Copper alloy sheet material, copper alloy sheet material for drawing, and drawn product

The copper alloy sheet material with controlled Ni and Si content, along with optional additives, addresses the challenge of achieving high tensile strength and electrical conductivity, reducing selvages and improving drawing workability in copper alloy sheets for electronic and automotive applications.

WO2024225165A1PCT designated stage expired Publication Date: 2024-10-31FURUKAWA ELECTRIC CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015456
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Copper alloy sheets used in electronic and automotive devices face challenges with high mechanical properties and electrical conductivity, particularly in drawing processes where large undulations and selvages form, leading to shape damage and cracks, with existing alloys not adequately addressing both high tensile strength and high electrical conductivity simultaneously.

Method used

A copper alloy sheet material with a composition of 1.00% to 5.00% Ni, 0.20% to 1.30% Si, and optional additions of Sn, Zn, Mg, Fe, and Cr, manufactured through specific processing steps including melting, reheating, hot rolling, intermediate annealing, and cold rolling, to achieve reduced anisotropy and improved drawing workability.

Benefits of technology

The copper alloy sheet material achieves high tensile strength, high electrical conductivity, and reduced selvages on drawn products, enhancing drawing workability and mechanical properties while maintaining excellent electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided are a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product, which have high tensile strength and high electrical conductivity. The present invention makes it possible to realize excellent drawability and, in particular, to reduce ears formed on the edges of the drawn product. The copper alloy sheet material has an alloy composition containing Ni in the range from 1.00 mass% to 5.00 mass% and Si in the range from 0.20 mass% to 1.30 mass%, with the remainder being Cu and unavoidable impurities. When a plate surface of the copper alloy sheet material is measured by the EBSD method for crystal orientation analysis, the maximum strength value found in the inverse polar figure pertaining to a crystal plane oriented in the normal direction (ND) of the plate surface obtained from the analysis is 3.0 or less. The copper alloy sheet material has a tensile strength in the range from 500 MPa to 900 MPa, and an electroconductivity of 30% IACS or more.
Need to check novelty before this filing date? Find Prior Art

Description

Copper alloy sheets, copper alloy sheets for drawing and drawn products

[0001] The present invention relates to a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product.

[0002] Copper alloy sheet materials are used, for example, in electronic devices or automotive connectors, lead frames, relays, switches, sockets, shield cases, shield cans, camera module cases, vibration device cases, heat dissipation parts for liquid crystal and organic EL displays, batteries, probe pins, and gas shut-off valves, and are often subjected to press working such as punching, bending, drawing, and bulging.

[0003] As an example of a copper alloy used in such press working, Patent Document 1 discloses a copper alloy containing, by mass%, 1.0 to 3.6% Ni, 0.2 to 1.0% Si, 0.05 to 3.0% Sn, and 0.05 to 3.0% Zn, with the remainder being copper and unavoidable impurities. The copper alloy has an average crystal grain size of 25 μm or less, and, as measured by SEM-EBSP, has a texture in which the average area ratio of the Cube orientation {001}<100> is 20 to 60%, and the average total area ratio of the three orientations, Brass orientation {011}<211>, S orientation {123}<634>, and Copper orientation {112}<111>, is 20 to 50%, and has a KAM value of 1.00 to 3.00. Patent Document 1 describes that a copper alloy having small strength anisotropy and excellent bending workability can be obtained by controlling the area ratio of the Cube orientation {001}<100>, the average total area ratio of the three orientations, i.e., the Brass orientation {011}<211>, the S orientation {123}<634>, and the Copper orientation {112}<111>, and the KAM value.

[0004] Patent Document 2 discloses a Cu-Ni-Si copper alloy sheet material with excellent deep drawability and fatigue resistance, which contains 1.0 to 3.0 mass% Ni, 1 / 6 to 1 / 4 of the mass% concentration of Ni, and the remainder Cu and unavoidable impurities, and has a Goss orientation density of 2.0 to 6.0% measured by EBSD using a scanning electron microscope equipped with a backscattered electron diffraction image system, an average KAM value of 0.9 to 1.5°, and a ratio (Lσ / L) of the total special grain boundary length Lσ of the special grain boundaries to the total grain boundary length L of the crystal grain boundaries of 60 to 70%. Patent Document 2 states that by controlling the Goss orientation density, KAM value, and total special grain boundary length of the Cu-Ni-Si alloy sheet, the fatigue properties and drawability of the copper alloy sheet can be improved.

[0005] JP 2011-162848 A JP 2012-122114 A

[0006] In recent years, with the increasing performance, current density, and miniaturization of electronic devices and on-board automotive devices, higher mechanical properties and electrical conductivity (or thermal conductivity) have been required for press-formed products, which are one of the components that make up these devices. In particular, for drawn parts used in electronic devices and on-board automotive devices, such as connectors, lead frames, relays, switches, sockets, shielding cases, shielding cans, camera module cases, vibration device cases, heat dissipation parts for liquid crystal and organic EL displays, batteries, probe pins, gas shut-off valves, etc., copper alloy sheet materials made of materials that combine higher mechanical properties and electrical conductivity (or thermal conductivity) than the copper alloys such as brass and nickel silver that have been conventionally used.

[0007] Here, "drawing" refers to a type of metal sheet forming method, and typically refers to a processing method in which a punch is pressed into a sheet of metal to form bottomed containers of various shapes, such as cylinders, square tubes, and cones. Also, "drawn product" refers to a processed product formed by drawing, and is characterized by having no seams in the formed processed product. Note that "drawn product" also includes processed products formed by combining drawing with other processing methods different from drawing, such as bending, crushing, and twisting.

[0008] Increasing the drawing depth often makes the material more susceptible to fracture, making processing difficult. Even if the process can be completed without fracture, the resulting drawn product is likely to have large undulations (ears) on its edge. In particular, when the drawing depth is large relative to the diameter of the punch used during the process, the drawn product must be formed through multiple drawing steps, which makes the ears particularly likely to become large. The formation of large ears not only impairs the shape of the drawn product, but also makes it more likely that adjacent ears will overlap or that cracks will form between adjacent ears during the drawing process. Furthermore, the formation of large ears requires an additional process for removing the ears from the drawn product. Therefore, there is a demand for a copper alloy sheet material that can reduce the ears formed on the edge of the drawn product.

[0009] In this regard, in the Cu—Ni—Si alloy described in Patent Document 1, the difference in mechanical properties between the direction parallel to the rolling direction (rolling parallel direction) and the direction perpendicular to the rolling direction (rolling perpendicular direction) is reduced by accumulating Cube orientation. Therefore, in applications where bending is performed with the rolling parallel direction and the rolling perpendicular direction as bending axes, such as connectors, terminals, switches, relays, and lead frames, anisotropy can be reduced by considering only these two directions. However, no consideration has been given to drawing, which is affected by anisotropy in all directions, not just the rolling parallel direction and the rolling perpendicular direction. Furthermore, there is no disclosure of achieving both high tensile strength and high electrical conductivity while reducing the size of the ears formed on the edge of a drawn product, nor are there any evaluation results for these properties. In this regard, the Cu—Ni—Si alloy of Patent Document 1 has an integrated Cube orientation, so that the mechanical properties along a direction forming an angle of 45° with respect to the rolling direction are significantly different from those along the rolling direction or perpendicular to the rolling direction. Therefore, when this copper alloy is used in drawing, large ears are formed on the edge of the resulting drawn product. Furthermore, even when looking at the manufacturing method of the Cu—Ni—Si alloy described in Patent Document 1, it is manufactured by performing the following steps in order: casting, ingot facing, soaking, hot rolling, cold rolling, solution treatment (recrystallization annealing), age hardening, cold rolling, and low-temperature annealing, but does not include an intermediate annealing step for coarsening the crystal grain size after the hot rolling step.

