Method for producing catalyst for methacrylic acid production, and method for producing methacrylic acid and methacrylic acid ester using same
The method of producing a catalyst with specific phosphorus, molybdenum, and vanadium ratios, along with an organic carboxylic acid, addresses the selectivity issues in existing catalysts, achieving high methacrylic acid yield and selectivity in the conversion of methacrolein.
Patent Information
- Application Number
- PCT/JP2024/015757
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Current catalysts for producing methacrylic acid from methacrolein have limitations in selectivity, necessitating the development of a more effective method for catalyst production to enhance methacrylic acid yield.
A method involving a slurry with specific liquid phase components, including phosphorus, molybdenum, and vanadium, with controlled molar ratios and vanadium concentration, and the addition of an organic carboxylic acid, is used to produce a catalyst with improved methacrylic acid selectivity, comprising a firing step to create a catalyst with a specific composition.
The method results in a catalyst that produces methacrylic acid with high selectivity and yield, allowing for efficient conversion of methacrolein to methacrylic acid and its subsequent esterification to methacrylic ester.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
METHOD FOR PRODUCING CATALYST FOR PRODUCING METHACRYLIC ACID, AND METHACRYLIC ACID AND METHACRYLIC ACID ESTER USING THE CATALYST
[0001] The present invention relates to a method for producing a catalyst for producing methacrylic acid, and a method for producing methacrylic acid and a methacrylic acid ester using the same.
[0002] Known examples of catalysts for producing methacrylic acid (hereinafter simply referred to as "catalysts") used in producing methacrylic acid by oxidizing methacrolein include heteropolyacid catalysts containing molybdenum and phosphorus. Heteropolyacids are condensed oxygen acids formed by the coordination atoms (hereinafter referred to as "polyatoms") that form the basic skeleton of a polyacid and oxides of the heteroatoms. Examples of heteropolyacid catalysts include proton-type heteropolyacids in which the counter cation is a proton, and heteropolyacid salts in which some of the protons are replaced with cations other than protons (hereinafter, proton-type heteropolyacids will be simply referred to as "heteropolyacids," and at least one selected from proton-type heteropolyacids and heteropolyacid salts will be simply referred to as "heteropolyacids (salts)").
[0003] Regarding the structure of heteropolyacids (salts), Non-Patent Document 1 describes that phosphorus, silicon, arsenic, germanium, titanium, antimony, etc. can be heteroatoms, and tungsten, molybdenum, vanadium, niobium, tantalum, etc. can be polyatoms of heteropolyacids (salts). Furthermore, the basic structures of heteropolyacids (salts) include Keggin type, Dawson type, Preysler type, etc.
[0004] Heteropolyacid catalysts are known as catalysts used in the production of methacrylic acid by oxidizing methacrolein. For example, Patent Document 1 discloses a heteropolyacid catalyst for producing methacrylic acid, which contains molybdenum, vanadium, phosphorus, and an alkali metal. The catalyst comprises a poorly water-soluble component and a water-soluble component, with 60 mol % or more of the total vanadium atoms contained in the catalyst being contained in the water-soluble component. Also disclosed is a method for producing a heteropolyacid catalyst for producing methacrylic acid, comprising the following steps (i) to (v): (i) adding at least a molybdenum source and a phosphorus source to water to prepare an aqueous slurry or solution containing a heteropolyacid (Solution A); and then adding to Solution A an alkali metal compound containing 0.8 to 2.5 alkali metal atoms per phosphorus atom contained in Solution A to prepare an aqueous slurry (Solution B) in which a heteropolyacid salt in which at least a portion of the protons of the heteropolyacid have been substituted with alkali metal ions is precipitated. (ii) a step of preparing an aqueous slurry or solution (liquid C) containing a heteropolyacid by adding to water at least a molybdenum source, a phosphorus source, and a vanadium source containing 1.2 to 2.5 vanadium atoms per phosphorus atom contained in the phosphorus source; (iii) a step of mixing the solutions B and C to prepare an aqueous slurry; (iv) a step of drying the aqueous slurry of the step (iii) to produce a dried product; and (v) a step of heat-treating the dried product of the step (iv).
[0005] JP 2011-255327 A
[0006] Toshio Okuhara, Noritaka Mizuno, Makoto Misono, Advances in Catalysis, volume 41 (1996).
[0007] However, from an industrial viewpoint, a catalyst with a higher selectivity for methacrylic acid is desired. The present invention aims to provide a method for producing a catalyst capable of producing methacrylic acid with high selectivity by oxidation of methacrolein, and a method for producing methacrylic acid using the catalyst.
