the window glass hydrophilic. This turns the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.

[0003] However, the surface of hydrophilic materials is prone to the adhesion of organic contaminants, such as those from automobile exhaust fumes or factory smoke. When organic contaminants adhere to the surface, water droplets adhere to the surface, significantly reducing visibility.

[0004] Therefore, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm.

[0005] Japanese Patent Publication No. 2018-77260

[0006] When the hydrophilic lens of Patent Document 1 is used for a long period of time, if dirt accumulates and the hydrophilic function is reduced, the hydrophilicity may not be restored even if it is irradiated with ultraviolet light (sunlight). Specifically, when the hydrophilic lens of Patent Document 1 is used for a long period of time, the hydrophilic layer may be damaged, which may reduce the function of restoring hydrophilicity. Furthermore, when the hydrophilic lens of Patent Document 1 is used in an environment where it is not sufficiently irradiated with ultraviolet light (sunlight), such as in an environment with continuous cloudy or rainy weather or in an environment where it is installed in a place with little light, it may not be possible to restore the hydrophilic function in the first place.

[0007] The present disclosure has been made in view of the above-mentioned problems, and an object of the present disclosure is to provide a hydrophilic film and an optical component that can be prevented from being scratched and can maintain the function of recovering hydrophilicity when irradiated with ultraviolet light (sunlight). Another object of the present disclosure is to provide a hydrophilic film and an optical component that can maintain the hydrophilic function for a longer period even when used in an environment where ultraviolet light (sunlight) is not sufficiently irradiated.

[0008] An exemplary hydrophilic film of the present disclosure includes a plurality of titanium particles and a plurality of silica particles, and has a surface roughness of 2.0 nm to 7.5 nm.

[0009] An exemplary optical member according to the present disclosure includes the hydrophilic film described above and a translucent member that transmits visible light. The hydrophilic film is disposed on the translucent member.

[0010] According to the exemplary embodiment of the present disclosure, for example, it is possible to suppress scratches, maintain the function of recovering hydrophilicity when irradiated with ultraviolet light (sunlight), and maintain hydrophilicity for a longer period even in an environment where ultraviolet light (sunlight) is not irradiated.

[0011] Fig. 1 is a schematic diagram showing an example of an optical unit according to this embodiment, Fig. 2 is a schematic diagram showing an example of an optical member according to this embodiment, and Fig. 3 shows an image taken using an atomic force microscope (AFM).

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals, and the description will not be repeated. The dimensions, shapes, and dimensional relationships between components in the drawings are not necessarily the same as the actual dimensions, shapes, and dimensional relationships between components. In particular, the thickness ratios and curvatures of the reflection adjustment film, hydrophilic film, and translucent member in the drawings may differ significantly from the actual products.

[0013] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the translucent member to the hydrophilic film. The "inside" of an optical member refers to the direction from the hydrophilic film to the translucent member.

[0014] The optical member according to this embodiment is suitable, for example, as an optical member used in an optical unit including one or more optical members (particularly an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit."

[0015] The optical element according to this embodiment may be used in an optical unit (particularly an optical unit for use outdoors) including the optical element 100 and an optical lens. The optical lens transmits light with a wavelength of 400 nm or more and 700 nm or less. The optical element 100 is disposed on the opposite side of the optical lens in the light traveling direction.

[0016] The static contact angle of the surface of the optical element 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be simply referred to as the "contact angle." Note that the contact angle of the surface of the optical element according to this embodiment is a value measured in an environment at a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0017] Furthermore, the reflectance for light with a wavelength of 400 nm or more and 700 nm or less is 3% or less. The maximum reflectance of the optical element 100 for light with a wavelength of 400 nm or more and 700 nm or less is preferably 1.5% or less, and more preferably 1.0% or less. The optical element 100 according to this embodiment can suppress the occurrence of image defects known as ghost phenomena and flare phenomena as the maximum reflectance described above decreases. In particular, the lower the maximum reflectance described above, the more effectively the occurrence of ghost phenomena can be suppressed. When the maximum reflectance described above is 3.0% or less, the occurrence of ghost phenomena can be suppressed. When the maximum reflectance described above is 1.0% or less, the occurrence of ghost phenomena can be more effectively suppressed. Note that light with a wavelength of 400 nm or more and 700 nm or less corresponds to light in the visible light region.