[0010] Furthermore, although Patent Document 2 describes that the drawing workability (deep drawing workability) of copper alloy sheet material is improved, the evaluation of drawing workability only evaluates the presence or absence of fracture when a punch having a large spherical tip with a diameter of 10 mm is pressed against a blank material taken from the copper alloy sheet material to produce a cup, and only evaluates the presence or absence of fracture under gentle drawing conditions, and does not show evaluation results under drawing conditions in which the depth of the drawn product is large relative to the diameter of the punch during drawing. Furthermore, Patent Document 2 does not consider at all the ears formed on the edge of the drawn product. Furthermore, it does not disclose how to achieve both high tensile strength and high electrical conductivity by reducing the ears formed on the edge of the drawn product, nor does it show evaluation results of these properties. Furthermore, even in terms of the manufacturing method, the copper alloy sheet material described in Patent Document 2 is manufactured by sequentially carrying out a hot rolling step, a cold rolling step, a solution treatment step, an aging treatment step, a pickling treatment step, a final cold rolling step, and a low-temperature annealing step, and does not include at least an intermediate annealing step for coarsening the crystal grain size after the hot rolling step.

[0011] Therefore, the present invention has been made in consideration of the above problems, and aims to provide a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product that have high tensile strength and high electrical conductivity, and also have excellent drawing workability, and in particular, that can reduce the size of the ears formed on the edges of the drawn product.

[0012] The present inventors have discovered that in a copper alloy sheet having an alloy composition containing 1.00 mass% or more and 5.00 mass% or less of Ni, 0.20 mass% or more and 1.30 mass% or less of Si, with the balance being Cu and inevitable impurities, by setting the maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface of the copper alloy sheet, obtained from crystal orientation analysis by the EBSD method described later, to 3.0 or less, setting the tensile strength to be in the range of 500 MPa or more and 900 MPa or less, and setting the electrical conductivity to be 30% IACS or more, the tensile strength and electrical conductivity of the copper alloy sheet can be increased, and the drawing workability can be improved, and in particular, the ears formed on the edge of the drawn product can be made smaller, and have completed the present invention.

[0013] (1) A copper alloy sheet material having an alloy composition containing 1.00% by mass or more and 5.00% by mass or less of Ni, 0.20% by mass or more and 1.30% by mass or less of Si, with the balance being Cu and inevitable impurities, wherein the maximum value of the strength of an inverse pole figure for a crystal plane facing the normal direction (ND) of the sheet surface, obtained by crystal orientation analysis using an EBSD method, measured on the sheet surface of the copper alloy sheet material, is 3.0 or less, the tensile strength is in the range of 500 MPa or more and 900 MPa or less, and the electrical conductivity is 30% IACS or more.

[0014] (2) The copper alloy sheet material according to (1) above, wherein in the inverse pole figure, the proportion of azimuth angles at which the strength is 2.0 or less to all azimuth angles is 50% or more.

[0015] (3) The copper alloy sheet material according to (1) or (2), wherein the alloy composition further contains at least one optional additional component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a total amount of 0.10 mass% or more and 1.00 mass% or less.

[0016] (4) A copper alloy sheet material for drawing, comprising the copper alloy sheet material according to any one of (1) to (3) above.

[0017] (5) A drawn product obtained by drawing the copper alloy sheet material according to any one of (1) to (3) above.

[0018] According to the present invention, it is possible to provide a copper alloy sheet material, a copper alloy sheet material for drawing, and a drawn product that have high tensile strength and high electrical conductivity, and also have excellent drawing workability, in particular, that can reduce the size of the ears formed on the edges of the drawn product.

[0019] FIG. 1 is a diagram illustrating a method for measuring the size of the selvage (waviness) formed on the edge of a typical drawn product made of copper alloy sheet material. FIG. 1(a) is a bottom view of the drawn product when a line segment extending in the radial direction from the center position of the bottom surface of the drawn product to the position of the circular outline of the bottom surface is drawn while rotating it by 45°. FIG. 1(b) is a perspective view of the drawn product of FIG. 1(a), showing the height from the bottom surface position of the drawn product to the position of the selvage present on the upper edge.

[0020] Next, an embodiment of the present invention will be described. The following description shows examples of embodiments of the present invention and does not limit the scope of the claims.

[0021] The copper alloy sheet according to the present invention has an alloy composition containing Ni in the range of 1.00 mass % or more and 5.00 mass % or less, Si in the range of 0.20 mass % or more and 1.30 mass % or less, with the balance being Cu and unavoidable impurities, and the copper alloy sheet has a maximum inverse pole figure intensity of 3.0 or less for a crystal plane facing the normal direction (ND) of the sheet surface, which is obtained by crystal orientation analysis using an EBSD method, measured on the sheet surface of the copper alloy sheet, a tensile strength of 500 MPa or more and 900 MPa or less, and an electrical conductivity of 30% IACS or more.

[0022] The copper alloy sheet of the present invention contains at least appropriate amounts of Ni and Si, and is manufactured under appropriate manufacturing conditions to suppress the development of texture, thereby reducing the maximum value of the inverse pole figure intensity to 3.0 or less, thereby reducing anisotropy and thereby reducing the selvage formed on the edge of a drawn product, i.e., the waviness of the edge of the drawn product. Furthermore, by containing at least appropriate amounts of Ni and Si, the copper alloy sheet of the present invention can increase the tensile strength and electrical conductivity of the copper alloy sheet. Therefore, the copper alloy sheet of the present invention can provide a copper alloy sheet, a copper alloy sheet for drawing, and a drawn product that have high tensile strength and high electrical conductivity, and can achieve excellent drawing workability, particularly reducing the selvage formed on the edge of the drawn product.

[0023] [1] Alloy composition of copper alloy sheet The copper alloy sheet of the present invention has an alloy composition containing, as essential components, Ni in the range of 1.00 mass% to 5.00 mass% and Si in the range of 0.20 mass% to 1.30 mass%. The reasons for limiting the alloy composition of the copper alloy sheet will be explained below.

[0024] (Ni: 1.00% by mass or more and 5.00% by mass or less) Ni (nickel) is an important component that has the effect of increasing the tensile strength of a copper alloy sheet material, and is contained in a range of 1.00% by mass or more and 5.00% by mass or less. Here, if the Ni content is less than 1.00% by mass, a high tensile strength of 500 MPa or more cannot be obtained. Furthermore, if the Ni content is more than 5.00% by mass, the tensile strength of the copper alloy sheet material exceeds 900 MPa, and a coarse second phase consisting of a compound with Si is easily formed, and this second phase is likely to become the starting point of cracks during drawing. Furthermore, if the Ni content is more than 5.00% by mass, the electrical conductivity of the copper alloy sheet material decreases. Therefore, from the viewpoint of increasing the tensile strength and electrical conductivity of the copper alloy sheet and making it difficult for cracks to occur in the drawn product, the Ni content is in the range of 1.00 mass% or more and 5.00 mass% or less, preferably in the range of 1.00 mass% or more and 4.50 mass% or less, more preferably in the range of 1.50 mass% or more and 4.50 mass% or less, and even more preferably in the range of 2.00 mass% or more and 4.00 mass% or less. In particular, from the viewpoint of further increasing the tensile strength of the copper alloy sheet, the Ni content is preferably 1.50 mass% or more. Furthermore, from the viewpoint of further increasing the electrical conductivity of the copper alloy sheet, the Ni content is preferably 4.50 mass% or less.

