Image forming method and image forming system
By using inks with controlled complex permittivity and drying rates, and applying microwaves for drying, the method achieves high-speed ink drying and stability, addressing the challenges of base material damage and uneven drying in conventional methods.
Patent Information
- Application Number
- PCT/JP2024/015692
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional image forming methods face challenges in achieving high-speed drying of ink while maintaining inkjet stability and preventing damage to the base material, as existing heating methods like hot air or infrared heating often damage the substrate, and microwave drying methods are expensive and can lead to uneven drying.
The method involves using a combination of two inks with controlled complex permittivity and drying rates, where the first ink and second ink have specific complex dielectric constants and drying rates, and are applied with a humectant and surfactant, and dried using microwaves to achieve high-speed drying without damaging the base material.
This approach allows for high-speed drying and stable ink ejection while preventing base material damage, ensuring uniform and high-quality images by controlling the drying properties of each ink based on their microwave absorption characteristics.
Smart Images

Figure JP2024015692_31102024_PF_FP_ABST
Abstract
Description
Image forming method and image forming system
[0001] The present invention relates to an image forming method and an image forming system, and more particularly to an image forming method and the like that can achieve both high-speed drying of ink and ejection stability, and that does not damage the substrate.
[0002] Recently, there has been a strong demand for faster printing of flexible packaging and labels. However, conventional methods of heating the atmosphere, such as applying hot air or using an infrared heater, heat not only the ink but also the substrate at the same time, making it impossible to apply heat that would significantly damage the substrate.
[0003] In order to improve the ejection stability of the ink, it is necessary to add a large amount of humectant with a high boiling point to the ink to prevent the ink from drying and solidifying in the head nozzles, but this requires an even larger amount of heat to dry the ink, so the only options are to extend the drying time with the limited amount of heat or to print at a slower speed. Therefore, there is a trade-off between drying ability and ink ejection stability.
[0004] Other methods for heating and drying the entire ink include, for example, the techniques disclosed in Patent Documents 1 and 2, in which microwaves are irradiated onto a water-based ink that does not contain a resin.
[0005] The microwave irradiation method heats the object to be dried by directly applying microwaves only to substances that have microwave absorption capabilities, making it a highly directional drying method that can dry only the object to be dried.It can heat the ink directly without heating the substrate, and it is a method that can apply the power required for high-speed drying without worrying about damaging the substrate.
[0006] However, in the techniques disclosed in Patent Documents 1 and 2, inkjet printing typically involves simultaneously ejecting multiple inks such as YMCKW and drying them all at once, but this method poses the problem of insufficient drying or excessive drying, which can damage the substrate depending on the drying properties of the ink material.
[0007] Patent Literature 3 discloses a technology for preventing sparks and controlling drying by combining ink containing highly conductive carbon black and resin with a dielectric heating method. However, there is still room for improvement, as drying control can be approached from a different perspective.
[0008] Japanese Patent Application Laid-Open No. 5-278259 Japanese Patent Application Laid-Open No. 2022-147052 Japanese Patent Application Laid-Open No. 2019-151071
[0009] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide an image forming method and an image forming system that can achieve both high-speed drying of ink and ejection stability, and that do not damage the substrate.
[0010] In order to solve the above-mentioned problems, the present inventors have investigated the causes of the above-mentioned problems and have found that the above-mentioned problems can be solved by irradiating microwaves to the first ink and the second ink, the complex dielectric constant and drying rate of which are controlled within specific ranges, and have arrived at the present invention. That is, the above-mentioned problems according to the present invention are solved by the following means.
[0011] 1. An image forming method having an ink coating step and a drying step, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating step is a step of ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying steps is a step of drying a coating film by irradiating with microwaves, wherein when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates when the first ink and the second ink are dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1.
[0012] 2. The image forming method described in item 1, wherein the complex dielectric constant ε''1 of the first ink and the complex dielectric constant ε''2 of the second ink satisfy the following formula (3): (ε''2 / ε''1)<20.
[0013] 3. The image forming method described in item 1, wherein the water-soluble solvent contains a humectant having a boiling point of 200°C or higher, the content of the humectant is within a range of 3 to 20% by mass relative to the first ink or the second ink, and the complex dielectric constant ε'' at 25°C when the first ink or the second ink is irradiated with microwaves at a frequency of 2.45 GHz is within a range of 13 to 60.0.
[0014] 4. The image forming method according to claim 3, wherein the content of the humectant in the second ink is greater than that in the first ink.
[0015] 5. The image forming method according to item 1, wherein the ink contains a surfactant having a hydroxy group.
[0016] 6. The image forming method according to item 1, wherein the ink contains a surfactant having a diol structure.
[0017] 7. The image forming method according to item 1, wherein the substrate is a resin film.
[0018] 8. The image forming method described in item 1, wherein an inkjet head having a water-repellent film is used in the ink application step, and the contact angles of the first ink and the second ink with the water-repellent film are within a range of 60 to 80°C at 25°C.
[0019] 9. The image forming method according to item 1, further comprising a step of applying a precoat liquid before the step of applying the ink.
[0020] 10. The image forming method according to item 8, wherein the inkjet head is provided with a nozzle circulation mechanism.
[0021] 11. The image forming method described in item 10, wherein the inkjet head comprises at least one pressure chamber into which ink is injected, pressure generating means for generating pressure fluctuations in the pressure chamber, a nozzle communicating with the pressure chamber and serving as a flow path for ink ejected from the pressure chamber to the outside due to the pressure fluctuations in the pressure chamber, and a circulation path communicating with the pressure chamber and discharging ink inside the nozzle and returning it to the injection path to the pressure chamber, and wherein there are two or more circulation paths.
[0022] 12. The image forming method according to item 1, wherein in the drying step using microwave irradiation, the coated materials of the first ink and the second ink are dried by applying air at a temperature of 100° C. or less.
[0023] 13. An image forming system having an ink coating means and a drying means, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating means is a means for ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying means is a means for drying a coating film by irradiating with microwaves, wherein when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates when the first ink and the second ink are dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1.
[0024] The above-described means of the present invention can provide an image forming method and an image forming system that can achieve both high-speed drying of ink and ejection stability, and that does not damage the substrate.
[0025] The mechanism by which the effects of the present invention are manifested or the mechanism of action is not clear, but is speculated as follows.
[0026] The image forming method of the present invention achieves both rapid drying of the ink and ejection stability during image formation by irradiating microwaves to the first ink and the second ink, whose complex dielectric constant and drying rate are controlled within a specific range, without damaging the substrate.
[0027] As mentioned above, in conventional techniques, drying control during image formation has been performed by heating the atmosphere or irradiating with microwaves. However, there are problems such as an inability to resolve the trade-off between drying property and ink ejection stability, and image defects such as roughening of the ink coating surface and damage to the substrate due to excessive drying of some inks over time.
[0028] In the image forming method of the present invention, ink is dried mainly by highly directional microwave irradiation, and therefore, nothing other than the object to be dried is directly heated, and therefore, the substrate is not damaged.
[0029] Furthermore, the ambient temperature does not need to be too high when the ink dries, and the ink does not dry in the nozzle of the head during ink ejection, which would result in a decrease in ejection performance.Furthermore, since the substrate is not heated, the ink ejection section is not heated by the heated substrate, and therefore ejection performance does not decrease.
[0030] However, it was found that while there is no significant difference in the microwave absorption capacity of images formed using multiple types of ink in the early drying stage when the inks have not yet dried, there are differences in the microwave absorption capacity of each ink in the later drying stage when the inks have dried. Since there are significant differences in the later drying stage depending on the ink color and the type of solid content, such as resin, if the drying time by microwave irradiation is extended, some inks will dry excessively, causing the surface of the coating film formed by the ink to become rough and damaging the substrate. It was thus found that differences in microwave absorption capacity in the later drying stage can lead to insufficient drying and substrate damage during batch drying.
[0031] Therefore, by controlling the complex dielectric constants of the first ink and the second ink within a specific range, the microwave absorption ability, which differs depending on the color of each ink and the type of solid content such as resin, and by taking the drying rate into consideration, it is possible to control the drying property to be quick and uniform, and it is presumed that this will enable the formation of high-quality images.
[0032] In other words, by drying by irradiation with microwaves that act directly on the ink and do not heat the substrate or the atmosphere, it has become possible to achieve both high-speed drying and ejection properties. However, even with drying by irradiation with microwaves, when multiple colors are printed and dried simultaneously, the drying speed varies greatly depending on the differences in microwave absorption of each ink, especially in the later stages of drying.
[0033] Therefore, if all the ink is dried at once using microwaves without any consideration, problems such as some ink being over-dried in the latter stages of drying, causing damage to the substrate, or insufficient drying may occur.
[0034] From this, it is presumed that the present invention solves this problem and enables the formation of high-quality images by taking into account the difference in microwave absorption in the later stage of drying and controlling the drying properties of each ink according to its complex dielectric constant.
[0035] A schematic diagram of an example of a recording device preferred for the present invention. A conceptual diagram showing how ink is drawn into a pressure chamber during maintenance of a circulation-type inkjet head H. A conceptual diagram showing how a meniscus formed by ink is restored during maintenance of a circulation-type inkjet head. An example of an image pattern for a solid area. An example of an image pattern in which solid areas are individually drawn.
[0036] The image forming method of the present invention is an image forming method having an ink coating step and a drying step, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating step is a step of ejecting and coating at least a first ink and a second ink onto a substrate, at least one of the drying steps is a step of drying a coating film by irradiating with microwaves, and is characterized in that, when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε"1 and ε"2, respectively, ε"1 and ε"2 satisfy the above formula (1), and when the drying rates when the first ink and the second ink are dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the above formula (2). This feature is a technical feature common to or corresponding to each of the following embodiments (aspects).
[0037] As an embodiment of the present invention, it is preferable from the viewpoint of uniform drying control that the complex dielectric constant ε''1 of the first ink and the complex dielectric constant ε''2 of the second ink satisfy the formula (3).
[0038] From the viewpoint of uniform drying control, it is preferable that the water-soluble solvent contains a humectant having a boiling point of 200°C or higher, the content of the humectant is within a range of 3 to 20% by mass relative to the first ink or the second ink, and the complex dielectric constant ε'' at 25°C when the first ink or the second ink is irradiated with microwaves at a frequency of 2.45 GHz is within a range of 13 to 60.0.
[0039] It is more preferable from the viewpoint of controlling uniform drying properties that the content of the humectant in the second ink is greater than that in the first ink.
[0040] From the viewpoint of the coatability of the first ink and the second ink, it is preferable that the ink contains a surfactant having a hydroxy group.
[0041] From the viewpoint of the coatability of the first ink and the second ink, it is more preferable that the ink contains a surfactant having a diol structure.
[0042] Even if the substrate is a resin film, it can be suitably used since it does not cause damage to the substrate.
[0043] In the ink application step, it is preferable to use an inkjet head having a water-repellent film, and to have the contact angles of the first ink and the second ink with the water-repellent film be within a range of 60 to 80°C at 25°C, from the viewpoint of improving the ejection stability of the ink and enabling high-speed drying.
[0044] It is preferable to have a step of applying a precoat liquid before the step of applying the inks, from the viewpoint of controlling the pinning properties and uniform drying properties of the first ink and the second ink.
[0045] It is preferable that the inkjet head includes a nozzle circulation mechanism from the viewpoint of ejection stability of the first ink and the second ink.
[0046] The inkjet head comprises at least one pressure chamber into which ink is injected, pressure generating means for generating pressure fluctuations in the pressure chamber, a nozzle that communicates with the pressure chamber and serves as a flow path for ink that is ejected from the pressure chamber to the outside due to the pressure fluctuations in the pressure chamber, and a circulation path that communicates with the pressure chamber and discharges ink that is inside the nozzle and returns it to the injection path to the pressure chamber, and it is preferable that there are two or more circulation paths from the viewpoint of ejection stability of the first ink and the second ink.
[0047] In the drying step using microwave irradiation, it is preferable from the viewpoint of controlling the drying property to dry the coated first ink and second ink by blowing air at 100° C. or less.
[0048] The image forming system of the present invention is an image forming system having an ink coating means and a drying means, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating means is a means for ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying means is a means for drying a coating film by irradiating with microwaves, wherein when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, the ε''1 and ε''2 satisfy the above formula (1), and when the drying rates of the first ink and the second ink when dried at 80°C for 20 seconds are D1 and D2, respectively, the D1 and D2 satisfy the above formula (2), and the image forming system is suitably used in the image forming method of the present invention.
[0049] The present invention, its components, and embodiments and modes for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0050] [Outline of Image Forming Method of the Present Invention] The image forming method of the present invention is an image forming method having an ink coating step and a drying step, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating step is a step of ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying steps is a step of drying a coating film by irradiating with microwaves, and is characterized in that when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates when the first ink and the second ink are dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1
[0051] As described above, simply controlling the drying property during image formation by heating the atmosphere or irradiating microwaves cannot resolve the trade-off between the drying property and the ejection stability of the ink, and there are problems such as image defects that occur due to excessive drying of some inks over time, causing roughness of the ink coating surface and damage to the substrate.
[0052] In the present invention, drying is performed by irradiating microwaves that act directly on the ink and do not heat the substrate or the atmosphere, thereby achieving both high-speed drying and ejection properties. However, even when drying is performed by irradiating microwaves, in an embodiment in which multiple colors are printed and dried simultaneously, the drying properties vary greatly depending on the differences in microwave absorption of each ink in the later stages of drying.
[0053] Therefore, if drying is performed all at once using microwaves without any consideration, some of the ink may be overdried in the later stages of drying, causing damage to the substrate or insufficient drying.
[0054] In contrast, in the image forming method of the present invention, this problem is solved by taking into account the difference in microwave absorption in the later stage of drying and controlling the drying properties of each ink according to its complex dielectric constant, thereby forming a high-quality image. Each step and component will be described below in order.
[0055] 1. Image Forming Method (1.1) Ink Coating Step The ink coating step according to the present invention is a step of ejecting and coating at least a first ink and a second ink onto a substrate. The application of the inks in the first ink coating step and the second ink coating step is performed almost simultaneously.
[0056] (1.1.1) Ink The inks according to the present invention vary in type depending on the purpose, such as the content ratio of pigment, resin, water, water-soluble solvent, and surfactant, and the complex dielectric constant of each ink at the later stage of drying, i.e., at a drying rate of 95% in the present invention, is different.
[0057] Therefore, the ink (first ink) having a relatively small complex dielectric constant in the later stage of drying compared to the other inks is more excellent in uniform drying control when the drying rate of the ink is relatively high.Furthermore, the ink (second ink) having a relatively large complex dielectric constant in the later stage of drying compared to the first ink is more excellent in uniform drying control when the drying rate of the ink is relatively low.
[0058] From this viewpoint, when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates of the first ink and the second ink when dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1 By doing this, it is possible to achieve both high-speed drying of the ink and ejection stability, and to eliminate damage to the substrate.
[0059] In the present invention, a plurality of inks having different components, contents, etc. are used as described above, but when focusing on two types of ink, for example, one ink is designated as the first ink and the other as the second ink. The first ink and the second ink are characterized in that their complex dielectric constants and drying rates in the later stage of drying are relatively different, as described above.