[0008] The present inventors conducted extensive research in light of the above-mentioned problems, and as a result, found that the above-mentioned problems can be solved by producing a catalyst using a method that uses a slurry having a specific liquid phase component, and thus completed the present invention. That is, the present invention includes the following: [1]: A method for producing a catalyst used in producing methacrylic acid by oxidizing methacrolein, comprising the following steps (i) to (iii): (i) mixing a phosphorus raw material, a molybdenum raw material, and a vanadium raw material with a solvent to prepare slurry A; (ii) drying the slurry A to obtain a dried product; and (iii) calcining the dried product. In the step (i), when the number of moles of molybdenum in the liquid phase of the slurry A is M1 and the number of moles of vanadium in the liquid phase of the slurry A is M2, the ratio M2 / M1 is 7.5 or less. [2]: The method for producing a catalyst for methacrylic acid production according to [1], wherein the M2 / M1 ratio is 1.4 to 3.5 in the step (i). [3]: The method for producing a catalyst for methacrylic acid production according to [1] or [2], wherein the vanadium concentration in the liquid phase of the slurry A in the step (i) is 0.005 to 0.1 mass%. [4]: The method for producing a catalyst for methacrylic acid production according to any of [1] to [3], wherein the vanadium concentration in the liquid phase of the slurry A in the step (i) is 0.01 to 0.08 mass%. [5]: The method for producing a catalyst for methacrylic acid production according to any of [1] to [4], wherein the pH of the slurry A in the step (i) is 1.1 to 2.0. [6]: The method for producing a catalyst for methacrylic acid production according to any of [1] to [5], wherein the slurry A in the step (i) is further prepared by mixing an organic carboxylic acid. [7]: The method for producing a catalyst for methacrylic acid production according to [6], wherein in the step (i), the organic carboxylic acid is mixed in an amount such that a carboxyl group of the organic carboxylic acid is 0.011 to 0.46 moles per mole of molybdenum in the slurry A. [8]: The method for producing a catalyst for methacrylic acid production according to [6] or [7], wherein the organic carboxylic acid contains oxalic acid or oxalic acid dihydrate.[9]: A method for producing a catalyst for use in producing methacrylic acid according to any one of [6] to [8], wherein the step (i) comprises the following steps (i-1) to (i-3): (i-1) a step of mixing a phosphorus raw material, a molybdenum raw material, and a vanadium raw material with a solvent to prepare a solution or slurry A1, (i-2) a step of mixing a raw material of an alkali metal element with the solution or slurry A1 to prepare a slurry A2, and (i-3) a step of mixing an organic carboxylic acid with the slurry A2 to prepare a slurry A.
[10] : A method for producing a catalyst for use in producing methacrylic acid according to any one of [1] to [9], wherein the catalyst has a composition represented by the following formula (I): a Mo b V c Cu d A e E f G g O h (I) In formula (I), P, Mo, V, Cu, and O represent phosphorus, molybdenum, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, silicon, and tungsten. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to h represent the molar ratios of each component, where b = 12, a = 0.5 to 3, c = 0.01 to 3, d = 0.01 to 2, e = 0 to 3, f = 0 to 3, and g = 0.01 to 3, and h represents the molar ratio of oxygen required to satisfy the valence of each component.
[11] : A method for producing methacrylic acid, comprising a step of oxidizing methacrolein to produce methacrylic acid using a catalyst for producing methacrylic acid produced by the method according to any one of [1] to
[10] .
[12] : A method for producing a methacrylic acid ester, comprising esterifying the methacrylic acid produced by the method according to
[11] .
[0009] According to the present invention, a catalyst capable of producing methacrylic acid with high selectivity can be provided.
[0010] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following. In this specification, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits, and "A to B" means A or more and B or less.
[0011] [Catalyst for producing methacrylic acid] The catalyst for producing methacrylic acid produced by the production method according to this embodiment is used when producing methacrylic acid by oxidizing methacrolein. From the viewpoint of improving the yield of methacrylic acid, the catalyst preferably has a composition represented by the following formula (I). Note that the catalyst may contain small amounts of elements not described in the following formula (I). P a Mo b V c Cu d A e E f G g O h(I) In formula (I), P, Mo, V, Cu, and O represent phosphorus, molybdenum, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, silicon, and tungsten. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to h represent the molar ratios of each component, where b = 12, a = 0.5 to 3, c = 0.01 to 3, d = 0.01 to 2, e = 0 to 3, f = 0 to 3, and g = 0.01 to 3, and h represents the molar ratio of oxygen required to satisfy the valence of each component. Preferably, a = 0.6 to 2.5, and more preferably a = 0.7 to 2. Preferably, c = 0.1 to 2.5, more preferably c = 0.15 to 2, and even more preferably c = 0.2 to 1.5. Preferably, d = 0.03 to 2.5, and more preferably d = 0.05 to 2. Preferably, e = 0.01 to 2.5, and more preferably e = 0.1 to 2. Preferably, f = 0 to 2, more preferably f = 0 to 1.5, and even more preferably f = 0 to 1. Preferably, g = 0.1 to 2.8, and more preferably g = 0.3 to 2.5.