[0025] (Si: 0.20 mass% or more and 1.30 mass% or less) Si (silicon) is an important component that has the effect of increasing the tensile strength of a copper alloy sheet material, and is contained in a range of 0.20 mass% or more and 1.30 mass% or less. Here, if the Si content is less than 0.10 mass%, a high tensile strength of 500 MPa or more cannot be obtained. Furthermore, if the Si content is more than 1.30 mass%, the tensile strength of the copper alloy sheet material exceeds 900 MPa, and a coarse second phase consisting of a compound with Ni is easily formed, and this second phase is likely to become the starting point of cracks during drawing. Furthermore, if the Si content is more than 1.30 mass%, the electrical conductivity of the copper alloy sheet material decreases. Therefore, from the viewpoint of increasing the tensile strength and electrical conductivity of the copper alloy sheet and making it difficult for cracks to occur in the drawn product, the Si content is in the range of 0.20 mass% or more and 1.30 mass% or less, preferably in the range of 0.20 mass% or more and 1.10 mass% or less, more preferably in the range of 0.30 mass% or more and 1.10 mass% or less, and even more preferably in the range of 0.50 mass% or more and 1.00 mass% or less. In particular, from the viewpoint of further increasing the tensile strength of the copper alloy sheet, the Si content is preferably 0.30 mass% or more. Furthermore, from the viewpoint of further increasing the electrical conductivity of the copper alloy sheet, the Si content is preferably 1.10 mass% or less.

[0026] <Optionally Added Component> Furthermore, the copper alloy sheet material of the present invention may further contain, as an optional added component, at least one optional added component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a range of 0.10 mass% or more and 1.00 mass% or less in total.

[0027] (Sn: 0.10% by mass or more and 0.30% by mass or less) Sn (tin) is a component that has the effect of improving stress relaxation resistance. To exert this effect, the Sn content is preferably 0.10% by mass or more. On the other hand, if the Sn content exceeds 0.30% by mass, the electrical conductivity tends to decrease. For this reason, the Sn content is preferably in the range of 0.10% by mass or more and 0.30% by mass or less.

[0028] (Zn: 0.10% by mass or more and 0.50% by mass or less) Zn (zinc) is a component that has the effect of improving the adhesion and migration properties of Sn plating. To exert this effect, the Zn content is preferably 0.10% by mass or more. On the other hand, if the Zn content exceeds 0.50% by mass, the electrical conductivity tends to decrease. For this reason, the Zn content is preferably in the range of 0.10% by mass or more and 0.50% by mass or less.

[0029] (Mg: 0.10% by mass or more and 0.30% by mass or less) Mg (magnesium) is a component that has the effect of improving stress relaxation resistance. To exert this effect, the Mg content is preferably 0.10% by mass or more. On the other hand, if the Mg content exceeds 0.30% by mass, the electrical conductivity tends to decrease. Therefore, the Mg content is preferably in the range of 0.10% by mass or more and 0.30% by mass or less.

[0030] (Fe: 0.05% by mass or more and 0.30% by mass or less) Fe (iron) is a component that has the effect of suppressing coarsening of crystal grains after dynamic recrystallization and the effect of preventing roughness of the surface of a drawn product in the hot rolling step [Step 3] described below. To exert this effect, the Fe content is preferably 0.05% by mass or more. Furthermore, if the Fe content exceeds 0.30% by mass, coarse crystallized products containing Fe are likely to be generated during casting, which makes it easier for cracks to form. For this reason, the Fe content is preferably in the range of 0.05% by mass or more and 0.30% by mass or less.

[0031] (Cr: 0.05% by mass or more and 0.30% by mass or less) Cr (chromium) is a component that has the effect of suppressing coarsening of crystal grains after dynamic recrystallization and the effect of preventing roughness of the surface of a drawn product in the hot rolling step [Step 3] described below. To exert this effect, the Cr content is preferably 0.05% by mass or more. Furthermore, if the Cr content exceeds 0.30% by mass, coarse crystallized products containing Cr are likely to be generated during casting, which makes it easier for cracks to form. For this reason, the Cr content is preferably in the range of 0.05% by mass or more and 0.30% by mass or less.

[0032] (Total content of optional components: 0.10 mass % or more and 1.00 mass % or less) In order to obtain the effects of the optional components described above, it is preferable that the total content of these optional components be 0.10 mass % or more. On the other hand, if these optional components are contained in large amounts, the electrical conductivity decreases, so it is preferable that the total content of the optional components be 1.00 mass % or less.

[0033] (Balance: Cu and inevitable impurities) The copper alloy constituting the copper alloy sheet material has an alloy composition consisting of the above-mentioned components, with the balance being Cu (copper) and inevitable impurities. The term "unavoidable impurities" as used herein generally refers to impurities present in raw materials for metal products or unavoidably mixed in during the manufacturing process. These impurities are essentially unnecessary but are tolerated in trace amounts because they do not affect the properties of the metal product. Examples of inevitable impurities include non-metallic elements such as sulfur (S), carbon (C), and oxygen (O), and metallic elements such as antimony (Sb). The upper limit of the content of these components can be, for example, 0.05% by mass for each of the above components, or 0.20% by mass for the total amount of the above components.

[0034] [2] Maximum Intensity of Inverse Pole Figure for Crystal Plane Oriented in the Normal Direction (ND) of the Sheet Surface In the copper alloy sheet of the present invention, the maximum intensity of the inverse pole figure for the crystal plane orientated in the normal direction (ND) of the sheet surface, obtained by crystal orientation analysis using the EBSD method, measured on the sheet surface of the copper alloy sheet, is 3.0 or less. When the maximum intensity of this inverse pole figure exceeds 3.0, the orientation to one of the atomic planes (crystal planes) becomes high, and the anisotropy increases depending on the oriented atomic plane. In other words, from the viewpoint of improving the drawing workability of the copper alloy sheet, particularly from the viewpoint of reducing the selvage (waviness) formed on the edge of the drawn product, it is important to suppress the orientation to all atomic planes (crystal planes). At this time, in order to evaluate the orientation of the copper alloy sheet, it is effective to evaluate the maximum value among the inverse poles. Here, from the viewpoint of improving drawing workability, the maximum intensity of the inverse pole figure for the crystal plane orientated in the normal direction (ND) of the sheet surface is preferably 2.6 or less, more preferably 2.5 or less, and even more preferably 2.0 or less. On the other hand, the lower limit of the maximum intensity of the inverse pole figure is not particularly defined, but can be 1.0 or 1.2.

[0035] Here, the maximum value of the intensity of the inverse pole figure can be obtained from crystal orientation analysis data calculated using analysis software (OIM Analysis, manufactured by TSL) from crystal orientation data continuously measured using an EBSD detector attached to a high-resolution scanning analytical electron microscope (JEOL Ltd., JSM-7001FA). "EBSD" stands for Electron Backscatter Diffraction, and refers to a crystal orientation analysis technique that utilizes reflected electron Kikuchi diffraction, which occurs when an electron beam is irradiated onto a copper alloy sheet sample in a scanning electron microscope (SEM). "OIM Analysis" is software for analyzing data measured by EBSD. Measurements can be performed on the surface of an electropolished copper alloy sheet. Measurements can also be performed on a cross section along the rolling direction of a copper alloy sheet that has been embedded in resin and finished by mechanical polishing and buffing (colloidal silica). The measurement area on these cross sections and plate surfaces is approximately 400 μm × 800 μm, and measurements can be performed with a step size of 0.5 μm. If the above field size cannot be obtained due to the sample size in both cross-sectional and plate surface measurements, measurements can be taken in multiple fields of view and the average value can be used.

[0036] Among the crystal orientation data obtained by the EBSD method in this way, measurement points where the reliability index (CI) value is 0.1 or more are targeted for analysis, and the intensities are measured at polar angles in the range of 0 to 90° and azimuthal angles in the range of 0 to 355° in 5° increments, and the maximum intensity value of the inverse pole figure can be obtained from the inverse pole figure for the atomic plane in the normal direction (ND) of the plate surface.