[0060] The complex dielectric constant and the drying rate can be controlled by, for example, the amount of coloring material contained in the ink or the amount of moisturizing agent contained in the water-soluble solvent.
[0061] The first ink and the second ink may be applied not only to the same location on the substrate, but also to different locations.
[0062] (Pigment) The ink according to the present invention preferably uses an anionic dispersed pigment, such as a self-dispersed pigment having anionic groups on its surface, a pigment dispersed with an anionic polymer dispersant, or a pigment dispersed with its surface coated with an anionic resin. It also preferably contains a pigment dispersant for dispersing the pigment. In particular, it is preferable to use a pigment dispersed with an anionic polymer dispersant, as this provides excellent dispersibility and allows the pigment to react appropriately with the precoat liquid to form pinning.
[0063] As the pigment, any conventionally known pigment can be used without any particular limitation. For example, inorganic pigments containing inorganic particles such as titanium oxide, insoluble pigments, and organic pigments containing organic particles such as lake pigments can be preferably used.
[0064] [Insoluble Pigment] The insoluble pigment is not particularly limited, but preferred examples include azo, azomethine, methine, diphenylmethane, triphenylmethane, quinacridone, anthraquinone, perylene, indigo, quinophthalone, isoindolinone, isoindoline, azine, oxazine, thiazine, dioxazine, thiazole, phthalocyanine, and diketopyrrolopyrrole.
[0065] [Organic Pigments] Specific examples of organic pigments that can be preferably used include the following pigments.
[0066] Examples of pigments for magenta or red include C.I. Pigment Red 2, C.I. Pigment Red 3, C.I. Pigment Red 5, C.I. Pigment Red 6, C.I. Pigment Red 7, C.I. Pigment Red 15, C.I. Pigment Red 16, C.I. Pigment Red 48:1, C.I. Pigment Red 53:1, C.I. Pigment Red 57:1, C.I. Pigment Red 122, C.I. Pigment Red 123, C.I. Pigment Red 139, C.I. Pigment Red 144, C.I. Pigment Red 149, C.I. Pigment Red 166, C.I. Pigment Red 177, C.I. Examples of suitable pigments include C.I. Pigment Red 178, C.I. Pigment Red 202, C.I. Pigment Red 222, and C.I. Pigment Violet 19.
[0067] Examples of orange or yellow pigments include C.I. Pigment Orange 31, C.I. Pigment Orange 43, C.I. Pigment Yellow 12, C.I. Pigment Yellow 13, C.I. Pigment Yellow 14, C.I. Pigment Yellow 15, C.I. Pigment Yellow 15:3, C.I. Pigment Yellow 17, C.I. Pigment Yellow 74, C.I. Pigment Yellow 93, C.I. Pigment Yellow 128, C.I. Pigment Yellow 94, C.I. Pigment Yellow 138, and C.I. Pigment Yellow 155. In particular, C.I. Pigment Yellow 155 is preferred in terms of the balance between color tone and lightfastness.
[0068] Examples of pigments for green or cyan include C.I. Pigment Blue 15, C.I. Pigment Blue 15:2, C.I. Pigment Blue 15:3, C.I. Pigment Blue 16, C.I. Pigment Blue 60, and C.I. Pigment Green 7.
[0069] Examples of black pigments include C.I. Pigment Black 1, C.I. Pigment Black 6, and C.I. Pigment Black 7.
[0070] [Inorganic Pigment] Inorganic pigments of various colors can be used as the inorganic pigment. In particular, it is preferable to use an inorganic pigment as a white pigment. The white pigment is not particularly limited as long as it is a pigment that causes the cured film formed by curing an ink containing the white pigment to exhibit a white color.
[0071] Examples of white pigments include titanium oxide, zinc oxide, zinc sulfide, calcium carbonate, calcium silicate, barium sulfate, aluminum hydroxide, antimony oxide, zirconium oxide, silicas such as finely powdered silicic acid and synthetic silicates, talc, clay, etc. Among these, from the viewpoint of whiteness (coloring ability), white metal oxides are preferred, and titanium oxide is more preferred. These may be used alone or in combination of two or more.
[0072] In addition, the present invention is particularly effective in preventing bleeding and improving adhesion in titanium oxide, which is generally difficult to ensure ink ejection stability and adhesion. Titanium oxide has three crystalline forms: anatase, rutile, and brookite, but commonly used forms can be broadly classified into anatase and rutile. Although not particularly limited, rutile forms are preferred, as they have a high refractive index and high hiding power. Specific examples include the TR series from Fuji Titanium Industry Co., Ltd., the JR series from Teika Corporation, and Typepaque from Ishihara Sangyo Co., Ltd.
[0073] [Pigment Dispersant] When the ink according to the present invention contains a pigment, it preferably contains a pigment dispersant for dispersing the pigment. The pigment dispersant for dispersing the pigment according to the present invention is not particularly limited, but is preferably a polymer dispersant having an anionic group, and one having a molecular weight in the range of 5,000 to 200,000 can be suitably used.
[0074] Examples of polymer dispersants include block copolymers and random copolymers having a structure derived from two or more monomers selected from styrene, styrene derivatives, vinylnaphthalene derivatives, acrylic acid, acrylic acid derivatives, maleic acid, maleic acid derivatives, itaconic acid, itaconic acid derivatives, fumaric acid, and fumaric acid derivatives, as well as salts thereof, polyoxyalkylenes, polyoxyalkylene alkyl ethers, etc. The polymer dispersant preferably has an acryloyl group, and is preferably neutralized with a neutralizing base before addition.
[0075] In particular, when the pigment is titanium oxide, the titanium oxide is preferably dispersed with a polymer dispersant having an acryloyl group. The neutralizing base is not particularly limited, but is preferably an organic base such as ammonia, monoethanolamine, diethanolamine, triethanolamine, or morpholine.
[0076] The amount of polymer dispersant added is preferably within a range of 10 to 100% by mass, more preferably within a range of 10 to 40% by mass, based on the pigment.
[0077] It is particularly preferred that the pigment be in the form of a so-called capsule pigment, which is a pigment coated with the polymer dispersant. As a method for coating a pigment with a polymer dispersant, various known methods can be used, and preferred examples include a phase inversion emulsification method, an acid precipitation method, and a method in which a pigment is dispersed in a polymerizable surfactant, a monomer is supplied thereto, and the monomer is polymerized to coat the pigment.
[0078] A particularly preferred method is to dissolve a water-insoluble resin in an organic solvent such as methyl ethyl ketone, partially or completely neutralize the acidic groups in the resin with a base, add a pigment and ion-exchanged water, disperse the pigment, remove the organic solvent, and add water as needed to prepare the dispersion.
[0079] The average particle size of the pigment dispersed in the ink is preferably 50 nm or more and less than 200 nm. This improves the dispersion stability of the pigment and the storage stability of the ink. The particle size of the pigment can be measured using a commercially available particle size measuring device that uses a dynamic light scattering method, electrophoresis method, or the like, but measurement by dynamic light scattering is simple and can accurately measure the particle size range.
[0080] The pigment can be dispersed in a dispersing machine together with a dispersant and other additives required for various desired purposes.
[0081] As the dispersing machine, a conventionally known ball mill, sand mill, line mill, high-pressure homogenizer, etc. can be used. Among them, dispersing the pigment using a sand mill is preferable because it results in a sharp particle size distribution. Furthermore, the material of the beads used for sand mill dispersion is not particularly limited, but from the viewpoint of preventing the generation of bead fragments and contamination of ionic components, zirconia or zircon is preferred. Furthermore, the diameter of the beads is preferably within the range of 0.3 to 3 mm.
[0082] The content of the pigment in the ink is not particularly limited, but for titanium oxide, the content is preferably in the range of 7 to 18% by mass, and for organic pigments, the content is preferably in the range of 0.5 to 7% by mass.
[0083] (Resin) When an ink contains a resin, the fixation of the ink to a recording medium can be improved. Examples of resins include vinyl chloride resins, (meth)acrylic resins, urethane resins, polyether resins, and polyester resins. Among these, it is preferable that the ink contains an ionic resin from the viewpoint of fixation, film-forming properties, etc.
[0084] When drying is performed using microwaves in the drying step described below, the ionic resin is directly heated by microwaves, thereby improving film-forming properties and adhesion to the substrate. The ionic resin is preferably water-insoluble resin fine particles, and the glass transition temperature (Tg) of the resin fine particles is preferably within the range of 40 to 90°C.
[0085] The glass transition temperature can be determined by reading the glass transition temperature (Tg) from an endothermic peak when the temperature is increased at a rate of 10°C / min in a temperature range of -30 to 200°C using a DSC (differential scanning calorimeter).
[0086] The water-insoluble resin preferably used in the present invention is a water-insoluble resin that can accept ink and exhibits solubility or affinity for the ink. The "water-insoluble resin microparticles" used in the present invention are essentially water-insoluble, but have a form in which the resin disperses in an aqueous medium as microparticles. These microparticles are water-insoluble resins that are forcibly emulsified using an emulsifier or the like and dispersed in water, or water-insoluble resins that have hydrophilic functional groups introduced into their molecules and are self-emulsifiable to form a stable aqueous dispersion without the use of an emulsifier or dispersion stabilizer. These resins are usually used in a state of being emulsified and dispersed in water or a water / alcohol mixed solvent.
[0087] In the present invention, "water-insoluble" refers to a resin that, when dried at 105° C. for 2 hours and then dissolved in 100 g of water at 25° C., dissolution amounts of the resin are 10 g or less, preferably 5 g or less, and more preferably 1 g or less. However, when the resin has salt-forming groups, the dissolution amount refers to the amount dissolved when the salt-forming groups of the resin are 100% neutralized with acetic acid or sodium hydroxide, depending on the type of resin.
[0088] The resin having a glass transition temperature (Tg) in the range of 40 to 90°C is preferably any one of acrylic resin, urethane resin, polyester, or a composite resin of urethane resin and acrylic resin. In particular, it is preferably an acrylic resin, urethane resin, polyester, or a composite resin of urethane resin and acrylic resin, and the average particle size of these resin particles is preferably 200 nm or less. Furthermore, the average particle size is more preferably in the range of 100 to 150 nm.
[0089] The polyester, urethane resin, acrylic resin, or composite resin particles of urethane resin and acrylic resin are preferably anionic. Among these, the resin particles contained in the ink preferably have an acid structure, which allows them to be dispersed in water even with a small amount of surfactant added, improving water resistance. This is called a self-emulsifying type, which means that the resin can be dispersed and stabilized in water using only molecular ionicity without using a surfactant or even with a small amount of surfactant added.
[0090] Examples of the acid structure include a carboxy group (—COOH), a sulfonic acid group (—SO 3 The acid structure may be present in a side chain of the resin or at the terminal thereof. The ink according to the present invention preferably contains a water-dispersible polyester having a sulfonic acid group, which provides high adhesion to the substrate.
[0091] It is preferable that the acid structures are partially or entirely neutralized, and neutralizing the acid structures can improve the aqueous dispersibility of the resin. As a neutralizing agent for neutralizing the acid structures, for example, organic amines are preferred, and it is preferable to use organic amines such as trimethylamine, triethylamine, tripropylamine, tributylamine, N-methyldiethanolamine, and triethanolamine. Furthermore, the ink according to the present invention preferably contains 3 to 15% by mass of resin fine particles having an agglomeration property of 0.2 or less with a 0.15% by mass aqueous solution of calcium acetate.
[0092] By using such resin particles with low aggregating properties, high wettability to the substrate is ensured while high ejection stability is obtained, resulting in higher image quality and excellent adhesion to the substrate.
[0093] Each resin will be described below.
[0094] [Polyester] The polyester having a polyester skeleton used as the water-insoluble resin particles can be obtained using a polyhydric alcohol component and a polycarboxylic acid component such as a polycarboxylic acid, a polycarboxylic acid anhydride, or a polycarboxylic acid ester.
[0095] The polyhydric alcohol component may be a dihydric alcohol (diol), specifically, an alkylene glycol having 2 to 36 carbon atoms (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, etc.), an alkylene ether glycol having 4 to 36 carbon atoms (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.), an alicyclic diol having 6 to 36 carbon atoms (diol), an alkylene ether glycol ...4 to 36 carbon atoms (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, etc.), an alkylene ether glycol having 6 to 36 carbon atoms (diol), an alkylene ether glycol having 6 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to 36 carbon atoms (diol), an alkylene ether glycol having 4 to Examples of suitable alkylene oxides include alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.), adducts of the above-mentioned alicyclic diols with alkylene oxides (ethylene oxide (hereinafter abbreviated as EO), propylene oxide (hereinafter abbreviated as PO), butylene oxide (hereinafter abbreviated as BO)) having 2 to 4 carbon atoms (number of added moles in the range of 1 to 30), and adducts of bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.) with alkylene oxides (EO, PO, BO, etc.) having 2 to 4 carbon atoms (number of added moles in the range of 2 to 30). These may be used alone or in combination of two or more.
[0096] Examples of the polyvalent carboxylic acid component include dicarboxylic acids (dicarboxylic acids), specifically alkanedicarboxylic acids having 4 to 36 carbon atoms (succinic acid, apidic acid, sebacic acid, etc.), alkenylsuccinic acids (dodecenylsuccinic acid, etc.), alicyclic dicarboxylic acids having 4 to 36 carbon atoms (dimer acids (dimerized linoleic acid), etc.), alkenedicarboxylic acids having 4 to 36 carbon atoms (maleic acid, fumaric acid, citraconic acid, mesaconic acid, etc.), and aromatic dicarboxylic acids having 8 to 36 carbon atoms (phthalic acid, isophthalic acid, terephthalic acid or derivatives thereof, naphthalenedicarboxylic acid, etc.). These may be used alone or in combination of two or more.
[0097] The polyester is preferably a polyester having an anionic group in the molecule, and more preferably a polyester containing a sulfonic acid group.
[0098] As a known synthesis method for obtaining a polyester containing a sulfonic acid group, for example, it can be obtained by a method such as a polycondensation reaction between a dicarboxylic acid having a sulfonic acid group and a diol, or a method such as a polycondensation reaction between a dicarboxylic acid and a diol having a sulfonate salt.
[0099] Examples of dicarboxylic acid components having a sulfonic acid group include 2-sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfonaphthaleneisophthalic-2,7-dicarboxylic acid, 5-(4-sulfophenoxy)isophthalic acid, and alkali metal salts thereof.
[0100] Examples of diols having a sulfonic acid group include 2-sulfo-1,4-butanediol, 2,5-dimethyl-3-sulfo-2,5-hexanediol, and alkali metal salts thereof.
[0101] The number average molecular weight of the polyester is preferably in the range of 1,000 to 50,000, and more preferably in the range of 2,000 to 20,000.