[0012] In the formula (I), from the viewpoint of improving the yield of methacrylic acid, the lower limit of a is preferably 0.6 or more, more preferably 0.7 or more. The upper limit of a is preferably 2.5 or less, more preferably 2 or less. The lower limit of c is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more. The upper limit of c is preferably 2.5 or less, more preferably 2 or less, and even more preferably 1.5 or less. The lower limit of d is preferably 0.03 or more, more preferably 0.05 or more. The upper limit of d is preferably 2.5 or less, more preferably 2 or less. The lower limit of e is preferably 0.01 or more, more preferably 0.1 or more. The upper limit of e is preferably 2.5 or less, more preferably 2 or less. The upper limit of f is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1 or less. The lower limit of g is preferably 0.1 or more, more preferably 0.3 or more. The upper limit of g is preferably 2.8 or less, more preferably 2.5 or less.
[0013] The molar ratio of each component is determined by dissolving the catalyst in aqueous ammonia and analyzing the resulting solution by ICP emission spectrometry.
[0014] [Method for producing a catalyst for producing methacrylic acid] The method for producing a catalyst for producing methacrylic acid according to this embodiment is a method for producing a catalyst used in producing methacrylic acid by an oxidation reaction of methacrolein, and includes the following steps: (i) a step of mixing a phosphorus raw material, a molybdenum raw material, and a vanadium raw material with a solvent to prepare a slurry A, (ii) a step of drying the slurry A to obtain a dried product, and (iii) a step of calcining the dried product.
[0015] In the method for producing a catalyst for producing methacrylic acid according to this embodiment, in the step (i), when the number of moles of molybdenum in the liquid phase of the slurry A is M1 and the number of moles of vanadium in the liquid phase of the slurry A is M2, M2 / M1 is 7.5 or less. By using a catalyst produced by such a method, methacrylic acid can be produced with high selectivity.
[0016] Each step will be described in detail below. <Step (i)> In step (i), a phosphorus source, a molybdenum source, and a vanadium source are mixed with a solvent to prepare slurry A. Slurry A may contain raw materials for catalyst components other than the phosphorus source, the molybdenum source, and the vanadium source, and preferably contains a raw material for the element represented by formula (I). Furthermore, in step (i), it is preferable to prepare slurry A by further mixing an organic carboxylic acid. This causes the metal element or ion in slurry A to form a complex with the carboxylate ion, increasing the proportion of solid phase in slurry A. Therefore, by mixing an organic carboxylic acid in step (i), the value of M2 / M1 of slurry A can be easily adjusted.
[0017] The organic carboxylic acid is an organic acid having a carboxyl group, and examples thereof include oxalic acid, oxalic acid dihydrate, acetic acid, citric acid, and formic acid. Among these, it is preferable to use oxalic acid or oxalic acid dihydrate, which have a low carbon content and are stable as a compound. By mixing the organic carboxylic acid in step (i-3), a catalyst with stable performance can be obtained regardless of the preparation scale of slurry A. The organic carboxylic acid is preferably mixed so that the carboxyl group is 0.011 to 0.46 mol, more preferably 0.023 to 0.27 mol, per 1 mol of molybdenum in slurry A.
[0018] Furthermore, step (i) preferably includes the following steps (i-1) to (i-3): (i-1) a step of mixing a phosphorus source, a molybdenum source, and a vanadium source with a solvent to prepare a solution or slurry A1; (i-2) a step of mixing a source of an alkali metal element with the solution or slurry A1 to prepare a slurry A2; and (i-3) a step of mixing an organic carboxylic acid with the slurry A2 to prepare a slurry A.
[0019] <<Step (i-1)>> In step (i-1), a phosphorus source, a molybdenum source, and a vanadium source are mixed with a solvent to prepare a solution or slurry A1. The solution or slurry A1 preferably contains sources of elements other than the G element in formula (I).
[0020] (Raw materials for catalyst components) The raw materials for the catalyst components are not particularly limited, and nitrates, carbonates, acetates, ammonium salts, oxides, halides, oxoacids, oxoacid salts, etc. of each constituent element of the catalyst can be used alone or in combination of two or more.
[0021] Examples of phosphorus raw materials include phosphoric acid, phosphorus pentoxide, ammonium phosphate, etc. Examples of molybdenum raw materials include molybdenum oxides such as molybdenum trioxide, ammonium molybdates such as ammonium paramolybdate and ammonium dimolybdate, and molybdenum chloride.