[0018] An example of the optical member 100 according to this embodiment will be described below with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to this embodiment. The optical member 100 includes a light-transmitting member 10, a hydrophilic film 70, and a reflection adjustment film 30.

[0019] <Light-Transmitting Member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0020] The light-transmitting member 10 functions as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 10 mm or more and 15 mm or less.

[0021] <Hydrophilic Film> The hydrophilic film 70 covers the light-transmitting member 10. Specifically, the hydrophilic film 70 is disposed on the reflection adjustment film 30. The hydrophilic film 70 has hydrophilic properties.

[0022] The hydrophilic film 70 contains a plurality of titanium particles and a plurality of silica particles.

[0023] Specifically, the hydrophilic film 70 includes a hydrophilic layer 20 and a coating layer 60. The hydrophilic layer 20 is an example of a "first layer." The coating layer 60 is an example of a "second layer."

[0024] <Hydrophilic Layer> The thickness of the hydrophilic layer 20 is preferably 20 nm or more and 200 nm or less, and more preferably 30 nm or more and 100 nm or less. If the thickness of the hydrophilic layer 20 is less than 20 nm, the function of restoring hydrophilicity tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, sufficient transmittance to visible light tends to be insufficient.

[0025] In the present specification, "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced across the surface to measure the step between areas with and without a layer (film). Steps are measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."

[0026] The hydrophilic layer 20 contains a plurality of titanium particles. The titanium particles have a photocatalytic function. For example, when the optical element 100 is used for a long period of time, dirt adheres to the optical element 100, reducing the hydrophilic function. When the optical element 100 is irradiated with ultraviolet light (sunlight), the dirt is decomposed and the hydrophilic function can be restored. The optical element 100 according to this embodiment exhibits a high hydrophilicity when exposed to ultraviolet light at a dose of 1 mW / cm when the contact angle exceeds 30.0°. 2 It is preferable that the contact angle becomes 30.0° or less by irradiating the surface with the light for 6 hours.

[0027] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferred.

[0028] The titanium particles preferably have an average particle size of 15 nm to 100 nm. Specifically, the titanium particles are, for example, primary or secondary particles of titanium dioxide. In particular, the hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of multiple primary particles of titanium dioxide.

[0029] The average particle size of the titanium primary particles is preferably 5 nm or more and 20 nm or less, more preferably 5 nm or more and 10 nm or less. If the average particle size of the titanium primary particles is less than 5 nm, sufficient hydrophilicity cannot be maintained. If the average particle size of the titanium primary particles is more than 20 nm, sufficient transmittance to visible light cannot be obtained, or a uniform film cannot be formed.

[0030] In the present specification, the "average particle size of primary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 primary particles that can be observed in their entirety, the maximum diameter and the minimum diameter of each primary particle are measured, and the average value of the maximum diameter and the minimum diameter is defined as the particle size of the single primary particle. The average value of the particle sizes of each of the 50 primary particles is defined as the "average particle size of primary particles."

[0031] The average particle size of the secondary particles of the titanium particles is 15 nm or more and 100 nm or less, and preferably 20 nm or more and 60 nm or less. If the average particle size of the secondary particles of the titanium particles is less than 15 nm, the hydrophilicity of the hydrophilic layer 20 cannot be sufficiently restored. If the average particle size of the secondary particles of the titanium particles is more than 100 nm, sufficient transmittance to visible light cannot be obtained.

[0032] In the present specification, the "average particle size of secondary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 secondary particles for which the entire particle can be observed, the maximum diameter and minimum diameter of each secondary particle are measured, the average value of the maximum diameter and minimum diameter is defined as the particle size of the single secondary particle, and the average value of the particle diameters of each of the 50 secondary particles is defined as the "average particle size of secondary particles."