[0102] As the polyester, commercially available products may be used. Examples of commercially available water-dispersible polyesters having sulfonic acid groups include Vylonal MD-1100, MD-1200, MD-1245, MD-1480, MD-1500, and MD-2000 manufactured by Toyobo Co., Ltd.; Plascoat Z-221, Z-446, Z-561, Z-880, and Z-3310 manufactured by Goo Chemical Co., Ltd.; and PESRESIN A-520, A-613D, A-615GE, A-640, A-645GH, A-647GEX, A-110F, and A-160P manufactured by Takamatsu Oil & Fats Co., Ltd.
[0103] Among the above, resins having a glass transition temperature (Tg) in the range of 40 to 90°C are particularly preferred, and examples thereof include Vylonal MD-1100, MD-1200, MD-1245, MD-1500, and MD-2000 manufactured by Toyobo Co., Ltd., Plascoat Z-221, Z-446, and Z-561 manufactured by Goo Chemical Co., Ltd., and PES Resin A-520, A-613D, A-615GE, A-640, A-645GH, and A-647GEX manufactured by Takamatsu Oil & Fat Co., Ltd. These may be used alone or in combination of two or more.
[0104] [Urethane Resin] The urethane resin used as the water-insoluble resin particles according to the present invention may be one having a hydrophilic group. The urethane resin is preferably an aqueous dispersion in which a self-emulsifying urethane having a water-soluble functional group, i.e., a hydrophilic group, is dispersed, or an aqueous dispersion in which a forced-emulsifying urethane is emulsified under strong mechanical shearing force in combination with a surfactant. The urethane resin in the aqueous dispersion can be obtained by reacting a polyol with an organic polyisocyanate and a hydrophilic group-containing compound.
[0105] Examples of polyols that can be used to prepare the aqueous dispersion of the urethane resin include polyester polyols, polyether polyols, polycarbonate polyols, and polyolefin polyols.
[0106] Examples of polyester polyols include low molecular weight polyols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2- and 1,3-propylene glycol, neopentyl glycol, 1,3- and 1,4-butanediol, 3-methylpentanediol, hexamethylene glycol, 1,8-octanediol, 2-methyl-1,3-propanediol, bisphenol A, hydrogenated bisphenol A, trimethylolpropane, and cyclohexanedimethanol; and condensates thereof with polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, tetrahydrofuran acid, endomethinetetrahydrofuran acid, and hexahydrophthalic acid.
[0107] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene polytetramethylene glycol, polypropylene polytetramethylene glycol, and polytetramethylene glycol.
[0108] Examples of polycarbonate polyols include those obtainable by reacting a carbonic acid derivative such as diphenyl carbonate, dimethyl carbonate or phosgene with a diol.
[0109] Examples of the diol include ethylene glycol, diethylene glycol, triethylene glycol, 1,2- and 1,3-propylene glycol, neopentyl glycol, 1,3- and 1,4-butanediol, 3-methylpentanediol, hexamethylene glycol, 1,8-octanediol, 2-methyl-1,3-propanediol, bisphenol A, hydrogenated bisphenol A, trimethylolpropane, and cyclohexanedimethanol.
[0110] Examples of organic polyisocyanates that can be used to prepare the aqueous dispersion of urethane resin include aromatic isocyanates such as tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymeric MDI, xylylene diisocyanate (XDI), and tetramethylxylylene diisocyanate (TMXDI); aliphatic isocyanates such as hexamethylene diisocyanate (HMDI); and alicyclic isocyanates such as isophorone diisocyanate (IPDI) and 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI, H12MDI). These may be used alone or in combination of two or more.
[0111] Examples of hydrophilic group-containing compounds that can be used to prepare the aqueous dispersion of the urethane resin include carboxylic acid-containing compounds such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, and glycine, and derivatives thereof such as sodium salts, potassium salts, and amine salts; and sulfonic acid-containing compounds such as taurine (i.e., aminoethylsulfonic acid) and ethoxypolyethylene glycol sulfonic acid, and derivatives thereof such as sodium salts, potassium salts, and amine salts.
[0112] The urethane resin can be obtained by a known method. For example, a urethane prepolymer can be obtained by mixing the above-mentioned polyol, organic polyisocyanate, and hydrophilic group-containing compound and reacting them at a temperature in the range of 30 to 130°C for 30 minutes to 50 hours. The urethane prepolymer is polymerized by chain extension using a chain extender, thereby becoming a urethane resin having hydrophilic groups.
[0113] The chain extender is preferably water and / or an amine compound. By using water or an amine compound as the chain extender, it is possible to react with free isocyanate in a short time and efficiently extend the isocyanate-terminated prepolymer.
[0114] Examples of the amine compound as a chain extender include aliphatic polyamines such as ethylenediamine and triethylenediamine, aromatic polyamines such as metaxylenediamine and toluylenediamine, and polyhydrazino compounds such as hydrazine and adipic acid dihydrazide. The amine compound may contain, together with the polyamine, a monovalent amine such as dibutylamine or methyl ethyl ketoxime as a reaction terminator to the extent that it does not significantly inhibit polymerization.
[0115] In addition, in the synthesis of the urethane prepolymer, a solvent that is inert to isocyanates and can dissolve the urethane prepolymer may be used. Examples of such solvents include dioxane, methyl ethyl ketone, dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, toluene, and propylene glycol monomethyl ether acetate. These hydrophilic organic solvents used in the reaction step are preferably finally removed.
[0116] In addition, in the synthesis of the urethane prepolymer, a catalyst such as an amine catalyst (e.g., triethylamine, N-ethylmorpholine, triethyldiamine, etc.), a tin-based catalyst (e.g., dibutyltin dilaurate, dioctyltin dilaurate, tin octoate, etc.), or a titanium-based catalyst (e.g., tetrabutyl titanate, etc.) may be added to promote the reaction.
[0117] The number-average molecular weight of the urethane resin is preferably increased as much as possible by introducing a branched structure or internal crosslinking structure, and is preferably within the range of 50,000 to 10,000,000. By keeping the molecular weight within this range, the urethane resin becomes less soluble in solvents, resulting in a coating film with excellent weather resistance and water resistance. Alternatively, commercially available urethane resins may be used. Examples of commercially available urethane resins with a glass transition temperature (Tg) within the range of 40 to 90°C include Neorez R-967, R-600, and R-9671 manufactured by Kusumoto Chemicals, Ltd., Evaphanol HA-560 manufactured by Nicca Chemical, Inc., and SF870 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.
[0118] The number average molecular weight (Mn) is a value measured by gel permeation chromatography (GPC), and can be determined from a calibration curve prepared using a polystyrene standard sample, for example, using a Shimadzu Corporation "RID-6A" (column: Tosoh Corporation "TSK-GEL", solvent: tetrahydrofuran (THF), column temperature: 40°C).
[0119] [Acrylic Resin] The acrylic resin used as the water-insoluble resin particles can be obtained by using a copolymer with an acrylic acid ester component, a methacrylic acid ester component, or a styrene component.
[0120] Examples of the acrylic acid ester component and the methacrylic acid ester component include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, and methyl (meth)acrylate. Examples of the acrylate copolymer include 2-hydroxybutyl acrylate, benzyl (meth)acrylate, glycidyl (meth)acrylate, (meth)acrylic acid, (di)ethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin di(meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and acrylamide.
[0121] Examples of the styrene component include styrene, 4-methylstyrene, 4-hydroxystyrene, 4-acetoxystyrene, 4-acetylstyrene, and styrenesulfonic acid, etc. These components may be used alone or in combination of two or more.
[0122] The number average molecular weight (Mn) of the acrylic resin is preferably in the range of 1,000 to 50,000, and more preferably in the range of 2,000 to 20,000. When the number average molecular weight (Mn) of the acrylic resin is 1,000 or more, the cohesive force of the coating film is strong and the adhesion is improved, and when it is 50,000 or less, the solubility in organic solvents is good and miniaturization of the particle size of the emulsion dispersion is promoted.
[0123] Commercially available acrylic resins having a glass transition temperature (Tg) in the range of 40 to 90°C include acrylic emulsions such as Mowinyl 6899D, 6969D, and 6800 manufactured by Japan Coating Resins Co., Ltd., and TOCRYL W-7146, W-7147, W-7148, W-7149, and W-7150 manufactured by Toyochem Co., Ltd.
[0124] The number average molecular weight (Mn) is a value measured by gel permeation chromatography (GPC), and can be determined from a calibration curve prepared using a polystyrene standard sample, for example, using a Shimadzu Corporation "RID-6A" (column: Tosoh Corporation "TSK-GEL", solvent: tetrahydrofuran (THF), column temperature: 40°C).
[0125] [Composite Resin Particles] The composite resin particles that can be contained in the ink are preferably composite resin particles in which an acrylic resin is emulsified in a urethane resin, i.e., composite resin particles having an inner layer made of an acrylic resin and a surface layer made of a urethane resin.
[0126] The urethane resin exists at the interface between the acrylic resin as the water-insoluble resin particles and the water as the continuous phase, and functions as a water-insoluble resin particle layer different from the resin that protects the water-insoluble resin particles. By emulsifying the acrylic resin with the urethane resin to form composite resin particles in this way, the physical properties of the image (coating film) can be improved, and the storage stability of the composite resin particles can also be improved, compared to when the acrylic resin and the urethane resin are separately emulsified and mixed.
[0127] In the composite resin microparticles obtained by emulsifying the acrylic resin in the urethane resin, the mass ratio (U / A) of the urethane resin (U) to the acrylic resin (A) is preferably within the range of (40 / 60) to (95 / 5). When the proportion of the urethane resin (U) is within this range, compatibility with the dispersant is improved, and solvent resistance is also improved.
[0128] Furthermore, when the content of the acrylic resin (A) is within the above range, the adhesiveness to the acrylic film is excellent. In the above content, the mass ratio (U / A) of the urethane resin (U) to the acrylic resin (A) is preferably within the range of (40 / 60) to (80 / 20).
[0129] The total resin concentration of the acrylic resin and the urethane resin in the composite resin particles is not particularly limited, but is preferably 5.0% by mass or more, and more preferably in the range of 10.0 to 70.0% by mass. When the resin concentration is within this range, the fixation of the ink to the recording medium is good.
[0130] Furthermore, when emulsifying an acrylic resin with a urethane resin, a surfactant acting as an emulsifier can be used together with the urethane resin. The addition of an emulsifier can improve the storage stability of the composite resin microparticles. Anionic surfactants and nonionic surfactants can be used as the emulsifier. The use of composite resin microparticles in which an acrylic resin is emulsified in a urethane resin can improve the fixability of an image (coating film) to an absorbent or non-absorbent substrate.
[0131] The average particle size of the composite resin microparticles is not particularly limited, but is preferably in the range of 10 to 500 nm, more preferably in the range of 10 to 300 nm, and even more preferably in the range of 10 to 200 nm. The average particle size can be measured using a commercially available particle size measuring device that uses a dynamic light scattering method, an electrophoresis method, or the like, but measurement by the dynamic light scattering method is simple and can measure the particle size range with high accuracy.
[0132] (Inorganic Particles) The inorganic particles contained in the ink according to the present invention are used as an inorganic pigment by being contained in, for example, a pigment. Examples of pigments containing inorganic particles include white inorganic pigments such as light calcium carbonate, heavy calcium carbonate, magnesium carbonate, kaolin, clay, talc, calcium sulfate, barium sulfate, titanium dioxide, zinc oxide, zinc hydroxide, zinc sulfide, zinc carbonate, hydrotalcite, aluminum silicate, diatomaceous earth, calcium silicate, magnesium silicate, synthetic amorphous silica, colloidal silica, alumina, colloidal alumina, pseudoboehmite, aluminum hydroxide, lithopone, zeolite, and magnesium hydroxide.
[0133] Generally, titanium oxide is used as an inorganic particle contained in ink, but it is difficult to ensure ink ejection stability and adhesion with titanium oxide, and its high complex dielectric constant makes it significantly affected by the heat-generating effect of microwaves in the drying process described below. In the present invention, for example, by applying the precoat liquid described above in an appropriate amount, the heat-generating effect of microwaves can be appropriately controlled, thereby compensating for the above-mentioned drawbacks of titanium oxide.
[0134] (Organic Particles) The organic particles contained in the ink according to the present invention are used as an organic pigment, for example, by being contained in a pigment. The organic particles according to the present invention are water-insoluble organic particles that dissolve or swell in a water-soluble organic solvent having a boiling point of 120°C or higher. The material thereof is selected from conventionally known materials, such as polyvinyl chloride, polyvinylidene chloride, polyacrylate, polymethacrylate, elastomer, ethylene-vinyl acetate copolymer, styrene-(meth)acrylic copolymer, polyester, polyvinyl ether, polyvinyl acetal, polyamide, polyurethane, polyolefin, SBR, NBR, polytetrafluoroethylene, chloroprene, protein, polysaccharide, rosin ester, and shellac resin.
[0135] Particularly preferred materials for the organic particles are polyvinyl acetal resins, polyurethane resins, rosin ester resins, (meth)acrylate resins, SBR, etc. Resins composed of two or more types of monomers obtained by modification or copolymerization are also preferably used. Furthermore, resins to which a specific modifying group has been added or from which a leaving group has been removed may also be used. Two or more types of materials may be mixed to form organic particles, and two or more types of organic particles may also be mixed and used.
[0136] In the present invention, "dissolution" refers to the state in which the organic particles and the water-soluble organic solvent in the ink are in equilibrium and form a single phase, and "swelling" refers to the state in which the organic particles absorb the water-soluble organic solvent and increase in volume.
[0137] The organic particles according to the present invention must be insoluble in water so as not to dissolve during inkjet recording. However, they are permitted to absorb water to the extent that it does not impair the ink absorption rate. They may absorb up to 20% by mass of water relative to the mass of the organic particles. Furthermore, a crosslinking agent may be used in the organic particles according to the present invention to the extent that it does not interfere with dissolution or swelling in a water-soluble organic solvent.
[0138] In the present invention, the crosslinking agent may be any of conventionally known crosslinking agents, whether organic or inorganic. The organic particles themselves are preferably hydrophilic but not water-soluble, and therefore are preferably adjusted to a content of 10% by mass or more but less than 50% by mass.
[0139] Inkjet recording paper is usually used at room temperature, but the storage conditions before use are not necessarily room temperature. In particular, inkjet recording paper can reach extremely high temperatures inside a closed car in the summer, so it is desirable that the paper can be used without any problems even after being exposed to such an environment. For this reason, the glass transition temperature (Tg) of the organic particles in the above-described embodiment must be 70°C or higher, preferably 80°C or higher, and more preferably within the range of 90 to 120°C.
[0140] If the glass transition temperature (Tg) of the organic particles is less than 70°C, the organic particles are likely to fuse together when heated, which results in a reduction in the voids on the surface of the recording paper and a decrease in the ink absorption rate.
[0141] (Water) The water according to the present invention constitutes the aqueous solution together with the surfactant, and any known water can be used as the water, and there are no particular limitations.