[0022] When a catalyst containing vanadium and copper is produced, examples of the vanadium raw material include ammonium metavanadate, vanadium pentoxide, vanadium chloride, vanadyl oxalate, etc. Examples of the copper raw material include copper sulfate, copper nitrate, copper oxide, copper carbonate, copper acetate, copper chloride, etc.
[0023] The concentration of the raw materials of the catalyst components in the slurry A1 is not particularly limited, but is preferably in the range of 5 to 90 mass %.
[0024] (Solvent) Examples of the solvent include water, ethyl alcohol, and acetone. These may be used alone or in combination of two or more. Among these, water is preferably used from an industrial viewpoint.
[0025] (Preparation of Solution or Slurry A1) The solution or slurry A1 is preferably prepared by adding raw materials for the catalyst components to a solvent in a preparation vessel and stirring the mixture while heating, thereby producing a sufficient amount of heteropolyacid suitable for the production of methacrylic acid.
[0026] The heating temperature can usually be in the range of 30 to 150°C, but is preferably in the range of 60 to 150°C. By setting the heating temperature to 60°C or higher, the rate of production of the heteropolyacid can be sufficiently increased, and by setting the heating temperature to 150°C or lower, evaporation of the solvent can be suppressed. The lower limit of the heating temperature is more preferably 80°C or higher, and even more preferably 90°C or higher. The upper limit of the heating temperature is more preferably 130°C or lower, and even more preferably 110°C or lower. Depending on the vapor pressure of the solvent used, the heating may involve concentration or reflux, or the heating may be carried out under pressurized conditions by operating in a sealed container.
[0027] The temperature rise rate is not particularly limited, but is preferably 0.8 to 15°C / min. When the temperature rise rate is 0.8°C / min or more, the time required for step (i) can be shortened. Furthermore, when the temperature rise rate is 15°C / min or less, the temperature can be raised using ordinary heating equipment.
[0028] The stirring power was 0.01 kW / m 3 It is preferable to operate at a power of 0.05 kW / m or more. 3 It is more preferable to carry out the stirring at a power of 0.01 kW / m or more. 3 By adjusting the temperature and components of the slurry A to the above level, local variations in temperature are reduced, and a structure suitable for a catalyst for producing an α,β-unsaturated carboxylic acid is stably formed. From the viewpoint of catalyst production costs, the stirring is usually performed at a stirring power of 3.5 kW / m 3 It is preferable to do the following:
[0029] <<Step (i-2)>> In step (i-2), an alkali metal element is mixed with the solution or slurry A1 obtained in step (i-1) to prepare slurry A2. Examples of the alkali metal include lithium, sodium, potassium, rubidium, and cesium, and the alkali metal preferably contains at least one selected from the group consisting of potassium and cesium, and more preferably contains cesium.
[0030] <<Step (i-3)>> In step (i-3), an organic carboxylic acid is mixed with the slurry A2 obtained in step (i-2) to prepare slurry A. The pH of the resulting slurry A is preferably 1.1 to 2.0, more preferably 1.3 to 2.0. This stabilizes the reaction for producing a heteropolyacid suitable for producing an α,β-unsaturated carboxylic acid. Examples of methods for adjusting the pH of slurry A within the above range include using molybdenum trioxide as the molybdenum raw material, or appropriately selecting a raw material compound to adjust the content of nitrate ions and oxalate ions. The pH of slurry A can be measured using a commercially available pH meter.
[0031] (Composition of Liquid and Solid Phases of Slurry A) When the number of moles of molybdenum in the liquid phase of slurry A is M1 and the number of moles of vanadium in the liquid phase of slurry A is M2, M2 / M1 is 7.5 or less. This makes it possible to obtain a catalyst with high methacrylic acid selectivity. The reason for this is thought to be as follows: The heteropolyacid formed in the solid phase of slurry A forms the main active site in the obtained catalyst. Here, when vanadium is present in the solid phase of slurry A so as to achieve the specified M2 / M1, vanadium is suitably distributed in the heteropolyacid formed in the solid phase, forming a chemical structure suitable for the production of methacrylic acid. This is thought to be why a catalyst with high methacrylic acid selectivity is obtained. It is more preferable that the lower limit of M2 / M1 is 1.4 or more and the upper limit is 3.5 or less. Preferred ranges for M2 / M1 include 0 to 7.5, 0.5 to 7.5, 0 to 3.5, 0.5 to 3.5, 1.4 to 7.5, and 1.4 to 3.5. Examples of methods for adjusting M2 / M1 include a method of changing the amount of the organic carboxylic acid used. Increasing the amount of the organic carboxylic acid used tends to decrease M2 / M1.