[0037] [3] Proportion of azimuth angles at which the intensity is 2.0 or less in all azimuth angles in an inverse pole figure for a crystal plane facing the normal direction (ND) of the sheet surface. In the copper alloy sheet of the present invention, the proportion of azimuth angles at which the intensity is 2.0 or less in all azimuth angles is preferably 50% or more in an inverse pole figure for a crystal plane facing the normal direction (ND) of the sheet surface obtained by crystal orientation analysis using the EBSD method, measured on the sheet surface of the copper alloy sheet. By making this proportion 50% or more, the orientation at a specific azimuth angle becomes smaller, thereby reducing anisotropy, thereby further improving the drawing workability of the copper alloy sheet, and in particular, further reducing the selvage formed on the edge of a drawn product. Here, from the viewpoint of improving the drawing workability of the copper alloy sheet, the proportion of azimuth angles at which the intensity is 2.0 or less in all azimuth angles is preferably 52% or more, more preferably 60% or more, and more preferably 70% or more.

[0038] The proportion of orientation angles at which the intensity is 2.0 or less to all orientation angles of the copper alloy sheet material can be obtained by calculating the proportion of the number of orientation angles at which the intensity is 2.0 or less to the number of all orientation angles measured in an inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface obtained from the crystal orientation analysis by the above-mentioned EBSD method.

[0039] [4] Tensile strength of copper alloy sheet The copper alloy sheet of the present invention has a tensile strength in the range of 500 MPa or more and 900 MPa or less. As a result, even when the copper alloy sheet is used for small or thin parts such as electrical and electronic components or automotive components, the desired tensile strength can be obtained, making the copper alloy sheet suitable for use in various drawn products. On the other hand, when the tensile strength exceeds 900 MPa, the fracture resistance of the copper alloy sheet also increases, but the deformation resistance during drawing also increases, and the copper alloy sheet tends to be more likely to break in drawing tests. Therefore, the tensile strength of the copper alloy sheet is in the range of 500 MPa or more and 900 MPa or less, and preferably in the range of 600 MPa or more and 900 MPa or less. Here, the tensile strength can be, for example, the tensile strength when pulled in a direction parallel to the rolling direction. The tensile strength is measured using two test pieces of No. 13B specified in JIS Z2241, cut out so that the longitudinal direction is parallel to the rolling direction, and the average value of the tensile strength obtained from the two test pieces is taken as the measured value of the tensile strength.

[0040] [5] Electrical Conductivity of Copper Alloy Sheet The copper alloy sheet of the present invention has an electrical conductivity of 30% IACS or more. This allows the copper alloy sheet to have high electrical conductivity, and therefore the copper alloy sheet can also be used for drawn products that require electromagnetic wave shielding and heat dissipation. Therefore, the electrical conductivity of the copper alloy sheet is 30% IACS or more, and preferably 33% IACS or more. Here, the electrical conductivity (IACS; International Annealed Copper Standard) is measured twice using a four-terminal method, and the average value of the electrical conductivity obtained by the two measurements is used as the measured electrical conductivity.

[0041] [6] Example of a manufacturing method for a copper alloy sheet The above-mentioned copper alloy sheet can be realized by controlling the alloy composition and the manufacturing process in combination, and the manufacturing process is not particularly limited. Among them, the following method can be mentioned as an example of a manufacturing process that can obtain such high tensile strength and excellent drawing workability.

[0042] In one example of the method for producing a copper alloy sheet of the present invention, a copper alloy material having an alloy composition equivalent to that of the above-mentioned copper alloy sheet is sequentially subjected to at least a melting and casting step (step 1), a reheating step (step 2), a hot rolling step (step 3), an intermediate annealing step (step 4), a first cold rolling step (step 5), a solution treatment step (step 6), an aging heat treatment step (step 7), a second cold rolling step (step 8), and a low-temperature annealing step (step 9).

[0043] (i) Melting and Casting Step [Step 1] In the melting and casting step [Step 1], a copper alloy material having an alloy composition equivalent to the above-mentioned alloy composition is melted and cast to produce an ingot of a predetermined shape (e.g., thickness 30 mm, width 100 mm, length 150 mm). In the melting and casting step [Step 1], the copper alloy material is preferably melted and cast in air, an inert gas atmosphere, or a vacuum using a high-frequency melting furnace. Note that the alloy composition of the copper alloy material may not necessarily be completely identical to that of the copper alloy sheet material produced due to the addition of components that adhere to or volatilize the melting furnace in each manufacturing step, but it has substantially the same alloy composition as the copper alloy sheet material.

[0044] (ii) Reheating Step [Step 2] The reheating step [Step 2] is a step of heat treating the ingot after the casting step [Step 1]. The conditions for the heat treatment in the reheating step [Step 2] are preferably such that the ultimate temperature (heat treatment temperature) is in the range of 900 ° C. to 1050 ° C., and the holding time at the ultimate temperature (heat treatment time) is in the range of 1 hour to 10 hours. Here, if the ultimate temperature is less than 900 ° C., dynamic recrystallization does not occur sufficiently in the hot rolling step [Step 3] described below, and therefore, a non-uniform structure is likely to occur. On the other hand, if the ultimate temperature exceeds 1050 ° C., the grain boundaries are weakened, and cracks are likely to occur in the hot-rolled material after the hot rolling step [Step 3].

[0045] (iii) Hot Rolling Step [Step 3] The hot rolling step [Step 3] is a step in which the ingot that has been subjected to the reheating step [Step 2] is hot rolled until it reaches a predetermined thickness to produce a hot-rolled material. The conditions for the hot rolling step [Step 3] can be set so that dynamic recrystallization occurs; for example, the rolling temperature can be set to 700°C or higher, and the total processing rate (total rolling reduction) can be set to 50% or higher. On the other hand, if dynamic recrystallization does not occur sufficiently in the hot rolling step [Step 3], the resulting copper alloy sheet material is likely to have a non-uniform structure.

[0046] The "working rate" (rolling reduction) in this specification is a value obtained by subtracting the cross-sectional area after rolling from the cross-sectional area before rolling, dividing the value by the cross-sectional area before rolling, and multiplying the result by 100, expressed as a percentage, and is expressed by the following formula: [Working rate] = {([cross-sectional area before rolling] - [cross-sectional area after rolling]) / [cross-sectional area before rolling]} x 100 (%)

[0047] As an example, when the rolling temperature in the hot rolling step [Step 3] is 700°C, the sum of the processing rate calculated from the cross-sectional area before the start of rolling and the cross-sectional area after the passes completed before reaching 700°C can be used as the total processing rate (total rolling reduction), and the total processing rate (total rolling reduction) in the temperature range from the heat treatment temperature to 700°C in the reheating step [Step 2] can be set to 50% or more.

[0048] The temperature of the ingot during the hot rolling step [step 3] can be measured with a radiation thermometer.

[0049] (iv) Intermediate Annealing Step [Step 4] The intermediate annealing step [Step 4] is a step in which the hot-rolled material after the hot working step [Step 3] is subjected to a heat treatment according to the alloy composition.