[0142] (Water-Soluble Solvent) Examples of water-soluble solvents contained in the ink according to the present invention include ethanol (boiling point: 78°C), ethylene glycol (boiling point: 198°C), propylene glycol (boiling point: 188°C), diethylene glycol monobutyl ether (boiling point: 230°C), 1,2-hexanediol (boiling point: 170°C), dipropylene glycol (boiling point: 230°C), glycerin (boiling point: 290°C), 1,3-propanediol (boiling point: 215°C), and 1,2-pentanediol (boiling point: 242°C). The water-soluble solvent may be a single solvent or multiple solvents. When multiple solvents are used, it is preferable that one of the solvents has a boiling point of 150°C or higher. This suppresses ink drying near the nozzles of the inkjet head and prevents solids from precipitating and clogging the nozzles, resulting in poor ejection performance. Furthermore, it is even more preferable that one of the water-soluble solvents is a humectant.
[0143] [Humectant] The term "humectant" as used herein refers to a solvent that has high microwave or high-frequency wave absorption and a high boiling point. When contained in the water-soluble solvent contained in the ink of the present invention, the humectant has the effect of suppressing evaporation of water in the ink composition and preventing aggregation of solid components such as pigments and polymer particles in the ink. The humectant also plays a role in slowing down the drying speed of the ink.
[0144] When a humectant with a high boiling point is contained in a water-soluble solvent, the humectant is difficult to evaporate, but the water-soluble solvent itself can be directly heated by using microwaves. The humectant is a solvent that dries easily when irradiated with microwaves, but is difficult to dry under normal atmosphere, so it is suitable for controlling uniform drying.
[0145] The humectant preferably has a boiling point of 200° C. or higher. Moisture retention can be achieved by adding an ink containing a solvent with a high boiling point that is easily heated directly by microwaves or high-frequency dielectric waves (high complex dielectric constant) and a boiling point of 200° C. or higher. This can then be dried at high speed by using microwaves and high-frequency dielectric waves, achieving both high-speed drying and stable ejection.
[0146] By including the above-mentioned humectant in the ink, when the ink is ejected from the inkjet head, nozzle clogging due to the ink drying in the nozzle part of the inkjet head can be prevented, thereby improving the ejection stability of the ink.
[0147] Furthermore, from the viewpoint of uniform drying control, it is preferable that the content of the humectant is within a range of 3 to 20 mass % relative to the first ink or the second ink, and that the complex dielectric constant ε'' at 25°C when the first ink or the second ink is irradiated with microwaves at a frequency of 2.45 GHz is within a range of 13 to 60.0.
[0148] Furthermore, from the viewpoint of uniform drying control, it is more preferable that the content of the humectant is greater in the second ink (ink having a relatively high complex dielectric constant) than in the first ink (ink having a relatively low complex dielectric constant).
[0149] Examples of humectants include dipropylene glycol (boiling point: 230°C), 1,4-butanediol (boiling point: 230°C), glycerin (boiling point: 290°C), 1,2-pentanediol (boiling point: 242°C), 1,5-pentanediol (boiling point: 242°C), and 1,3-propanediol (boiling point: 215°C).
[0150] (Surfactant) The ink according to the present invention contains a surfactant, which improves the ejection stability of the ink and makes it possible to control the spread (dot diameter) of ink droplets that land on a recording medium.
[0151] The surfactant is not particularly limited, but when an anionic compound is included in the constituent components of the ink, the ionicity of the surfactant may be anionic, nonionic (also called "nonionic"), or amphoteric, and as an amphoteric surfactant, a betaine type is preferable. In the present invention, if an anionic surfactant contains an alkaline component, the resin particles contained as a fixing resin tend to aggregate, resulting in a decrease in fixing property, and therefore, it is preferable that the surfactant be nonionic.
[0152] The surfactant is preferably a fluorine-based or silicone-based surfactant having a high static surface tension reducing ability, an anionic surfactant such as dioctyl sulfosuccinate having a high dynamic surface tension reducing ability, or a nonionic surfactant such as a relatively low molecular weight polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, acetylene glycol, Pluronic (registered trademark) surfactant, sorbitan derivative, etc. Note that a surfactant having a high static surface tension reducing ability and a surfactant having a high dynamic surface tension reducing ability may be used in combination.
[0153] In the present invention, it is preferable to use, for example, TEGOWET-KL245 (polyether-modified siloxane copolymer; manufactured by Evonik Co., Ltd.) as the surfactant.
[0154] It is preferable that the ink contains a surfactant having a hydroxy group, as this appropriately controls the surface tension and viscosity of the ink according to the present invention and improves the coatability of the ink, and it is more preferable that the surfactant has a diol structure. The surfactant that remains after the ink dries has high microwave absorption capacity, which results in the unexpected effect of rapid drying and improved film uniformity. In addition, the complex dielectric constant is high in the later stage of drying. Furthermore, this effect is further enhanced when the surfactant has a diol structure.
[0155] (Other Components) The ink according to the present invention may contain various known additives depending on other purposes such as ejection stability, compatibility with print heads and ink cartridges, storage stability, image preservability, etc. The ink according to the present invention may also contain pH adjusters, crosslinking agents, antifungal agents, bactericides, and other components as appropriate.
[0156] (1.1.2) Physical Properties of Ink (Complex Dielectric Constant) The term "complex dielectric constant" as used herein refers to a numerical value that indicates the response of molecules when an electric field is applied from the outside (degree of dielectric polarization), and is specific to a substance and is expressed as the dielectric constant ε in a vacuum. 0 It is a dimensionless quantity when the electrical constant is used as the standard.
[0157] The higher the complex dielectric constant of microwaves, the greater the heat-generating effect. Therefore, it is possible to control the drying property by using an appropriate formulation that uses an ink (first ink) with a relatively low complex dielectric constant and an ink (second ink) with a relatively high complex dielectric constant.
[0158] If the complex dielectric constants of the first ink and the second ink according to the present invention are lower than the complex dielectric constant of the precoat liquid described below, when drying is performed using microwaves in the drying step described below, the precoat liquid will be more strongly affected by the heat generating effect of microwaves than the first ink and the second ink.
[0159] This allows the precoat liquid to mix with the first ink and the second ink, improving the drying properties of each ink, thereby imparting quick-drying properties to areas where increased drying properties are desired in the image forming method of the present invention. This allows for uniform drying control, and also allows for the formation of uniform dots without graininess, resulting in the formation of images with excellent gloss and color gamut. Furthermore, applying the precoat liquid to areas where the first ink and the second ink are not applied is preferable because it allows the effect of microwaves to be controlled in accordance with the areas where the first ink and the second ink are applied.
[0160] In the present invention, when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1):
[0161] Formula (1): ε′′1<ε′′2
[0162] Note that the higher the complex dielectric constant of microwaves, the greater the heat-generating effect. Therefore, it is preferable for the complex dielectric constant ε''1 of the first ink and the complex dielectric constant ε''2 of the second ink to satisfy the relationship of the following formula (3) in order to keep the heat-generating effect within an appropriate range and to control the drying property uniformly.
[0163] Equation (3): (ε′′2 / ε′′1)<20
[0164] The complex dielectric constant is measured using a complex dielectric constant measuring device (for example, a material impedance analyzer MIA-5M (SH2-Z type 4-terminal sample holder) manufactured by Toyo Corporation).
[0165] (Viscosity, surface tension, etc.) The physical properties of the ink of the present invention are not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges.
[0166] The viscosity of the ink at 25°C is preferably in the range of 5 to 30 mPa·s, and more preferably in the range of 5 to 25 mPa·s, from the viewpoints of improving print density and character quality and obtaining good ejection stability from the nozzles of the inkjet head. The viscosity can be measured, for example, using a rotational viscometer "RE-80L" manufactured by Toki Sangyo Co., Ltd., under measurement conditions of 25°C, a standard cone rotor (1°34' x R24), a sample liquid volume of 1.2 mL, a rotation speed of 50 rpm, and 3 minutes.
[0167] The surface tension of the ink is preferably in the range of 1 to 55 mN / m, more preferably 1 to 40 mN / m or less, and even more preferably 1 to 35 mN / m at 25° C., from the viewpoint of ensuring good ink leveling on the recording medium and shortening the drying time of the ink. The surface tension can be measured by the Wilhelmy method using a surface tensiometer such as the "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd.
[0168] The pH value of the ink is preferably in the range of 3 to 9, and more preferably in the range of 6 to 9, from the viewpoint of achieving the effects of the present invention.
[0169] (1.1.3) Ink Application Method As with the precoat liquid described above, the method for applying the first ink and the second ink according to the present invention onto a substrate, or onto a substrate to which a precoat liquid has been applied, is not particularly limited. However, application by an inkjet method is preferred from the viewpoint of controlling the uniformity and density of the ink.
[0170] When the second ink is applied after the first ink, it is preferable that the second ink is applied within 0.1 to 5 seconds after the first ink is applied. By applying the second ink immediately after the first ink is applied, the first ink and the second ink diffuse and improve wettability.
[0171] (1.2) Ink Drying Process The drying process according to the present invention includes a process of drying the first ink and the second ink (hereinafter simply referred to as the "ink drying process"). In the ink drying process, microwaves are irradiated onto the first ink and the second ink, and, if necessary, the precoat liquid, etc., that have been applied to the substrate, to control the drying properties uniformly.
[0172] The term "uniform drying control" used here means imparting quick drying properties to a specific area to be dried, and controlling the drying of areas other than the specific area to be dried uniformly.
[0173] (1.2.1) Drying Method The first ink and second ink applied to the substrate are dried by being irradiated with microwaves in the ink drying process to form a coating film. Note that the above-mentioned "coating film" includes not only one formed from the first ink and the second ink, but also one formed from the precoat liquid, the first ink, and the second ink.
[0174] The thickness of the coating film obtained as described above is preferably in the range of 0.3 to 3.0 μm, and more preferably in the range of 0.3 to 2.0 μm. When the thickness of the coating film is 0.3 μm or more, the adhesion and abrasion resistance of the image are easily improved. Furthermore, when the thickness of the coating film is 3.0 μm or less, the deformation stress applied to the ink layer can be reduced, so the adhesion of the image is less likely to be impaired.
[0175] (Microwave) At least one of the drying steps according to the present invention, that is, the ink drying step, is a step of drying the coating film by irradiating microwaves.
[0176] In the image forming method of the present invention, microwaves are used to dry the ink. Microwaves have high directionality and act directly on materials with high complex dielectric constants, resulting in high drying efficiency and no damage to plastic substrates and the like.
[0177] In addition, since there is no need to apply atmospheric conditions (conditions due to wind, temperature, etc.) to dryness control, it is possible to prevent the nozzle from drying out during inkjet coating, and it is possible to dry immediately after printing without worrying about nozzle drying. Furthermore, if the precoat liquid contains metal salts, etc., the coagulation effect is enhanced, improving durability and fastness.
[0178] In this specification, the above-mentioned "coating film" includes a liquid state having fluidity such as wetting and spreading properties or permeability immediately after the precoat liquid is applied to the area outside the ink application area on the substrate, immediately after the ink is applied to the substrate, or immediately after the precoat liquid and the ink are mixed on the substrate, as well as the state thereafter (state after drying).
[0179] The term "fluid liquid state" refers to a state in which a liquid (including a semi-solid liquid in the present invention) moves so as to wet, spread, or penetrate onto a substrate or a coating film.
[0180] Microwave irradiation tends to generate Joule heat and easily generate heat when the ink has a high complex dielectric constant. In the present invention, the heat generation effect caused by microwave irradiation can be uniformly controlled by controlling the complex dielectric constants of the first ink and the second ink, and the properties and combinations of the pigment, resin, water, water-soluble solvent, surfactant, etc., in order to control the drying properties.
[0181] For the microwave irradiation according to the present invention, a microwave generator manufactured by Shimada Rika Kogyo Co., Ltd. can be used, but a commercially available microwave dryer such as a batch microwave dryer manufactured by Yamamoto Vinita Co., Ltd. may also be used.
[0182] In addition to the drying by microwave irradiation, the present invention may also be carried out using a non-contact heating type drying device such as a drying oven or a hot air blower, or a contact heating type drying device such as a hot plate or a heat roller. Similar effects can also be expected when drying is carried out by irradiating high frequency waves (13 to 50 MHz) instead of microwaves.
[0183] The heating temperature is preferably within a range of 60 to 120°C, and the heating time is adjusted appropriately depending on the type of substrate, the amount of the precoat liquid to be applied, and the amount of the first ink and the second ink to be applied.
[0184] The drying temperature can be obtained by measuring any one of the following throughout the drying period of the precoat liquid and ink: (a) when a non-contact heating drying device such as a drying oven or a hot air blower is used, the ambient temperature such as the temperature inside the oven or the hot air temperature; (b) when a contact heating drying device such as a hot plate or a heated roller is used, the temperature of the contact heating part; or (c) the surface temperature of the surface to be dried. It is more preferable to measure the surface temperature of the surface to be dried (c).
[0185] As described above, by heating the applied amount of the precoat liquid and the area where the ink is applied, the solvent components of the precoat liquid and the ink are removed, and at the same time, in the case of a metal substrate in particular, the polyvalent metal salt is dried and thermally decomposed at a temperature equal to or higher than the thermal decomposition temperature, thereby improving the abrasion resistance of the image and the adhesion to the substrate.
[0186] (Air drying) In the drying step using microwave irradiation, it is preferable to dry the coated first ink and second ink by blowing air at a temperature of 100° C. or less from the viewpoint of controlling drying properties. The air speed is preferably 5 to 40 m / s.
[0187] (1.2.2) Drying rate The first ink and second ink according to the present invention are characterized in that when the inks are applied to a substrate and then dried at 80°C for 20 seconds, their drying rates are defined as D1 and D2, respectively, and D1 and D2 satisfy the following formula (2): D2<D1.
[0188] For example, if drying properties are not taken into consideration, during microwave irradiation, there is no significant difference in the complex dielectric constant between the first ink and the second ink in the early drying stage when drying has not progressed, but in the later drying stage, the complex dielectric constant of the second ink according to the present invention is significantly higher than that of the first ink, and therefore the second ink dries more quickly. However, by making the drying rate (D1) of the first ink greater than the drying rate (D2) of the second ink, the drying properties of the first ink and the second ink are balanced, making it possible to control the drying properties uniformly.
[0189] The drying rate when the first ink and the second ink are dried at 80° C. for 20 seconds is measured and calculated as follows.
[0190] The ink is applied to a PET substrate cut to 10 cm x 10 cm using a wire bar to obtain a sample for measuring the drying rate. The mass of the sample is then immediately measured using an electronic balance, and this measurement is the "mass before drying" of the sample. The sample is dried in a hot air oven at 80°C for 20 seconds, and then the mass is measured again using the electronic balance, and this measurement is the "mass after drying" of the sample.
[0191] The total mass of the ink is calculated from the amount of ink applied to a PET substrate cut to 10 cm x 10 cm, and the total mass of the solvent in the ink is calculated from the ratio of the solvent to the total ink.
[0192] Since (mass before drying - mass after drying) is considered to be the mass lost by the ink due to evaporation, the drying rate can be expressed by the following formula:
[0193] Drying rate [%] = (mass before drying - mass after drying) / total mass of solvents in ink × 100
[0194] (1.3) Other Steps It is preferable to have a step of applying a precoat liquid before the step of applying the ink and the step of drying the ink. The precoat liquid according to the present invention plays a role in fixing (pinning) the first ink and the second ink on the recording medium.