[0032] From the viewpoint of methacrylic acid selectivity, the vanadium concentration in the liquid phase of slurry A is preferably 0.005 to 0.1 mass %. The vanadium concentration in the liquid phase of slurry A is more preferably 0.01 to 0.08 mass %. Examples of methods for adjusting the vanadium concentration in the liquid phase of slurry A include a method of changing the amount of the organic carboxylic acid used and a method of changing the pH of slurry A. Increasing the amount of the organic carboxylic acid used or lowering the pH of slurry A tends to decrease the vanadium concentration in the liquid phase of slurry A.
[0033] The number of moles and molar concentration of each element in the liquid phase of Slurry A are values determined by elemental analysis of the liquid phase of Slurry A by ICP atomic emission spectrometry. The number of moles of each element in the solid phase of Slurry A is a value obtained by subtracting the number of moles of each element in the liquid phase determined by ICP atomic emission spectrometry from the amount of each raw material charged.
[0034] <Step (ii)> In step (ii), the slurry A obtained in step (i) is dried to obtain a dried product. There are no particular limitations on the method for drying the slurry A, and examples thereof include a method of drying using a box dryer, a method of drying using a spray dryer, a method of drying using a slurry dryer, a method of drying using a drum dryer, and a method of pulverizing the massive solid obtained by evaporation to dryness. There are no particular limitations on the drying conditions, and when using a box dryer, for example, it is preferable to dry at a temperature of 30 to 150°C. Furthermore, when using a spray dryer, it is preferable to set the inlet temperature to 100 to 500°C and the outlet temperature to 100 to 300°C.
[0035] The drying is preferably carried out so that the moisture content of the resulting dried product is 4.5% by mass or less, more preferably 0.1 to 4.5% by mass. The dried product obtained in step (ii) may be shaped as described below, if necessary.
[0036] <Shaping Step> In the shaping step, the dried product obtained in the step (ii) is shaped as needed. Note that shaping may be performed after the step (iii) described below.
[0037] The molding method is not particularly limited, and known dry and wet molding methods can be applied, such as tablet molding, press molding, extrusion molding, and granulation molding. The shape of the molded product is not particularly limited, and examples include cylindrical, ring-shaped, spherical, and other shapes. Furthermore, during molding, it is preferable to mold only the dried product without adding a carrier or the like to the dried product, but known additives such as graphite and talc may be added as necessary. When a carrier is used, the carrier is not particularly limited, but silica is preferred.
[0038] <Step (iii)> In the firing step, the dried product obtained in the step (ii) or the dried product after shaping obtained in the shaping step is fired to obtain a fired product.
[0039] The calcination can be carried out under a flow of at least one of an oxygen-containing gas such as air and an inert gas, and is preferably carried out under a flow of an oxygen-containing gas such as air. Here, the inert gas refers to a gas that does not reduce the catalytic activity, and examples thereof include nitrogen, carbon dioxide, helium, and argon. These gases may be used alone or in combination of two or more.
[0040] The shape of the firing vessel is not particularly limited, but a box-shaped, tubular, or other vessel can be used. Furthermore, the material can be divided and filled into multiple vessels for firing. Among these, a vessel with a cross-sectional area of 1 to 100 cm is particularly suitable. 2 It is preferable to use a tubular container in which
[0041] The firing temperature (maximum temperature during firing) is preferably 200 to 700°C, more preferably 320 to 450°C.
[0042] The calcined product obtained as described above can be used as a catalyst for producing methacrylic acid. The calcined product may also be molded as described in the molding step. In this embodiment, the calcined product and the calcined product after molding are collectively referred to as catalysts.
[0043] [Method for producing methacrylic acid] In the method for producing methacrylic acid according to the present embodiment, methacrolein is oxidized using the catalyst for producing methacrylic acid produced by the production method according to the present embodiment. According to these methods, methacrylic acid can be produced in a high yield.
[0044] The method for producing methacrylic acid according to this embodiment can be carried out by contacting a catalyst for producing methacrylic acid produced by the production method according to this embodiment with a raw material gas containing methacrolein. A fixed-bed reactor can be used for this reaction. The reaction can be carried out by filling the reactor with a catalyst and supplying the raw material gas to the reactor. The catalyst layer may be a single layer, or multiple catalysts with different activities may be packed in multiple layers. In addition, the catalyst may be diluted with an inert carrier and packed to control the activity.
[0045] The methacrolein concentration in the raw material gas is preferably 1 to 20% by volume, more preferably 3 to 10% by volume. The raw material methacrolein may contain small amounts of impurities such as lower saturated aldehydes that do not substantially affect the reaction.
[0046] The oxygen source for the raw material gas is not particularly limited, but it is industrially advantageous to use air. If necessary, a gas obtained by mixing pure oxygen with air or the like can also be used. The ratio of oxygen in the raw material gas is not particularly limited, but is preferably 0.4 to 4 moles, more preferably 0.5 to 3 moles, per mole of methacrolein.