[0050] The annealing conditions in the intermediate annealing step [Step 4] are preferably such that the ultimate temperature is in the range of 800°C or higher and 1000°C or lower, and the holding time at the ultimate temperature is in the range of 30 seconds to 1 hour. By growing crystal grains through heat treatment at a high temperature of 800°C or higher, the development of the rolling texture obtained in the first cold rolling step [Step 5] described below and the recrystallization texture obtained in the subsequent solution treatment step [Step 6] is suppressed. When an inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface is obtained by crystal orientation analysis using the EBSD method, the maximum intensity of the inverse pole figure becomes a low value of 3.0 or lower. Therefore, the anisotropy of the copper alloy sheet can be reduced, and as a result, the drawing workability of the copper alloy sheet can be improved. Here, if the ultimate temperature is less than 800°C, the crystal grain growth becomes insufficient and the anisotropy of the copper alloy sheet increases, resulting in a decrease in the drawing workability of the copper alloy sheet. In particular, the temperature reached in the intermediate annealing step [Step 4] is preferably 850°C or higher, more preferably 900°C or higher, from the viewpoint of further reducing the maximum value of the intensity of the inverse pole figure obtained by crystal orientation analysis using the EBSD method for the crystal plane facing the normal direction (ND) of the sheet surface. On the other hand, it is not desirable for the temperature to exceed 1000°C because there is a possibility of partial melting of the material.

[0051] Furthermore, the heat treatment time (holding time at the ultimate temperature) in the intermediate annealing step [step 4] has less effect on the anisotropy of the copper alloy sheet material than the heat treatment temperature, and therefore can be carried out in the range of 30 seconds to 1 hour depending on the characteristics of the equipment, such as a continuous running annealing furnace or a batch furnace. Here, if the holding time at the ultimate temperature is less than 30 seconds, the growth of crystal grains becomes insufficient. On the other hand, even if the holding time at the ultimate temperature is longer than 1 hour, the change in crystal grains becomes small, and therefore heat treatment for a longer time than this is not desirable from the viewpoint of productivity.

[0052] After the intermediate annealing step [step 4], the cold-rolled material is preferably cooled from the ultimate temperature to a temperature of 300°C or less, which is a temperature at which new precipitation is unlikely to occur. In this case, the cold-rolled material can be cooled at a cooling rate of 1°C / s or more, for example, by water cooling.

[0053] The hot-rolled material after the hot working step [step 3] or the intermediate annealing step [step 4] may be subjected to facing, in which the surface is scraped off. By performing facing, it is possible to remove surface oxide films and defects that have occurred in the hot working step [step 3] or the intermediate annealing step [step 4]. The conditions for facing are not particularly limited as long as they are commonly used conditions. The amount of material scraped off from the surface of the hot-rolled material by facing can be adjusted appropriately based on the state of oxidation of the surface, and can be, for example, about 1 mm to 5 mm from both the front and back sides of the hot-rolled material.

[0054] (v) First cold rolling step [step 5] The first cold rolling step [step 5] is a step of cold rolling the hot rolled material after the intermediate annealing step [step 4]. Here, the rolling in the first cold rolling step [step 5] is performed in two stages.

[0055] In the first stage of rolling, the hot rolled material is rolled in the same direction as the rolling direction in the hot working step [Step 3]. Here, the working ratio d 1 are the plate thicknesses before and after the first rolling stage, respectively. 0 , t 1 When d is set, it is expressed by the following equation (1). 1 = 100 × (t 0 -t 1 ) / t 0 ...(1)

[0056] The second rolling stage is performed by rolling the cold rolled material after the first rolling stage. The rolling direction in the second rolling stage may be the same as or different from the rolling direction in the first rolling stage. 2 are the thicknesses of the plates after the second rolling stage, respectively. 2 When d is set, it is expressed by the following equation (2). 2 = 100 × (t 1 -t 2 ) / t 1 ...(2)

[0057] At this time, the second stage processing rate d 2 The first stage processing rate d 1 The ratio (d 1 / d 2) is set to a processing rate d in the range of 0.3 to 2.0. 1 , d 2 Adjust the processing rate d 2 Processing rate d 1 The ratio (d 1 / d 2 If the working ratio d is out of the range of 0.3 or more and 2.0 or less, when an inverse pole figure is obtained for a crystal plane facing the normal direction (ND) of the sheet surface, the maximum value of the intensity of the inverse pole figure becomes large, and the anisotropy of the material increases, so that the drawing workability of the copper alloy sheet material deteriorates, and in particular, the ears formed on the edge of the drawn product become large. 2 Processing rate d 1 The ratio (d 1 / d 2 From the viewpoint of reducing the size of the edge formed on the edge of the drawn product, the working ratio d is preferably in the range of 0.5 to 1.5, more preferably in the range of 0.7 to 1.3, and even more preferably in the range of 0.9 to 1.1. 2 Processing rate d 1 The ratio (d 1 / d 2 ) in the range of 0.5 or more and 1.5 or less, when an inverse pole figure for a crystal plane facing the normal direction (ND) of the plate surface is obtained by crystal orientation analysis using the EBSD method, the proportion of azimuth angles at which the intensity is 2.0 or less among all azimuth angles can be made 50% or more.

[0058] In addition, the total processing rate d in the first cold rolling step [step 5] 0 The total working ratio d in the first cold rolling step [step 5] can be expressed by the following formula (3), and is preferably 80% or more. 0 If the strain is less than 80%, sufficient strain is not introduced, and the recrystallized structure with non-uniform grain size is likely to be formed in the solution treatment step [Step 6] described later. As a result, the copper alloy sheet material is likely to break due to stress concentration during drawing, which may lead to a decrease in the workability of the copper alloy sheet material. 0 = 100 × (t 0 -t 2 ) / t 0 ...(3)

[0059] (vi) Solution Treatment Step [Step 6] The solution treatment step [Step 6] is a step in which the cold-rolled material after the first cold rolling step [Step 5] is subjected to heat treatment to recrystallize and then cooled. Here, the heat treatment conditions in the solution treatment step [Step 6] can be, for example, a temperature range of 700 ° C. to 1000 ° C., and a holding time at the temperature range of 10 seconds to 60 seconds. Here, if the temperature is less than 700 ° C. or the holding time is less than 10 seconds, the amount of precipitation strengthening in the aging heat treatment step [Step 7] described later decreases, thereby reducing the tensile strength of the copper alloy sheet. On the other hand, if the temperature exceeds 1000 ° C. or the holding time exceeds 60 seconds, the crystal grain size becomes coarse, and the tensile strength of the copper alloy sheet tends to decrease.

[0060] The solution-treated material after the solution treatment step [Step 6] is preferably cooled immediately. More specifically, the solution-treated material after the solution treatment step [Step 6] is preferably cooled at a cooling rate of 40°C / s or more. Here, if the cooling rate is less than 40°C / s, coarse precipitates are formed during cooling, which reduces the amount of precipitation strengthening in the aging heat treatment step [Step 7], and the tensile strength of the copper alloy sheet tends to decrease.

[0061] (vii) Aging Heat Treatment Step [Step 7] The aging heat treatment step [Step 7] is a step of precipitation strengthening by heat treatment of the cooled solution-treated material. Here, the conditions for the heat treatment in the aging heat treatment step [Step 7] are that the ultimate temperature is in the range of 400 ° C or higher and 600 ° C or lower, and the holding time at the ultimate temperature is in the range of 1 hour or higher and 10 hours or lower. Here, if the ultimate temperature is lower than 400 ° C or the holding time is shorter than 1 hour, precipitation strengthening is difficult to achieve, and the tensile strength and electrical conductivity of the copper alloy sheet material are likely to decrease. On the other hand, if the ultimate temperature exceeds 600 ° C or the holding time exceeds 10 hours, the precipitates become coarse, and the tensile strength of the copper alloy sheet material is likely to decrease.

[0062] (viii) Second cold rolling step [step 8] The second cold rolling step [step 8] is a step of further cold rolling the cold-rolled material after the aging heat treatment step [step 7]. Here, the total working ratio in the second cold rolling step [step 8] is preferably in the range of 5% to 20%. Here, if the total working ratio is less than 5%, the amount of work hardening is small, making it difficult to obtain the effect of increasing the tensile strength of the copper alloy sheet. Furthermore, if the total working ratio is greater than 20%, the rolling texture develops and the anisotropy of the copper alloy sheet increases. When an inverse pole figure for a crystal plane facing the normal direction (ND) of the sheet surface is obtained by crystal orientation analysis using the EBSD method, the maximum value of the inverse pole figure intensity becomes greater than 3.0, thereby reducing the drawing workability of the copper alloy sheet or making the copper alloy sheet more susceptible to fracture during drawing.