[0195] The precoat liquid can be applied before the first ink and the second ink are applied to the substrate, or can be applied after the first ink and the second ink are applied to the substrate.
[0196] Furthermore, for example, by applying a precoat liquid having a high complex dielectric constant before the ink is ejected, the drying property of the applied portion of the precoat liquid can be improved. The drying property can also be controlled by adjusting the amount of precoat depending on the difference in the complex dielectric constant between the first ink and the second ink.
[0197] Therefore, it is preferable to have a precoat liquid application step before the ink application step, from the viewpoint of controlling the pinning properties and uniform drying properties of the first ink and the second ink.
[0198] A precoat liquid is usually used for the purpose and perspective of aggregating the ink appropriately, suppressing aggregation unevenness, improving the pinning property of the ink, etc. For example, when the precoat liquid plays a role in fixing (pinning) the ink on the recording medium, the precoat liquid is applied to a substrate before applying the ink, and after drying, the precoat liquid mixes with the ink on the substrate to form an ink aggregation layer.
[0199] In the image forming method of the present invention, the precoat liquid may not be used, but by utilizing the aggregation effect due to the reaction between the precoat liquid and the ink and by providing quick drying properties, the use of the precoat liquid makes it possible to control the drying property more uniformly. Furthermore, by applying a precoat liquid having a high complex dielectric constant to a desired location, it becomes possible to control the drying property uniformly.
[0200] (1.3.1) Precoat Liquid The precoat liquid according to the present invention contains, for example, a resin, a metal salt, an organic acid, an inorganic acid, a solvent, a surfactant, and the like. Among these, a metal salt, a resin (especially a cationic resin), or an organic acid reacts with the ink to thicken it and has the effect of acting as a flocculant, so that a high-quality image can be formed even when the image is formed on a non-absorbent substrate. Furthermore, these can be contained alone or in combination of two or more kinds.
[0201] When drying is performed using microwaves in the drying step described below, the complex dielectric constant of the precoat liquid can be changed by combining these materials, making it possible to control the heat generation effect of microwaves. In addition to the aggregation pinning effect of the precoat liquid and ink, the drying pinning effect of microwaves is superimposed, making it possible to form an image with less graininess, higher gloss, and a higher color gamut.
[0202] It is preferable that the complex dielectric constant of the precoat liquid is equal to or greater than the complex dielectric constants of the first ink and the second ink, in order to improve the drying properties of a mixed coating film of the precoat liquid and the ink, form uniform dots without graininess, and achieve gloss and color gamut.
[0203] (Resin) The resin in the precoat liquid according to the present invention may be, for example, a vinyl chloride resin, a (meth)acrylic resin, a urethane resin, a polyether resin, a polyester resin, etc. Among these, it is preferable that the precoat liquid contains an ionic resin from the viewpoint of fixing property, film-forming property, etc.
[0204] The resin contained in the precoat liquid according to the present invention may be water-soluble. Since pigments are usually anionic components, it is preferable that the resin contained in the precoat liquid is a cationic resin, since it mixes with the ink and forms an ink aggregation layer.
[0205] (Metal Salt) The precoat liquid according to the present invention preferably contains an inorganic or organic polyvalent metal salt as the metal salt. When the precoat liquid contains such a polyvalent metal salt, anionic components in the ink mixed with the precoat liquid on the substrate are coagulated by salting out.
[0206] The polyvalent metal salt may be a salt of a metal having a valence of two or more. The type of metal (cation) constituting the polyvalent metal salt is not particularly limited. For example, Ca 2+ , Cu 2+ , Ni 2+ , Mg 2+ , Zn 2+ , Ba 2+ divalent metal ions such as Al 3+ , Fe 3+ , Cr 3+ , Y 3+ Trivalent metal ions such as Zr 4+ and the like.
[0207] The type of salt constituting the polyvalent metal salt is not particularly limited, and known salts such as carbonates, sulfates, nitrates, hydrochlorides, organic acid salts, borates, and phosphates can be used. Particularly preferred are calcium or magnesium salts of carboxylic acids such as calcium chloride, magnesium chloride, calcium nitrate, magnesium nitrate, magnesium acetate, calcium acetate, magnesium lactate, and calcium pantothenate.
[0208] Examples of metal salts other than polyvalent metal salts include monovalent metal salts such as sodium salts and potassium salts, such as sodium sulfate and potassium sulfate.
[0209] (Organic Acid) The organic acid is capable of aggregating pigments that may be contained in the ink. When an organic acid is contained in the precoat liquid as an aggregating agent, it can aggregate anionic components in the ink by changing the pH.
[0210] As the organic acid, a monocarboxylic acid is preferred from the viewpoint of not weakening the cohesive force of the polyvalent metal salt, and examples thereof include formic acid, malonic acid, acetic acid, propionic acid, isobutyric acid, and benzoic acid.
[0211] Furthermore, the use of an organic acid makes it easier to maintain the storage stability of the precoat liquid, and makes it less likely that blocking will occur after the precoat liquid is applied and dried. From this perspective, preferred organic acids include formic acid, malonic acid, acetic acid, propionic acid, and benzoic acid.
[0212] (Inorganic Acid) Examples of acids other than organic acids include inorganic acids, such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. These may be used alone or in combination of two or more.
[0213] (Solvent) In the precoat liquid according to the present invention, both water-soluble and non-water-soluble solvents can be used as the solvent.
[0214] [Water-soluble solvent] The precoat liquid according to the present invention may contain, as a solvent, a water-soluble solvent having a boiling point in the range of 150 to 250° C. If a water-soluble solvent with such a high boiling point is contained, the precoat liquid becomes difficult to evaporate, and the drying property decreases, which is preferable from the viewpoint of controlling the drying property uniformly.
[0215] Therefore, for example, in the image forming method of the present invention, by applying a precoat liquid containing a water-soluble solvent having a high boiling point as described above to a location where it is desired to reduce the drying speed, it is possible to slow down the drying speed of the specific location, which is suitable for controlling the drying speed uniformly.
[0216] Examples of the water-soluble solvent include alcohols, polyhydric alcohols, amines, amides, glycol ethers, and 1,2-alkanediols having 4 or more carbon atoms. Among these, it is preferable to contain a water-soluble solvent having a boiling point of 180° C. or higher from the viewpoint of controlling drying properties.
[0217] Examples of water-soluble solvents having a boiling point in the range of 180 to 300° C. include ethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, and glycerin.
[0218] [Non-Water-Soluble Solvent] The precoat liquid according to the present invention may contain, as a solvent, a non-water-soluble solvent other than the water-soluble solvent having a boiling point in the range of 150 to 250° C. Examples of the non-water-soluble solvent include trimethylolpropane, triethylene glycol, and tetraethylene glycol.
[0219] (Surfactant) The precoat liquid according to the present invention preferably contains a surfactant. The surfactant is not particularly limited, but is preferably at least one selected from the group consisting of polysiloxane-based surfactants and acetylene glycol-based surfactants.
[0220] Among these, polysiloxane surfactants are more preferred because they have a high solubility in the precoat liquid and are less likely to produce foreign matter in the precoat liquid.
[0221] The polysiloxane surfactant is not particularly limited, but examples thereof include TEGOWET-KL245 (polyether-modified siloxane copolymer; manufactured by Evonik), BYK-347 (manufactured by BYK), BYK-348 (manufactured by BYK), BYK-349 (manufactured by BYK), BYK-3550 (manufactured by BYK), and BYK-UV3510 (manufactured by BYK).
[0222] The acetylene glycol surfactant is not particularly limited, but is preferably at least one selected from, for example, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, alkylene oxide adducts of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, and alkylene oxide adducts of 2,4-dimethyl-5-decyne-4-ol, and alkylene oxide adducts of 2,4-dimethyl-5-decyne-4-ol.
[0223] These are available as commercial products such as E series such as Olfine 104 series and Olfine E1010 (manufactured by Air Products Japan, Inc.), Olfine PD-002W, Surfynol 465 and Surfynol 61 (manufactured by Nissin Chemical Industry CO., Ltd.).
[0224] The content of the surfactant is preferably within a range of 0.1 to 10% by mass relative to the total mass of the reaction liquid (100% by mass).
[0225] (Other Constituents) The precoat liquid according to the present invention may contain water, a crosslinking agent, an antifungal agent, a bactericide, and other components as appropriate, provided that the effects of the present invention are not impaired.
[0226] Further, for example, ultraviolet absorbers described in JP-A Nos. 57-74193, 57-87988 and 62-261476, anti-fading agents described in JP-A Nos. 57-74192, 57-87989, 60-72785, 61-146591, JP-A Nos. 1-95091 and 3-13376, anions, It is also possible to contain various known additives such as various cationic or nonionic surfactants, fluorescent brightening agents described in JP-A Nos. 59-42993, 59-52689, 62-280069, 61-242871, and JP-A No. 4-219266, antifoaming agents, lubricants such as diethylene glycol, preservatives, thickeners, antistatic agents, etc.
[0227] (1.3.2) Physical Properties of Precoat Liquid (Complex Dielectric Constant) It is preferable that the complex dielectric constant of the precoat liquid according to the present invention is equal to or greater than the complex dielectric constants of the first ink and the second ink, in order to improve the drying properties of a mixed coating film of the precoat liquid with the first ink and the second ink, form uniform dots without graininess, and improve gloss and color gamut. Details of the complex dielectric constant are as explained in the section on physical properties of the inks.
[0228] The physical properties of the precoat liquid according to the present invention are not particularly limited and can be appropriately selected depending on the purpose. For example, the viscosity of the precoat liquid at 25°C is preferably in the range of 5 to 30 mPa·s, from the viewpoint of obtaining good ejection stability from the nozzle of the inkjet head.
[0229] The surface tension of the precoat liquid is preferably within the range of 1 to 55 mN / m at 25° C., in order to ensure that the ink is properly leveled on the recording medium and the drying time of the ink is shortened.
[0230] (1.3.3) Method of Applying Precoat Liquid The method of applying the precoat liquid to the substrate is not particularly limited, but preferred examples include an inkjet method, a roller coating method, a curtain coating method, and a spray coating method.
[0231] In an embodiment of the present invention, the precoat liquid is preferably applied by an inkjet method, from the viewpoint of freely controlling the amount and application range of the precoat liquid, for example, by using a printer equipped with an inkjet head loaded with the precoat liquid.
[0232] Examples of inks with low complex dielectric constants that are close to insulating include yellow ink (Y), magenta ink (M), and cyan ink (C), while examples of inks with high complex dielectric constants include black ink (K) and white ink (W). Inks containing highly conductive metal oxides or metals also have high complex dielectric constants.
[0233] Here, by appropriately controlling the application amount of the precoat liquid according to the present invention by a method such as inkjet printing in accordance with the application amount of the ink with a low complex dielectric constant that is close to insulating and the application amount of the ink with a high complex dielectric constant, the ink with a high complex dielectric constant is not dried excessively compared to the ink with a low complex dielectric constant that is close to insulating, and uniform drying control can be performed, resulting in a high-quality printed matter.
[0234] (1.4) Other (1.4.1) Substrate The substrate (recording medium) applicable to the present invention is not particularly limited, and examples thereof include substrates that are non-ink-absorbent or have low ink absorbency. In the present invention, microwaves are used to dry the first ink and the second ink, and therefore substrates that do not absorb microwaves do not generate heat. Therefore, damage to the substrate can be suppressed.
[0235] Furthermore, since the first ink and the second ink are dried using microwaves, there is no need to dry the first ink and the second ink under atmospheric conditions (conditions due to wind, temperature, etc.), and therefore drying of the nozzles during inkjet coating can be prevented. Therefore, even if the substrate is a resin film that is easily affected by heat, damage to the substrate can be avoided and ink ejection stability can be ensured.
[0236] Examples of non-ink-absorbent substrates include resin films that have not been surface-treated for inkjet printing (i.e., no ink-absorbing layer formed thereon), substrates such as paper that are coated with a resin, and substrates that have a resin film adhered thereto.
[0237] Examples of the resin film include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyethylene, polypropylene, cellophane, cellulose esters such as cellulose diacetate, cellulose triacetate (TAC), cellulose acetate butyrate, cellulose acetate propionate (CAP), cellulose acetate phthalate, and cellulose nitrate, or derivatives thereof, polyvinylidene chloride, polyvinyl alcohol, polyethylene vinyl alcohol, syndiotactic polystyrene, polycarbonate, norbornene resin, polymethylpentene, polyether ketone, polyimide, polyethersulfone (PES), polyphenylene sulfide, polysulfones, polyetherimide, polyether ketone imide, polyamide, fluororesin, nylon, polymethyl methacrylate, acrylics or polyarylates, and cycloolefin resins such as Arton (trade name, manufactured by JSR Corporation) or Apel (trade name, manufactured by Mitsui Chemicals, Inc.).
[0238] Examples of low ink absorbency substrates include printing papers such as art paper, coated paper, and matte paper. In this specification, the term "non-ink absorbency and low ink absorbency substrates" refers to substrates that are "non-ink absorbency and low ink absorbency substrates that are non-ink absorbent and low ink absorbent ... 1/2 Water absorption up to 10 mL / m 2 The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also adopted by the Japan Pulp and Paper Technical Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and Paperboard - Liquid Absorbency Test Method - Bristow Method" of the "JAPAN TAPPI Paper and Pulp Test Methods 2000 Edition."
[0239] (1.4.2) Inkjet Head The method for ejecting and applying the ink according to the present invention is preferably an inkjet method.
[0240] In the image forming method of the present invention, microwaves are used to dry the ink. Because microwaves have high directionality, there is no need to apply excessive atmospheric conditions (conditions due to wind, temperature, etc.) to control drying, and for example, there is no need to unnecessarily dry the nozzle part of the inkjet head, which is a part other than the ink. Therefore, excellent ink ejection properties can be maintained, and drying can be performed immediately after printing without worrying about nozzle drying.
[0241] (Water-repellent film) An ink-jet head used in an ink-jet system preferably has a water-repellent film. This water-repellent film is formed on the surface of the ink-jet head on the ink-ejecting side, and improves and maintains the ink-ejecting performance.
[0242] Here, the ink ejection performance of an inkjet head is largely influenced by the surface characteristics of the liquid ejection surface of the nozzles of the inkjet head. Therefore, ink ejection performance can be improved by generally forming a water-repellent film (also called a "liquid-repellent film" or "liquid-repellent layer") on the surface of the ink ejection surface of the nozzle to prevent liquid from adhering to the periphery of the nozzle.
[0243] The water-repellent film according to the present invention is preferably formed by applying or depositing a fluorine-based silane coupling agent. n Six 4-n In the silicon compound represented by the formula (n = 1 to 3), Y is a group containing fluorine such as a fluorinated alkyl group, and X is a group capable of bonding by condensation with a hydroxy group on the substrate surface or adsorbed water, such as a halogen, methoxy group, ethoxy group, or acetoxy group.
[0244] Specific examples include perfluorooctylethyltrimethoxysilane, perfluorooctylethyltripropoxysilane, perfluorooctylethyltriaminosilane, and perfluorooctylethyltrichlorosilane.