[0047] From an economical viewpoint, the raw material gas may be diluted with an inert gas such as nitrogen or carbon dioxide. Furthermore, water vapor may be added to the raw material gas. By carrying out the reaction in the presence of water vapor, methacrylic acid can be obtained in a higher yield. The concentration of water vapor in the raw material gas is preferably 0.1 to 50% by volume, more preferably 1 to 40% by volume.
[0048] The contact time between the raw material gas and the catalyst for producing methacrylic acid is preferably 1.5 to 15 seconds, more preferably 2 to 10 seconds. The reaction pressure is preferably 0.1 to 1 MPa (G), where (G) means gauge pressure. The reaction temperature is preferably 200 to 450°C, more preferably 250 to 400°C.
[0049] In the production of methacrylic acid, the position of the catalyst in the reactor, the proportion of the catalyst in the reactor, etc. are not particularly limited, and a commonly used form can be applied.
[0050] [Method for producing methacrylic acid ester] In the method for producing a methacrylic acid ester according to the present embodiment, the methacrylic acid produced by the method for producing the methacrylic acid according to the present embodiment is esterified. That is, the method for producing a methacrylic acid ester according to the present embodiment includes a step of producing methacrylic acid by the method for producing the methacrylic acid according to the present embodiment and a step of esterifying the methacrylic acid.
[0051] The alcohol to be reacted with methacrylic acid is not particularly limited, and examples thereof include methanol, ethanol, n-propanol, isopropanol, n-butanol, and isobutanol. Examples of the methacrylic acid ester obtained include methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, and isobutyl methacrylate. The esterification reaction can be carried out in the presence of an acidic catalyst such as a sulfonic acid-type cation exchange resin. The temperature during the esterification reaction is preferably 50 to 200°C.
[0052] The pressure during the esterification reaction, the position of the catalyst in the reactor, the proportion of the catalyst in the reactor, etc. are not particularly limited, and any commonly used form can be applied.
[0053] Hereinafter, examples of producing the catalyst according to this embodiment and examples of reactions using the catalyst will be described together with comparative examples. In the following examples and comparative examples, "parts" means parts by mass.
[0054] (Collection of Liquid and Solid Phases in Slurry A) 30 g of the slurry was collected in a centrifuge tube and centrifuged using a centrifuge (high-speed refrigerated centrifuge CR22N (manufactured by Hitachi Koki)). The supernatant was filtered through a 0.45 μm PTFE filter to obtain a filtrate (liquid phase). The precipitate, together with the centrifuge tube, was vacuum dried overnight at 60°C to obtain a dry powder (solid phase). (Analysis of Liquid and Solid Phases of Slurry A) The liquid phase of Slurry A was subjected to elemental analysis using ICP atomic emission spectrometry to calculate the concentrations (mass%) of molybdenum and vanadium in the liquid phase of Slurry A. The M2 / M1 ratio was calculated from the obtained molybdenum and vanadium concentrations (mass%) and atomic weights. Note that the deficiency in the total concentration of all metal elements in the liquid phase of Slurry A obtained by elemental analysis relative to 100% was assumed to be water.
[0055] (Composition Ratio of Catalyst) The molar ratio of each component was determined by dissolving the catalyst in aqueous ammonia and then subjecting the resulting solution to elemental analysis by ICP emission spectrometry.
[0056] (Analysis of Feed Gas and Products) The feed gas and products were analyzed using the following gas chromatography: GC-2014 manufactured by Shimadzu Corporation (column: DB-FFAP manufactured by J&W, 30 m×0.32 mm, film thickness 1.0 μm) GC-8A manufactured by Shimadzu Corporation (column: molecular sieve, 2.0 M×3.0 mm ID) GC-8A manufactured by Shimadzu Corporation (column: Porapak Q, 2.0 M×3.0 mm ID) The conversion rate of methacrolein and the selectivity of the produced methacrylic acid were calculated using the following formulas: Methacrolein conversion rate (%) = (N2 / N1) × 100 Methacrylic acid selectivity (%) = (N3 / N2) × 100 Here, N1 is the number of moles of methacrolein supplied, N2 is the number of moles of methacrolein reacted, and N3 is the number of moles of methacrylic acid produced.
[0057] (pH of Slurry A) The pH of Slurry A was measured using a portable pH meter LAQUAact D-71 manufactured by HORIBA.