[0063] (ix) Low-temperature annealing step [step 9] The low-temperature annealing step [step 9] is an annealing step in which heat treatment is performed on the cold-rolled material after the second cold rolling step [step 8]. The conditions for the heat treatment in this low-temperature annealing step [step 9] are preferably such that the ultimate temperature is in the range of 200 ° C. or higher and 600 ° C. or lower, and the holding time at the ultimate temperature is in the range of 10 seconds or higher and 30 minutes or lower. Here, if the ultimate temperature is lower than 200 ° C. or the holding time is shorter than 10 seconds, excessive strain remains in the cold-rolled material after annealing, thereby reducing the drawing workability of the copper alloy sheet material. On the other hand, if the ultimate temperature exceeds 600 ° C. or the holding time at the ultimate temperature exceeds 30 minutes, work hardening due to cold rolling disappears.

[0064] The heating and cooling rates before and after the annealing in the low-temperature annealing step [step 9] are not particularly limited, but can be, for example, in the range of 1° C. / s to 100° C. / s.

[0065] [7] Uses of Copper Alloy Sheet The copper alloy sheet of the present invention is preferably used as a copper alloy sheet for drawing. That is, the copper alloy sheet of the present invention is particularly suitable for obtaining drawn products by drawing, and is suitable for forming drawn parts used in electronic devices and automotive on-board equipment, for example. More specifically, it is suitable for use in connectors, lead frames, relays, switches, sockets, shielding cases, shielding cans, camera module cases, vibration device cases, heat dissipation parts for liquid crystal and organic EL displays, batteries, probe pins, gas shut-off valves, etc. for electronic devices and automotive on-board equipment that require high performance, high current, and miniaturization.

[0066] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, but includes all aspects encompassed by the concept of the present invention and the scope of the claims, and can be modified in various ways within the scope of the present invention.

[0067] Next, in order to further clarify the effects of the present invention, examples of the present invention and comparative examples will be described, but the present invention is not limited to these examples of the present invention.

[0068] (Inventive Examples 1 to 21 and Comparative Examples 1 to 10) Various copper alloy materials having the alloy compositions shown in Table 1 were melted, cooled in an air atmosphere, and cast to obtain ingots through a melting and casting process [Step 1]. The ingots were then subjected to a reheating process [Step 2] in which heat treatment was performed at an ultimate temperature (heat treatment temperature) of 1000°C and a holding time at the ultimate temperature (heat treatment time) of 1 hour. Then, a hot-rolling process [Step 3] was immediately performed in which the ingot was rolled in the longitudinal direction of the rolling direction at a temperature in the range of 700°C to 1000°C, with a total working ratio of 50% or more. The rolled materials after the hot-rolling process [Step 3] were subjected to an intermediate annealing process [Step 4] in which heat treatment was performed at the ultimate temperature and holding time shown in Table 2, and then cooled to room temperature by water cooling.

[0069] The cooled hot rolled material is subjected to facing by removing about 1 mm to 2 mm from both the front and back surfaces to remove the oxide film on the surface, and then the first stage working rate d 1 , the plate thickness after the first rolling stage t1 , the second stage processing rate d 2 , the thickness of the plate after the second rolling stage t 2 , the ratio of the first-stage processing rate to the second-stage processing rate (d 1 / d 2 ) in such a way that the longitudinal direction of the hot-rolled material was the rolling direction in both cases, a first cold-rolling step [step 5] was carried out in which the hot-rolled material was rolled in two stages.

[0070] The cold-rolled material after the first cold rolling step [step 5] was subjected to a solution treatment step [step 6] in which the material was heat-treated at the temperature and holding time shown in Table 2, and then cooled to room temperature at a cooling rate of 100°C / s.

[0071] The cooled solution-treated material was subjected to an aging heat treatment step [Step 7] in which heat treatment was performed at the temperature and holding time shown in Table 2, and then a second cold rolling step [Step 8] in which rolling was performed so that the longitudinal direction was the rolling direction under the conditions of the plate thickness after rolling and the total processing rate shown in Table 2, to obtain a rolled material with a plate thickness of 0.20 mm.

[0072] The rolled material after the second cold rolling step [step 8] was subjected to a low-temperature annealing step [step 9] in which the material was heat-treated at the attained temperature and for the holding time shown in Table 2, thereby producing the copper alloy sheet material of the present invention.

[0073] On the other hand, in Comparative Example 10, a copper alloy sheet material was produced without performing the intermediate annealing step [Step 4].

[0074] In Table 1, among the constituent elements other than copper (Cu), Ni (nickel), and Si (silicon), Sn (tin), Zn (zinc), Mg (magnesium), Fe (iron), and Cr (chromium) are designated as optional added elements. In Table 1, a horizontal line "-" is entered in the column for an element not included in the alloy composition of the copper alloy material, indicating that the element is not included, or if it is included, its amount is below the detection limit.

[0075] [Various Measurement and Evaluation Methods] The copper alloy sheets according to the above-described invention examples and comparative examples were used to carry out the following characteristic evaluations. The evaluation conditions for each characteristic were as follows.

[0076] [1] Maximum Intensity of Inverse Pole Figures for Crystal Planes Facing the Normal Direction (ND) of the Sheet Surface The maximum intensity of the inverse pole figure for the crystal planes facing the normal direction (ND) of the sheet surface of the copper alloy sheet was obtained from crystal orientation analysis data calculated using analysis software (TSL, OIM Analysis) from crystal orientation data continuously measured using an EBSD detector attached to a high-resolution scanning analytical electron microscope (JEOL Ltd., JSM-7001FA) for the copper alloy sheets obtained in the present invention and comparative examples. The measurement was performed on samples whose surface (sheet surface) was mirror-finished by electrolytic polishing in a field of view of approximately 400 μm × 800 μm with a step size of 0.5 μm.

[0077] Among the crystal orientation data obtained by the EBSD method in this way, measurement points with a reliability index (CI) value of 0.1 or more were analyzed. The strength was measured at 5° increments for polar angles ranging from 0 to 90° and azimuthal angles ranging from 0 to 355°, and an inverse pole figure for the atomic plane in the normal direction (ND) of the sheet surface was obtained. In this example, the maximum strength value for the inverse pole figure for the atomic plane in the normal direction (ND) of the sheet surface was determined, and inverse pole figures with a maximum strength value of 3.0 or less were considered acceptable. The results are shown in Table 3. The rolling direction (RD) in this example was based on the rolling direction in the second cold rolling step [step 8].

[0078] [2] Proportion of azimuth angles with an intensity of 2.0 or less in all azimuth angles The proportion of azimuth angles with an intensity of 2.0 or less in all azimuth angles of the copper alloy sheet material was determined by calculating the proportion of the number of azimuth angles with an intensity of 2.0 or less among all measured azimuth angles in the inverse pole figure for the atomic plane in the normal direction (ND) of the sheet surface, and a proportion of 50% or more was considered to be acceptable. The results are shown in Table 3.

[0079] [3] Measurement of tensile strength of copper alloy sheet material Tensile strength was measured using two test pieces of type 13B specified in JIS Z2241, cut out from the test material so that the longitudinal direction was parallel to the rolling direction, and the average value of the tensile strength obtained from the two test pieces when pulled in the direction parallel to the rolling direction was taken as the measured value. In this example, a tensile strength in the range of 500 MPa or more and 900 MPa or less was considered to be acceptable. The results are shown in Table 3.