[0033] The content of titanium particles in the hydrophilic layer 20 is preferably 50% by mass or more and 70% by mass or less. By having the content of titanium particles of 50% by mass or more and 70% by mass or less, the hydrophilicity of the hydrophilic layer 20 can be more effectively restored and an increase in reflectance can be more effectively suppressed.

[0034] The hydrophilic layer 20 may further contain a binder, which further improves the abrasion resistance of the optical member 100. The binder preferably further contains tetraethoxysilane and silicon dioxide.

[0035] <Coating Layer> The coating layer 60 is disposed on the hydrophilic layer 20. The coating layer 60 contains a plurality of silica particles.

[0036] Specifically, the coating layer 60 contains a plurality of primary silica particles. At least a portion of the hydrophilic layer 20 is partially or completely coated with the primary silica particles. As a result, the abrasion resistance of the optical element 100 is further improved, and the durability of maintaining hydrophilicity is improved. The coating layer 60 may further contain tetraethoxysilane.

[0037] The average particle size of the primary silica particles is preferably 5 nm or more and 20 nm or less. If the average particle size of the primary silica particles is less than 5 nm, the cost tends to increase. If the average particle size of the primary silica particles is more than 20 nm, sufficient transmittance for visible light tends to be insufficient.

[0038] The thickness of the coating layer 60 is preferably 5 nm or more and 20 nm or less. If the thickness of the coating layer 60 is less than 5 nm, sufficient durability tends to be insufficient. If the thickness of the coating layer 60 is more than 20 nm, the coating is easily scratched.

[0039] The surface roughness of the hydrophilic film 70 is 2.0 nm or more and 7.5 nm or less. If the surface roughness of the hydrophilic film 70 is less than 2.0 nm, the coating is easily scratched. If the surface roughness of the hydrophilic film 70 is more than 7.5 nm, sufficient durability tends to be insufficient.

[0040] 1 and 2, in this embodiment, the surface roughness of the hydrophilic film 70 is 2.0 nm or more and 7.5 nm or less, so that the hydrophilic film 70 is highly durable and can be prevented from being scratched. As a result, even if the hydrophilicity is reduced, the function of recovering the hydrophilicity when irradiated with ultraviolet light (sunlight) can be maintained for a long period of time.

[0041] Furthermore, since the hydrophilic film 70 includes the hydrophilic layer 20 and the coating layer 60, it has higher durability, and even if the hydrophilicity is reduced, it can recover its hydrophilicity more easily by being irradiated with ultraviolet light (sunlight). Furthermore, even in an environment where ultraviolet light (sunlight) is not irradiated, the hydrophilicity can be maintained for a longer period of time.

[0042] Furthermore, the average particle size of the titanium particles in the hydrophilic layer 20 is 15 nm or more and 100 nm or less, and the average particle size of the primary silica particles in the coating layer 60 is 5 nm or more and 20 nm or less, so that scratches can be further suppressed, and when irradiated with ultraviolet light (sunlight), hydrophilicity can be further restored.

[0043] <Reflection adjustment film> The reflection adjustment film 30 is disposed below the hydrophilic layer 20. The reflection adjustment film 30 covers the light-transmitting member 10. The reflection adjustment film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The reflection adjustment film 30 suppresses reflection of light. Specifically, by including the reflection adjustment film 30, the optical member 100 suppresses light that attempts to enter the light-transmitting member 10 from the reflection adjustment film 30 from being reflected by the surface on the reflection adjustment film 30 side.

[0044] The reflection adjustment film 30 has a multilayer structure. Specifically, the reflection adjustment film 30 includes low refractive index layers and high refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low refractive index layers and high refractive index layers are not limited as long as the combination allows the reflection adjustment film 30 to exhibit an anti-reflection effect. The refractive index of the low refractive index layers is, for example, 1.80 or less. The refractive index of the high refractive index layers is, for example, greater than 1.80. The outermost layer of the low refractive index layers and high refractive index layers is the low refractive index layer. The innermost layer of the low refractive index layers and high refractive index layers is the low refractive index layer.