[0058] Example 1: 1,200 parts of room-temperature pure water were mixed with a dilution of 300 parts of molybdenum trioxide, 10.2 parts of ammonium metavanadate, and 30.0 parts of an 85% by weight aqueous phosphoric acid solution diluted with 36 parts of pure water, and a solution of 6.3 parts of copper (II) nitrate trihydrate dissolved in 9.0 parts of pure water. Next, 13.5 parts of oxalic acid dihydrate were added so that the carboxyl group concentration per mole of molybdenum was 0.10 moles. The resulting slurry was heated to 95°C at a rate of 2°C / min and stirred for 2 hours to obtain Slurry A1. The resulting Slurry A1 was mixed with a solution of 40.4 parts of cesium bicarbonate dissolved in 60 parts of room-temperature pure water and stirred at 95°C for 15 minutes. Next, a solution of 27.5 parts of ammonium carbonate dissolved in 78 parts of pure water was mixed with the mixture and stirred at 95°C for 15 minutes to obtain Slurry A. The pH of Slurry A was 1.65. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The obtained slurry A was evaporated to dryness, and the resulting lumpy solid was pulverized to obtain a dried product. The obtained dried product was calcined at 380°C for 5 hours in an air stream to obtain a catalyst. The composition of the catalyst excluding oxygen was P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 The catalyst obtained was diluted to a weight ratio of catalyst to silicon carbide of 4:5 and packed into a fixed-bed reactor. A feed gas consisting of 5% by volume of methacrolein, 10% by volume of oxygen, 30% by volume of steam, and 55% by volume of nitrogen was passed through the reactor for a contact time of 178 h g / mol, and an oxidation reaction of methacrolein was carried out at a reaction temperature of 300°C. The amount of catalyst packed was adjusted so that the conversion rate of methacrolein in the oxidation reaction was 70%. The results of the methacrylic acid selectivity are shown in Table 1.
[0059] Example 2 A catalyst was obtained in the same manner as in Example 1, except that 21.0 parts of oxalic acid dihydrate was used. The pH of Slurry A was 1.43. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained Slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0060] Example 3 A catalyst was obtained in the same manner as in Example 1, except that 30.0 parts of oxalic acid dihydrate was used. The pH of Slurry A was 1.25. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained Slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0061] Example 4: 1,200 parts of room-temperature pure water were mixed with 36 parts of pure water containing 300 parts of molybdenum trioxide, 10.2 parts of ammonium metavanadate, and 30.0 parts of an 85% by weight aqueous phosphoric acid solution, and a solution containing 6.3 parts of copper (II) nitrate trihydrate in 9.0 parts of pure water. The resulting slurry was heated to 95°C at a rate of 2°C / min and stirred for 2 hours to obtain Slurry A1. A solution containing 40.4 parts of cesium bicarbonate in 60 parts of room-temperature pure water was then mixed with the resulting slurry A1 and stirred for 15 minutes at 95°C. A solution containing 27.5 parts of ammonium carbonate in 78 parts of pure water was then mixed with the resulting slurry A2 and stirred for 15 minutes at 95°C to obtain Slurry A2. 6.0 parts of oxalic acid dihydrate was added to the resulting slurry A2 so that the carboxyl group ratio was 0.05 moles per mole of molybdenum, and the resulting mixture was stirred for 15 minutes to obtain Slurry A. The pH of the slurry A was 1.71. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The obtained slurry A was dried and calcined in the same manner as in Example 1 to obtain a catalyst. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0062] Example 5 A catalyst was obtained in the same manner as in Example 4, except that 3.4 parts of oxalic acid dihydrate was used. The pH of Slurry A was 1.56. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained Slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0063] Example 6 A catalyst was obtained in the same manner as in Example 4, except that 13.5 parts of oxalic acid dihydrate was used. The pH of Slurry A was 1.53. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained Slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0064] Example 7 A catalyst was obtained in the same manner as in Example 4, except that the oxalic acid dihydrate was changed to 21.0. The pH of the slurry A was 1.47. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0065] Example 8 A catalyst was obtained in the same manner as in Example 1, except that 11.2 parts of ammonium metavanadate was used. The pH of the slurry A was 1.47. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.55 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0066] Example 9 A catalyst was obtained in the same manner as in Example 1, except that 12.2 parts of ammonium metavanadate was used. The pH of the slurry A was 1.49. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.6 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0067] Example 10 A catalyst was obtained in the same manner as in Example 1, except that 24.8 parts of ammonium carbonate was used. The pH of Slurry A was 1.30. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained Slurry A and the amount of water charged. The results are shown in Table 1. The composition of the catalyst excluding oxygen was: P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0068] Comparative Example 1 Slurry A1 was obtained in the same manner as in Example 4. A solution of 40.4 parts of cesium bicarbonate dissolved in 60 parts of pure water at room temperature was mixed with the obtained slurry, and the mixture was stirred at 95°C for 15 minutes. Next, a solution of 36.3 parts of ammonium carbonate dissolved in 78 parts of pure water was mixed with the mixture, and the mixture was stirred at 95°C for 15 minutes to obtain slurry A. The pH of slurry A was 2.43. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The obtained slurry A was dried and calcined in the same manner as in Example 1 to obtain a catalyst. The composition of the catalyst excluding oxygen was P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0069] Comparative Example 2 Slurry A1 was obtained in the same manner as in Example 4. A solution of 40.4 parts of cesium bicarbonate dissolved in 60 parts of pure water at room temperature was mixed with the obtained slurry, and the mixture was stirred at 95°C for 15 minutes. Next, a solution of 40.7 parts of ammonium carbonate dissolved in 78 parts of pure water was mixed with the mixture, and the mixture was stirred at 95°C for 15 minutes to obtain slurry A. The pH of slurry A was 2.91. The vanadium concentration and M2 / M1 were calculated from the elemental analysis results of the obtained slurry A and the amount of water charged. The results are shown in Table 1. The obtained slurry A was dried and calcined in the same manner as in Example 1 to obtain a catalyst. The composition of the catalyst excluding oxygen was P 1.5 Mo 12 V 0.5 Cu 0.15 Cs 1.2 Using the obtained catalyst, an oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The results of the methacrylic acid selectivity are shown in Table 1.