[0245] Methods for forming the water-repellent film of the present invention using a silane coupling agent include applying a solution of the silane coupling agent or immersing the substrate in a solution of the silane coupling agent and then drying, or spraying the silane coupling agent.
[0246] The solvent for the fluorine-based silane coupling agent may be selected from the group consisting of isopropyl alcohol, acetone, and fluorine-based alcohols such as hydrofluoroether, perfluoropolyether, hydrofluorocarbon, perfluorocarbon, hydrofluoropolyether, etc. Specific examples of the silane coupling agent that can be used include Optool manufactured by Daikin Industries, Ltd., WR4 manufactured by Merck, and FG-5080 and FG-5010 manufactured by Fluorotechnology.
[0247] The water-repellent film according to the present invention may contain a Group 4 or Group 5 element, a nitrogen element, and an oxygen element. Examples of the Group 4 element include titanium (Ti), zirconium (Zr), and hafnium (Hf). Examples of the Group 5 element include vanadium (V), niobium (Nb), and tantalum (Ta). Among these, tantalum (Ta), titanium (Ti), and zirconium (Zr) are preferred, with tantalum (Ta) being particularly preferred.
[0248] [Method for Forming Water-Repellent Film] As a method for forming a water-repellent film, for example, a thin film formation method such as a wet method or a dry method can be appropriately selected. Wet methods that can be used include spray coating, spin coating, brush coating, dip coating, and wire bar coating. Dry methods (a general term for vacuum film-forming methods) include physical vapor deposition (PVD) and chemical vapor deposition (CVD). Physical vapor deposition (PVD) methods include, for example, resistance heating vacuum deposition, electron beam heating vacuum deposition, ion plating, ion beam assisted vacuum deposition, and sputtering. Chemical vapor deposition (CVD) methods include, for example, plasma CVD, thermal CVD, metalorganic CVD, and photo-assisted CVD.
[0249] It is preferable that the water-repellent film is a vapor-deposited film from the viewpoints of adhesion between the water-repellent film and the substrate and manufacturability. In this specification, the term "vapor-deposited film" refers to a film formed by a vapor deposition method, i.e., a film formed by the above-mentioned physical vapor deposition (PVD) or chemical vapor deposition (CVD).
[0250] Plasma treatment may be performed as a pretreatment before the formation of the water-repellent film. The plasma treatment can be performed using oxygen gas, argon gas, or a mixture of these gases. Plasma treatment can remove contaminants from the surface of the primer layer or activate the surface, improving reactivity and adhesion, and enhancing alkali resistance and durability against chemical mechanical polishing.
[0251] [Contact Angle] In the present invention, the term "contact angle" quantifies the degree of wetting, and is defined as the angle between the liquid surface and the solid surface (the angle inside the liquid) where the free surface of a stationary liquid comes into contact with a solid wall.
[0252] The wettability of a liquid with respect to a solid surface (including a semi-solid state) is generally quantitatively expressed by the contact angle of the liquid. As mentioned above, inkjet heads used in inkjet systems preferably have a water-repellent film, which improves and maintains the ink ejection performance. If the ink has low wettability with respect to this water-repellent film, the ink will not wet the inkjet head and then dry, which will likely clog the nozzles.
[0253] From this perspective, if the contact angles of the first ink and the second ink with respect to the water-repellent film are within the range of 60 to 80 degrees at 25° C., the ink can be prevented from adequately repelling from the head surface and drying and adhering to the nozzle surface, resulting in ink with good ejection properties.
[0254] As an inkjet head having a water-repellent film, an independently driven inkjet head manufactured by Konica Minolta, Inc., as disclosed in JP 2018-202768 A, was used to measure the contact angle with the water-repellent film of the inkjet head. The contact angles at 25°C with the precoat liquid [P1], yellow ink [Y1], magenta ink [M1], cyan ink [C1], and black ink [K1] prepared in the examples described below were as follows:
[0255] Precoat liquid [P1]: Contact angle at 25°C is 65° Yellow ink [Y1]: Contact angle at 25°C is 75° Magenta ink [M1]: Contact angle at 25°C is 76° C Cyan ink [C1]: Contact angle at 25°C is 74° Black ink [K1]: Contact angle at 25°C is 75°
[0256] The contact angle according to the present invention was measured as follows.
[0257] The nozzle plate on which the water-repellent film was formed was peeled off from an inkjet head having the water-repellent film. The contact angle at 25°C was measured 60 ms after ink was dropped onto the water-repellent film formed on the nozzle plate. The contact angle was measured using a DM500 water contact angle meter manufactured by Kyowa Interface Science Co., Ltd.
[0258] (Circulation Mechanism) The inkjet head is provided with a nozzle circulation mechanism, which is expected to have the following effects: removal of air bubbles in the pressure chamber, prevention of settling of ink particles, reduction in the amount of ink wasted at the time of initial introduction, and prevention of decapsulation. Therefore, it is preferable from the viewpoint of ejection stability of the first ink and the second ink.
[0259] In inkjet technology, it is important to maintain a stable and good ejection state for a long period of time, and in the case of ejection failure, conventional technology requires long-term maintenance. However, the inkjet head of the present invention is equipped with a nozzle circulation mechanism, so that maintenance is not necessary.
[0260] A typical inkjet head has a structure in which a circulation flow path is provided on only one side, which can easily lead to problems such as ink being unable to be discharged due to ink stagnation on the other side, etc. In contrast, the "nozzle circulation mechanism" according to the present invention refers to a mechanism in which circulation flow paths are provided on both ends of the ink channel, one of which is used for discharging ink.
[0261] In an inkjet head equipped with the nozzle circulation mechanism of the present invention, ink is constantly discharged from a circulation flow path that is connected to the ink channel, thereby refreshing the ink in the ink channel and nozzle, and making it possible to suppress ejection failures due to particle settling, drying of ink in the nozzle, and air bubbles.
[0262] The inkjet head comprises at least one pressure chamber into which ink is injected, pressure generating means for generating pressure fluctuations in the pressure chamber, a nozzle that communicates with the pressure chamber and serves as a flow path for ink that is ejected from the pressure chamber to the outside due to the pressure fluctuations in the pressure chamber, and a circulation path that communicates with the pressure chamber and discharges ink that is inside the nozzle and returns it to the injection path to the pressure chamber, and it is more preferable from the viewpoint of ejection stability of the first ink and the second ink to have two or more circulation paths, as this further improves the performance of the nozzle circulation mechanism described above.
[0263] Fig. 2 is a cross-sectional view conceptually showing the maintenance operation of the circulation type inkjet head H, and shows the maintenance operation of controlling the ink discharge pressure by a return pressure control pump (not shown). In Fig. 2, 121 represents the nozzle plate, 122 the nozzle, 123 the ink channel (pressure chamber), 126a the individual ink circulation path, and 126b the common ink circulation path. Also, h represents a groove, and 1S represents the ink ejection surface.
[0264] Individual ink circulation paths 126a are connected to the ink channels (pressure chambers) 123. The individual ink circulation paths 126a connected to the ink channels (pressure chambers) 123 are joined by connecting to a common ink circulation path 126b. The pressure difference between the ink channels (pressure chambers) 123 and the common ink circulation path 126b causes ink to flow from the ink channels (pressure chambers) 123 to the common ink circulation path 126b.
[0265] Although not shown, the partition between the ink channel (pressure chamber) 123 and the dummy channel (not shown) is composed of a pair of piezoelectric elements. The piezoelectric elements undergo shear deformation when a voltage is applied from a power supply circuit (not shown) via the wiring patterns of the FPC board and the wiring board. The shear deformation of the piezoelectric elements that form both walls of the ink channel (pressure chamber) 123 causes pressure fluctuations in the ink channel (pressure chamber) 123 (reduced pressure due to expansion or increased pressure due to contraction). The pressure fluctuations (reduced pressure or increased pressure) in the ink channel (pressure chamber) 123 apply pressure to the ink inside the nozzle 122, i.e., inside the ink channel (pressure chamber) 123, and this ink is ejected through the nozzle 122.
[0266] In this maintenance operation, the return pressure control pump generates a negative pressure greater than the meniscus break head value, increasing the ink discharge pressure and drawing all of the ink remaining in the nozzle 122 into the ink channel (pressure chamber) 123, as shown in Figure 2A. At this time, the meniscus of the ink remaining in the nozzle 122 is broken and the ink is moved into the ink channel (pressure chamber) 123, emptying the nozzle 122. At this time, outside air is often drawn into the ink channel (pressure chamber) 123 from the nozzle 122 as air bubbles together with the ink.
[0267] The meniscus (curved interface) formed by the ink inside the nozzle 122 is usually fixed at its outer periphery to the periphery (edge) on the outlet side of the nozzle 122. Therefore, destruction of the meniscus means that the outer periphery of the meniscus becomes separated from the periphery on the outlet side of the nozzle 122. When the meniscus is destroyed in this way, its shape is often not maintained as a smooth curved surface, and at this time, outside air is drawn in as bubbles.
[0268] Thereafter, when the ink ejection pressure is returned to its normal strength, the meniscus formed by the ink in the nozzle 122 returns to its original state, as shown in Fig. 2B. When the meniscus returns in this manner, the ink that had been remaining in the nozzle 122 has been sufficiently replaced by new ink in the ink channel (pressure chamber) 123.
[0269] If a state in which ink is not being ejected onto the recording medium (non-printing state) continues, a maintenance operation is repeatedly performed at a predetermined regular interval. By repeatedly performing the maintenance operation at a predetermined regular interval, settling of ink particles in the nozzles 122 and an increase in ink viscosity are prevented.
[0270] By performing the above-described maintenance operation, either one or both of the ink injection pressure and the ink discharge pressure are controlled, the meniscus formed by the ink remaining in the nozzle 122 is destroyed, the ink is moved to the area surrounding the ejection side outlet of the nozzle 122 or inward from the nozzle 122 (inside the pressure chamber 123), and then the meniscus is restored, and at least a portion of the ink remaining in the nozzle 122 is replaced with ink inward from the nozzle 122 (inside the pressure chamber 123).
[0271] As an example of such an inkjet head, the inkjet head disclosed in JP-A-2018-202768 can be mentioned, and can be suitably used in the image forming method of the present invention.
[0272] 2. Image Forming System The image forming system of the present invention is an image forming system having an ink coating means and a drying means, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating means is a means for ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying means is a means for drying a coating film by irradiating with microwaves, and wherein when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates when the first ink and the second ink are dried at 80°C for 20 seconds are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1
[0273] The ink application means according to the present invention is not particularly limited, and any conventionally known application device capable of applying the first ink and the second ink described in the image forming method can be used.
[0274] Furthermore, there are no particular limitations on the means for drying the ink according to the present invention, and any conventionally known drying device capable of realizing the drying method described in the image forming method can be used.
[0275] 3. Recording Apparatus A recording apparatus that can be used in the image forming method and image forming system of the present invention is a recording apparatus that has an ink applying means and a drying means, and may have a precoat liquid applying means in front of the ink applying means.
[0276] 1 is a schematic diagram of an example of a recording apparatus that is preferred for the present invention, although the present invention is not limited to this example.
[0277] (3.1) Configuration of the Recording Apparatus The recording apparatus 1 is mainly composed of a precoat liquid application unit 10, an ink application unit 20, and an ink drying unit 30.
[0278] In the recording apparatus 1 of FIG. 1, for example, in a precoat liquid application section 10, a precoat liquid 12 is applied as needed by an inkjet head Hp onto a substrate F fed from a feed roller 40.
[0279] Next, in the ink application section 20, the ink is applied onto the precoat liquid 12 or the substrate F by the inkjet head H Y , H M , H C The first ink 21 is applied from the inkjet head H W , H K and H Ag The second ink 22 is applied from the first ink 22 .
[0280] Then, in the ink drying section 30, the area where the precoat liquid 12, the first ink 21, and the second ink 22 have been applied is heated and dried by irradiating at least microwaves using a drying device 35, thereby controlling the drying property uniformly and performing image recording.
[0281] Thereafter, the substrate F on which the image has been recorded as described above is wound up by the winding roller 41 to obtain an image-recorded product.
[0282] Although FIG. 1 shows a case where the substrate F is a film substrate, in the case of a metal substrate or the like, the metal substrate can be placed on a conveyor belt, and the above-mentioned precoat liquid 12, first ink 21, and second ink 22 can be applied in one pass while conveying the belt, thereby forming a mixed coating film before drying.
[0283] In the present invention, since there may be cases where the precoat liquid 12 is not applied, the above-mentioned precoat liquid application section 10 can be omitted, but the following explanation will be given assuming that the precoat liquid application section 10 is present.
[0284] (3.2) Precoat Liquid Application Portion As the precoat liquid 12, the precoat liquid explained in the image forming method can be used.
[0285] In the image recording procedure, first, in a precoat liquid application section 10, a precoat liquid 12 is applied onto a substrate F. At this time, if necessary, the coating film of the precoat liquid formed in the area where the precoat liquid 12 has been applied may be partially dried.
[0286] The method of applying the precoat liquid in the precoat liquid application unit 10 is not particularly limited as long as it is configured to be able to apply the precoat liquid 12 to the substrate, and may be a roll coater method using a bar coater, etc., but an inkjet method using an inkjet head Hp is preferred from the perspective of drying control.
[0287] (3.3) Ink Coated Portion As described above, the ink according to the present invention varies in type depending on the purpose, with respect to the content ratio of pigment, resin, water, water-soluble solvent, and surfactant, and the complex dielectric constant of each ink in the later stage of drying, i.e., the complex dielectric constant of each ink at a drying rate of 95% in the present invention, varies.
[0288] Therefore, the ink (first ink) having a relatively small complex dielectric constant in the later stage of drying compared to the other inks is more excellent in uniform drying control when the drying rate of the ink is relatively high.Furthermore, the ink (second ink) having a relatively large complex dielectric constant in the later stage of drying compared to the first ink is more excellent in uniform drying control when the drying rate of the ink is relatively low.
[0289] In the present invention, a plurality of inks having different components, contents, etc. are used as described above, but when focusing on two types of ink, for example, one ink is designated as the first ink and the other as the second ink. The first ink and the second ink are characterized in that their complex dielectric constants and drying rates in the later stage of drying are relatively different, as described above.
[0290] The first ink and the second ink may be applied not only to the same location on the substrate, but also to different locations.
[0291] In FIG. 1, the ink application unit 20 applies the first ink 21 and the second ink 22 using an inkjet head H Y , H M , HC , H W , H K and H Ag It is an inkjet method using an inkjet head H Y Yellow ink, inkjet head H M magenta ink, inkjet head H C From cyan ink, inkjet head H W White ink, inkjet head H K From black ink, inkjet head H Ag The ink containing silver nanoparticles is ejected from the nozzle.
[0292] In addition, in Figure 1, the precoat liquid 12 is applied to the substrate F before the first ink 21 and the second ink 22, but the first ink and the second ink may be applied to the substrate F before the precoat liquid in a configuration other than that shown in Figure 1.
[0293] In the ink application section 20, the first ink 21 and the second ink 22 are applied to a desired area on the substrate F, or the first ink 21 and the second ink 22 are applied to a desired area on the precoat liquid 12.