[0045] The refractive index of the low-refractive index layer may be less than the refractive index of the high-refractive index layer. For example, the refractive index of the low-refractive index layer is preferably 1.30 or more and 1.80 or less, and more preferably 1.40 or more and 1.60 or less. When the refractive index of the low-refractive index layer is 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low-refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.

[0046] The refractive index of the high refractive index layer may be higher than the refractive index of the low refractive index. For example, the refractive index of the high refractive index layer is preferably 1.80 or more and 3.00 or less, and more preferably 2.00 or more and 2.80 or less. When the refractive index of the high refractive index layer is 1.80 or more and 3.00 or less, the reflectance of the optical member 100 is further reduced. The high refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4.

[0047] The refractive indices of the low-refractive-index layer and the high-refractive-index layer described above are merely examples and are not limited to these. The refractive indices of the low-refractive-index layer and the high-refractive-index layer may be set to values ​​that are optimal for the refractive index of the light-transmitting member 10.

[0048] The thickness of the reflection adjustment film 30 is at least 5 times the thickness of the hydrophilic layer 20. From the viewpoint of productivity, the thickness of the reflection adjustment film 30 is preferably no more than 100 times the thickness of the hydrophilic layer 20. The total film thickness of the reflection adjustment film 30 is preferably 20 nm or more and 2000 nm or less, and more preferably 200 nm or more and 750 nm or less. If the total film thickness of the reflection adjustment film 30 is less than 20 nm, a sufficient anti-reflection effect tends to be insufficient. If the total film thickness of the reflection adjustment film 30 exceeds 2000 nm, film formation takes a long time, and the productivity of the optical element 100 tends to decrease. Furthermore, if the total film thickness exceeds 2000 nm, the production cost of the optical element 100 tends to increase.

[0049] The thickness of one low refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less, and the thickness of one high refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less.

[0050] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.

[0051] <Method for Manufacturing Optical Member> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a reflection adjustment film formation step, a coating step, and a drying step.

[0052] <Preparation Step> Prepare the light-transmitting member 10. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0053] <Reflection Adjustment Film Formation Step> A low refractive index material is prepared. The low refractive index material preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2. The SiO2 content in the low refractive index material is preferably 95 mass% or more. The low refractive index material is preferably formed by vapor deposition or sputtering.

[0054] A high refractive index material is prepared. The high refractive index material preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4. The content of Si3N4 in the high refractive index material is preferably 95 mass% or more. The high refractive index material is preferably formed by vapor deposition or sputtering.

[0055] The low refractive index layers and the high refractive index layers are alternately laminated. The total number of low refractive index layers and high refractive index layers is usually an odd number, although the total number of low refractive index layers and high refractive index layers may be an even number.

[0056] <Coating Step> A hydrophilic material is coated. The hydrophilic material contains a plurality of titanium particles. The average particle size of the primary titanium particles is preferably 5 nm or more and 20 nm or less.

[0057] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0058] The content of the solvent in the hydrophilic material is preferably 50% by mass or more and 99.9% by mass or less. By having the content of the solvent in the hydrophilic material be 50% by mass or more and 99.9% by mass or less, coating can be easily performed.

[0059] The method for applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of two or more of these (e.g., dip spin coating). Preferred wet processes are spin coating, dip coating, and dip spin coating.

[0060] <Drying Step> The hydrophilic material is dried to produce the hydrophilic layer 20. The hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of a plurality of primary particles of photocatalyst particles. The average particle diameter of the secondary particles of the photocatalyst particles is 15 nm or more and 100 nm or less.

[0061] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.

[0062] <Coating Material Application Step> A coating material is applied. The coating material contains a plurality of primary silica particles. The average particle size of the primary silica particles is 5 nm or more and 20 nm or less.