[0070]
[0071] As shown in Table 1, in Examples 1 to 10, in which the catalyst was produced using Slurry A in which the molar ratio of molybdenum and vanadium in the liquid phase was within a specific range, methacrylic acid was produced with high selectivity. Note that methacrylic acid esters can be obtained by esterifying the methacrylic acid obtained in these examples.
[0072] According to the present invention, it is possible to provide a method for producing a catalyst capable of producing methacrylic acid with high selectivity by oxidizing methacrolein, and a method for producing methacrylic acid using the catalyst.
Claims
1. A method for producing a catalyst used in producing methacrylic acid by oxidation of methacrolein, comprising the following steps (i) to (iii): (i) mixing a phosphorus raw material, a molybdenum raw material and a vanadium raw material with a solvent to prepare slurry A; (ii) drying the slurry A to obtain a dried product; and (iii) firing the dried product. In the step (i), when the number of moles of molybdenum in the liquid phase of the slurry A is M1 and the number of moles of vanadium in the liquid phase of the slurry A is M2, M2 / M1 is 7.5 or less.
2. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein in the step (i), the M2 / M1 is 1.4 to 3.
5.
3. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein in the step (i), the vanadium concentration in the liquid phase of the slurry A is 0.005 to 0.1 mass%.
4. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein in the step (i), the vanadium concentration in the liquid phase of the slurry A is 0.01 to 0.08 mass%.
5. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein in the step (i), the pH of the slurry A is 1.1 to 2.
0.
6. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein in the step (i), an organic carboxylic acid is further mixed to prepare slurry A.
7. The method for producing a catalyst for producing methacrylic acid according to claim 6, wherein in the step (i), the organic carboxylic acid is mixed in an amount such that the amount of carboxyl group of the organic carboxylic acid is 0.011 to 0.46 moles per mole of molybdenum in the slurry A.
8. The method for producing a catalyst for producing methacrylic acid according to claim 6, wherein the organic carboxylic acid includes oxalic acid or oxalic acid dihydrate.
9. A method for producing a catalyst for producing methacrylic acid according to claim 6, wherein the step (i) comprises the following steps (i-1) to (i-3): (i-1) a step of mixing a phosphorus raw material, a molybdenum raw material and a vanadium raw material with a solvent to prepare a solution or slurry A1; (i-2) a step of mixing a raw material of an alkali metal element with the solution or slurry A1 to prepare a slurry A2; and (i-3) a step of mixing an organic carboxylic acid with the slurry A2 to prepare a slurry A.
10. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein the catalyst has a composition represented by the following formula (I): a M.O. b V c Cu d A e E f G g O h (I) In formula (I), P, Mo, V, Cu, and O represent phosphorus, molybdenum, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, silicon, and tungsten. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to h represent the molar ratio of each component, where b = 12, a = 0.5 to 3, c = 0.01 to 3, d = 0.01 to 2, e = 0 to 3, f = 0 to 3, and g = 0.01 to 3, and h represents the molar ratio of oxygen required to satisfy the valence of each of the components.
11. A method for producing methacrylic acid, comprising a step of oxidizing methacrolein to produce methacrylic acid using a catalyst for producing methacrylic acid produced by the method according to any one of claims 1 to 10.
12. A method for producing a methacrylic acid ester, comprising the step of esterifying the methacrylic acid produced by the method according to claim 11.
Citation Information
Patent Citations
JP1975096522A
Production of methacrolein oxication catalyst
JP1978109889A
Prepaeation of methacrylic acid
JP1979022319A
Preparation of unsaturated carboxylic acid
JP1979106419A
Production of catalyst for producing acrylic acid
JP2000317309A