[0294] There may be a plurality of first inks 21 and second inks 22, and either may be applied first, but the first ink 21 or the second ink 22 is applied immediately after the application of the first ink 21 or the second ink 22. In this case, the substrate F may have regions where the precoat liquid 12, the first ink 21, and the second ink 22 are applied individually, and regions where they are mixed and applied in different combinations.
[0295] In the ink application unit 20, various combinations of yellow ink, magenta ink, cyan ink, white ink, black ink, and ink containing silver nanoparticles are applied, and then dried all at once in the ink drying unit described below. At this time, the first ink and the second ink are determined based on the relative relationships between the complex dielectric constants and drying rates of these inks.
[0296] For example, when yellow ink, magenta ink, cyan ink, and black ink are applied in the ink application unit 20, the yellow ink, magenta ink, and cyan ink become the first inks, and the black ink becomes the second ink. When yellow ink, magenta ink, cyan ink, and white ink are applied, the yellow ink, magenta ink, and cyan ink become the first inks, and the white ink becomes the second ink. When white ink and black ink are applied, the white ink becomes the first ink, and the black ink becomes the second ink.
[0297] For example, when yellow ink, magenta ink, cyan ink, and black ink are applied in the ink application section 20, the inks are the first inks and the inks are the second inks.
[0298] (3.4) Ink Drying Section In the ink drying section 30, the precoat liquid, the first ink, and the second ink applied to the substrate are dried by a drying device 35. There are no particular limitations on the drying device 35 as long as it is an apparatus that can realize the drying method described in the image forming method described above. In the present invention, the drying device 35 dries the coating film formed by the precoat liquid, the first ink, and the second ink by irradiating at least microwaves.
[0299] (3.5) Others Furthermore, as an apparatus other than the recording apparatus shown in Fig. 1, a flatbed type printer may also be preferably used to apply the precoat liquid 12, the first ink 21, and the second ink 22. In a flatbed type printer, the substrate is fixed, and the inkjet head can be moved in the main scanning direction and the sub-scanning direction that intersects with the main scanning direction, and printing can be performed without transporting the substrate.
[0300] For metal substrates such as tinplate, roll-to-roll transport is not possible as with resin film substrates, so it is preferable to use a flatbed printer that does not require transporting the substrate. Examples of such flatbed printers include the printers shown in FIG. 1 of JP-A-2015-74161 and FIG. 1 of JP-A-2017-177578.
[0301] The inkjet head may be either an on-demand type or a continuous type. Examples of on-demand type inkjet heads include electro-mechanical conversion type inkjet heads, such as single-cavity type, double-cavity type, bender type, piston type, shear mode type, and shared wall type inkjet heads, and electro-thermal conversion type inkjet heads, such as thermal inkjet type and bubble jet type inkjet heads ("Bubble Jet" is a registered trademark of Canon Inc.).
[0302] Among the above ink jet heads, ink jet heads using a piezoelectric element as the electromechanical conversion element used in the electromechanical conversion system (also called piezo type ink jet heads) are preferred.
[0303] The inkjet printer may be of either a scan type or a single pass type, but in the case of a single pass type, it is preferable to use a line head type inkjet head.
[0304] A line head type inkjet head is an inkjet head having a length equal to or greater than the width of the printing range (including the application range of the precoat liquid). As a line head type inkjet head, a single head having a width equal to or greater than the printing range (including the application range of the precoat liquid) may be used, or multiple heads may be combined to form a configuration having a width equal to or greater than the printing range (including the application range of the precoat liquid). Furthermore, multiple heads may be arranged side by side with their nozzles in a staggered arrangement to increase the overall resolution of these heads.
[0305] The transport speed of the recording medium, which is the substrate, can be set within a range of, for example, 1 to 120 m / min. The faster the transport speed, the faster the image formation speed.
[0306] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. In the examples, the terms "parts" and "%" are used, but unless otherwise specified, they represent "parts by mass" or "% by mass."
[0307] A. Preparation of Precoat Solution (A.1) Preparation of Precoat Solution [P1] 3.00% by mass of calcium acetate monohydrate as a flocculant, 12.00% by mass of dipropylene glycol (DPG) and 20.00% by mass of propylene glycol (PG) (1,2-HDO) as solvents, 1.00% by mass of "TEGOWET-KL245" (polyether-modified siloxane copolymer; manufactured by Evonik) as a surfactant, 0.10% by mass of "Proxel GXL(S)" (1,2-benzisothiazolin-3-one; manufactured by Daiwa Chemical Industry Co., Ltd.) as an antifungal agent, and ion-exchanged water (the balance; the total amount was 100% by mass) were added with stirring, and the resulting mixture was filtered through a 1 μm filter to prepare precoat solution [P1]. The formulation of precoat solution [P1] is summarized in Table I below. The abbreviations in Table I are as follows:
[0308]
[0309] <Abbreviations> (Flocculant) "Calcium acetate": calcium acetate monohydrate (Solvent) "DPG": dipropylene glycol "PG": propylene glycol (Surfactant) "KL245": TEGOWET-KL245 (polyether-modified siloxane copolymer; manufactured by Evonik) (Antifungal agent) "Proxel GXL": "Proxel GXL(S)" (1,2-benzisothiazolin-3-one; manufactured by Daiwa Chemical Industry Co., Ltd.)
[0310] B. Preparation of pigment dispersions to be contained in each ink (B.1) Preparation of white pigment dispersion [W] A mixed liquid was premixed by adding 40% by mass of white pigment (titanium oxide CR-50-2; manufactured by Ishihara Sangyo Kaisha) as the pigment, 4% by mass of "Joncryl 819" (anionic polymer dispersant, acrylic dispersant having a carboxy group neutralized with dimethylaminoethanol, acid value 75 mg KOH / g, solids content 20% by mass; manufactured by BASF) and 4% by mass of "Disperbyk-2019" (solvent-free wetting dispersant; manufactured by BYK-Chemie) as pigment dispersants, 20% by mass of propylene glycol (PG) as a solvent, 0.1% by mass of 1,2-benzisothiazolin-3-one (Proxel GXL(S)) as an antifungal agent, and ion-exchanged water (the remainder; an amount that made the total amount 100% by mass).
[0311] Thereafter, the mixture was dispersed using a bead mill filled with 0.3 mm zirconia beads at a volume ratio of 50% to prepare a white pigment dispersion [W] having a pigment content of 20% by mass.
[0312] The average particle size of the pigment particles contained in this pigment dispersion was 250 nm, and the average particle size was measured using a Zetasizer Nano S-90 manufactured by Maruballoon Co., Ltd.
[0313] (B.2) Preparation of Magenta Pigment Dispersion [M] A magenta pigment dispersion [M] having a pigment content of 20% by mass was prepared in the same manner as for the white pigment dispersion [W], except that the type of pigment was changed to a magenta pigment (a mixed crystal of Pigment Red 122 and Pigment Violet 19) and that only "Joncryl 819" was added in an amount of 8% by mass as the pigment dispersant.
[0314] The average particle size of the pigment particles contained in this pigment dispersion was 250 nm, and the average particle size was measured using a Zetasizer Nano S-90 manufactured by Maruballoon Co., Ltd.
[0315] (B.3) Preparation of Yellow Pigment Dispersion [Y], Cyan Pigment Dispersion [C], and Black Pigment Dispersion [K] Yellow pigment dispersion [Y], cyan pigment dispersion [C], and black pigment dispersion [K], each having a pigment content of 20% by mass, were prepared in the same manner as in the preparation of Magenta Pigment Dispersion [M], except that the magenta pigment was changed to a yellow pigment (Pigment Yellow 150; manufactured by Lanxess K.K.), a cyan pigment (Pigment Blue 15; manufactured by Tokyo Chemical Industry Co., Ltd.), or a black pigment (Pigment Black 7; manufactured by Mitsubishi Chemical Corporation), respectively.
[0316] The average particle size of the pigment particles contained in these pigment dispersions was all 250 nm. The average particle size was measured using a Zetasizer Nano S-90 manufactured by Maruballoon Co., Ltd.
[0317] (B.4) Preparation of Silver Nanoparticle Pigment Dispersion [Ag] A silver nanoparticle pigment dispersion ("Picosil R" manufactured by Daicel Corporation) was adjusted with water to prepare a silver nanoparticle dispersion [Ag] having a pigment content of 20 mass %.
[0318] C. Preparation of Ink (C.1) Preparation of White Ink A white ink was prepared using 40.00% by mass of white pigment dispersion [W] as the pigment dispersion, 5.00% by mass (solids content equivalent) of PLASCOAT Z-446 (manufactured by GOO Chemical Industry Co., Ltd.) as the resin particle dispersion, 15.00% by mass of propylene glycol (PG) as the water-soluble solvent, 10.00% by mass of dipropylene glycol (DPG) as the humectant, 1.00% by mass of "TEGOWET-KL245" (polyether-modified siloxane copolymer; manufactured by Evonik) as the surfactant, 0.05% by mass of silicone-modified surfactant KF-351A (manufactured by Shin-Etsu Silicones Co., Ltd.) as the antifungal agent, and "Proxel": "Proxel GXL(S)" (1,2-benzisothiazolin-3-one) as the antifungal agent. 0.10% by mass of acrylic acid acrylate (manufactured by Daiwa Kasei Co., Ltd.) and ion-exchanged water (the remainder; an amount such that the total amount was 100% by mass) were added with stirring, and the resulting mixture was filtered through a 1 μm filter to prepare a white ink [W1].
[0319] There was no substantial change in composition before and after filtration.
[0320] (C.2) Preparation of Yellow, Magenta, Cyan, and Black Inks Yellow ink [Y1], magenta inks [M1] to [M8], cyan ink [C1], and black inks [K1] to [K20] were prepared in the same manner as white ink [W1], except that the pigment dispersion, resin particle dispersion, water-soluble solvent, humectant, type of surfactant, type and amount of antifungal agent, and water were changed as shown in Tables II and III.
[0321] (C.3) Preparation of Silver Nanoparticle-Containing Ink To 20.00% by mass of a silver nanoparticle pigment dispersion [Ag] as a pigment dispersion, 15.00% by mass of propylene glycol (PG) as a water-soluble solvent, 10.00% by mass of dipropylene glycol (DPG) as a humectant, 1.00% by mass of "TEGOWET-KL245" (polyether-modified siloxane copolymer; manufactured by Evonik) as a surfactant, 0.10% by mass of "Proxel": "Proxel GXL(S)" (1,2-benzisothiazolin-3-one; manufactured by Daiwa Chemical Industry Co., Ltd.) as an antifungal agent, and ion-exchanged water (the balance; the total amount was 100% by mass) were added with stirring, and the resulting mixture was filtered through a 1 μm filter to prepare a silver nanoparticle-containing ink [Ag1]. There was no substantial change in composition before and after filtration.
[0322] Table II shows the contents (mass %) of the pigment dispersion, resin, water-soluble solvent, humectant, surfactant, preservative, and water in the ink. PLASCOAT Z-446 (manufactured by GOO Chemical Industry Co., Ltd.) was added as the resin particle dispersion. The "pigment amount" values in Table II are the amounts added in solid content terms. For example, in the case of yellow ink [Y1], 20% by mass of yellow pigment dispersion [Y] with a solid content of 20% by mass was added, resulting in a pigment content of 4% by mass in solid content terms, and this value is listed. The value for resin Z-446 is the amount added in solid content terms. The abbreviations in Table II are as follows:
[0323]
[0324] <Abbreviations> (Resin particle dispersion) "Z-446": Plascoat Z-446 (manufactured by GOO Chemical Industry Co., Ltd.) (Water-soluble solvent) "PG": Propylene glycol "HexDo": 1,2-hexanediol "DEGBE": Diethylene glycol monobutyl ether (Humectant) "DPG": Dipropylene glycol "PenDO": 1,2-pentanediol "Gly": Glycerin "PDO": 1,3-propanediol (Surfactant) "KL245": TEGOWET-KL245 (Polyether-modified siloxane copolymer; manufactured by Evonik) "SF-8428": SF-8428 (Carbinol-modified silicone; manufactured by Dow-Toray) "E1010": Olfine E1010 (Acetylene glycol; manufactured by Nissin Chemical Industry Co., Ltd.) (Antifungal agent) "Proxel GXL": Proxel GXL(S) (1,2-benzisothiazolin-3-one; manufactured by Daiwa Chemical Industry Co., Ltd.)
[0325] D. Complex dielectric constants and boiling points of water, water-soluble solvents, and humectants The complex dielectric constants and boiling points of water, water-soluble solvents, and humectants are shown in Table III.
[0326]
[0327] E. Measurement of drying rate and complex dielectric constant of each ink (E.1) Complex dielectric constant The ink was applied to separate locations on a PET substrate (FE2001, manufactured by Futamura Chemical Co., Ltd.) using a wire bar at an amount of 13 g / m 2 and dried in a hot air oven at 80° C. for 3 minutes to prepare a sample for measuring the complex dielectric constant of each ink.
[0328] The measurement of the drying rate and complex dielectric constant of the ink will be explained using the yellow ink [Y1] as an example.
[0329] Yellow ink [Y1] was applied to a PET substrate (mass: 0.168 g) cut to 10 cm x 10 cm with a wire bar at a coating amount of 13 g / m 2 A sample [Y1] was obtained.
[0330] Immediately afterwards, the mass of sample [Y1] was measured using an electronic balance and found to be 0.298 g, which was taken as the "mass before drying" of sample [Y1].
[0331] Sample [Y1] was dried in a hot air oven at 80°C for 3 minutes, and then the mass was measured again using an electronic balance, and 0.187 g was taken as the "mass after drying" of sample [Y1].
[0332] Therefore, the mass of the yellow ink [Y1] evaporated by drying is the above-mentioned "mass before drying" - "mass after drying".
[0333] The yellow ink [Y1] was applied in an amount of 13 g / m onto a PET substrate cut to 10 cm x 10 cm. 2 Therefore, the total mass of the yellow ink [Y1] is 13×0.01=0.130 g.
[0334] Since 89.9% of the yellow ink [Y1] is solvent, the total mass of the solvent in the yellow ink [Y1] is 0.130×0.899=0.117 g.
[0335] When this was substituted into the following formula, the drying rate was calculated to be 95%.
[0336] Drying rate [%] = (mass before drying - mass after drying) / total mass of solvents in ink × 100
[0337] The complex dielectric constant of the sample [Y1] was measured at a drying rate of 95% for the yellow ink [Y1] using a material impedance analyzer MIA-5M (SH2-Z type 4-terminal sample holder) manufactured by Toyo Corporation. The measurement results of the complex dielectric constant are shown in Table IV.
[0338] (E.2) Drying rate: The first ink and the second ink were applied to separate locations on a PET substrate (FE2001, manufactured by Futamura Chemical Co., Ltd.) using a wire bar at a coating amount of 13 g / m. 2 The ink was applied to a substrate at a rate of 1000 ppm and dried for 20 seconds in a hot air oven at 80°C to prepare a sample for measuring the drying rate of each ink. The results of the drying rate measurements are shown in Table V.