[0063] The coating material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0064] The content of the solvent in the coating material is preferably 50% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50% by mass or more and 99.9% by mass or less, the coating material can be easily applied.

[0065] The coating material is preferably applied by a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of two or more of these (e.g., dip spin coating). Preferred wet processes are spin coating, dip coating, and dip spin coating.

[0066] The above describes embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments and can be implemented in various forms without departing from the spirit and scope of the present disclosure. The drawings mainly show each component in a schematic manner for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings may differ from the actual components due to the convenience of creating the drawings. Furthermore, the materials, shapes, dimensions, etc. of each component shown in the above embodiments are merely examples and are not particularly limited. Various modifications are possible within a scope that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiments may be appropriately modified within a scope that does not deviate from the technical concept of the present disclosure. Furthermore, the embodiments may be implemented in combination within the scope of possibility.

[0067] The present technology can also employ the following configuration.

[0068] (1) A hydrophilic film containing a plurality of titanium particles and a plurality of silica particles, wherein the surface roughness of the hydrophilic film is 2.0 nm or more and 7.5 nm or less.

[0069] (2) The hydrophilic film according to (1), comprising a first layer and a second layer disposed on the first layer, wherein the first layer contains the plurality of titanium particles, and the second layer contains the plurality of silica particles.

[0070] (3) The hydrophilic film according to (1) or (2), wherein the titanium particles have an average particle size of 15 nm or more and 100 nm or less, and the silica particles have an average particle size of 5 nm or more and 20 nm or less.

[0071] (4) The hydrophilic film according to (2), wherein the first layer further contains a binder, and the content of the titanium particles in the first layer is 50% by mass or more and 70% by mass or less.

[0072] (5) An optical member comprising: the hydrophilic film according to any one of (1) to (4); and a translucent member that transmits visible light, wherein the hydrophilic film covers the translucent member.

[0073] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.

[0074] <Production of Optical Members> Optical members according to Examples 1 and 2, and optical members according to Comparative Examples 1 and 2 were produced.

[0075] Example 1 Preparation Steps A lens (manufactured by HOYA Corporation, "TAFD-5G", composition: glass, diameter: 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was convex (radius of curvature: 12 mm) and the other surface was concave (radius of curvature: 3.07 mm).

[0076] <Reflection Adjustment Film Formation Step> A low refractive index material containing SiO2 and a high refractive index material containing Si3N4 were alternately laminated to form a reflection adjustment film having a total of 11 low refractive index layers and high refractive index layers.

[0077] <Coating Step> A hydrophilic material according to Example 1 containing 0.5 parts by mass of titanium dioxide particles, 0.5 parts by mass of silicon dioxide, 2 parts by mass of water, 76 parts by mass of isopropyl alcohol, 20 parts by mass of methanol, and 1 part by mass of nitric acid was prepared.

[0078] A hydrophilic material was applied onto the reflection adjustment film. Specifically, 60 μL of the hydrophilic material was dropped onto the optical axis of the light-transmitting member. Next, using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), the light-transmitting member was rotated at a rotation speed of 5000 rpm. At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.

[0079] <Drying Step> A hydrophilic layer was formed by heating at 90° C. for 30 minutes. The surface roughness of the hydrophilic layer was 7.56 nm.

[0080] <Coating Material Application Step> A coating material containing 1 part by weight of silica particles (average primary particle diameter of 5 nm), 99 parts by weight of water, and 0.2 parts by weight of ammonia was prepared. The coating material was applied to the hydrophilic layer. Specifically, 60 μL of the coating material was dropped onto the optical axis of the light-transmitting member. Next, using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), the light-transmitting member was rotated at a rotation speed of 5000 rpm. At this time, the rotation axis was aligned with the optical axis of the light-transmitting member. A heat treatment was performed at 120°C for 30 minutes to form a coating layer, thereby obtaining the optical member according to Example 1. The surface roughness of the hydrophilic film was 2.50 nm. An image taken using an atomic force microscope (AFM) is shown in FIG. 3(a).