[0080] [4] Measurement of electrical conductivity of copper alloy sheet The electrical conductivity of the copper alloy sheet was measured twice using the four-terminal method, and the average value obtained by the two measurements was used as the measured electrical conductivity. The results are shown in Table 3.

[0081] [5] Evaluation of drawing workability of copper alloy sheet material The drawing workability of the copper alloy sheet material was evaluated by using a blank having a diameter of 45 mm formed by press punching from the obtained copper alloy sheet material having a thickness of 0.20 mm, applying a lubricating oil (product name: Pleton R-303P, manufactured by Sugimura Chemical Industry Co., Ltd.) to the sheet surface, attaching the blank to a die having a radius of curvature of the shoulder of 3 mm, and pushing a punch having a cylindrical shape with a diameter of 30 mm at the tip, a radius of curvature of the corner of the tip of 3 mm, and a clearance between the punch and the die of 0.27 mm into the center of the blank, thereby performing a first drawing process.

[0082] Furthermore, in the case of an example in which no cracks occurred in the first drawing process, the blank after the first drawing process was attached to a die with a shoulder radius of curvature of 3 mm so that the centers of the blank and the die overlapped, and a punch that was cylindrical with a tip diameter of 20 mm, had a tip corner radius of curvature of 3 mm, and the clearance between the punch and the die was 0.27 mm was pressed into the center of the blank to perform a second drawing process, thereby obtaining a cylindrical cup as a drawn product.

[0083] As shown in FIG. 1(a), the drawn product is drawn by a line segment L extending from the center C of the bottom surface 11 of the drawn product 1 to one side of the rolling direction X of the copper alloy plate material constituting the bottom surface. 1 Draw this line segment L 1 is set as the reference angle (0°). 1The height from the bottom surface 11 to the edge 13 of the side surface 12 of the drawn product 1 at the position where the butt is measured, and the height is H 0 Next, a line segment L is drawn from the center C of the bottom surface 11 of the drawn product 1. 1 Line segment L in a direction that forms a 45° angle clockwise with respect to 2 Draw this line segment L 1 The height from the bottom surface 11 to the edge 13 of the side surface 12 of the drawn product 1 at the position where the butt is measured, and the height is H 45 Similarly, from the center C, the line segment L 1 A line segment L is drawn in a direction that forms angles of 90°, 135°, 180°, 225°, 270°, and 315° clockwise with respect to 3 ~L 8 These line segments L 3 ~L 8 As shown in FIG. 1(b), the heights from the bottom surface 11 to the edge 13 of the side surface 12 of the drawn product 1 at the position where the ends abut are measured, and these heights are respectively calculated as H 90 , H 135 , H 180 , H 225 , H 270 , H 315 It was decided.

[0084] These heights H 0 , H 45 , H 90 , H 135 , H 180 , H 225 , H 270 , H 315 Using the above, the magnitude E [%] of the waviness (edge) on the edge of the drawn product was calculated from the following formulas (4) to (6). 1 = (2 x H 0 +H 90 +H 180 +H 270 ) / 5...(4) H 2 = (H 45 +H 135 +H 225 +H 315 ) / 4...(5) E=(H 1 -H 2 ) / {(H 1 +H 2) / 2} × 100 ... (6)

[0085] The size of the waviness (edge) on the edge of the drawn product was evaluated according to the following evaluation criteria. The results are shown in Table 3.

[0086] <Evaluation criteria for the size of waviness (edges) on the edges of drawn products> "4" (Excellent): When the waviness (edges) is 3.0% or less "3" (Good): When the waviness (edges) is more than 3.0% and 6.0% or less "2" (Acceptable): When the waviness (edges) is more than 6.0% and 10.0% or less "1" (Fail): When the waviness (edges) is more than 10.0% or when the blank breaks during drawing

[0087]

[0088]

[0089]

[0090] From the results in Tables 1 to 3, the copper alloy sheets of Inventive Examples 1 to 21 have alloy compositions within the appropriate range of the present invention, and the maximum value of the strength of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface is 3.0 or less, the tensile strength is in the range of 500 MPa or more and 900 MPa or less, and the electrical conductivity is 30% IACS or more, and at this time, the evaluation of the drawing workability is also "2", "3" or "4".

[0091] Therefore, the copper alloy sheet materials of Examples 1 to 21 of the present invention had high tensile strength and high electrical conductivity, and also had excellent drawing workability, and in particular, it was possible to reduce the ears formed on the edges of the drawn products.

[0092] In particular, when comparing the copper alloy sheets of Inventive Examples 1 and 2, the copper alloy sheet of Inventive Example 1 has a lower working ratio d 2 The first stage processing rate d 1 The ratio (d 1 / d 2) was within the preferred range of 0.5 or more and 1.5 or less, which was a smaller value than that of Inventive Example 2, in which this ratio was 1.6. In this case, the copper alloy sheet material of Inventive Example 1 had a ratio of azimuth angles in the inverse pole figure in which the intensity was 2.0 or less to all azimuth angles in a range of 50% or more, which was larger than that of Inventive Example 2, in which this ratio was 48%. Furthermore, in the copper alloy sheet material of Inventive Example 1, the waviness (ear) at the edge of the drawn product was also smaller than that of Inventive Example 2.

[0093] Furthermore, when comparing the copper alloy sheets of Inventive Examples 1 and 3, the copper alloy sheet of Inventive Example 3 achieved a temperature in the intermediate annealing step [Step 4] that was within the preferred range of 850°C to 1000°C, which was higher than the temperature achieved in Inventive Example 1, which achieved a temperature of 800°C. In this case, the copper alloy sheet of Inventive Example 3 had a maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface that was within the more preferred upper limit of 2.5 or less, which was smaller than that of Inventive Example 1. Furthermore, in the copper alloy sheet of Inventive Example 3, the waviness (ear) at the edge of the drawn product was also smaller than that of Inventive Example 1.

[0094] Furthermore, when comparing the copper alloy sheets of Inventive Examples 3 and 4, the copper alloy sheet of Inventive Example 4 achieved a temperature in the intermediate annealing step [Step 4] that was within a more preferable range of 900°C or higher and 1000°C or lower, which was higher than the temperature achieved in Inventive Example 3, which achieved a temperature of 850°C. In this case, the copper alloy sheet of Inventive Example 4 had a maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface that was within a more preferable upper limit range of 2.0 or lower, which was smaller than that of Inventive Example 3. Furthermore, in the copper alloy sheet of Inventive Example 4, the waviness (ear) at the edge of the drawn product was also smaller than that of Inventive Example 3.

[0095] In addition, when comparing the copper alloy sheets of Inventive Examples 1 and 5, the copper alloy sheet of Inventive Example 5 had a reduction ratio d 2 The first stage processing rate d 1 The ratio (d 1 / d 2 ) is 0.8, which is within a more preferable range of 0.7 to 1.3, and this ratio (d 1 / d 2 ) was 1.5, which was lower than that of Inventive Example 1. In this case, the copper alloy sheet of Inventive Example 5 had a ratio of azimuth angles in which the intensity was 2.0 or less to all azimuth angles in the inverse pole figure that was in the range of 60% or more, which is the preferable lower limit, and was higher than that of Inventive Example 1. Furthermore, in the copper alloy sheet of Inventive Example 5, the waviness (ear) at the edge of the drawn product was also smaller than that of Inventive Example 3.

[0096] In addition, when comparing the copper alloy sheets of Inventive Examples 1 and 6, the copper alloy sheet of Inventive Example 6 had a reduction ratio d 2 The first stage processing rate d 1 The ratio (d 1 / d 2 ) was 0.4, which was outside the preferred range of 0.5 or more and 1.5 or less. Therefore, in the copper alloy sheet material of Inventive Example 6, the proportion of azimuth angles in which the intensity was 2.0 or less to all azimuth angles in the inverse pole figure was small, and the waviness (ear) at the edge of the drawn product was also large.