[0339] The drying rate when the first ink and the second ink were dried at 80° C. for 20 seconds was calculated using the following formula.
[0340] Drying rate [%] = (mass before drying - mass after drying) / total mass of solvent in ink × 100
[0341]
[0342] F. Image formation preparation 1 Preparation for image formation was carried out using a recording apparatus configured as shown in Figure 1. The substrate was conveyed in the direction D in Figure 1, the conveyance speed was set to 300 mm / sec, and the recording medium F was a PP substrate ("#20 FOR" manufactured by Futamura Chemical Co., Ltd.).
[0343] Five independently driven inkjet heads (360 npi, ejection volume 6 pL or 14 pL, 1024 nozzles) manufactured by Konica Minolta Inc. (JP 2018-202768 A) (H W , H Y , H M , H C , H K In addition to the scanning printer equipped with the inkjet head H for ink containing metal nanoparticles, Ag A scan type printer with a total of six inkjet heads was prepared. In addition, an inkjet head H was used for applying the precoat liquid. P The nozzle plate provided in each inkjet head had a water-repellent film.
[0344] (Preparation for Image Formation in Example 1) The inkjet head (H M ) with magenta ink [M1], and inkjet head (H K ) was filled with black ink [K1].
[0345] (Preparation for Image Formation in Examples 2 to 21 and Comparative Examples 1 and 2) Ink jet heads suitable for each ink used in the ink application section 20 were filled with inks in the combinations shown in Table V.
[0346] (Preparation for Image Formation in Example 22) Inkjet head H used in the precoat liquid application unit 10 P The inkjet head (H M ) magenta ink [M3], inkjet head (H K ) was filled with black ink [K8].
[0347] G. Image Formation Preparation 2 Image formation preparation was performed using the recording apparatus configuration shown in Figure 1. The same preparation as in Image Formation Preparation 1 was performed, but unlike Image Formation Preparation 1, drying was performed using not only microwave irradiation in the drying device 35 but also hot air and an infrared heater.
[0348] (Preparation for Image Formation in Example 23) The inkjet head (H M ) magenta ink [M3], inkjet head (H K ) was filled with black ink [K8].
[0349] (Preparation for Image Formation in Examples 24 and 25) Ink jet heads suitable for each ink used in the ink application section 20 were filled with inks in the combinations shown in Table V.
[0350] (Preparation for Image Formation in Comparative Example 3) The inkjet head (H M ) and inkjet head (H K ) was filled with the same ink as in Example 23.
[0351] (Preparation for Image Formation in Comparative Example 4) The inkjet head (H M ) and inkjet head (H K ) was filled with the same ink as in Example 23.
[0352] (Preparation for Image Formation in Comparative Example 5) The inkjet head (H M ) and inkjet head (H K ) was filled with the same ink as in Example 23.
[0353] (Preparation for Image Formation in Comparative Example 6) In the ink application section 20, an inkjet head (H M ) with magenta ink [M8], inkjet head (H K ) was filled with black ink [K20].
[0354] H. Image Formation and Various Evaluations (Formation of Evaluation Images) Images were formed using a recording apparatus having the configuration shown in FIG.
[0355] <Image Forming Method 1 (Image Formation in Examples 1 to 21 and Comparative Examples 1 and 2)> A PP substrate ("#20 FOR" manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the precoat liquid application section 10, no special treatment was performed, and in the ink application section 20, each ink was applied from each inkjet head in the combinations shown in Table V at an application amount of 13 g / m. 2 A solid image was printed, and the image formation patterns shown in FIGS. 3 and 4 were printed.
[0356] Both the image patterns in Figures 3 and 4 are mainly composed of yellow solid area y, magenta solid area m, cyan solid area c, black solid area k, red solid area r, green solid area g, and blue solid area b.
[0357] The primary color solid areas, namely, yellow solid area y, magenta solid area m, cyan solid area c, and black solid area k, were formed by applying only yellow ink, magenta ink, cyan ink, and black ink, respectively.
[0358] The secondary color solid areas, red solid area r, green solid area g, and blue solid area b, were each formed by applying two types of ink in layers. The red solid area r was formed by applying yellow ink and magenta ink in layers. The green solid area g was formed by applying yellow ink and cyan ink in layers. The blue solid area b was formed by applying magenta ink and cyan ink in layers.
[0359] Figure 3 shows an image pattern composed of the above-mentioned solid color areas, where the solid color areas are adjacent to each other and where outline characters (4 pt, 6 pt, 8 pt) are drawn. In either recording method, the amount of ink applied in the image based on Figure 3 is 13 g / m for the primary color solid areas y, m, c, and k. 2 , 13.0 g / m for the secondary color solid areas r, g, b 2 It was decided.
[0360] Figure 4 shows an image pattern in which each of the solid color areas is individually printed. In either printing method, the amount of ink applied in the image based on Figure 4 is 13 g / m for the primary color solid areas y, m, c, and k. 2 , 13.0 g / m for the secondary color solid areas r, g, b 2 It was decided.
[0361] The white ink and the ink containing silver nanoparticles were printed in the same areas as the black ink (k) in FIG.
[0362] Thereafter, in the ink drying section 30, microwave treatment was performed in the drying device 35 to dry the ink and form an image for evaluation. Note that a microwave generator (ESG-2450S-2A, manufactured by Shimada Rika Kogyo Co., Ltd.) was used as the drying device, and the ink was dried by irradiating it with microwaves (oscillation frequency: 2.45 GHz, output: 100 W) for 3 seconds.
[0363] <Image Forming Method 2 (Image Formation in Example 22)> A PP substrate (#20 FOR, manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the coating section 10 of the precoat liquid, an inkjet head H P Coating amount: 4g / m 2 In the ink application section 20 and the ink drying section 30, an image for evaluation was formed in the same procedure as in image forming method 1.
[0364] <Image Forming Method 3 (Image Formation of Examples 23 to 25)> A PP substrate ("#20 FOR" manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the precoat liquid application section 10, nothing in particular was done, and in the ink application section 20, a solid image was printed using the same procedure as in Image Forming Method 1. Thereafter, in the ink drying section 30, microwave treatment and hot air treatment were simultaneously performed in the drying device 35 to dry the ink, thereby forming an image for evaluation. In the drying device 35, microwave treatment (oscillation frequency: 2.45 GHz, output: 100 W) and hot air treatment (temperature: 100°C, air speed: 16 m / sec) were performed for 3 seconds.
[0365] <Image Forming Method 4 (Image Formation of Comparative Examples 3 and 6)> A PP substrate ("#20 FOR", manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the precoat liquid application section 10, nothing in particular was done, and in the ink application section 20, a solid image was printed using the same procedure as in Image Forming Method 1. Thereafter, in the ink drying section 30, only hot air treatment (at a temperature of 70°C and an air velocity of 16 m / sec) was performed for 3 seconds in the drying device 35 to dry the image, forming an image for evaluation.
[0366] <Image Forming Method 5 (Image Formation of Comparative Example 4)> A PP substrate ("#20 FOR" manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the precoat liquid application section 10, nothing in particular was done, and in the ink application section 20, a solid image was printed in the same procedure as in Image Forming Method 1. Thereafter, in the ink drying section 30, neither microwave treatment nor hot air treatment was performed in the drying device 35, and only treatment with an infrared heater was performed for 3 seconds to dry the image for evaluation, forming an image for evaluation. The treatment with the infrared heater in the drying device was performed using a medium wavelength infrared heater of 100 kW / m manufactured by Heraeus. 2 The measurement was carried out under the condition that the gap between the substrate and the sheet was 20 mm.
[0367] <Image Forming Method 6 (Image Formation of Comparative Example 5)> A PP substrate ("#20 FOR" manufactured by Futamura Chemical Co., Ltd.) was used as the substrate. In the precoat liquid application section 10, nothing special was done, and in the ink application section 20, a solid image was printed in the same procedure as in Image Forming Method 1. Thereafter, in the ink drying section 30, hot air treatment and treatment with an infrared heater were simultaneously carried out in the drying device 35 to dry the ink, thereby forming an image for evaluation. In the drying device 35, hot air treatment (temperature 100°C, air speed 16 m / sec) and treatment with an infrared heater (medium wavelength infrared heater 100 kW / m manufactured by Heraeus) were carried out. 2 The adhesive was applied for 3 seconds with the gap between the adhesive and the substrate being 20 mm.
[0368] (H.1) Drying Property (Evaluation Method) The evaluation method was to evaluate the drying property of an image formed as an evaluation image in each Example and Comparative Example, as shown in Figure 3, by rubbing the solid area of the corresponding color 10 times with Asahi Kasei Bemcot AZ-8. Evaluation was made according to the following evaluation criteria, with results A and B being deemed practical, and C being deemed problematic for practical use. The evaluation results are shown in Table V.
[0369] (Evaluation criteria) A: No fading on the print sample for both of the relevant colors. B: The surface of the print sample for both of the relevant colors is slightly fading, reducing gloss, and there is no color transfer to the Bemcot. C: One of the relevant colors is fading and coming off. Color transfer to the Bemcot occurs.
[0370] (H.2) Substrate Damage (Evaluation Method) Images like those shown in Figure 3 were used for evaluating substrate damage. The samples were visually inspected to determine whether there was any deformation or shrinkage of the substrate, and evaluated according to the following evaluation criteria. Results of A were deemed usable, and results of C were deemed problematic for practical use. The evaluation results are shown in Table V.
[0371] (Evaluation criteria) A: No damage to the substrate. No waviness when laid flat. C: The substrate is significantly deformed in one of the colors. Waviness is present when laid flat.
[0372] (H.3) Ejectability (Evaluation method) An image like the one shown in Figure 3 was printed continuously for 30 minutes, and then left to stand for 5 minutes, repeating this process three times. The final solid image from the third print was visually observed and evaluated for ejectability according to the following evaluation criteria. Results A and B were deemed to be suitable for practical use, and C was deemed to be problematic for practical use. The evaluation results are shown in Table V.
[0373] (Evaluation criteria) A: No chips or bends (white spots). B: One chip or bend or less. C: Many chips or bends.
[0374] (H.4) Image Quality (Evaluation Method) Images such as those shown in Figures 3 and 4 were printed, and the solid image patterns were visually observed to evaluate the graininess of the images. White ink and silver nanoparticle ink were printed in the place of the K ink and evaluated according to the following evaluation criteria. The silver nanoparticle ink used was "TEC-PA-010" (manufactured by InkTec).
[0375] (Evaluation Criteria) A: The dots are uniform and there is no graininess even in the light density areas of the solid areas. B: There is no graininess in the dark density areas of the solid areas, but there is some graininess in the light density areas. C: There is a strong graininess overall.
[0376]
[0377] I. Summary As can be seen from Table V above, there were no examples rated C (problems in practical use), and the examples were generally superior to the comparative examples, achieving both high-speed ink drying and ejection stability, and forming high-quality images without damaging the substrate.
[0378] It is possible to provide an image forming method and an image forming system that can achieve both high-speed drying of ink and ejection stability, and that does not damage the substrate.
[0379] REFERENCE SIGNS LIST 1 Recording device 10 Precoat liquid application section 12 Precoat liquid 20 Ink application section 21 First ink 22 Second ink 30 Ink drying section 35 Drying device 40 Delivery roller 41 Take-up roller 121 Nozzle plate 122 Nozzle 123 Ink channel (pressure chamber) 126a Individual ink circulation path 126b Common ink circulation path F Substrate, recording medium D Transport direction of substrate H Circulation type inkjet head H w , H Y , H M , H C , H K Inkjet head for ink application H P Inkjet head for applying pre-coat liquid H Ag Inkjet head for applying ink containing metal nanoparticles 1S Ink ejection surface h Groove
Claims
1. An image forming method having an ink coating step and a drying step, wherein the ink contains at least one or more of a pigment, inorganic particles, organic particles, and a resin, as well as water and a water-soluble solvent, the ink coating step is a step of ejecting and coating at least a first ink and a second ink onto a substrate, and at least one of the drying steps is a step of drying a coating film by irradiating with microwaves, wherein when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, the ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates of the first ink and the second ink when dried for 20 seconds at 80°C are D1 and D2, respectively, the D1 and D2 satisfy the following formula (2): Formula (2): D2<D1.
2. The image forming method according to claim 1, wherein the complex dielectric constant ε''1 of the first ink and the complex dielectric constant ε''2 of the second ink satisfy the following formula (3): (ε''2 / ε''1)<20.
3. The image forming method according to claim 1, wherein the water-soluble solvent contains a humectant having a boiling point of 200°C or higher, the content of the humectant is within the range of 3 to 20% by mass relative to the first ink or the second ink, and the complex dielectric constant ε'' at 25°C when the first ink or the second ink is irradiated with microwaves at a frequency of 2.45 GHz is within the range of 13 to 60.
0.
4. The image forming method according to claim 3, wherein the content of the moisturizing agent is greater in the second ink than in the first ink.
5. The image forming method according to claim 1, wherein the ink contains a surfactant having a hydroxyl group.
6. The image forming method according to claim 1, wherein the ink contains a surfactant having a diol structure.
7. The image forming method according to claim 1, wherein the substrate is a resin film.
8. The image forming method according to claim 1, characterized in that in the ink application step, an inkjet head having a water-repellent film is used, and the contact angles of the first ink and the second ink with respect to the water-repellent film are within the range of 60 to 80 at 25°C.
9. The image forming method according to claim 1, further comprising a step of applying a precoat liquid prior to the step of applying the ink.
10. The image forming method according to claim 8, wherein the ink-jet head is provided with a nozzle circulation mechanism.
11. The image forming method according to claim 10, characterized in that the inkjet head comprises: at least one pressure chamber into which ink is injected; a pressure generating means for generating pressure fluctuations in the pressure chamber; a nozzle communicating with the pressure chamber and serving as a flow path for ink ejected from the pressure chamber to the outside due to the pressure fluctuations in the pressure chamber; and a circulation path communicating with the pressure chamber and discharging ink inside the nozzle and returning it to an injection path into the pressure chamber, wherein there are two or more circulation paths.
12. The image forming method according to claim 1, characterized in that in the drying step using microwave irradiation, the coated materials of the first ink and the second ink are dried by applying air at a temperature of 100° C. or less.
13. An image forming system having an ink application means and a drying means, wherein the ink contains at least one or more of pigment, inorganic particles, organic particles, and resin, as well as water and a water-soluble solvent, the ink application means is a means for ejecting and applying at least a first ink and a second ink onto a substrate, and at least one of the drying means is a means for drying a coating film by irradiating with microwaves, and when the complex dielectric constants of the first ink and the second ink at a drying rate of 95% are ε''1 and ε''2, respectively, ε''1 and ε''2 satisfy the following formula (1): Formula (1): ε''1<ε''2 When the drying rates of the first ink and the second ink when dried for 20 seconds at 80°C are D1 and D2, respectively, D1 and D2 satisfy the following formula (2): Formula (2): D2<D1.
Citation Information
Patent Citations
Ink jet recording picture forming method
JP1982074192A
Ink jet recording picture forming method
JP1982074193A
Ink jet recording paper
JP1982087988A
Ink jet recording paper
JP1982087989A
Ink jet recording method
JP1984042993A