[0081] Example 2 In the coating material application step of Example 1, instead of preparing a coating material containing 1 part by mass of silica particles (average primary particle size of 5 nm), 98.8 parts by mass of water, and 0.2 parts by mass of ammonia, a coating material containing 0.5 parts by mass of silica particles (average primary particle size of 5 nm), 93.3 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The surface roughness of the hydrophilic film was 4.08 nm. An image taken using an atomic force microscope (AFM) is shown in Figure 3(b).

[0082] Comparative Example 1: The coating material application step of Example 1 was not performed. The surface roughness of the hydrophilic film was 7.6 nm. An image taken with an atomic force microscope (AFM) is shown in FIG. 3(c).

[0083] Comparative Example 2: In the coating material application step of Example 1, instead of preparing a coating material containing 1 part by mass of silica particles (average primary particle size of 5 nm), 98.8 parts by mass of water, and 0.2 parts by mass of ammonia, a coating material containing 5 parts by mass of silica particles (average primary particle size of 5 nm), 94.8 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The surface roughness of the hydrophilic film was 0.87 nm. An image taken using an atomic force microscope (AFM) is shown in FIG. 3(d).

[0084] <Evaluation> The reflectance and scratch resistance of the optical members according to Examples 1 and 2 and the optical members according to Comparative Examples 1 and 2 were evaluated by the following methods. The measurement results are shown in Table 1. All measurements were carried out in an environment of a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0085] <Abrasion test> An optical element was placed in pure water and subjected to 500 reciprocating abrasion tests using a scrubbing brush with a 300 g load on the surface. The optical element was then observed under a laser microscope at 466x magnification. The durability of the optical element was evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0086] 〇: No optical influence ×: Optical influence present

[0087] <Contact Angle> Before using the optical member, the static contact angle with pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). In addition, after the optical member was subjected to a thermal cycle test for 265 hours at -40°C for 30 minutes and 85°C for 30 minutes, the static contact angle with pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). The evaluation results are shown in Table 1.

[0088]

[0089] The optical element according to Comparative Example 1 lost its hydrophilicity after 256 hours of thermal shock. The optical element according to Comparative Example 2 had poor abrasion resistance, and scratches caused deterioration of its optical properties. In contrast, the optical elements according to Examples 1 and 2 were able to suppress scratches and maintain the ability to recover hydrophilicity upon irradiation with ultraviolet light (sunlight) for a long period of time. Furthermore, the hydrophilicity could be maintained for a longer period of time even in an environment where ultraviolet light (sunlight) was not irradiated.

[0090] 10... Transparent member 20... Hydrophilic layer 60... Covering layer 70... Hydrophilic film 100... Optical member

Claims

1. A hydrophilic film containing a plurality of titanium particles and a plurality of silica particles, the hydrophilic film having a surface roughness of 2.0 nm or more and 7.5 nm or less.

2. The hydrophilic film according to claim 1, comprising a first layer and a second layer disposed on the first layer, the first layer containing the plurality of titanium particles, and the second layer containing the plurality of silica particles.

3. The hydrophilic film according to claim 2, wherein the average particle size of the titanium particles is 15 nm or more and 100 nm or less, and the average particle size of the silica particles is 5 nm or more and 20 nm or less.

4. The hydrophilic film according to claim 2, wherein the first layer further contains a binder, and the content of the titanium particles in the first layer is 50% by mass or more and 70% by mass or less.

5. An optical component comprising: a hydrophilic film according to any one of claims 1 to 4; and a translucent member that transmits visible light, said hydrophilic film covering said translucent member.

Citation Information

Patent Citations

  • Hydrophilic photocatalytic member

    JP2000239047A

  • Optical member and method for manufacturing the same

    JP2022078385A

  • Photocatalyst element, method and device for preparing the same

    WO2003028885A1

  • Hydrophilic member and method for producing same

    WO2014080726A1