[0097] In the copper alloy sheets of Inventive Examples 7 to 11, the temperature reached in the intermediate annealing step [Step 4] was 1000° C., which was within a more preferable range of 900° C. or more and 1000° C. or less. In addition, in the copper alloy sheets of Inventive Examples 7 to 11, the working ratio d 2 The first stage processing rate d 1 The ratio (d 1 / d 2 ) was 1.0, which was within the more preferable range of 0.9 or more and 1.1 or less. Therefore, the evaluation results of the drawing workability of the copper alloy sheets of Inventive Examples 7 to 11 were all "4".

[0098] Furthermore, when comparing the copper alloy sheets of Inventive Examples 7 and 8, the copper alloy sheet of Inventive Example 7 had a solution treatment step [Step 6] reached at a temperature of 800° C., and thus had a higher tensile strength value than Inventive Example 8, which had a solution treatment step [Step 6] reached at a lower temperature of 700° C. The reason for this is thought to be that the solution amounts of Ni and Si necessary for precipitation strengthening were insufficient in Inventive Example 8 due to the low temperature reached in the solution treatment step [Step 6].

[0099] Furthermore, when comparing the copper alloy sheets of Inventive Examples 7 and 9, the copper alloy sheet of Inventive Example 7 had a solution treatment step [Step 6] reached at a temperature of 800° C., and thus had a higher tensile strength value than Inventive Example 9, which had a solution treatment step [Step 6] reached at a higher temperature of 1000° C. The reason for this is thought to be that in Inventive Example 9, the crystal grains were coarsened due to the high temperature reached in the solution treatment step [Step 6].

[0100] Furthermore, the copper alloy sheet material of Inventive Example 10 had low tensile strength and electrical conductivity due to the low temperature reached in the aging heat treatment step [Step 7] of 400° C. This is thought to be because the amount of precipitation was insufficient due to the low temperature reached in the aging heat treatment step [Step 7].

[0101] Furthermore, the copper alloy sheet material of Inventive Example 11 had high electrical conductivity due to the high temperature reached in the aging heat treatment step [Step 7] of 560° C., but the tensile strength was low. This is thought to be because the electrical conductivity increased due to the increased amount of precipitation, while the tensile strength decreased due to the coarsening of the precipitates.

[0102] The copper alloy sheets of Inventive Examples 12 to 14 have high tensile strength due to the high working ratio of 20% in the second cold rolling step [Step 8], but the evaluation results for drawing workability were all "2." The reason for the evaluation result of drawing workability being "2" is thought to be that texture was developed by cold rolling.

[0103] Furthermore, when comparing the copper alloy sheets of Inventive Examples 12 and 13, the copper alloy sheet of Inventive Example 13 reached a higher temperature in the low-temperature annealing step [Step 9] than Inventive Example 12, and therefore the recovery of strain was more likely to proceed than Inventive Example 12. As a result, the tensile strength of the copper alloy sheet of Inventive Example 13 was lower than that of Inventive Example 12.

[0104] Furthermore, when comparing the copper alloy sheets of Inventive Examples 12 and 14, the copper alloy sheet of Inventive Example 14 reached a lower temperature in the low-temperature annealing step [Step 9] than Inventive Example 12, and therefore strain recovery was more difficult to occur than in Inventive Example 12. As a result, the tensile strength of the copper alloy sheet of Inventive Example 14 was higher than that of Inventive Example 12.

[0105] For Inventive Examples 15 to 20, the contents of the essential added components Ni and Si and the contents of the optional added elements were within the ranges of the present invention, and therefore it can be seen that the desired effects were obtained, similar to Inventive Examples 1 to 14.

[0106] On the other hand, in the copper alloy sheets of Comparative Examples 1 to 10, at least one of the alloy composition, tensile strength, electrical conductivity, and the maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface was outside the appropriate range of the present invention, and therefore the tensile strength or electrical conductivity did not reach an acceptable level, or the overall evaluation of the drawing workability was evaluated as "1".

[0107] In particular, in the copper alloy sheets of Comparative Examples 1, 2, and 9, the maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface exceeded 3.0 due to the low temperature reached in the intermediate annealing step [step 4], and the evaluation of the drawing workability was also evaluated as "1".

[0108] Furthermore, in the copper alloy sheet material of Comparative Example 3, the total working ratio in the second cold rolling step [Step 8] was high, and therefore the waviness (ear) at the edge of the drawn product became large. This is thought to be because the texture was developed due to the high total working ratio in the second cold rolling step [Step 8].

[0109] Furthermore, the copper alloy sheet material of Comparative Example 4 had a Ni (nickel) content in the alloy composition that was greater than the range of the present invention, and had a high tensile strength, so it broke during the first drawing process.

[0110] In addition, the copper alloy sheet material of Comparative Example 5 had a Si (silicon) content in the alloy composition that was lower than the range of the present invention, and the tensile strength did not reach an acceptable level.

[0111] The copper alloy sheet material of Comparative Example 6 is an example in which the electrical conductivity does not reach the acceptable level.

[0112] In addition, the copper alloy sheet material of Comparative Example 7 had a Si (silicon) content in the alloy composition that was higher than the range of the present invention, and had a high tensile strength, so it broke in the first drawing process. In addition, the electrical conductivity did not reach an acceptable level.

[0113] In addition, the copper alloy sheet material of Comparative Example 8 had a Ni (nickel) content in the alloy composition that was lower than the range of the present invention, and the tensile strength did not reach an acceptable level.

[0114] In addition, since the copper alloy sheet material of Comparative Example 10 was not subjected to the intermediate annealing step [step 4], the maximum value of the intensity of the inverse pole figure for the crystal plane facing the normal direction (ND) of the sheet surface exceeded 3.0, and the evaluation of the drawing workability was also evaluated as "1".

[0115] 1 Drawn product 11 Bottom surface of drawn product 12 Side surface of drawn product 13 Edge of drawn product C Center of bottom surface of drawn product H 0 , H 45 , H 90 , H 135 , H 180 , H 225 , H 270 , H 315 Height from the bottom to the edge L 1 ~L 8 Line drawn on the bottom surface of the drawn product X: Rolling direction of the copper alloy sheet material

Claims

1. A copper alloy sheet material having an alloy composition containing Ni in the range of 1.00 mass% to 5.00 mass%, Si in the range of 0.20 mass% to 1.30 mass%, and the balance consisting of Cu and unavoidable impurities, wherein the maximum value of the strength of an inverse pole figure for a crystal plane facing the normal direction (ND) of the sheet surface obtained by crystal orientation analysis using an EBSD method, measured on the sheet surface of the copper alloy sheet material, is 3.0 or less, the tensile strength is in the range of 500 MPa to 900 MPa, and the electrical conductivity is 30% IACS or more.

2. The copper alloy sheet material according to claim 1, wherein in the inverse pole figure, the proportion of azimuth angles at which the strength is 2.0 or less to all azimuth angles is 50% or more.

3. The copper alloy sheet material according to claim 1, wherein the alloy composition further contains at least one optional added component selected from the group consisting of Sn, Zn, Mg, Fe, and Cr in a range of 0.10 mass% or more and 1.00 mass% or less in total.

4. A copper alloy sheet material for drawing, comprising the copper alloy sheet material according to any one of claims 1 to 3.

5. A drawn product obtained by drawing the copper alloy sheet material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Copper alloy material and method for producing copper alloy material

    JP2010202946A

  • Copper alloy sheet material and method for manufacturing the same

    JP4563495B1